Trimming and punching method and trimming and punching die for thermal forming part

After hot stamping and quenching in the hot stamping mold, the workpiece is moved to the edge cutting punching mold for local heating and liquid cooling control, which solves the problem of cutting punching in the traditional technology that is difficult to process high-strength steel plates, achieving more efficient cutting edges and punching effects.

CN119056953AActive Publication Date: 2024-12-03SAIC GM WULING AUTOMOBILE CO LTD

Patent Information

Application Number
CN202411389562.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

Traditional edge cutting punching technology is difficult to meet the processing requirements of hot stamping parts, especially when the material has high strength and high hardness, resulting in low processing accuracy and efficiency.

Method used

After hot stamping, first quenching and insulation in the hot stamping mold, move the workpiece to the edge cutting punching mold for local heating, reduce the tensile strength of the edge cutting and punching positions, and control the cooling through liquid cooling Liquid flow, achieve rapid edge cutting and punching.

Benefits of technology

Improves the efficiency of cutting edges and punching, and improves 50% to 70%, ensuring processing quality and efficiency, while preventing deformation or cracks caused by uneven cooling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056953A_ABST
    Figure CN119056953A_ABST
Patent Text Reader

Abstract

The trimming and punching method comprises the following steps that S1, in a hot stamping die, a workpiece is subjected to hot stamping, primary quenching and heat preservation; s2, when the temperature is reduced to the preset temperature, the workpiece is taken out and moved into a trimming and punching die; s3, determining the position to be trimmed and the position to be punched, and heating the position to be trimmed and the position to be punched; s4, after a set condition is met, trimming and punching are conducted on the workpiece; and S5, the workpiece is quenched for the second time. The hot stamping part can be rapidly punched and trimmed, meanwhile, the cooling speed of the workpiece in the machining process is accurately controlled, the temperature of all positions of the workpiece can be cooled in a controllable mode, deformation or cracks can be prevented, and the performance of key positions of the workpiece is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mechanical processing and manufacturing, and in particular to a method for trimming and punching a hot-formed part and a trimming and punching die. Background Art

[0002] As the automotive industry's requirements for vehicle performance, safety and lightweight are increasing, high-strength steel plates have become one of the important ways to meet these requirements due to their light weight and high strength. However, high-strength steel plates have a small plastic deformation range at room temperature and poor formability, which poses a challenge to traditional cold stamping methods. Hot stamping technology makes the steel plate material soft and easy to form in a heated state by stamping the steel plate at high temperature. This technology can not only solve the problem of high-strength steel plates being difficult to form at room temperature, but also improve the dimensional accuracy and mechanical properties of parts. With the widespread application of hot stamping technology, the trimming and punching technology of hot-formed parts has gradually become an important link in the manufacture of automotive stamping parts. Due to the high strength and hardness of the material of hot stamping parts, traditional trimming and punching methods are difficult to meet the processing requirements. Therefore, advanced trimming and punching technologies, such as laser cutting and water cutting, are needed to ensure the processing accuracy and surface quality of hot-formed parts. Although the current laser cutting technology has significant advantages over traditional cutting technology, such as fast cutting speed, high precision, and strong material adaptability, it also has some problems:

[0003] The technical threshold is high, laser cutting technology requires professional technicians to operate and maintain, and the cost is higher. The trimming time is long, and it takes longer to cut parts using laser cutting technology.

[0004] How to quickly punch and trim hot stamping parts is one of the important issues that need to be solved urgently in this field. Summary of the invention

[0005] The purpose of the present invention is to provide a method for trimming and punching of hot-formed parts and a trimming and punching die, which can quickly punch and trim the hot-stamped parts.

[0006] The present invention provides a method for trimming and punching a thermoformed part, which comprises the following steps:

[0007] S1, in the hot stamping die, the workpiece is hot stamped, first quenched and kept warm;

[0008] S2, when the temperature cools to the preset temperature, the workpiece is taken out and moved to the trimming and punching die;

[0009] S3, determining the positions to be trimmed and punched, and heating the positions to be trimmed and punched;

[0010] S4, when the set condition is met, trimming and punching the workpiece; wherein the set condition is that the temperature of the area within the set distance from the incision corresponding to the position to be trimmed and punched on the workpiece is within the set temperature range;

[0011] S5, quenching the workpiece for the second time.

[0012] The method for trimming and punching a hot-formed part as described above, wherein, optionally, during the first quenching or the second quenching process, the workpiece is liquid-cooled; the liquid cooling uses a plurality of cooling channels;

[0013] Methods for liquid cooling of workpieces include:

[0014] S01, determining the cooling time and the initial coolant flow rate at the entrance of each cooling channel according to the heat dissipation requirements of the key points pre-selected on the workpiece and the initial coolant temperature;

[0015] S02, according to the cooling time, determine the time variation relationship of the target flow rate at the entrance of each cooling channel and the target temperature of each key point at different times during the cooling time, and monitor the actual temperature of each key point;

[0016] S03, controlling the flow rate at the inlet of each cooling channel according to the relationship between the target flow rate at the inlet of each cooling channel and time;

[0017] S04, during the cooling process, the actual temperature of each key point at the current moment is compared with the target temperature, and the relationship between the target flow rate at the entrance of each cooling channel and time is corrected according to the comparison result;

[0018] S05, controlling the coolant flow at the inlet of each cooling channel according to the modified relationship between the target flow at the inlet of each cooling channel and time; repeating steps S04 and S05 until the cooling time ends.

[0019] In the method for trimming and punching a hot-formed part as described above, optionally, in step S02, the step of determining the relationship between the target flow rate at the entrance of each cooling channel and time includes:

[0020] S021, determining the cooling capacity of each cooling channel for each key point;

[0021] S022, respectively determining the ratio of the degree of influence of each key point on each cooling channel;

[0022] S023, determine the cooling intensity requirements of each key point;

[0023] S024, determining the relationship between the total target flow rate at the entrance of each cooling channel and time according to the cooling intensity requirements of each key point, the cooling capacity of each cooling channel to each key point, and the ratio of the degree of influence of each key point on each cooling channel;

[0024] S025, allocating the target flow rate at the entrance of each cooling channel according to the ratio between the cooling intensity requirement of each key point and the target flow rate at the entrance of each cooling channel.

[0025] The method for trimming and punching a hot-formed part as described above, wherein, optionally, in step S021, the relationship between the target flow rate at the entrance of each cooling channel and time is determined by the cooling capacity of each cooling channel for each key point;

[0026] The cooling capacity of each cooling channel to each key point is determined by the following formula:

[0027]

[0028] Among them, sa is the cooling capacity, a1 is the constant coefficient, c is the specific heat capacity of the coolant, S is the cross-sectional area of ​​the cooling channel, v is the flow rate of the coolant, T m is the temperature of the coolant channel wall, T s is the temperature of the coolant; t1 is the time for the coolant to flow from the inlet of the cooling channel to the first end point of the cooling section; t2 is the time for the coolant to flow from the inlet to the second end point of the cooling section; l(t) is the distance between the position of the coolant at a certain point starting from the inlet and the corresponding key point at time t.

[0029] In the method for trimming and punching hot-formed parts as described above, optionally, the cooling section is selected by making a sphere with the key point as the center and a preset distance as the radius, and the portion of the cooling channel located within the spherical surface is the cooling section.

[0030] In the method for trimming and punching a hot-formed part as described above, optionally, the formula for correcting the relationship between the target flow rate at the entrance of each cooling channel and the time change according to the comparison result is:

[0031] q(t)=Sv=Q(t)+bΔq;

[0032] Among them, q(t) is the change relationship between the target flow rate at the inlet of the cooling channel and time after correction, Q(t) is the change relationship between the target flow rate at the inlet of the cooling channel and time before correction, b is the adjustment factor, and Δq is the unit adjustment amount;

[0033] The calculation formula of the adjustment factor is:

[0034]

[0035] a2 is a constant coefficient, T sj is the actual temperature of the corresponding key point, T mb is the target temperature of the corresponding key point.

[0036] In the method for trimming and punching hot-formed parts as described above, optionally, a middle portion of at least one of the cooling channels has a plurality of branches.

[0037] In the method for trimming and punching a thermoformed part as described above, optionally, step S1 includes the following steps:

[0038] S11, placing the blank into a hot stamping die and heating the blank;

[0039] S12, punching the blank to form a workpiece;

[0040] S13, perform the first quenching and keep the temperature for a set time;

[0041] The heating processes in step S11 and step S3 are both controlled by PID.

[0042] The present invention also provides a trimming and punching die for use in any of the above methods, which includes a first die, a second die and a third die;

[0043] The first die and the second die are used to press on the workpiece to be trimmed and punched from both sides;

[0044] The first die is provided with a plurality of first holes, a punching portion is provided on a side of the first die close to the workpiece, and the first holes penetrate the punching portion; a first heating element is embedded in the punching portion; the first heating element is used to heat the temperature of the area to be punched to a set temperature range before punching;

[0045] The second mold is provided with a plurality of second holes corresponding to the first holes;

[0046] The side wall of the first mold is provided with a trimming area, and at least one second heating element is provided in the trimming area;

[0047] The third mold and the first mold are located on the same side of the workpiece, and the third mold is distributed along the circumference of the first mold. The third mold is provided with a second heating element for heating the trimming position;

[0048] The first mold is provided with a cooling channel for liquid cooling for executing steps S01 to S05.

[0049] As described above, the trimming and punching die, wherein, optionally, a groove is provided in the trimming area, and the second heating element is arranged in the groove; the second heating element is used to heat the trimming area of ​​the workpiece; and a gap is provided between the peripheral side of the second heating element and the wall of the groove.

[0050] Compared with the prior art, the present invention moves the formed workpiece to the trimming and punching die after hot stamping, first quenching and heat preservation of the workpiece in the hot stamping die. When the workpiece is heated in the trimming and punching die, and the corresponding area of ​​the workpiece is heated to within the set temperature range, the tensile strength of the corresponding position of the workpiece is reduced to below 600MPa, so as to facilitate trimming and punching operations. By locally heating the workpiece, it is helpful to reduce the tensile strength of the position to be trimmed and punched, and to achieve rapid punching and trimming to ensure processing quality and efficiency. Since local heating can reduce the tensile strength of the position to be trimmed and punched, it has been verified that the efficiency of trimming and punching can be improved by about 50% to 70%.

[0051] In addition, during the cooling process through liquid cooling, the coolant flow rate at the inlet of each cooling channel is controlled based on the cooling of key points, so that the entire workpiece can be cooled proportionally in a controllable manner, thereby preventing the workpiece from deformation or cracking due to uneven changes in the internal structure during the cooling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 is a flow chart of the steps of the method for trimming and punching of a thermoformed part proposed by the present invention;

[0053] Figure 2 is a flow chart of the steps of the method for liquid cooling a workpiece proposed by the present invention;

[0054] Figure 3 is a specific step flow chart of step S02 proposed by the present invention;

[0055] Figure 4 is a specific step flow chart of step S1 proposed by the present invention;

[0056] Figure 5 It is a three-dimensional diagram of the trimming and punching die proposed by the present invention;

[0057] Figure 6 yes Figure 5 Disassembly diagram of

[0058] Figure 7 It is a schematic diagram of the structure of a workpiece before trimming and punching proposed by the present invention;

[0059] Figure 8 It is a schematic diagram of the structure of a workpiece after trimming and punching proposed by the present invention;

[0060] Fig. 9 It is a three-dimensional diagram of the first mold proposed by the present invention.

[0061] Description of reference numerals:

[0062] 1-first mold, 2-second mold, 3-third mold;

[0063] 11-first hole, 12-punching portion, 13-trimming area, 14-groove, 15-first heating element;

[0064] 21 - second hole, 22 - second heating element. DETAILED DESCRIPTION

[0065] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, but should not be construed as limiting the present invention.

[0066] Example 1

[0067] In view of the problems in the background technology, since the material strength of hot stamping parts is high, it is not convenient to trim and punch holes. The present invention proposes a method for trimming and punching holes of hot stamping parts. Please refer to Figures 1 to 4 , which includes the following steps,

[0068] S1, in a hot stamping die, hot stamping, first quenching and heat preservation are performed on the workpiece. Through this step, hot stamping forming of the workpiece is achieved.

[0069] For details, please refer to Figure 2 , this step includes the following steps,

[0070] S11, placing the blank into a hot stamping die and heating the blank.

[0071] In the specific implementation, the blank is placed in a hot stamping die for hot stamping. The hot stamping die is preheated to an appropriate molding temperature using a high-temperature heating unit. The specific value of the molding temperature can be obtained based on an empirical value or an experimental value or by looking up a table. The temperature sensor and the heating / cooling pipeline control system cooperate with each other to collect the temperature data of the mold fed back by the temperature sensor in real time, and automatically adjust as needed to ensure the consistency of the hot stamping workpiece. In the specific implementation, the hot stamping die is embedded with a high-temperature heating unit, a cooling channel, and a temperature sensor. In this step, the heating of the blank can be controlled by PID, and error accumulation can be prevented by limiting the integral term or using integral anti-saturation technology.

[0072] S12, punching the blank to form a workpiece. In the specific implementation, the punching speed and time of the punching machine are accurately controlled by using a high-performance servo motor and a control system to ensure that the parts are subjected to uniform force and pressure during the forming process. The blank is formed by the punching in this step.

[0073] S13, perform the first quenching and keep warm for a set time.

[0074] The quenching process can change the internal structure of the workpiece, thereby improving the strength of the workpiece. In practical applications, the first quenching process and heat preservation are carried out in the hot stamping die, which can ensure that the workpiece will not be deformed during the quenching process. In specific implementation, through this step, the blank can be formed by hot stamping.

[0075] S2, when the temperature cools to the preset temperature, the workpiece is taken out and moved to the trimming and punching die; in the specific implementation, the preset temperature is 360°C to 400°C, wherein the optional temperature values ​​are 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C, 400°C, etc., wherein 380°C is preferred. Since punching and trimming are performed after hot stamping, the workpiece does not need to be completely cooled to room temperature during this process. Therefore, it is possible to avoid increasing the workpiece from room temperature to the set temperature range in the subsequent steps, which is beneficial to saving energy.

[0076] S3, determine the position of the edge to be trimmed and the position of the hole to be punched, and heat the position of the edge to be trimmed and the position of the hole to be punched. In specific implementation, the edge trimming position and the hole punching position can be heated in a targeted manner by a heating component pre-set in the edge trimming and hole punching die. Since the first quenching of hot stamping has been completed, the strength of the workpiece has reached the required level. The purpose of this step is to reduce the strength of the edge trimming and the position to be punched by heating.

[0077] S4, when the set conditions are reached, the workpiece is trimmed and punched; wherein the set conditions are that the temperature of the area within the set distance from the corresponding incision is within the set temperature range; in the specific implementation, the set temperature range is 550°C to 600°C, specifically, the temperature in the area should be between 550°C and 600°C, that is, in the area, the highest temperature and the lowest temperature are both set at 550°C to 600°C. When the workpiece is within this temperature range, its tensile strength is reduced to below 600MPa, which is convenient for trimming and punching operations. In the specific implementation, after the corresponding area of ​​the workpiece reaches the set temperature range, the trimming and punching process is started. Use precise trimming and punching dies and control systems to ensure the accuracy and consistency of trimming and punching. During the entire process, keep the parts within the set temperature range to ensure processing quality and efficiency. In the specific implementation, the set distance can be 2-5 cm to ensure that the tensile strength of the workpiece is lower than 600MPa in the area corresponding to the incision position. Since local heating can reduce the tensile strength of the positions to be trimmed and punched, it has been verified in practice that the efficiency of trimming and punching can be increased by about 50% to 70%.

[0078] S5, quench the workpiece for the second time. The second quenching process is carried out in the trimming and punching die. By carrying out the second quenching in the trimming and punching die, the workpiece can be prevented from being deformed during the second quenching process. Since the second quenching is carried out in the trimming and punching die, that is, a cooling channel is provided in the trimming and punching die. After this step, the workpiece is cooled to room temperature. In practical applications, before trimming and punching, the heating position is local heating. For workpieces of specific shapes, the punching position and trimming position are fixed. Therefore, corresponding cooling channels can be directly provided at corresponding positions according to different heating areas.

[0079] In specific implementation, trimming and punching are performed through the above steps S1 to S5, and the first quenching and the second quenching need to be performed in the hot stamping die and the trimming and punching die respectively. During the first quenching and the second quenching process, since the temperature drop rate of each part of the workpiece is difficult to accurately control, when the temperature drop rate is uneven, it is easy to cause uneven changes in the internal structure of the workpiece, thereby causing deformation and cracks in the workpiece. In order to solve this problem, in this implementation, the workpiece is liquid-cooled during the first quenching and the second quenching process; the liquid cooling uses multiple cooling channels. Taking the first quenching as an example, please refer to Figure 3 , methods for liquid cooling of workpieces include:

[0080] S01, according to the heat dissipation requirements and initial coolant temperature of the key points predetermined on the workpiece, determine the cooling time and the initial coolant flow rate at the entrance of each cooling channel. In the specific implementation, the key points are first selected according to factors such as the shape of the workpiece, the heat dissipation requirements and the design strength. The key point can be the geometric center point or characteristic point of the key heat dissipation area. In the specific implementation, the key heat dissipation area is one or more areas on the workpiece that are difficult to dissipate heat after the hot stamping die is stamped and formed. For example, in the mold closing state, the area close to the center of the entire hot stamping die, the area with a larger thickness of the hot stamping die, and the area with a relatively concentrated mass on the workpiece. One or more key points are selected in each area where heat dissipation is difficult to dissipate, and together constitute a set of key points, such as n key points are respectively recorded as K1, K2, K3, K4, K5, K6...Kn.

[0081] In specific implementation, the initial coolant temperature refers to the coolant temperature when it enters the cooling channel entrance. When in use, tap water or the like can be used directly for cooling. It is only necessary to ensure the coolant temperature when it enters the cooling channel. During the entire cooling process, the coolant is not circulated. Therefore, it is only necessary to ensure that the coolant temperature at the cooling channel entrance is basically constant. Of course, in some implementations, the temperature at the cooling channel entrance can also be controlled as needed.

[0082] The initial coolant flow rate at the entrance of each cooling channel is only used at the beginning of cooling. This is because during the cooling process, the target flow rate at the entrance of each cooling channel needs to be calculated based on the cooling capacity, and the cooling capacity of the coolant channel to the key points is related to the coolant flow rate. Therefore, at the beginning of cooling, cooling is performed by the initial coolant flow rate at the entrance of each cooling channel. In the subsequent cooling process, precise control is performed by continuously correcting the target flow rate at the entrance of each cooling channel. The selection of the initial coolant flow rate at the entrance of each cooling channel directly affects the control accuracy, and it can be selected based on experience.

[0083] S02, according to the cooling time, determine the time variation relationship of the target flow rate at the entrance of each cooling channel and the target temperature of each key point at different times during the cooling time, and monitor the actual temperature of the key point.

[0084] In the hot stamping die, multiple cooling channels are set, and each cooling channel is counted as C1, C2, C3, C4...Cm. For each key point, multiple cooling channels can affect the key point, but due to the cooling capacity of the cooling channel itself and the distance from the key point, the cooling capacity of each cooling channel to the same key point is different.

[0085] In this step, in order to make each key point cool down evenly or in a certain proportion, please refer to Figure 4 , This step includes the following specific steps: S021, determining the cooling capacity of each cooling channel to each key point. In this step, the cooling capacity of any cooling channel to any key point is characterized by the following formula:

[0086]

[0087] Where a1 is a constant coefficient, the specific value can be obtained based on experience, experiment or table, c is the specific heat capacity of the coolant, S is the cross-sectional area of ​​the cooling channel, v is the flow rate of the coolant, T m is the temperature of the coolant channel wall, T s is the temperature of the coolant; t1 is the time for the coolant to flow from the inlet to the first endpoint of the cooling section; t2 is the time for the coolant to flow from the inlet to the second endpoint of the cooling section; l(t) is the distance between the coolant at a certain point at time t and the corresponding key point starting from the inlet. For ease of expression, sa(i,j) is used to represent the cooling capacity of the jth cooling channel to the ith key point. In specific implementation, the cooling section is the part of the corresponding cooling channel that has a greater impact on a certain key point. Specifically, the method for selecting the cooling section is to make a sphere with the key point as the center and the preset distance as the radius. The part of the cooling channel located within the spherical surface is the cooling section, that is, the section of the cooling channel that has the greatest cooling effect on the key point. The intersection of the cooling section and the spherical surface are the first endpoint and the second endpoint respectively.

[0088] In some implementations, for a single cooling channel, the cross-sectional area of ​​the cooling channel can also be set as a variable cross-sectional structure, that is, the cross section S is set as a variable. In specific implementation, the cross section S can also be transformed into the relationship between the distance between the cooling channel entrance, and further, the relationship between the cross section S and the time and flow rate is substituted into the above formula to obtain the cooling capacity of the variable cross-sectional cooling liquid channel for the key point. In specific implementation, the entrance of the cooling channel is not always located on the same side of the mold. For the upper mold, the entrance of the cooling channel can be set in the middle of the upper mold top surface. For the lower mold, the entrance of the cooling channel can also be set in the middle of the upper mold bottom surface, and the outlet is set on the side of the mold. Of course, the inlet and outlet can also be set on the opposite sides of the mold respectively. By setting the entrance of the cooling channel in the middle of the top surface or the bottom surface, the coolant can directly reach the corresponding key point to improve the cooling capacity of the key point.

[0089] For the i-th key point, the influence of each cooling channel is

[0090] S022, respectively determine the ratio of the degree of influence of each key point on each cooling channel; for the i-th key point, the ratio of the degree of influence of each cooling channel is:

[0091] sa(i,1):sa(i,2):...:sa(i,j):...:sa(i,m).

[0092] By determining the ratio of the degree of influence of each key point on each cooling channel, it is convenient to select the cooling channel with a greater influence on a key point according to the ratio, which is conducive to quickly determining the target flow at the entrance of each cooling channel.

[0093] S023, determine the cooling intensity requirement of each key point; in specific implementation, the cooling intensity requirement can be determined according to the position of each key point and the temperature change requirements. Specifically, when each key point needs to be cooled down synchronously and the initial temperature of each key point is different, the cooling intensity requirement can be determined according to the actual temperature of each key point, the required quenching conditions, etc. For example, it can be related to the difference between the actual temperature of the key point at the beginning of quenching and the temperature that the key point needs to reach at the end of quenching, the quenching time, and the specific heat capacity of the material used for the workpiece; more specifically, the cooling intensity requirement is proportional to the difference between the actual temperature of the key point at the beginning of quenching and the temperature that the key point needs to reach at the end of quenching, the cooling intensity requirement is inversely proportional to the quenching time, and the cooling intensity requirement is proportional to the specific heat capacity of the material used for the workpiece. In other aspects, the cooling intensity requirement of the key point is also related to its position. The closer to the middle position, the greater the cooling intensity requirement.

[0094] S024, determining the relationship between the total target flow rate at the entrance of each cooling channel and time according to the cooling intensity requirements of each key point, the cooling capacity of each cooling channel to each key point, and the ratio of the degree of influence of each cooling channel on each key point.

[0095] Specifically, the purpose of this step is to determine the relationship between the total target flow rate at the inlet of each cooling channel and its change over time. As the cooling progresses, at different times, the difference between the temperature of the workpiece and the temperature of the coolant gradually decreases. In order to make the workpiece have the same cooling rate at different times, it is necessary to change the total coolant flow rate, that is, the total target flow rate at the inlet of each cooling channel changes with time.

[0096] S025, according to the ratio of the cooling intensity requirements of each key point and the flow rate at the entrance of each cooling channel, the target flow rate at the entrance of each cooling channel is allocated, and the flow rate at the entrance of the corresponding cooling channel is controlled according to the target flow rate.

[0097] In this step, the purpose is to control the flow rate at the entrance of each cooling channel in a differentiated manner at the same time so that the temperature of each key point drops synchronously.

[0098] Specifically, when it is necessary to cool down the key points synchronously and the initial temperatures of the key points are the same, the inlet flow of each cooling channel is determined according to the ratio of the degree to which each key point is affected by the cooling channel, so that each key point is affected by all cooling channels to a substantially similar degree, thereby achieving the purpose of synchronously reducing the temperature at each key point and avoiding deformation and cracks caused by different temperature change rates and different changes in the internal organizational structure.

[0099] When the key points need to be cooled synchronously and the initial temperatures of the key points are the same, as long as each key point is affected by each cooling channel to the same extent, synchronous cooling can be guaranteed, that is, it is necessary to ensure that sa1=sa2=...sa i ...=sa n ;

[0100] The above equation is satisfied by adjusting the flow rate of each cooling channel. That is, the flow rate at the entrance of each cooling channel that satisfies the above equation can be used as the target flow rate at the entrance of each cooling channel. When the number of cooling channels is small and the number of key points is large, there may be no solution. In this case, the target flow rate at the entrance of each cooling channel at different times can be changed to achieve basically synchronous cooling of each key point.

[0101] When each key point needs to be cooled at the same proportional rate, the cooling capacity of each cooling channel can be adjusted in the same way to achieve the purpose of proportional temperature reduction. In this way, different key points of the workpiece can have corresponding performance.

[0102] In practical applications, since the number of cooling channels may be less than the number of key points, it may be difficult to achieve synchronous control of the temperature of each key point by controlling the cooling channel inlet flow rate with a fixed flow rate. Therefore, the cooling channel inlet flow rate is set to change with time, thereby achieving the purpose of cooling multiple key points basically as needed.

[0103] S03, controlling the flow rate at the inlet of each cooling channel according to the relationship between the target flow rate at the inlet of each cooling channel and time. In specific implementation, the relationship between the target flow rate at the inlet of each cooling channel and time is a functional relationship obtained through theoretical calculation, in which many factors are ignored, such as cooling channel resistance, natural heat dissipation, coolant evaporation, etc. In practical applications, the relationship between the target flow rate and time also needs to be adjusted.

[0104] S04, during the cooling process, the actual temperature of each key point at the current moment is compared with the target temperature, and the relationship between the target flow rate and time at the entrance of each cooling channel is corrected according to the comparison result; in the specific implementation, due to factors such as errors, the actual temperature may deviate from the relationship between the target flow rate and time. Therefore, in the actual control process, the relationship between the target flow rate and time is corrected in real time. Specifically, the formula is as follows:

[0105] q(t)=Sv=Q(t)+bΔq;

[0106] Among them, q(t) is the change relationship of the corrected target flow rate with time, Q(t) is the change relationship of the target flow rate with time, b is the adjustment factor, and Δq is the unit adjustment amount of the target flow rate.

[0107] The adjustment factor is related to the actual temperature and the target temperature. Specifically, the calculation formula of the adjustment factor is:

[0108]

[0109] Where a2 is a constant coefficient, and the specific value can be obtained from experience, experiment or table. sj is the actual temperature of the corresponding key point, T mb is the target temperature of the corresponding key point. The adjustment factor b is used to correct the relationship between the target flow rate and time, so that the corrected relationship between the target flow rate and time is more accurate. Among them, the role of a2 is to determine the size of the adjustment factor. Used to determine the sign of the adjustment factor. b is a dimensionless parameter; the size of a2 is related to factors such as the thermal conductivity. In practical applications, the size of this value can be determined by combining experiments with theoretical calculations. More specifically, in practical applications, the relationship between the change of the target flow rate over time and the change of the actual flow rate over time are recorded in a coordinate system with time as the horizontal axis and flow rate as the vertical axis. The goal is to minimize the sum of the areas enclosed by the change curve of the target flow rate over time and the change curve of the actual flow rate over time to solve a2 in order to obtain a better a2 value.

[0110] S05, controlling the flow rate at the inlet of each cooling channel according to the relationship between the target flow rate of each cooling channel after repair and time change; and repeating steps S04 and S05 until the cooling time is over.

[0111] In specific implementation, the cooling intensity of each key point is represented by the sum of the cooling capacity of each cooling channel to the corresponding key point; the same cooling channel has different cooling capacity for different key points. Only when the cooling capacity of the cooling channel at different key points is different, can the purpose of synchronously cooling each key point at a specific ratio be achieved by adjusting the inlet flow of each cooling channel.

[0112] At least one of the cooling channels has a plurality of tributaries in the middle. When the cooling channel has tributaries, the coolant flowing into the tributaries can help to dissipate heat in a larger area. When there are tributaries, especially when the cooling section includes tributaries, the cooling capacity of the key points corresponding to all tributaries on the cooling channel can be calculated by superimposing each tributary.

[0113] In this method, the heating process, the insulation process and the second quenching process of the aforementioned steps are all controlled by PID (proportional-integral-differential), and error accumulation is prevented by limiting the integral term or using integral anti-saturation technology. The PID algorithm is used to realize the automatic dynamic adjustment of parameters such as the mold temperature, the quenching temperature and insulation temperature of the part in the mold, the quenching and insulation time, the coolant flow rate, flow rate, the pipe diameter, the distance between the pipe and the mold surface, and the energy loss rate. Confirm the input: For mold temperature control, the input is the set temperature. For temperature control, the output may be the power of the heating / cooling device; of course, for cooling equipment, it can also be the coolant flow rate or flow rate at the entrance of each cooling channel.

[0114] The control of stamping speed and stamping time can also be PID control, which adjusts the speed or position of the servo motor according to the output of the PID controller.

[0115] Example 2

[0116] Please refer to Figures 5 to 9This embodiment proposes a trimming and punching die for the method described in Embodiment 1, wherein the die includes a first die 1, a second die 2, and a third die 3. Specifically, the first die 1 and the second die 2 are used to press on the workpiece to be trimmed and punched from both sides. During implementation, the first die 1 and the second die 2 are both adapted to the workpiece.

[0117] The first mold 1 is provided with a plurality of first holes 11, and a punching portion 12 is provided on the side of the first mold 1 close to the workpiece, and the first hole 11 passes through the punching portion 12; a first heating element 15 is embedded in the punching portion 12; the first heating element 15 is used to heat the temperature of the area to be punched to a set temperature range before punching. In a specific implementation, the first heating element 15 is used to heat the position to be punched to 550°C to 600°C, so that the tensile strength at this location is lower than 600MPa, so as to facilitate punching. In this way, the punching cost can be reduced, so as to achieve low-cost punching of hot stamping parts.

[0118] The second mold 2 is provided with a plurality of second holes 21 corresponding to the first holes 11; in a specific implementation, the center lines of the second holes 21 and the corresponding first holes 11 are located on the same line, and preferably, the second holes 21 and the corresponding first holes 11 have the same cross-sectional shape and size.

[0119] A trimming area 13 is provided around the first mold 1, and at least one second heating element 22 is provided in the trimming area 13; the second heating element 22 heats the portion of the workpiece located in the trimming area 13 to reduce the tensile strength of the portion to less than 600 MPa.

[0120] The third mold 3 and the first mold 1 are located on the same side of the workpiece and are distributed along the circumference of the first mold 1. The third mold 3 is provided with a second heating element 22 for heating the trimming position. In a specific implementation, when heated to 550° C. to 600° C., the punching position is punched by a punching device. The third mold 3 is removed and the trimming position is cut.

[0121] In a specific implementation, a groove 14 is provided in the trimming area 13, and the second heating element 22 is provided in the groove 14; the second heating element 22 is used to heat the position of the workpiece to be trimmed; a gap is provided between the peripheral side of the second heating element 22 and the wall of the groove 14. Specifically, the shape of the groove 14 is U-shaped, and by providing a gap between the peripheral side of the second heating element 22 and the wall of the groove 14, it is possible to reduce the diffusion of heat to the second mold 2 and transfer more heat to the workpiece.

[0122] In a specific implementation, a cooling channel is provided in the first mold 1. By passing a coolant into the cooling channel, the workpiece is cooled. In combination with the first heating element 15 and the second heating element 22, the local temperature of the workpiece is accurately controlled. For the specific control method, reference can be made to Example 1.

[0123] The above describes in detail the structure, features and effects of the present invention based on the embodiments shown in the drawings. The above is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown in the drawings. Any changes made according to the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the description and drawings, should be within the protection scope of the present invention.

Claims

1. A method for trimming and punching a thermoformed part, characterized in that: The following steps are included: S1, in the hot stamping die, the workpiece is hot stamped, first quenched and kept warm; S2, when the temperature cools to the preset temperature, the workpiece is taken out and moved to the trimming and punching die; S3, determining the positions to be trimmed and punched, and heating the positions to be trimmed and punched; S4, when the set condition is met, trimming and punching the workpiece; wherein the set condition is that the temperature of the area within the set distance from the incision corresponding to the position to be trimmed and punched on the workpiece is within the set temperature range; S5, quenching the workpiece for the second time.

2. The method for trimming and punching a thermoformed part according to claim 1, characterized in that: During the first quenching or the second quenching process, the workpiece is liquid-cooled; the liquid cooling uses multiple cooling channels; Methods for liquid cooling of workpieces include: S01, determining the cooling time and the initial coolant flow rate at the entrance of each cooling channel according to the heat dissipation requirements of the key points pre-selected on the workpiece and the initial coolant temperature; S02, according to the cooling time, determine the time variation relationship of the target flow rate at the entrance of each cooling channel and the target temperature of each key point at different times during the cooling time, and monitor the actual temperature of each key point; S03, controlling the flow rate at the inlet of each cooling channel according to the relationship between the target flow rate at the inlet of each cooling channel and time; S04, during the cooling process, the actual temperature of each key point at the current moment is compared with the target temperature, and the relationship between the target flow rate at the entrance of each cooling channel and time is corrected according to the comparison result; S05, controlling the coolant flow at the inlet of each cooling channel according to the modified relationship between the target flow at the inlet of each cooling channel and time; repeating steps S04 and S05 until the cooling time ends.

3. The method for trimming and punching a thermoformed part according to claim 2, characterized in that: In step S02, the step of determining the relationship between the target flow rate at the inlet of each cooling channel and time includes: S021, determining the cooling capacity of each cooling channel for each key point; S022, respectively determining the ratio of the degree of influence of each key point on each cooling channel; S023, determine the cooling intensity requirements of each key point; S024, determining the relationship between the total target flow rate at the entrance of each cooling channel and time according to the cooling intensity requirements of each key point, the cooling capacity of each cooling channel to each key point, and the ratio of the degree of influence of each key point on each cooling channel; S025, allocating the target flow rate at the entrance of each cooling channel according to the ratio between the cooling intensity requirement of each key point and the target flow rate at the entrance of each cooling channel.

4. The method for trimming and punching a thermoformed part according to claim 3, characterized in that: In step S021, the relationship between the target flow rate at the inlet of each cooling channel and time is determined by the cooling capacity of each cooling channel to each key point; The cooling capacity of each cooling channel to each key point is determined by the following formula: Among them, sa is the cooling capacity, a1 is the constant coefficient, c is the specific heat capacity of the coolant, S is the cross-sectional area of ​​the cooling channel, v is the flow rate of the coolant, T m is the temperature of the coolant channel wall, T s is the temperature of the coolant; t1 is the time for the coolant to flow from the inlet of the cooling channel to the first end point of the cooling section; t2 is the time for the coolant to flow from the inlet to the second end point of the cooling section; l(t) is the distance between the position of the coolant at a certain point starting from the inlet and the corresponding key point at time t.

5. The method for trimming and punching a thermoformed part according to claim 4, characterized in that: The method for selecting the cooling section is to make a sphere with the key point as the center and the preset distance as the radius, and the part of the cooling channel located within the sphere is the cooling section.

6. The method for trimming and punching a thermoformed part according to claim 3, characterized in that: According to the comparison results, the formula for correcting the relationship between the target flow rate at the entrance of each cooling channel and time is: q(t)=Sv=Q(t)+bΔq; Among them, q(t) is the change relationship of the target flow rate at the inlet of the cooling channel with time after correction, Q(t) is the change relationship of the target flow rate at the inlet of the cooling channel with time before correction, b is the adjustment factor, and Δq is the unit adjustment amount of the target flow rate; The calculation formula of the adjustment factor is: a2 is a constant coefficient, T sj is the actual temperature of the corresponding key point, T mb is the target temperature of the corresponding key point.

7. The method for trimming and punching a thermoformed part according to claim 3, characterized in that: At least one of the cooling channels has a plurality of branches in the middle portion.

8. The method for trimming and punching a thermoformed part according to claim 1, characterized in that: Step S1 includes the following steps, S11, placing the blank into a hot stamping die and heating the blank; S12, punching the blank to form a workpiece; S13, perform the first quenching and keep the temperature for a set time; The heating processes in step S11 and step S3 are both controlled by PID.

9. A trimming and punching die for the method according to any one of claims 2 to 8, characterized in that: It comprises a first mold (1), a second mold (2) and a third mold (3); The first mold (1) and the second mold (2) are used to press on the workpiece to be trimmed and punched from both sides; The first mold (1) is provided with a plurality of first holes (11); a punching portion (12) is provided on a side of the first mold (1) close to the workpiece, and the first holes (11) penetrate the punching portion (12); a first heating element (15) is embedded in the punching portion (12); the first heating element (15) is used to heat the temperature of the area to be punched to a set temperature range before punching; The second mold (2) is provided with a plurality of second holes (21) corresponding to the first holes (11); The side wall of the first mold (1) is provided with a trimming area (13), and at least one second heating element (22) is arranged in the trimming area (13); The third mold (3) and the first mold (1) are located on the same side of the workpiece, and the third mold (3) is distributed along the circumference of the first mold (1), and the third mold (3) is provided with a second heating element (22) for heating the trimming position; The first mold (1) is provided with a cooling channel for liquid cooling for executing steps S01 to S05.

10. The trimming and punching die according to claim 9, characterized in that: A groove (14) is provided in the trimming area (13), and the second heating element (22) is arranged in the groove (14); the second heating element (22) is used to heat the trimming area of ​​the workpiece; and a gap is provided between the peripheral side of the second heating element (22) and the wall of the groove (14).

Citation Information

Patent Citations

  • Hot forming apparatus and hot forming method

    CN101342559A

  • Hot-punching forming die and machining system used for hot-punching forming of special-shaped plate

    CN107876640A

  • Machining method for brake clamp

    CN110480275A

  • Hot stamping formation method and pre-cooling device

    CN111014398A

  • Parameter calculation method for cooling water channel of thermal forming multi-cavity mold

    CN111136169A

Cited By

  • Edge-trimming and punching method for hot-formed part, and edge-trimming and punching die

    WO2026065879A1