Polycrystalline silicon production method and application thereof
By adjusting the molar ratio of hydrogen and trichlorosilicon in real time, the problem of low quality of dense materials in polycrystalline silicon production is solved, and the proportion and performance of dense materials of the product are improved.
Patent Information
- Application Number
- CN202411066501.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-12-03
AI Technical Summary
At this stage, the quality of dense materials accounts for a low proportion in the polycrystalline silicon production process, resulting in poor performance of polycrystalline silicon products.
Through the reduction reaction between hydrogen and trichlorosilicon gas, the concentration of silicon powder in the exhaust gas is detected in real time, and the molar ratio of hydrogen to trichlorosilicon is adjusted according to the preset silicon powder concentration, and the flow of hydrogen is increased to promote the reaction to move in the forward direction, thereby increasing the flow of hydrogen. The proportion of the mass of dense materials.
It effectively increases the proportion of dense materials in polysilicon products, improves product performance, and ensures that the quality of dense materials accounts for a high proportion.
Smart Images

Figure CN119059525A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polysilicon production method, in particular to a polysilicon production method and application thereof, belonging to the field of applied chemical industry. Background Art
[0002] In the production of polysilicon, trichlorosilane gas is often reacted with hydrogen to obtain polysilicon products. According to the density of silicon accumulation, it can be divided into dense material, loose material and coral material. Among them, dense material has the best performance and is the target product in the production process.
[0003] However, the current polysilicon production process has the defect that the quality proportion of dense material in polysilicon products is relatively low.
[0004] Therefore, developing a method for producing polysilicon containing a higher proportion of dense material has become a research direction. Summary of the invention
[0005] The invention provides a polysilicon production method, which has the characteristic of increasing the proportion of dense material in the polysilicon product.
[0006] The present invention also provides a polysilicon production device, which has the characteristic of being able to increase the proportion of dense materials in the polysilicon product.
[0007] The present invention also provides a polysilicon production system, which has the characteristic of increasing the proportion of dense materials in polysilicon products.
[0008] The present invention provides a method for producing polycrystalline silicon, which comprises the following steps:
[0009] 1) Hydrogen and trichlorosilane gas undergo a reduction reaction to obtain polycrystalline silicon and tail gas; wherein the molar ratio of hydrogen to trichlorosilane is A;
[0010] 2) Obtaining the silicon powder concentration in the exhaust gas at M moments, and comparing it with the preset silicon powder concentration B, if the silicon powder concentration at any moment is higher than the value of the preset silicon powder concentration B, increasing the value of A;
[0011] M≥1,0wt%≤B≤0.5wt%.
[0012] The method as described above, wherein 2≤A≤6.
[0013] In the method as described above, the value of the preset silicon powder concentration B is 0.5wt%.
[0014] As described above, in step 1), the temperature of the hydrogen and the trichlorosilane gas is 120-150° C., and the pressure is 0.7-1.0 MPa.
[0015] In the method as described above, the treatment temperature of the reduction reaction is 1050-1200°C.
[0016] The present invention also provides a polysilicon production device, which is used to perform any of the above-mentioned polysilicon production methods, wherein the device comprises a reaction unit, a silicon powder concentration detection unit, a hydrogen flow rate adjustment unit, and a control unit;
[0017] The silicon powder concentration detection unit is connected to the tail gas outlet of the reaction unit; the hydrogen flow rate regulating unit is connected to the raw material inlet of the reaction unit, and the hydrogen flow rate regulating unit and the silicon powder concentration detection unit are electrically connected to the control unit respectively;
[0018] The silicon powder concentration detection unit is used to detect the silicon powder concentration of the tail gas;
[0019] The hydrogen flow regulating unit is used to regulate the hydrogen flow entering the reaction unit;
[0020] The control unit controls the hydrogen flow rate regulating unit to regulate the hydrogen flow rate according to the silicon powder concentration;
[0021] If the silicon powder concentration is higher than a preset silicon powder concentration B, the control unit controls the hydrogen flow rate regulating unit to increase the hydrogen flow rate.
[0022] The device as described above, wherein it further comprises a hydrogen supply unit, wherein the hydrogen outlet of the hydrogen supply unit is connected to the raw material inlet of the reaction unit through the hydrogen flow regulating unit.
[0023] The silicon powder concentration detection unit obtains the silicon powder concentration in the exhaust gas at M moments, and the control unit compares the silicon powder concentration with the value of the preset silicon powder concentration B. If the silicon powder concentration at any moment is higher than the value of the preset silicon powder concentration B, the control unit controls the hydrogen flow regulating unit to increase the hydrogen flow.
[0024] The device as described above, wherein it further comprises a trichlorosilane supply unit, wherein a raw material outlet of the trichlorosilane supply unit is connected to a raw material inlet of the reaction unit.
[0025] The device as described above, wherein it further comprises a mixing unit, and the hydrogen outlet of the hydrogen supply unit and the raw material outlet of the trichlorosilane supply unit are respectively connected to the raw material inlet of the reaction unit through the mixing unit.
[0026] The present invention also provides a polysilicon production system, wherein the system comprises any one of the polysilicon production devices mentioned above.
[0027] The polysilicon production method provided by the present invention has the characteristic of increasing the proportion of dense material in the polysilicon product. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced one by one below. Obviously, the drawings in the following description are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0029] Figure 1 A structural diagram of a first polysilicon production device provided by the present invention;
[0030] Figure 2 A structural diagram of a second polysilicon production device provided by the present invention;
[0031] Figure 3 This is an equipment diagram of the second polysilicon production device provided by the present invention.
[0032] Description of reference numerals:
[0033] A-reaction unit;
[0034] B-Silicon powder concentration detection unit;
[0035] C-hydrogen flow regulating unit;
[0036] D-control unit;
[0037] E-hydrogen supply unit;
[0038] G-trichlorosilane supply unit;
[0039] H-mixing unit;
[0040] A1-reduction furnace;
[0041] B1-Silicon powder concentration detector;
[0042] C1-hydrogen flow regulating valve;
[0043] E1-plant hydrogen interface;
[0044] G1-trichlorosilane interface in the plant area;
[0045] H1 - Mixer. DETAILED DESCRIPTION
[0046] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0047] The first aspect of the present invention protects a method for producing polysilicon, the method comprising the following steps:
[0048] 1) causing hydrogen and trichlorosilane gas to undergo a reduction reaction to obtain polycrystalline silicon and tail gas; wherein the molar ratio of hydrogen to trichlorosilane is A;
[0049] 2) Obtain the silicon powder concentration in the tail gas at M times, and compare it with the preset silicon powder concentration B. If the silicon powder concentration at any time is higher than the preset silicon powder concentration B, increase the value of A. M≥1, 0wt%≤B≤0.5wt%.
[0050] The present invention does not limit the reaction conditions such as the temperature, pressure and reduction reaction temperature of the raw materials, and common reaction conditions in the art may be used as long as the requirement that polysilicon can be produced using raw materials including hydrogen and trichlorosilane is met.
[0051] When hydrogen reacts with trichlorosilane, hydrogen can reduce trichlorosilane to solid silicon and generate tail gas. The reduced solid silicon is deposited as a polycrystalline silicon product. Specifically,
[0052] In the reduction furnace, hydrogen reacts with trichlorosilane gas, and trichlorosilane gas is reduced to silicon at high temperature and deposited on silicon rods. Polysilicon products can be divided into dense materials, loose materials and coral materials according to their density. Among them, dense materials have the best performance. However, the current polysilicon production process has the defect that dense materials account for a relatively low proportion of the quality of polysilicon products.
[0053] The inventors found that when the reduction reaction is carried out to the point where the reduction tail gas contains a large amount of silicon powder, increasing the hydrogen flow rate can reduce the trichlorosilane gas more thoroughly. At the same time, since the hydrogen temperature is lower than the temperature in the reduction furnace, the reaction temperature in the reduction furnace can be reduced, so that the reduction reaction is carried out at the optimal reaction temperature. Therefore, the proportion of dense material in the polysilicon product can be increased.
[0054] The inventor speculates that the reason for the above phenomenon is that when using a reduction furnace to produce polysilicon, when the mass of dense material in the polysilicon product accounts for a large proportion, the silicon powder that constitutes the dense material is not easy to fall off and enter the exhaust gas, and the concentration of silicon powder in the exhaust gas is relatively small; when the mass of dense material in the polysilicon product accounts for a small proportion, due to the relatively loose texture of coral material and loose material, the silicon element generated by the reaction is easy to enter the reducing exhaust gas in the form of silicon powder, resulting in a higher concentration of silicon powder in the exhaust gas.
[0055] Therefore, the inventors found that the proportion of dense polysilicon in the polysilicon product can be obtained by observing the concentration of silicon powder in the tail gas. When the silicon powder concentration is higher than the preset silicon powder concentration, it means that the mass proportion of dense material in the polysilicon product is low. At this time, the A value can be increased to increase the molar ratio of hydrogen to trichlorosilane, promote the reaction to move in the positive direction, and increase the mass proportion of dense material in the polysilicon.
[0056] Specifically, the silicon powder concentration in the tail gas at M moments can be obtained and compared with the preset silicon powder concentration B. If the silicon powder concentration at any moment is higher than the B value, the A value is increased, that is, the molar ratio of hydrogen to trichlorosilane is increased.
[0057] The preset silicon powder concentration B is a preset value, which can be set according to production experience. In one embodiment, 0wt%≤B≤0.5wt%, preferably 0.5wt%.
[0058] The polysilicon production method provided by the present invention does not limit the sampling intervals between the M moments, and the sampling intervals between the M moments may be the same or different. For example, in one embodiment, M=1000, sampling is performed every 1 second, and after each sampling is completed, the sampling result is compared with the preset silicon powder concentration B. If the sampling result at any moment is higher than the B value, the A value is increased to increase the molar ratio of hydrogen to trichlorosilane, promote the reaction to move in the forward direction, and increase the proportion of dense material in the polysilicon product.
[0059] In another embodiment, M is infinitely large and the sampling interval is infinitely small, that is, the silicon powder concentration in the exhaust gas is continuously sampled and compared with the preset silicon powder concentration B in real time. If the sampling result at any moment is higher than the B value, the A value is increased.
[0060] In one embodiment, the A value can be increased by increasing the concentration of hydrogen in the raw material. Specifically, when using a reduction furnace to produce trichlorosilane, the flow rate of trichlorosilane in the raw material entering the reduction furnace can be kept unchanged, while increasing the flow rate of hydrogen in the raw material entering the reduction furnace, thereby achieving an increase in the A value.
[0061] Accordingly, the present invention does not specifically limit the initial value of A at the beginning of the reduction reaction, and can be set according to production experience. In one embodiment, the initial value of A is between 2 and 4, that is, when the reduction reaction starts, the molar ratio of hydrogen to trichlorosilane in the raw material is between 2 and 4. The present invention also does not limit the single increase of the A value. In one embodiment, the A value increases by 2% of the original value each time, that is, when the A value is adjusted for the Nth time, the adjusted A value is 102% of the A value obtained after the A value is adjusted for the N-1th time.
[0062] Furthermore, among the M moments, when the silicon powder concentration obtained at any moment is less than or equal to the B value, it means that the silicon powder concentration in the exhaust gas has dropped to an appropriate level, that is, the mass of dense material in the obtained polysilicon product accounts for a high proportion. At this time, the A value is no longer adjusted, and the molar ratio of hydrogen and polysilicon is fixed.
[0063] The method for producing polysilicon provided by the present invention obtains the silicon powder concentration in the tail gas, compares it numerically with the preset silicon powder concentration, and adjusts the molar ratio of hydrogen and trichlorosilane in the raw material according to the comparison result, so that the proportion of dense material in the obtained polysilicon product is relatively high, which has the characteristic of increasing the proportion of dense material in the polysilicon product.
[0064] In one embodiment, 2≤A≤6, that is, in the raw material, the molar ratio of hydrogen to trichlorosilane is in the range of 2 to 6. The above range helps to increase the reaction rate of hydrogen and trichlorosilane, and increase the mass proportion of dense materials in the polysilicon product, so that the polysilicon production method provided by the present invention can obtain a polysilicon product with a higher proportion of dense materials, which is more prominent.
[0065] Furthermore, in one embodiment, the B value is 0.5wt%, that is, the preset silicon powder concentration in the tail gas is 0.5wt%. The inventors found that when the preset silicon powder concentration is controlled to be lower than 0.5wt%, the proportion of dense material in the obtained polysilicon product is higher, so that the polysilicon production method provided by the present invention can further highlight the characteristic of obtaining a polysilicon product with a higher proportion of dense material.
[0066] In one embodiment, the temperature of hydrogen and trichlorosilane gas is 120-150° C., the pressure of the raw material is 0.7-1.0 MPa, and further, the reaction temperature of the reduction reaction is 1050-1200° C. The above reaction conditions can make the reduction reaction have a higher reaction rate, and further increase the mass proportion of dense material in the polysilicon product.
[0067] A second aspect of the present invention provides a polysilicon production device, which is used to execute any of the above-mentioned polysilicon production methods. Figure 1 is a structural diagram of the first polysilicon production device provided by the present invention, such as Figure 1As shown, the polysilicon production device includes A-reaction unit, B-silicon powder concentration detection unit, C-hydrogen flow regulation unit, and D-control unit;
[0068] The B-silicon powder concentration detection unit is connected to the tail gas outlet of the A-reaction unit; the C-hydrogen flow rate adjustment unit is connected to the raw material inlet of the A-reaction unit, and the C-hydrogen flow rate adjustment unit and the B-silicon powder concentration detection unit are electrically connected to the D-control unit respectively;
[0069] B-Silicon powder concentration detection unit is used to detect the silicon powder concentration of tail gas;
[0070] C-hydrogen flow regulating unit is used to regulate the hydrogen flow entering the A-reaction unit;
[0071] D-control unit controls C-hydrogen flow rate regulating unit to adjust hydrogen flow rate according to silicon powder concentration;
[0072] B-silicon powder concentration detection unit obtains the silicon powder concentration in the exhaust gas at M moments, and D-control unit compares the silicon powder concentration with the preset silicon powder concentration B. If the silicon powder concentration at any moment is higher than the B value, the D-control unit controls C-hydrogen flow regulation unit to increase the hydrogen flow.
[0073] The A-reaction unit is used for the reduction reaction of hydrogen and trichlorosilane gas. The present invention does not limit the specific equipment selection of the A-reaction unit. In one embodiment, the A-reaction unit is a reduction furnace.
[0074] The B-silicon powder concentration detection unit is connected to the tail gas outlet of the A-reaction unit and is used to detect the silicon powder concentration in the tail gas discharged from the A-reaction unit. The present invention also does not limit the specific equipment selection of the B-silicon powder concentration detection unit. In one embodiment, the B-silicon powder concentration detection unit is a silicon powder concentration detector.
[0075] The C-hydrogen flow regulating unit is connected to the raw material inlet of the A-reaction unit and acts as a valve to regulate the flow of hydrogen entering the A-reaction unit. The present invention also does not limit the specific equipment selection of the C-hydrogen flow regulating unit. In one embodiment, the C-hydrogen flow regulating unit is a C1-hydrogen flow regulating valve.
[0076] The B-silicon powder concentration detection unit and the C-hydrogen flow rate adjustment unit are electrically connected to the D-control unit, respectively. The D-control unit receives the silicon powder concentration transmitted by the D-control unit from the B-silicon powder concentration detection unit at least once, and compares the concentration with the preset silicon powder concentration B. If the silicon powder concentration is higher than the B value, the D-control unit controls the C-hydrogen flow rate adjustment unit to increase the hydrogen flow rate, thereby increasing the molar ratio A value of the raw hydrogen to trichlorosilane. The present invention also does not limit the specific equipment selection of the D-control unit. In one embodiment, the D-control unit is a master control computer.
[0077] The inventors found that the concentration of silicon powder in the tail gas is negatively correlated with the mass proportion of dense materials in the polysilicon product. Therefore, the concentration of silicon powder in the tail gas can be observed to obtain the proportion of dense materials in the polysilicon product, and the mass proportion of dense materials in the polysilicon product can be increased by adjusting the molar ratio of hydrogen to trichlorosilane. Specifically, the B-silicon powder concentration detection unit obtains the silicon powder concentration in the tail gas at M moments, and compares it with the preset silicon powder concentration B value. If the silicon powder concentration is higher than the B value at any moment, the A value is increased, that is, the molar ratio of hydrogen to trichlorosilane is increased. In one embodiment, under the premise that the flow rate of trichlorosilane in the raw material remains unchanged, the D-control unit controls the C-hydrogen flow regulating unit to increase the hydrogen flow in the raw material, thereby increasing the A value, increasing the ratio of the molar ratio of hydrogen to trichlorosilane, promoting the reaction to move in the forward direction, and increasing the mass proportion of dense materials in polysilicon.
[0078] The present invention does not specifically limit the initial value of A at the beginning of the reduction reaction, and can be set according to production experience. In one embodiment, the initial value of A is between 2 and 4, that is, when the reduction reaction starts, the molar ratio of hydrogen to trichlorosilane in the raw material is between 2 and 4. The present invention also does not limit the single increase in the A value. In one embodiment, the A value increases by 2% of the original value each time, that is, when the A value is adjusted for the Nth time, the adjusted A value is 102% of the A value obtained after the A value is adjusted for the N-1th time.
[0079] Furthermore, among the M moments, when the A value and silicon powder concentration obtained at any moment are less than or equal to the B value, it means that the silicon powder concentration in the exhaust gas has dropped to an appropriate level, that is, the mass of dense material in the obtained polysilicon product accounts for a high proportion. At this time, the A value is no longer adjusted, and the molar ratio of hydrogen and polysilicon is fixed.
[0080] The polysilicon production device provided by the present invention obtains the silicon powder concentration in the tail gas, compares it numerically with the preset silicon powder concentration, and adjusts the molar ratio of hydrogen and trichlorosilane in the raw material according to the comparison result, so that the obtained polysilicon product has a higher proportion of dense material. The device has the characteristic of being able to obtain a polysilicon product with a higher proportion of dense material.
[0081] It can be understood that, since the raw material includes trichlorosilane, in one embodiment, the A-reaction unit also includes a trichlorosilane inlet, and the raw material trichlorosilane enters the A-reaction unit through the trichlorosilane inlet of the A-reaction unit and reacts after mixing with hydrogen.
[0082] In one embodiment, the polysilicon production device provided by the present invention further includes an E-hydrogen supply unit, and the hydrogen outlet of the E-hydrogen supply unit is connected to the raw material inlet of the A-reaction unit through the C-hydrogen flow regulating unit.
[0083] The raw materials used to produce polysilicon include hydrogen and trichlorosilane, which are obtained by mixing hydrogen and trichlorosilane in a certain proportion. Among them, the flow ratio of hydrogen to trichlorosilane is positively correlated with the molar ratio A of hydrogen to trichlorosilane. The E-hydrogen supply unit is used to provide the hydrogen required for the raw materials. The present invention does not specifically limit the specific selection of the E-hydrogen supply unit. In one embodiment, the E-hydrogen supply unit is a plant hydrogen interface, and the hydrogen outlet of the E-hydrogen supply unit is the hydrogen outlet of the plant hydrogen interface. The hydrogen outlet of the E-hydrogen supply unit is connected to the raw material inlet of the A-reaction unit through the C-hydrogen flow regulating unit. The C-hydrogen flow regulating unit can adjust the hydrogen flow provided by the E-hydrogen supply unit to enter the A-reaction unit, thereby realizing the adjustment of the molar ratio A of hydrogen to trichlorosilane. The present invention does not limit the manner in which trichlorosilane and hydrogen are mixed. In one embodiment, trichlorosilane can be mixed with hydrogen between the C-hydrogen flow regulating unit and the raw material inlet of the A-reaction unit to obtain a raw material for producing polysilicon, which enters the A-reaction unit for a reduction reaction.
[0084] In one embodiment, the polysilicon production device provided by the present invention further includes a G-trichlorosilane supply unit, and the raw material outlet of the G-trichlorosilane supply unit is connected to the raw material inlet of the A-reaction unit.
[0085] The G-trichlorosilane supply unit is used to provide trichlorosilane required for raw materials. The present invention does not specifically limit the specific selection of the G-trichlorosilane supply unit. In one embodiment, the G-trichlorosilane supply unit is a plant trichlorosilane interface, and the raw material outlet of the G-trichlorosilane supply unit is the raw material outlet of the plant trichlorosilane interface.
[0086] The raw material outlet of the G-trichlorosilane supply unit is connected to the raw material inlet of the A-reaction unit, and the G-trichlorosilane supply unit can adjust the trichlorosilane flow rate provided by the E-hydrogen supply unit entering the A-reaction unit, thereby adjusting the molar ratio A of hydrogen to trichlorosilane. The present invention does not limit the way in which trichlorosilane and hydrogen are mixed. In one embodiment, trichlorosilane can be mixed with hydrogen between the C-hydrogen flow rate adjustment unit and the raw material inlet of the A-reaction unit to obtain a raw material for producing polysilicon, which enters the A-reaction unit for reduction reaction.
[0087] Figure 2 is a structural diagram of a second polysilicon production device provided by the present invention, such as Figure 2 As shown, the polysilicon production device includes not only A-reaction unit, B-silicon powder concentration detection unit, C-hydrogen flow regulation unit, E-hydrogen supply unit, G-trichlorosilane supply unit, and D-control unit, but also H-mixing unit.
[0088] The hydrogen outlet of the E-hydrogen supply unit and the raw material outlet of the G-trichlorosilane supply unit are respectively connected to the raw material inlet of the A-reaction unit through the H-mixing unit.
[0089] Further, in one embodiment, the H-mixing unit includes a hydrogen inlet, a trichlorosilane inlet, and a raw material outlet, the E-hydrogen supply unit is connected to the hydrogen inlet of the H-mixing unit through the C-hydrogen flow regulating unit, the G-trichlorosilane supply unit is connected to the trichlorosilane inlet of the H-mixing unit, and the raw material outlet of the H-mixing unit is connected to the raw material inlet of the A-reaction unit.
[0090] The H-mixing unit is used to mix hydrogen and trichlorosilane, further improving the uniformity of distribution of hydrogen and trichlorosilane in the raw materials, helping to increase the reaction rate of hydrogen and trichlorosilane in the reduction reaction, and further increasing the mass proportion of dense material in polysilicon products.
[0091] The present invention does not limit the specific equipment selection of the H-mixing unit, as long as it can achieve the mixing of hydrogen and trichlorosilane. In one embodiment, the H-mixing unit is an H1-mixer.
[0092] The hydrogen outlet of the E-hydrogen supply unit and the raw material outlet of the G-trichlorosilane supply unit are respectively connected to the raw material inlet of the A-reaction unit through the H-mixing unit, that is, the hydrogen provided by the E-hydrogen supply unit and the trichlorosilane provided by the G-trichlorosilane supply unit are mixed in the H-mixing unit and then enter the A-reaction unit.
[0093] It is understandable that when the polysilicon production device includes a C-hydrogen flow regulating unit, in order to achieve effective regulation of the flow of hydrogen and trichlorosilane, the C-hydrogen flow regulating unit is located between the E-hydrogen supply unit and the H-mixing unit.
[0094] Figure 3 is a diagram of the equipment of the second polysilicon production device provided by the present invention, such as Figure 3 As shown, the polysilicon production device includes A1-reduction furnace, B1-silicon powder concentration detector, C1-hydrogen flow control valve, E1-plant area hydrogen interface, G1-plant area trichlorosilane interface, H1-mixer, wherein the E1-plant area hydrogen interface is connected to the hydrogen inlet of the H1-mixer through the C1-hydrogen flow control valve, the G1-plant area trichlorosilane interface is connected to the trichlorosilane hydrogen inlet of the H1-mixer, and the raw material outlet of the H1-mixer is connected to the raw material inlet of the A1-reduction furnace. The B1-silicon powder concentration detector is connected to the tail gas outlet of the A1-reduction furnace and is used to detect the silicon powder content in the tail gas. In addition, the equipment also includes a master control computer ( Figure 3 The master control computer is electrically connected to the B1-silicon powder concentration detector and the C1-hydrogen flow control valve.
[0095] When using the above equipment for polysilicon production, the E1-plant hydrogen interface provides hydrogen, which enters the H1-mixer through the C1-hydrogen flow control valve; the G1-plant trichlorosilane interface provides trichlorosilane, which enters the H1-mixer. After hydrogen and trichlorosilane are mixed in the H1-mixer, they enter the A1-reduction furnace through the raw material inlet of the A1-reduction furnace. Hydrogen and trichlorosilane react in the A1-reduction furnace to generate silicon and tail gas. The tail gas leaves the A1-reduction furnace from the tail gas outlet of the A1-reduction furnace and passes through the B1-silicon powder concentration detector to the subsequent tail gas treatment process.
[0096] During the operation of the A1-reduction furnace, the B1-silicon powder concentration detector obtains the silicon powder concentration in the exhaust gas at M moments. Each time the silicon powder concentration is obtained, the silicon powder concentration is compared with the preset silicon powder concentration B. If the silicon powder concentration is higher than the preset silicon powder concentration B at any moment, the master control computer controls the C1-hydrogen flow control valve to adjust the hydrogen flow, so that the hydrogen flow entering the H1-mixer increases, the molar ratio A of hydrogen to trichlorosilane increases, and the reaction is driven to move in the forward direction, so that the mass proportion of dense material in polysilicon increases.
[0097] If the silicon powder concentration is less than or equal to the preset silicon powder concentration B at any time, the master control computer will not issue any instructions to the C1-hydrogen flow control valve, and the hydrogen flow rate will remain unchanged.
[0098] The third aspect of the present invention provides a polysilicon production system, which includes any of the above-mentioned polysilicon production devices. Since the polysilicon production device provided by the present invention has the characteristic of increasing the proportion of dense materials in the polysilicon production, the polysilicon production system provided by the present invention also has the characteristic of increasing the proportion of dense materials in the polysilicon production.
[0099] The present invention does not further limit other devices included in the polysilicon production system, which may include common devices in the art. For example, in one embodiment, the polysilicon production system also includes a distillation device and a slurry processing device.
[0100] The polysilicon production method and its application provided by the present invention are further described in detail using specific embodiments below:
[0101] Example 1
[0102] This embodiment will Figure 3 The polysilicon production equipment shown is used for the production of polysilicon. Wherein, 2≤A≤6, the initial value is 2, when the A value is adjusted for the Nth time, the adjusted A value is 102% of the A value obtained after the A value is adjusted for the N-1th time; B=0.5wt%.
[0103] The polysilicon production device includes an A1-reduction furnace, a B1-silicon powder concentration detector, a C1-hydrogen flow control valve, an E1-plant hydrogen interface, a G1-plant trichlorosilane interface, and an H1-mixer, wherein the E1-plant hydrogen interface is connected to the hydrogen inlet of the H1-mixer via the C1-hydrogen flow control valve, the G1-plant trichlorosilane interface is connected to the trichlorosilane hydrogen inlet of the H1-mixer, and the raw material outlet of the H1-mixer is connected to the raw material inlet of the A1-reduction furnace. The B1-silicon powder concentration detector is connected to the tail gas outlet of the A1-reduction furnace and is used to detect the silicon powder content in the tail gas. In addition, the device also includes a master control computer ( Figure 3 The master control computer is electrically connected to the B1-silicon powder concentration detector and the C1-hydrogen flow regulating valve.
[0104] When using the above equipment for polysilicon production, the E1-plant hydrogen interface provides hydrogen, which enters the H1-mixer through the C1-hydrogen flow control valve; the G1-plant trichlorosilane interface provides trichlorosilane, which enters the H1-mixer. After hydrogen and trichlorosilane are mixed in the H1-mixer, they enter the A1-reduction furnace through the raw material inlet of the A1-reduction furnace. Hydrogen and trichlorosilane react in the A1-reduction furnace to generate silicon and tail gas. The tail gas leaves the A1-reduction furnace from the tail gas outlet of the A1-reduction furnace and passes through the B1-silicon powder concentration detector to the subsequent tail gas treatment process.
[0105] The method of using the polysilicon production device provided in this embodiment is as follows: B1-silicon powder concentration detector continuously obtains the silicon powder concentration in the exhaust gas, and each time the silicon powder concentration is obtained, the silicon powder concentration is compared with the preset silicon powder concentration B. If the silicon powder concentration is higher than the preset silicon powder concentration B at any moment, the main control computer controls C1-hydrogen flow control valve to adjust the hydrogen flow, so that the hydrogen flow entering the H1-mixer is increased, and the molar ratio A of hydrogen to trichlorosilane is increased, which drives the reaction to move in the forward direction, thereby increasing the mass proportion of dense material in the polysilicon.
[0106] If the silicon powder concentration is less than or equal to the preset silicon powder concentration B at any time, the master control computer will not issue any instructions to the C1-hydrogen flow control valve, and the hydrogen flow rate will remain unchanged.
[0107] In the description of the embodiments of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, or it can be an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0108] The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some or all of the technical features can be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.
Claims
1. A method for producing polycrystalline silicon, characterized in that: The steps include: 1) causing hydrogen and trichlorosilane gas to undergo a reduction reaction to obtain polycrystalline silicon and tail gas; wherein the molar ratio of hydrogen to trichlorosilane is A; 2) Obtaining the silicon powder concentration in the exhaust gas at M moments, and comparing it with the preset silicon powder concentration B, if the silicon powder concentration at any moment is higher than the value of the preset silicon powder concentration B, increasing the value of A; M≥1,0wt%≤B≤0.5wt%.
2. The method according to claim 1, characterized in that 2≤A≤6。 3. The method according to claim 1 or 2, characterized in that: The preset silicon powder concentration B is 0.5 wt %.
4. The method according to any one of claims 1 to 3, characterized in that In step 1), the temperature of the hydrogen and the trichlorosilane gas is 120-150° C., and the pressure is 0.7-1.0 MPa.
5. The method according to claim 4, characterized in that The reaction temperature of the reduction reaction is 1050-1200°C.
6. A polysilicon production device for executing the method according to any one of claims 1 to 5, characterized in that: It includes a reaction unit, a silicon powder concentration detection unit, a hydrogen flow regulating unit, and a control unit; The silicon powder concentration detection unit is connected to the tail gas outlet of the reaction unit; the hydrogen flow rate regulating unit is connected to the raw material inlet of the reaction unit, and the hydrogen flow rate regulating unit and the silicon powder concentration detection unit are electrically connected to the control unit respectively; The silicon powder concentration detection unit is used to detect the silicon powder concentration of the tail gas; The hydrogen flow rate regulating unit is used to regulate the hydrogen flow rate entering the reaction unit; The control unit controls the hydrogen flow rate regulating unit to regulate the hydrogen flow rate according to the silicon powder concentration; The silicon powder concentration detection unit obtains the silicon powder concentration in the exhaust gas at M moments, and the control unit compares the silicon powder concentration with the value of the preset silicon powder concentration B. If the silicon powder concentration at any moment is higher than the value of the preset silicon powder concentration B, the control unit controls the hydrogen flow regulating unit to increase the hydrogen flow.
7. The device according to claim 6, characterized in that It also includes a hydrogen supply unit, and the hydrogen outlet of the hydrogen supply unit is connected with the raw material inlet of the reaction unit through the hydrogen flow regulating unit.
8. The device according to claim 7, characterized in that The invention also comprises a trichlorosilane supply unit, wherein a raw material outlet of the trichlorosilane supply unit is connected with a raw material inlet of the reaction unit.
9. The device according to claim 8, characterized in that It also includes a mixing unit, and the hydrogen outlet of the hydrogen supply unit and the raw material outlet of the trichlorosilane supply unit are respectively connected to the raw material inlet of the reaction unit through the mixing unit.
10. A polysilicon production system, characterized in that: A device comprising any one of claims 5-9.
Citation Information
Patent Citations
Method for producing polysilicon
CN101717086A
Improvement method for the preparation of highly dense structure polycrystalline silicon and the device thereof
CN101748482A
Method for manufacturing polysilicon
CN101759182A
Temperature control and energy saving system and process for polycrystalline silicon reduction furnaces
CN103466629A
Polycrystalline silicon production system and method
CN105293501A