Continuous reaction system, manganese iron carbonate precursor and preparation method thereof, lithium manganese iron phosphate and preparation method thereof, positive plate and battery

Through the continuous reaction system, the reaction conditions are controlled, and the problems of low production efficiency and unstable quality in the preparation of ferromanganese carbonate precursors are solved, and efficient and simple preparation of ferromanganese carbonate precursors are achieved. Improve product consistency and quality.

CN119059566AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310637424.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The existing preparation methods for ferromanganese carbonate precursors have problems such as low production efficiency, cumbersome processes, and unstable product quality, resulting in poor batch consistency.

Method used

Using a continuous reaction system, the reaction conditions such as temperature, pH and flow rate are controlled through the series connection of the kettle reactor and the tube reactor, so as to achieve efficient preparation of the precursor of manganese carbonate, and obtain small particle size, narrow particle size distribution and crystallization. High-degree and single crystal phase.

Benefits of technology

It improves the production efficiency and product quality of the manganese ferrocarbonate precursor, achieves high batch consistency, simple process and high energy efficiency, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059566A_ABST
    Figure CN119059566A_ABST
Patent Text Reader

Abstract

The invention discloses a continuous reaction system, a manganese iron carbonate precursor and a preparation method thereof, lithium manganese iron phosphate and a preparation method thereof, a positive plate and a battery. The continuous reaction system comprises a first material dissolving kettle, a second material dissolving kettle, a kettle type reactor and a tubular reactor, and the kettle type reactor and the tubular reactor are connected in series.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a continuous reaction system, a ferromanganese carbonate precursor and a preparation method thereof, lithium ferromanganese phosphate and a preparation method thereof, a positive electrode sheet, and a battery. Background Art

[0002] In recent years, batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. Lithium iron manganese phosphate has become one of the most popular positive electrode active materials due to its advantages such as high capacity and abundant sources of raw materials. As one of the important raw materials for preparing lithium iron manganese phosphate, the performance of ferromanganese carbonate precursor is crucial to the performance of lithium iron manganese phosphate and battery performance. However, at present, ferromanganese carbonate precursors are obtained by intermittent preparation methods, which have problems such as low production efficiency, cumbersome procedures, difficult to control production processes, large fluctuations in product quality, and poor batch consistency. The above statements are only used to provide background technical information related to this application, and do not necessarily constitute prior art. Summary of the invention

[0003] The present application provides a continuous reaction system, a ferromanganese carbonate precursor and a preparation method thereof, a lithium ferromanganese phosphate and a preparation method thereof, a positive electrode sheet, and a battery, which can improve the production efficiency of the ferromanganese carbonate precursor and obtain a ferromanganese carbonate precursor with small particle size, narrow particle size distribution, high crystallinity, single crystal phase, uniform element distribution, and high batch consistency.

[0004] In a first aspect, the present application provides a continuous reaction system for preparing a ferromanganese carbonate precursor, wherein the continuous reaction system comprises a first dissolving kettle, a second dissolving kettle, a kettle reactor and a tubular reactor, wherein the kettle reactor and the tubular reactor are connected in series.

[0005] The first dissolving kettle is used to contain the metal salt solution required for preparing the ferromanganese carbonate precursor, and the second dissolving kettle is used to contain the precipitant solution required for preparing the ferromanganese carbonate precursor. The first dissolving kettle has a first discharge port, and the second dissolving kettle has a second discharge port.

[0006] The kettle reactor has a first feed port and a first overflow port. The first feed port of the kettle reactor is connected to the first dissolving kettle and the second dissolving kettle through a first pipe and a second pipe respectively, so that the kettle reactor can accommodate the metal salt solution and the precipitant solution and mix them to produce a precipitation reaction to generate a first reaction liquid. The first pipe is provided with a first stop valve and a first metering pump to adjust the flow rate of the metal salt solution, and the second pipe is provided with a second stop valve and a second metering pump to adjust the flow rate of the precipitant solution. The kettle reactor is also connected to a pH control device to monitor and adjust the pH value of the first reaction liquid.

[0007] The tubular reactor has a second feed port and a third discharge port. The second feed port of the tubular reactor is connected to the first overflow port of the tank reactor through a third pipeline, so that the tubular reactor can accommodate the first reaction liquid from the tank reactor and continue to precipitate it to form a second reaction liquid. The third discharge port of the tubular reactor is used to allow the second reaction liquid to flow out. The tubular reactor is also connected to one or more pH control devices to monitor and adjust the pH value of the second reaction liquid.

[0008] In any embodiment, the tubular reactor is a horizontal tubular reactor.

[0009] The second aspect of the present application provides a method for preparing a ferromanganese carbonate precursor through the continuous reaction system of the first aspect of the present application, comprising at least the following steps: connecting a kettle reactor and a tubular reactor in series, the kettle reactor having a first feed port and a first overflow port, the first feed port of the kettle reactor being connected to a first dissolving kettle and a second dissolving kettle through a first pipeline and a second pipeline respectively, the first pipeline being provided with a first stop valve and a first metering pump, the second pipeline being provided with a second stop valve and a second metering pump, the kettle reactor being also connected to a pH control device, the first dissolving kettle having a first discharge port, the second dissolving kettle having a second discharge port, the tubular reactor having a second feed port and a third discharge port, the second feed port of the tubular reactor being connected to the first overflow port of the kettle reactor through a third pipeline, the tubular reactor being also connected to one or more pH control devices. The device is connected; the metal salt solution required for preparing the ferromanganese carbonate precursor is added into the first dissolving kettle, and the precipitant solution required for preparing the ferromanganese carbonate precursor is added into the second dissolving kettle; the metal salt solution in the first dissolving kettle and the precipitant solution in the second dissolving kettle are respectively transported to the kettle reactor through the first pipeline and the second pipeline to mix them and then cause precipitation reaction to generate a first reaction liquid, when the liquid level of the first reaction liquid is higher than the first overflow port of the kettle reactor, the first reaction liquid is transported to the tubular reactor, and then the first reaction liquid continues to precipitate in the tubular reactor to form a second reaction liquid, and the second reaction liquid flows out through the third discharge port of the tubular reactor; the second reaction liquid obtained from the third discharge port of the tubular reactor is washed and dried to obtain the ferromanganese carbonate precursor.

[0010] The preparation method of the ferromanganese carbonate precursor provided in the present application is a continuous preparation method, which has the advantages of high production efficiency, high energy efficiency, simple process, easy operation and low labor cost, and is particularly suitable for large-scale industrial production. The ferromanganese carbonate precursor obtained by the preparation method of the ferromanganese carbonate precursor provided in the present application can have the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, uniform element distribution, and high batch consistency. The preparation method of the ferromanganese carbonate precursor provided in the present application can also flexibly adjust the particle size and morphology of the ferromanganese carbonate precursor, which is conducive to meeting different production needs so as to prepare lithium iron manganese phosphate with different particle sizes.

[0011] In any embodiment, a complexing agent is further added to the first dissolving kettle. When a complexing agent is further added to the first dissolving kettle, the method for preparing the ferromanganese carbonate precursor provided by the present application can obtain ferromanganese carbonate precursor particles with high purity and uniform element distribution, and the molar ratio of each metal element in the obtained ferromanganese carbonate precursor particles is less different from the molar ratio of each metal element in the raw material, which is conducive to further precise control of the content of metal elements and is conducive to better achieving the preset value of the ratio of metal elements.

[0012] In any embodiment, the complexing agent includes one or more of aminocarboxylates, hydroxycarboxylates and organic phosphonates. Optionally, the complexing agent includes one or more of sodium ethylenediaminetetramethylenephosphate, sodium ethylenediaminetetraacetate, sodium gluconate and sodium citrate.

[0013] In any embodiment, the reaction temperature in the autoclave reactor is less than or equal to the reaction temperature in the tubular reactor. By adjusting the reaction temperature in the autoclave reactor to be less than or equal to the reaction temperature in the tubular reactor, it is helpful to obtain ferromanganese carbonate precursor particles with narrow particle size distribution, uniform element distribution, high crystallinity and regular morphology.

[0014] In any embodiment, the reaction temperature in the autoclave reactor is 50-80° C. When the reaction temperature in the autoclave reactor is within the above range, it is beneficial for the rapid precipitation of metal ions and carbonate ions to form a large number of crystal nuclei, and it is also beneficial to reduce the precipitation rate difference of different metal ions during the precipitation reaction process, thereby facilitating uniform co-precipitation of metal ions.

[0015] In any embodiment, the reaction temperature in the tubular reactor is 50-80° C. When the reaction temperature in the tubular reactor is within the above range, the ferromanganese carbonate grains grown in the autoclave reactor can be further grown and the crystallinity of the ferromanganese carbonate grains can be improved, thereby facilitating the acquisition of a ferromanganese carbonate precursor with high crystallinity and regular morphology.

[0016] In any embodiment, the volume of the autoclave reactor is smaller than that of the tubular reactor. The ferromanganese carbonate precursor particles stay in the tubular reactor for a longer time, which helps to make the obtained ferromanganese carbonate precursor particles have a narrower particle size distribution, and also helps to make the obtained ferromanganese carbonate precursor particles have a higher crystallinity and a more regular morphology.

[0017] In any embodiment, the volume ratio of the autoclave reactor to the tubular reactor is 1:5-1:7. This helps to make the obtained ferromanganese carbonate precursor particles have a smaller particle size and a narrower particle size distribution, and also helps to make the obtained ferromanganese carbonate precursor particles have a higher crystallinity and a more regular morphology.

[0018] In any embodiment, the residence time of the ferromanganese carbonate precursor in the autoclave reactor during the growth process is 0.5-4h.

[0019] In any embodiment, the residence time of the ferromanganese carbonate precursor in the tubular reactor during the growth process is 2.5-28 hours.

[0020] In any embodiment, the concentration of the metal salt solution is 0.5-2 mol / L.

[0021] In any embodiment, the concentration of the precipitant solution is 0.5-2 mol / L.

[0022] In any embodiment, the molar ratio of the metal salt to the precipitant is 1:1-1:2.

[0023] In any embodiment, the flow rate of the metal salt solution is 0.5-4 L / min.

[0024] In any embodiment, the flow rate of the precipitant solution is 0.5-4 L / min.

[0025] In any embodiment, the flow rates of the metal salt solution and the precipitant solution are the same.

[0026] In any embodiment, the method further comprises the following steps: during the reaction, a pH adjusting liquid is added to the kettle reactor through a pH control device connected to the kettle reactor, so that the pH of the first reaction liquid in the kettle reactor is 6-8, optionally 7-7.5. When the pH in the kettle reactor is within the above range, it is conducive to the rapid precipitation of metal ions and carbonate ions to form a large number of crystal nuclei, and it is also conducive to reducing the difference in precipitation rates of different metal ions during the precipitation reaction, thereby facilitating the uniform coprecipitation of metal ions. In addition, when the pH in the kettle reactor is within the above range, it is also conducive to forming a spherical (or spherical) morphology of ferromanganese carbonate precursor, which is also conducive to improving the tap density.

[0027] In any embodiment, the method further comprises the following steps: during the reaction, a pH adjusting liquid is added to the tubular reactor through a pH control device connected to the tubular reactor so that the pH of the second reaction liquid in the tubular reactor is 6-8, optionally 7-7.5. When the pH of the second reaction liquid in the tubular reactor is within the above range, it is beneficial to reduce the difference in precipitation rates of different metal ions during the precipitation reaction, thereby facilitating uniform coprecipitation of metal ions. In addition, when the pH in the tubular reactor is within the above range, it is also beneficial to form a spherical (or spherical) morphology of the ferromanganese carbonate precursor, which is also beneficial to improve the tap density.

[0028] In any embodiment, during the reaction process, the first dissolving kettle, the second dissolving kettle, the kettle reactor and the tubular reactor are all placed under a protective gas atmosphere.

[0029] In any embodiment, during the reaction process, the first dissolving kettle, the second dissolving kettle and the kettle reactor are all kept in a stirring state, thereby reducing the aggregation growth of the ferromanganese carbonate precursor particles and facilitating the acquisition of a ferromanganese carbonate precursor with a narrow particle size distribution and a high tap density.

[0030] In any embodiment, the stirring speed of the first dissolving kettle is 300-800r / min.

[0031] In any embodiment, the stirring speed of the second dissolving kettle is 300-800r / min.

[0032] In any embodiment, the stirring speed of the tank reactor is 300-800 r / min.

[0033] In any embodiment, the metal salt required for preparing the manganese ferrocarbonate precursor includes a water-soluble divalent iron salt, a water-soluble divalent manganese salt and an optional divalent salt of a water-soluble doping element M, where M represents the doping element at the manganese position and / or iron position of the manganese ferrocarbonate precursor, optionally including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr.

[0034] In any embodiment, the water-soluble divalent iron salt includes one or more of ferrous chloride, ferrous nitrate, ferrous sulfate, and ferrous acetate.

[0035] In any embodiment, the water-soluble divalent manganese salt includes one or more of manganous chloride, manganous nitrate, manganous sulfate, and manganous acetate.

[0036] In any embodiment, the divalent salt of the water-soluble doping element M includes one or more of the hydrochloride, nitrate, sulfate, and acetate of the doping element M.

[0037] In any embodiment, the precipitating agent comprises a carbonate, optionally comprising one or more of ammonium bicarbonate, sodium bicarbonate, ammonium carbonate and sodium carbonate.

[0038] In any embodiment, the shielding gas includes nitrogen, an inert gas, or a combination thereof.

[0039] The third aspect of the present application provides a ferromanganese carbonate precursor prepared by the method of the second aspect of the present application, which has a chemical formula of Fe x Mn y M 1-x-yCO3, 0<x<1, optionally, 0.199≤x≤0.5; 0<y<1, optionally, 0.499≤y≤0.8; 0≤1-xy<1, optionally, 0<1-xy≤0.05; M represents the doping element of the manganese position and / or iron position of the manganese ferrocarbonate precursor, optionally including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr.

[0040] The ferromanganese carbonate precursor provided in the present application has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, uniform element distribution, and high batch consistency.

[0041] In any embodiment, the volume distribution particle sizes Dv90 and Dv50 of the manganese ferrocarbonate precursor satisfy 1<Dv90 / Dv50≤1.4.

[0042] The fourth aspect of the present application provides a method for preparing lithium iron manganese phosphate, which comprises at least the following steps: uniformly mixing the ferromanganese carbonate precursor prepared by the method of the second aspect of the present application or the ferromanganese carbonate precursor of the third aspect of the present application with a lithium source, a phosphorus source, an optional source of doping element N, an optional source of doping element Q and an optional source of doping element R to obtain a mixed raw material, wherein N represents the doping element at the lithium site of the lithium iron manganese phosphate, optionally including one or more of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents the doping element at the phosphorus site of the lithium iron manganese phosphate, optionally including one or more of B, S, Si and N; R represents the doping element at the oxygen site of the lithium iron manganese phosphate, optionally including one or more of S, F, Cl and Br; sintering the obtained mixed raw material to obtain the lithium iron manganese phosphate, wherein the lithium iron manganese phosphate has a chemical formula of Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n, M represents the doping element of the manganese site and / or iron site of the lithium iron manganese phosphate, optionally including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr; N represents the doping element of the lithium site of the lithium iron manganese phosphate, optionally including one or more of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents the doping element of the phosphorus site of the lithium iron manganese phosphate, optionally including one or more of B, S, Si and N; R represents the doping element of the oxygen site of the lithium iron manganese phosphate The heteroatom elements may optionally include one or more of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1, optionally, 0<b≤0.05; 0<x<1, optionally, 0.199≤x≤0.5; 0<y<1, optionally, 0.499≤y≤0.8; 0≤1-xy<1, optionally, 0<1-xy≤0.05; 0≤m≤0.1, optionally, 0<m≤0.05; 0≤n≤0.1, optionally, 0<n≤0.05.

[0043] The lithium manganese iron phosphate obtained by the preparation method provided by the present application can achieve a uniform mixture of lithium elements and a variety of metal elements, thereby making the lithium ions diffuse faster and more easily embedded in the lithium manganese iron phosphate precursor, thereby enabling the prepared lithium manganese iron phosphate to have excellent electrochemical properties. The lithium manganese iron phosphate obtained by the preparation method provided by the present application also has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, and high batch consistency, which is conducive to improving the capacity and electrochemical performance of the battery.

[0044] In any embodiment, a carbon source is further added to the mixed raw material, thereby preparing carbon-coated lithium manganese iron phosphate.

[0045] The fifth aspect of the present application provides lithium manganese iron phosphate prepared by the method of the fourth aspect of the present application.

[0046] The lithium manganese iron phosphate provided in the present application has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, uniform element distribution, and high batch consistency, which is beneficial to improving the capacity and electrochemical performance of the battery.

[0047] The sixth aspect of the present application provides a positive electrode sheet, including a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes lithium manganese iron phosphate prepared by the method of the fourth aspect of the present application or the lithium manganese iron phosphate of the fifth aspect of the present application.

[0048] The seventh aspect of the present application provides a battery, comprising the positive electrode sheet of the sixth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some implementation methods of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0050] Figure 1 A continuous reaction system for preparing a ferromanganese carbonate precursor is shown.

[0051] Figure 2 The scanning electron microscope (SEM) image of the ferromanganese carbonate precursor prepared in Example 1 is shown. Figure 2 The magnification of a is 2000 times. Figure 2 The magnification of b is 5000 times.

[0052] Figure 3 The scanning electron microscope (SEM) image of the ferromanganese carbonate precursor prepared in Comparative Example 1 is shown. Figure 3 The magnification of a is 2000 times. Figure 3 The magnification of b is 5000 times.

[0053] In the drawings, the drawings are not necessarily drawn to scale.

[0054] The reference numerals are as follows: 1. first dissolving kettle; 2. second dissolving kettle; 3. kettle reactor; 4. tubular reactor; 5. first discharge port; 6. second discharge port; 7. first stop valve; 8. first metering pump; 9. second stop valve; 10. second metering pump; 11. first feed port; 12. first overflow port; 13. second feed port; 14. pH control device; 15. third discharge port. DETAILED DESCRIPTION

[0055] Hereinafter, the continuous reaction system, ferromanganese carbonate precursor and its preparation method, lithium ferromanganese phosphate and its preparation method, positive electrode sheet, and battery implementation methods of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0056] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0057] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0058] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form a new technical solution, and such a technical solution should be deemed to be included in the disclosure of the present application.

[0059] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0060] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0061] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0062] If not otherwise specified, in this application, the terms "first", "second", "third", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.

[0063] In the present application, the terms "plurality" and "multiple" refer to two or more.

[0064] Unless otherwise specified, the terms used in this application have the commonly understood meanings that are commonly understood by those skilled in the art.

[0065] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured by various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise specified, the test temperature of each parameter is 25°C.

[0066] The embodiment of the present application provides a continuous reaction system for preparing a ferromanganese carbonate precursor.

[0067] like Figure 1 As shown, the continuous reaction system includes a first dissolving kettle 1, a second dissolving kettle 2, a kettle reactor 3 and a tubular reactor 4, and the kettle reactor 3 and the tubular reactor 4 are connected in series.

[0068] The first dissolving kettle 1 is used to contain the metal salt solution required for preparing the ferromanganese carbonate precursor, and the second dissolving kettle 2 is used to contain the precipitant solution required for preparing the ferromanganese carbonate precursor. The first dissolving kettle 1 has a first discharge port 5, and the second dissolving kettle 2 has a second discharge port 6.

[0069] The kettle reactor 3 has a first feed port 11 and a first overflow port 12. The first feed port 11 of the kettle reactor 3 is connected to the first dissolving kettle 1 and the second dissolving kettle 2 through the first pipeline and the second pipeline respectively, so that the kettle reactor 3 can contain the metal salt solution and the precipitant solution and mix them to produce a precipitation reaction to generate a first reaction liquid. The first pipeline is provided with a first stop valve 7 and a first metering pump 8 to adjust the flow rate of the metal salt solution. The second pipeline is provided with a second stop valve 9 and a second metering pump 10 to adjust the flow rate of the precipitant solution. The kettle reactor 3 is also connected to a pH control device 14 to monitor and adjust the pH value of the first reaction liquid.

[0070] The tubular reactor 4 has a second feed port 13 and a third discharge port 15. The second feed port 13 of the tubular reactor 4 is connected to the first overflow port 12 of the tank reactor 3 through a third pipeline, so that the tubular reactor 4 can accommodate the first reaction liquid from the tank reactor 3 and allow it to continue to precipitate to form a second reaction liquid. The third discharge port 15 of the tubular reactor 4 is used to allow the second reaction liquid to flow out. The tubular reactor 4 is also connected to one or more pH control devices 14 to monitor and adjust the pH value of the second reaction liquid.

[0071] The first feed port 11 is located at the bottom of the tank reactor 3 , and the first overflow port 12 is located at the top of the tank reactor 3 .

[0072] When preparing the ferromanganese carbonate precursor, the first stop valve 7 and the second stop valve 9 can both be kept in an open state, thereby ensuring continuous feeding and continuous discharging, so that multiple reactors can react simultaneously.

[0073] In some embodiments, the tubular reactor 4 is a horizontal tubular reactor. The horizontal tubular reactor can be formed by connecting a plurality of straight tubes and a plurality of U-shaped tubes.

[0074] In some embodiments, the first dissolving kettle 1 , the second dissolving kettle 2 , and the kettle reactor 3 are all provided with stirring devices.

[0075] In some embodiments, a heating device may be further provided in the kettle reactor 3 and the tubular reactor 4 to adjust the reaction temperature in the reactor according to actual needs. The location of the heating device may be adjusted according to actual needs, and the embodiments of the present application do not limit this.

[0076] The embodiment of the present application also provides a method for preparing a ferromanganese carbonate precursor using the continuous reaction system provided in the embodiment of the present application.

[0077] The method comprises at least the following steps.

[0078] like Figure 1 As shown, the tank reactor 3 and the tubular reactor 4 are connected in series, the tank reactor 3 has a first feed port 11 and a first overflow port 12, the first feed port 11 of the tank reactor 3 is connected to the first dissolving tank 1 and the second dissolving tank 2 through a first pipeline and a second pipeline respectively, the first pipeline is provided with a first stop valve 7 and a first metering pump 8, the second pipeline is provided with a second stop valve 9 and a second metering pump 10, the tank reactor 3 is also connected to a pH control device 14, the first dissolving tank 1 has a first discharge port 5, the second dissolving tank 2 has a second discharge port 6, the tubular reactor 4 has a second feed port 13 and a third discharge port 15, the second feed port 13 of the tubular reactor 4 is connected to the first overflow port 12 of the tank reactor 3 through a third pipeline, and the tubular reactor 4 is also connected to one or more pH control devices 14.

[0079] The metal salt solution required for preparing the ferromanganese carbonate precursor is added into the first dissolving kettle 1 , and the precipitant solution required for preparing the ferromanganese carbonate precursor is added into the second dissolving kettle 2 .

[0080] The metal salt solution in the first dissolving kettle 1 and the precipitant solution in the second dissolving kettle 2 are respectively transported to the kettle reactor 3 through the first pipe and the second pipe so that they are mixed and a precipitation reaction occurs to generate a first reaction liquid. When the liquid level of the first reaction liquid is higher than the first overflow port 12 of the kettle reactor 3, the first reaction liquid is transported to the tubular reactor 4, and then the first reaction liquid continues to precipitate in the tubular reactor 4 to form a second reaction liquid, and the second reaction liquid flows out through the third discharge port 15 of the tubular reactor 4.

[0081] The second reaction liquid obtained from the third discharge port 15 of the tubular reactor 4 is washed and dried to obtain a manganese iron carbonate precursor.

[0082] The existing reaction systems for preparing ferromanganese carbonate precursors mostly adopt a single reactor (aqueous reactor) or an intermittent production process with multiple reactors in parallel, so there is a defect of low production efficiency. In addition, when multiple reactors are used in parallel for production, it is necessary to switch between different reactors at regular intervals, which also has the defects of complicated production process and high labor cost.

[0083] The present application embodiment adopts Figure 1 The continuous reaction system shown is used to prepare a ferromanganese carbonate precursor. In the continuous reaction system provided in the embodiment of the present application, the kettle reactor and the tubular reactor are connected in series, and the two reactors can react at the same time, thereby ensuring continuous feeding and continuous discharging. Therefore, the preparation method of the ferromanganese carbonate precursor provided in the embodiment of the present application has the advantages of high production efficiency, high energy efficiency, simple process, easy operation and low labor cost, and is particularly suitable for large-scale industrial production.

[0084] In the process of intermittent preparation of ferromanganese carbonate precursor, the solubility product constant of ferromanganese carbonate is low and the precipitation rate is fast, which easily leads to problems such as wide particle size distribution of ferromanganese carbonate precursor particles, difficult to control particle size, and uneven element distribution.

[0085] The preparation method of the ferromanganese carbonate precursor provided in the embodiment of the present application is a continuous preparation method. In the continuous preparation process, the time of staying in the autoclave reactor and the tubular reactor during the growth of each ferromanganese carbonate precursor particle can be kept consistent. In addition, the premixing and rapid prenucleation of metal salt solution and precipitant solution mainly occur in the autoclave reactor. The tubular reactor and the autoclave reactor are connected in series, and the heat transfer area per unit volume of the tubular reactor is large, the reaction speed of the material in the tubular reactor is fast, the flow rate is fast, and the production capacity is high, and the residence time of the material in the tubular reactor is more equal, so the material concentration and chemical reaction speed at any point in the tubular reactor do not change with time, only with the tube length. Therefore, compared with making the reaction solution flow into another autoclave reactor connected in series from the autoclave reactor, after making the reaction solution flow into the tubular reactor from the autoclave reactor, it is possible to reduce the aggregation growth of crystal nuclei, and the ferromanganese carbonate precursor thus obtained can have the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystalline phase, uniform element distribution, and high batch consistency.

[0086] In the continuous preparation method of the ferromanganese carbonate precursor provided in the embodiment of the present application, the flow rate of the metal salt solution and the precipitant solution, the residence time of the ferromanganese carbonate precursor particles in each reactor during the growth process, the reaction temperature in each reactor, and the pH and other parameters can all be precisely adjusted. Therefore, the preparation method provided in the embodiment of the present application also has good production flexibility.

[0087] The residence time of the ferromanganese carbonate precursor particles in each reactor (a kettle reactor and a tubular reactor) during the growth process is negatively correlated with the flow rate of the metal salt solution and the precipitant solution, and positively correlated with the volume of each reactor. When the flow rate of the metal salt solution and the precipitant solution is high, the residence time of the ferromanganese carbonate precursor particles in each reactor is short; when the flow rate of the metal salt solution and the precipitant solution is low, the residence time of the ferromanganese carbonate precursor particles in each reactor is long; when the volume of each reactor is small, the residence time of the ferromanganese carbonate precursor particles in each reactor is short; when the volume of each reactor is large, the residence time of the ferromanganese carbonate precursor particles in each reactor is long. Therefore, the size of the ferromanganese carbonate precursor particles can be adjusted by adjusting the flow rate of the metal salt solution and the precipitant solution and the volume of each reactor.

[0088] The reaction temperature and / or pH of each reactor will also affect the morphology, crystallinity, particle size, particle size distribution and tap density of the obtained ferromanganese carbonate precursor. Therefore, the morphology, crystallinity, particle size, particle size distribution and tap density of the ferromanganese carbonate precursor can also be adjusted by adjusting the reaction temperature and / or pH of each reactor.

[0089] Therefore, the preparation method of the ferromanganese carbonate precursor provided in the embodiment of the present application can also flexibly adjust the particle size and morphology of the ferromanganese carbonate precursor, thereby facilitating meeting different production needs so as to prepare lithium iron manganese phosphate with different particle sizes.

[0090] The preparation method of the ferromanganese carbonate precursor provided in the embodiment of the present application is a coprecipitation reaction method, and the ferromanganese carbonate precursor obtained by the preparation method provided in the embodiment of the present application can also have a regular spherical (or quasi-spherical) morphology. The spherical (or quasi-spherical) morphology of the ferromanganese carbonate precursor is conducive to the lithium ions to penetrate the center of the ferromanganese carbonate precursor uniformly and synchronously from all directions through the micropores on the surface of the spherical (or quasi-spherical) particles during the subsequent sintering treatment of lithium iron manganese phosphate, and it helps to obtain lithium iron manganese phosphate with a spherical (or quasi-spherical) morphology and uniform distribution of various elements; in addition, a complete, uniform and firm carbon coating layer can also be formed, thereby improving the conductivity of the obtained lithium iron manganese phosphate.

[0091] In some embodiments, a complexing agent may also be added to the first dissolving kettle.

[0092] The complexing agent can complex metal ions to achieve the purpose of controlling free metal ions, thereby improving the precipitation conversion efficiency of metal ions and reducing the difference in precipitation rates of different metal ions in the reaction solution, thereby facilitating uniform coprecipitation. Therefore, when a complexing agent is also added to the first dissolving kettle, the preparation method of the ferromanganese carbonate precursor provided by the present application can obtain ferromanganese carbonate precursor particles with high purity (purity greater than 99.7%) and uniform element distribution, and the molar ratio of each metal element in the obtained ferromanganese carbonate precursor particles is less different from the molar ratio of each metal element in the raw material, which is conducive to further precise control of the metal element content and helps the ratio of the metal elements to better reach the preset value.

[0093] Alternatively, the complexing agent may include one or more of aminocarboxylates, hydroxycarboxylates, and organic phosphonates.

[0094] More optionally, the complexing agent may include one or more of sodium ethylenediaminetetramethylenephosphate, sodium ethylenediaminetetraacetate, sodium gluconate, and sodium citrate. This helps to obtain ferromanganese carbonate precursor particles with high purity and uniform element distribution, and the molar ratio of each metal element in the obtained ferromanganese carbonate precursor particles is less different from the molar ratio of each metal element in the raw material, which is conducive to further precise control of the metal element content and helps the ratio of the metal elements to better reach the preset value.

[0095] Optionally, the mass concentration of the complexing agent may be below 5 wt %, more preferably 1-5 wt %, based on the total mass of the metal salt solution.

[0096] In some embodiments, the reaction temperature in the tank reactor 3 may be less than or equal to the reaction temperature in the tube reactor 4 .

[0097] In some embodiments, the reaction temperature in the tank reactor 3 may be equal to the reaction temperature in the tube reactor 4 .

[0098] In some embodiments, the reaction temperature in the tank reactor 3 may be lower than the reaction temperature in the tubular reactor 4. Optionally, the difference between the reaction temperature in the tubular reactor 4 and the reaction temperature in the tank reactor 3 may be less than or equal to 20°C, and more preferably less than or equal to 15°C.

[0099] In the preparation method of the ferromanganese carbonate precursor provided in the embodiment of the present application, the kettle reactor and the tubular reactor are connected in series, and the reaction temperature in the kettle reactor is set to be less than or equal to the reaction temperature in the tubular reactor, so that different reactors in the continuous reaction system can mainly play different functions. The reaction temperature in the kettle reactor is low, so in the kettle reactor, the premixing and rapid prenucleation of the metal salt solution and the precipitant solution mainly occur; and the lower reaction temperature is also conducive to reducing the crystal nucleus aggregation growth in the first reaction solution, so that the metal ions and carbonate ions can also be coprecipitated to form a large number of crystal nuclei with uniform size and uniform element distribution, which is conducive to better growth and crystallization of the crystal nucleus in the tubular reactor. The reaction temperature in the tubular reactor is equal to or higher than the reaction temperature in the kettle reactor, so when the reaction solution flows from the kettle reactor into the tubular reactor, the equal or higher reaction temperature can provide enough energy to promote the further growth and crystallization of the crystal nucleus, and it is also conducive to improving the crystallinity of the formed ferromanganese carbonate precursor under the premise of reducing the crystal nucleus aggregation growth.

[0100] Therefore, by adjusting the reaction temperature in the autoclave reactor to be less than or equal to the reaction temperature in the tubular reactor, it is helpful to obtain ferromanganese carbonate precursor particles with narrow particle size distribution, uniform element distribution, high crystallinity and regular morphology.

[0101] In some embodiments, the reaction temperature in the autoclave reactor 3 may be 50-80° C. When the reaction temperature in the autoclave reactor is within the above range, it is beneficial for the metal ions and carbonate ions to precipitate rapidly, forming a large number of crystal nuclei, and also beneficial for reducing the precipitation rate difference of different metal ions during the precipitation reaction, thereby facilitating uniform co-precipitation of metal ions.

[0102] In some embodiments, the reaction temperature in the tubular reactor 4 may be 50-80° C. When the reaction temperature in the tubular reactor is within the above range, the ferromanganese carbonate grains grown in the autoclave reactor can be further grown and the crystallinity of the ferromanganese carbonate grains can be improved, thereby facilitating the acquisition of a ferromanganese carbonate precursor with high crystallinity and regular morphology.

[0103] In some embodiments, the concentration of the metal salt solution may be 0.5-2 mol / L, optionally 0.5-1 mol / L.

[0104] In some embodiments, the concentration of the precipitant solution may be 0.5-2 mol / L, optionally 0.5-1 mol / L.

[0105] In some embodiments, the molar ratio of the metal salt to the precipitant may be 1:1 to 1:2.

[0106] In some embodiments, the flow rate of the metal salt solution (or the pumping speed of the first metering pump) may be 0.5-4 L / min, and may be optionally 1-2 L / min.

[0107] In some embodiments, the flow rate of the precipitant solution (or the pumping speed of the second metering pump) may be 0.5-4 L / min, optionally 1-2 L / min.

[0108] In some embodiments, the flow rates of the metal salt solution and the precipitant solution may be the same (ie, the pumping speeds of the first metering pump and the second metering pump may be the same), thereby helping to improve the consistency of the obtained ferromanganese carbonate precursor particles.

[0109] In some embodiments, the volume of the autoclave reactor 3 may be smaller than the volume of the tubular reactor 4. The ferromanganese carbonate precursor particles stay in the tubular reactor for a longer time, which helps to make the obtained ferromanganese carbonate precursor particles have a narrower particle size distribution, and also helps to make the obtained ferromanganese carbonate precursor particles have a higher crystallinity and a more regular morphology.

[0110] In some embodiments, the volume ratio of the autoclave reactor 3 to the tubular reactor 4 may be 1:5-1:7. This helps to make the obtained ferromanganese carbonate precursor particles have both smaller particle size and narrower particle size distribution, and also helps to make the obtained ferromanganese carbonate precursor particles have higher crystallinity and more regular morphology.

[0111] In some embodiments, the residence time of the ferromanganese carbonate precursor in the autoclave reactor 3 during the growth process can be 0.5-4 hours. The residence time of the ferromanganese carbonate precursor in the autoclave reactor during the growth process is inversely proportional to the flow rate of the metal salt solution and the flow rate of the precipitant solution, and is proportional to the volume of the autoclave reactor.

[0112] In some embodiments, the residence time of the ferromanganese carbonate precursor in the tubular reactor 4 during the growth process can be 2.5-28 hours. The residence time of the ferromanganese carbonate precursor in the tubular reactor during the growth process is inversely proportional to the flow rate of the metal salt solution and the flow rate of the precipitant solution, and is proportional to the volume of the tubular reactor.

[0113] In some embodiments, during the reaction, a pH adjusting liquid can be added to the kettle reactor 3 by a pH control device 14 connected to the kettle reactor 3, so that the pH of the first reaction solution in the kettle reactor 3 is 6-8, optionally 7-7.5. When the pH in the kettle reactor is within the above range, it is conducive to the rapid precipitation of metal ions and carbonate ions to form a large number of crystal nuclei, and it is also conducive to reducing the precipitation rate difference of different metal ions during the precipitation reaction, so as to facilitate the uniform coprecipitation of metal ions. In addition, when the pH in the kettle reactor is within the above range, it is also conducive to forming a spherical (or spherical) morphology of ferromanganese carbonate precursor, and then it is also conducive to improving the tap density.

[0114] In some embodiments, during the reaction process, a pH regulating liquid can be added to the tubular reactor 4 through a pH control device 14 connected to the tubular reactor 4, so that the pH of the second reaction liquid in the tubular reactor 4 is 6-8, optionally 7-7.5. When the pH of the second reaction liquid in the tubular reactor is within the above range, it is beneficial to reduce the difference in precipitation rates of different metal ions during the precipitation reaction, thereby facilitating uniform coprecipitation of metal ions. In addition, when the pH in the tubular reactor is within the above range, it is also beneficial to form a spherical (or spherical) morphology of the ferromanganese carbonate precursor, which is also beneficial to improve the tap density.

[0115] The pH adjusting solution may include an acid solution (eg, dilute sulfuric acid) or an alkaline solution (eg, aqueous ammonia).

[0116] During the reaction, the first dissolving kettle 1, the second dissolving kettle 2 and the kettle reactor 3 can all be kept in a stirring state, thereby reducing the aggregation growth of the ferromanganese carbonate precursor particles and facilitating the acquisition of a ferromanganese carbonate precursor with a narrow particle size distribution and a high tap density.

[0117] In some embodiments, the stirring speed of the first dissolving kettle 1 can be 300-800 r / min. In some embodiments, the stirring speed of the second dissolving kettle 2 can be 300-800 r / min. In some embodiments, the stirring speed of the kettle reactor 3 can be 300-800 r / min.

[0118] In some embodiments, no stirring device is provided in the tubular reactor 4. Thus, the reaction liquid can flow in the form of plug flow, which is beneficial to the further growth of ferromanganese carbonate grains and the improvement of the crystallinity of ferromanganese carbonate grains, and further beneficial to obtaining a ferromanganese carbonate precursor with high crystallinity and regular morphology.

[0119] In some embodiments, during the reaction process, the first dissolving material kettle 1, the second dissolving material kettle 2, the kettle reactor 3 and the tubular reactor 4 may all be under a protective gas atmosphere. In some embodiments, the protective gas may include nitrogen, an inert gas or a combination thereof. Alternatively, the inert gas includes helium, argon or a combination thereof.

[0120] In some embodiments, the metal salts required for preparing the manganese ferrocarbonate precursor may include water-soluble divalent iron salts, water-soluble divalent manganese salts, and optional divalent salts of water-soluble doping elements M, where M represents the doping elements at the manganese and / or iron positions of the manganese ferrocarbonate precursor, optionally including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr.

[0121] In some embodiments, the water-soluble ferrous salt may include one or more of ferrous chloride, ferrous nitrate, ferrous sulfate, and ferrous acetate.

[0122] In some embodiments, the water-soluble divalent manganese salt may include one or more of manganous chloride, manganous nitrate, manganous sulfate, and manganous acetate.

[0123] In some embodiments, the divalent salt of the water-soluble doping element M may include one or more of hydrochloride, nitrate, sulfate, and acetate of the doping element M.

[0124] In some embodiments, the precipitating agent may include a carbonate, for example, may include one or more of ammonium bicarbonate, sodium bicarbonate, ammonium carbonate, and sodium carbonate.

[0125] In the preparation method of the ferromanganese carbonate precursor provided in the examples of the present application, unless otherwise specified, all raw materials can be directly purchased.

[0126] The embodiment of the present application also provides a ferromanganese carbonate precursor prepared by the above preparation method.

[0127] The ferromanganese carbonate precursor may have the chemical formula Fe x Mn y M 1-x-y CO3, 0<x<1, 0<y<1, 0≤1-xy<1, M represents the doping element at the manganese site and / or iron site of the manganese ferrocarbonate precursor.

[0128] Optionally, M includes one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr.

[0129] Optionally, 0.199≤x≤0.5.

[0130] Optionally, 0.499≤y≤0.8.

[0131] Optionally, 0<1-xy≤0.05.

[0132] The ferromanganese carbonate precursor provided in the embodiment of the present application is prepared by the above method, and therefore has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, uniform element distribution, and high batch consistency.

[0133] In some embodiments, the volume distribution particle sizes Dv90 and Dv50 of the manganese ferrocarbonate precursor satisfy 1<Dv90 / Dv50≤1.4.

[0134] The present application also provides a method for preparing lithium iron manganese phosphate.

[0135] The method comprises at least the following steps: uniformly mixing the ferromanganese carbonate precursor prepared by the above preparation method or the above ferromanganese carbonate precursor with a lithium source, a phosphorus source, an optional source of doping element N, an optional source of doping element Q and an optional source of doping element R to obtain a mixed raw material, wherein N represents the doping element at the lithium site of lithium iron manganese phosphate, optionally including one or more of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents the doping element at the phosphorus site of lithium iron manganese phosphate, optionally including one or more of B, S, Si and N; R represents the doping element at the oxygen site of lithium iron manganese phosphate, optionally including one or more of S, F, Cl and Br; sintering the obtained mixed raw material, and lithium iron manganese phosphate is obtained after the sintering process. Lithium iron manganese phosphate has the chemical formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n , M represents the doping element of the manganese site and / or iron site of the lithium iron manganese phosphate, optionally including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr; N represents the doping element of the lithium site of the lithium iron manganese phosphate, optionally including one or more of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents the doping element of the phosphorus site of the lithium iron manganese phosphate, optionally including one or more of B, S, Si and N; R represents the doping element of the oxygen site of the lithium iron manganese phosphate, Optionally includes one or more of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1, optionally, 0<b≤0.05; 0<x<1, optionally, 0.199≤x≤0.5; 0<y<1, optionally, 0.499≤y≤0.8; 0≤1-xy<1, optionally, 0<1-xy≤0.05; 0≤m≤0.1, optionally, 0<m≤0.05; 0≤n≤0.1, optionally, 0<n≤0.05.

[0136] The lithium manganese iron phosphate obtained by the preparation method provided in the embodiment of the present application can achieve a uniform mixture of lithium elements and multiple metal elements, thereby making lithium ions diffuse faster and more easily embedded in the lithium iron phosphate precursor, thereby enabling the prepared lithium manganese iron phosphate to have excellent electrochemical properties.

[0137] The lithium manganese iron phosphate obtained by the preparation method provided in the embodiment of the present application also has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, and high batch consistency, which is beneficial to improving the capacity and electrochemical properties of the battery, such as cycle performance and rate performance.

[0138] In some embodiments, a carbon source is also added to the mixed raw material, thereby preparing carbon-coated lithium manganese iron phosphate.

[0139] In some embodiments, the carbon source includes one or more of an organic carbon source and an inorganic carbon source, and may optionally include a combination of one or more of glucose, sucrose, starch, fructose, polyvinyl alcohol, polyethylene glycol, and citric acid.

[0140] In some embodiments, the lithium source may be a lithium-containing compound known in the art that can be used to prepare phosphate positive electrode active materials. For example, the lithium source may include one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, lithium hydrogen phosphate, lithium nitrate, and lithium acetate.

[0141] In some embodiments, the phosphorus source may be a phosphorus-containing compound known in the art for preparing a phosphate positive active material. For example, the phosphorus source may include one or more of phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate.

[0142] In some embodiments, the source of the doping element N may include one or more of sulfate, nitrate, hydrochloride, and acetate of the doping element N.

[0143] In some embodiments, the source of the doping element Q may include one or more of sulfates, borates, nitrates, and silicates of the doping element Q.

[0144] In some embodiments, the source of the doping element R may include one or more of a simple substance of the doping element R and an ammonium salt.

[0145] In some embodiments, the sintering process may include a pre-sintering process and a high temperature sintering process.

[0146] In some embodiments, the temperature of the pre-sintering process may be 350°C-550°C, and optionally 400°C-500°C.

[0147] In some embodiments, the pre-sintering treatment time may be 2-12 hours, and optionally 3-10 hours.

[0148] In some embodiments, the pre-sintering process can be performed under a protective gas atmosphere. In some embodiments, the protective gas can include nitrogen, an inert gas, or a combination thereof. Optionally, the inert gas includes helium, argon, or a combination thereof.

[0149] In some embodiments, the temperature of the high temperature sintering process may be 600°C-800°C, and optionally 650°C-750°C.

[0150] In some embodiments, the high temperature sintering treatment time may be 5-24 hours, and optionally 8-12 hours.

[0151] In some embodiments, the high temperature sintering process can be performed under a protective gas atmosphere. In some embodiments, the protective gas can include nitrogen, an inert gas, or a combination thereof. Optionally, the inert gas includes helium, argon, or a combination thereof.

[0152] In some embodiments, the pre-sintering process and the high temperature sintering process may be performed in a tube furnace.

[0153] The amount of each raw material added may conform to the stoichiometric ratio of the target product. In some embodiments, the amount of lithium source added may be slightly excessive, for example, 100%-110% of the theoretical mass of the lithium source, where the theoretical mass of the lithium source refers to the mass of the lithium source calculated based on the stoichiometric ratio of lithium iron manganese phosphate.

[0154] In the preparation method of lithium manganese iron phosphate provided in the embodiment of the present application, unless otherwise specified, all raw materials and instruments used can be purchased directly. Each raw material may contain crystal water or may not contain crystal water.

[0155] The present application also provides a lithium manganese iron phosphate prepared by the above method.

[0156] The lithium manganese iron phosphate provided in the embodiments of the present application has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystal phase, uniform element distribution, and high batch consistency, which is beneficial to improving the capacity and electrochemical properties of the battery, such as cycle performance and rate performance.

[0157] In some embodiments, the surface of the lithium iron manganese phosphate is further coated with carbon, thereby improving the conductivity of the lithium iron manganese phosphate.

[0158] The embodiment of the present application also provides a positive electrode sheet.

[0159] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0160] The positive electrode film layer includes the above-mentioned lithium iron manganese phosphate or the lithium iron manganese phosphate prepared by the above-mentioned preparation method. Of course, the positive electrode film layer may also include other positive electrode active materials, for example, it may also include lithium transition metal oxides and the like. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. The modified compound may be a doping modification and / or surface coating modification of the positive electrode active material.

[0161] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0162] In some embodiments, the positive electrode film layer may further include a positive electrode binder. The present application has no particular restrictions on the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0163] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0164] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, the optional positive electrode conductive agent, the optional positive electrode binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.

[0165] The embodiment of the present application also provides a battery.

[0166] The battery mentioned in the embodiments of the present application may be a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module or a battery pack.

[0167] A battery cell is the smallest unit of a battery, which can independently realize the functions of charging and discharging. The battery cell can be cylindrical, rectangular or in other shapes, etc., which is not limited in the embodiments of the present application.

[0168] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed connection through a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a case and battery cells, and the battery cells or battery modules are accommodated in the case. In some embodiments, the case may serve as part of the chassis structure of the vehicle. For example, part of the case may become at least a part of the floor of the vehicle, or part of the case may become at least a part of the crossbeam and longitudinal beam of the vehicle.

[0169] In some embodiments, the battery may be an energy storage device, which includes an energy storage container, an energy storage cabinet, and the like.

[0170] The battery cells mentioned in the embodiments of the present application include lithium-ion battery cells, lithium metal battery cells, negative electrode-free lithium metal battery cells, etc., which are not limited in the embodiments of the present application.

[0171] The battery cell includes an electrode assembly and an electrolyte. The electrode assembly can be a winding structure or a stacked structure, which is not limited in the present application.

[0172] The battery cell also includes an outer package, which can be used to encapsulate the electrode assembly and the electrolyte. The outer package can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS).

[0173] The battery cell includes the above-mentioned positive electrode sheet. The battery cell also includes a negative electrode sheet. The structure and composition of the negative electrode sheet can be selected according to the type of the battery cell, and the embodiment of the present application does not limit this.

[0174] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0175] The negative electrode active material may adopt materials known in the art. As an example, the negative electrode active material may include, but is not limited to, one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials may also be used.

[0176] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent. As an example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0177] In some embodiments, the negative electrode film layer may further include a negative electrode binder. The present application has no particular restrictions on the type of negative electrode binder. As an example, the negative electrode binder may include styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS). One or more.

[0178] In some embodiments, the negative electrode film layer may further include other additives. As an example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.

[0179] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0180] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional negative electrode conductive agent, optional negative electrode binder, other optional auxiliary agents, etc. in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0181] The negative electrode sheet does not exclude other additional functional layers besides the negative electrode film layer. For example, in some embodiments, the negative electrode sheet may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode sheet may further include a protective layer covering the surface of the negative electrode film layer.

[0182] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a metal layer disposed on at least one surface of the negative electrode current collector, and the metal layer may include one or more of lithium single substance and lithium alloy.

[0183] The lithium alloy may be an alloy formed by metallic lithium and other metallic elements or non-metallic elements. As an example, the other metallic elements in the lithium alloy may include one or more of tin, zinc, aluminum, magnesium, silver, gold, gallium, indium, and platinum, and the non-metallic elements in the lithium alloy may include one or more of boron, carbon, and silicon.

[0184] In some embodiments, the negative electrode sheet may further include a negative electrode current collector but not a metal layer, thereby forming a negative electrode metal-free battery cell.

[0185] In some embodiments, the negative electrode sheet may also be directly made of a sheet (or foil) of lithium or a lithium alloy.

[0186] The battery cell includes an electrolyte. The electrolyte plays a role in conducting active ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can include one or more of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte).

[0187] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0188] As an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0189] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the solvent may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE) One or more.

[0190] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature power performance.

[0191] Battery cells using electrolytes and some battery cells using solid electrolytes also include a separator. The separator is arranged between the positive electrode and the negative electrode, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The present application has no particular restrictions on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0192] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different.

[0193] The preparation method of battery cells is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the above-mentioned electrolyte is injected after drying. After vacuum packaging, standing, formation, shaping and other processes, a battery cell is obtained. Multiple battery cells can also be further connected in series, in parallel or in mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.

[0194] The embodiment of the present application also provides an electrical device, which includes the battery of the present application. The battery can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0195] The electrical device can select a specific type of battery, such as a battery cell, a battery module or a battery pack, according to its usage requirements.

[0196] As an example, the electric device may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used as a power source.

[0197] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a battery cell may be used as a power source.

[0198] Example

[0199] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present application will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0200] Example 1

[0201] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0202] A 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle, and 3% of ethylenediaminetetramethylene phosphate sodium is added; a 2 mol / L sodium carbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 400 r / min.

[0203] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 400 r / min. The reaction temperature in the reactor was 55°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 55°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH control device in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0204] After reacting in the horizontal tubular reactor for 12 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0205] Example 2

[0206] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0207] A 1 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle, and 3% of the complexing agent sodium ethylenediaminetetraacetate is added; a 1 mol / L sodium bicarbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 2L / min. Both the first dissolving kettle and the second dissolving kettle are kept in a nitrogen-filled and stirred state, and the stirring speed is 600r / min.

[0208] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 600 r / min. The reaction temperature in the reactor was 60°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 1 hour of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 60°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH controller in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0209] After reacting in the horizontal tubular reactor for 6 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0210] Example 3

[0211] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0212] A manganese sulfate / ferrous sulfate mixed metal salt solution with a concentration of 1 mol / L (the molar ratio of manganese to iron is 7:3) is prepared in the first dissolving kettle, and 3 wt% of the complexing agent sodium gluconate is added, and an ammonium bicarbonate aqueous solution with a concentration of 1 mol / L is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 600 r / min.

[0213] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 600 r / min. The reaction temperature in the reactor was 70°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 70°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH controller in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0214] After reacting in the horizontal tubular reactor for 12 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0215] Example 4

[0216] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0217] A manganese sulfate / ferrous sulfate mixed metal salt solution with a concentration of 0.5 mol / L (the molar ratio of manganese: iron: cobalt elements is 7:2.9:0.1) is prepared in the first dissolving kettle, and 3%wt of the complexing agent sodium citrate is added, and a 0.5 mol / L ammonium bicarbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 700 r / min.

[0218] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 700 r / min, a reaction temperature of 70°C, and a pH value of 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 70°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH controller in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0219] After reacting in the horizontal tubular reactor for 12 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0220] Example 5

[0221] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0222] A manganese sulfate / ferrous sulfate mixed metal salt solution (the molar ratio of manganese: iron element is 6:4) with a concentration of 1 mol / L is prepared in the first dissolving kettle, and 3 wt% of the complexing agent sodium ethylenediaminetetraacetate is added, and a sodium bicarbonate aqueous solution with a concentration of 1.2 mol / L is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 2 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 600 r / min.

[0223] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 600 r / min. The reaction temperature in the reactor was 60°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 1 hour of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 60°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH controller in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0224] After reacting in the horizontal tubular reactor for 6 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0225] Example 6

[0226] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0227] A 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle; a 2 mol / L sodium carbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. Both the first dissolving kettle and the second dissolving kettle are kept in a nitrogen-filled and stirred state, and the stirring speed is 400 r / min.

[0228] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 400 r / min. The reaction temperature in the reactor was 55°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 55°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH control device in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0229] After reacting in the horizontal tubular reactor for 12 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0230] Example 7

[0231] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0232] A 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle, and 3% of ethylenediaminetetramethylene phosphate sodium is added; a 2 mol / L sodium carbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 400 r / min.

[0233] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 400 r / min. The reaction temperature in the reactor was 55°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 55°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH control device in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0234] After reacting in the horizontal tubular reactor for 10 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a manganese ferrocarbonate precursor.

[0235] Example 8

[0236] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0237] A 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle, and 3% of ethylenediaminetetramethylene phosphate sodium is added; a 2 mol / L sodium carbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 400 r / min.

[0238] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 400 r / min. The reaction temperature in the reactor was 55°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 55°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH control device in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0239] After reacting in the horizontal tubular reactor for 14 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0240] Example 9

[0241] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0242] A 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle, and 3% of ethylenediaminetetramethylene phosphate sodium is added; a 2 mol / L sodium carbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 400 r / min.

[0243] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 400 r / min. The reaction temperature in the reactor was 55°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 55°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH control device in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0244] After reacting in the horizontal tubular reactor for 16 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0245] Example 10

[0246] use Figure 1 The continuous reaction system shown is used to prepare ferromanganese carbonate precursor.

[0247] A 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) is prepared in the first dissolving kettle, and 3% of ethylenediaminetetramethylene phosphate sodium is added; a 2 mol / L sodium carbonate aqueous solution is prepared in the second dissolving kettle. The metal salt aqueous solution and the sodium carbonate aqueous solution are continuously injected from the first dissolving kettle and the second dissolving kettle into the kettle reactor through two liquid inlet pipes, and the flow rate of the two liquid inlet pipes is 1 L / min. The first dissolving kettle and the second dissolving kettle are both kept in a nitrogen-filled and stirred state, and the stirring speed is 400 r / min.

[0248] The reactor was kept in a nitrogen-filled and stirred state, with a stirring speed of 400 r / min. The reaction temperature in the reactor was 55°C and the pH value was 7.5 (ammonia or dilute sulfuric acid can be added during the reaction to adjust the pH). In the reactor, manganese iron metal ions and carbonate ions quickly formed manganese iron carbonate precipitation and formed a large number of crystals. After 2 hours of reaction, the liquid level of the reactor was higher than the first overflow port, and the reaction liquid flowed out of the first overflow port and entered the horizontal tubular reactor to continue the precipitation reaction. During the precipitation reaction, nitrogen was kept in the horizontal tubular reactor, and the reaction temperature in the horizontal tubular reactor was kept at 55°C by controlling the external heat exchanger. The pH value of the reaction liquid was monitored by the pH control device in each pipeline area, and the pH value in the reactor was kept at 7.5.

[0249] After reacting in the horizontal tubular reactor for 8 hours (i.e., the time from when the reaction liquid enters the horizontal tubular reactor to when it flows out of the horizontal tubular reactor), the reaction liquid flows out from the third discharge port. The obtained reaction liquid is filtered and washed multiple times by a filter press, and then the washed material is transferred to a dryer and dried at 120° C. for 6 hours to obtain a ferromanganese carbonate precursor.

[0250] Comparative Example 1

[0251] Prepare a 2 mol / L manganese sulfate / ferrous sulfate mixed metal salt aqueous solution (the molar ratio of manganese: iron is 6:4) and a 2 mol / L sodium carbonate aqueous solution. Inject the metal salt aqueous solution and the sodium carbonate aqueous solution into the reactor at the same time, start rapid stirring, the stirring speed is 400r / min, the reaction temperature in the reactor is 55°C, the reaction time is 14h, and it is naturally cooled to room temperature after the end. The slurry is discharged from the discharge port of the reactor, filtered and washed by a filter press for multiple times, and then the washed material is transferred to a dryer and dried at 120°C for 6h to obtain a manganese ferrocarbonate precursor.

[0252] Test Section

[0253] (1) Volume distribution particle size Dv50 and Dv90 test

[0254] The volume distribution particle size of the ferromanganese carbonate precursor prepared above was tested using a Malvern Master Size 3000 laser particle size analyzer. Dv50 and Dv90 refer to the particle sizes corresponding to when the cumulative volume distribution percentage of the material reaches 50% and 90%. The test basis can refer to GB / T 19077-2016.

[0255] (2) Mn / Fe molar ratio test

[0256] The contents of manganese and iron in the ferromanganese carbonate precursor prepared above were tested by ICP-OES using a Plasma 3000 inductively coupled plasma optical emission spectrometer and their molar ratios were calculated.

[0257] The contents of manganese and iron in the ferromanganese carbonate precursor are measured by an inductively coupled plasma optical emission spectrometer, such as Plasma 3000, using an ICP-OES method and calculating their molar ratio.

[0258] (3) Tap density test

[0259] The tap density test method and steps can refer to GB / T5162-2006. The test instrument can be Dandong Better BT-311 tap density tester.

[0260] Table 1

[0261]

[0262] Figure 2 The scanning electron microscope (SEM) image of the ferromanganese carbonate precursor prepared in Example 1 is shown. Figure 2 The magnification of a is 2000 times. Figure 2 The magnification of b is 5000 times.

[0263] Figure 3 The scanning electron microscope (SEM) image of the ferromanganese carbonate precursor prepared in Comparative Example 1 is shown. Figure 3 The magnification of a is 2000 times. Figure 3 The magnification of b is 5000 times.

[0264] Comprehensive test results in Table 1 and Figure 2 It can be seen that the ferromanganese carbonate precursor prepared by the continuous preparation method provided in the embodiment of the present application has the advantages of small particle size, narrow particle size distribution, regular morphology, etc.

[0265] Comprehensive test results in Table 1 and Figure 3 It can be seen that the ferromanganese carbonate precursor prepared by the existing intermittent preparation method has a large particle size and a wide particle size distribution.

[0266] Based on the test results of Example 1, Example 6 and Comparative Example 1, it can be seen that the Mn / Fe molar ratio in the ferromanganese carbonate precursor particles prepared by the continuous preparation method provided in the embodiment of the present application is smaller than the Mn / Fe molar ratio in the metal salt solution, which is conducive to achieving precise control of the content of manganese and iron elements. Based on the test results of Example 1, Example 6 and Comparative Example 1, it can also be seen that when a complexing agent is also added to the first dissolving kettle, it is helpful to further accurately control the content of manganese and iron elements in the prepared ferromanganese carbonate precursor particles.

[0267] Based on the test results of Example 1 and Examples 7-10, it can be seen that the particle size and particle size distribution of the obtained ferromanganese carbonate precursor particles can be adjusted by adjusting the volume ratio of the autoclave reactor and the tubular reactor (ie, the reaction time ratio).

[0268] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A continuous reaction system for preparing a ferromanganese carbonate precursor, wherein: The continuous reaction system comprises a first dissolving kettle, a second dissolving kettle, a kettle reactor and a tubular reactor, wherein the kettle reactor and the tubular reactor are connected in series; The first dissolving kettle is used to contain the metal salt solution required for preparing the ferromanganese carbonate precursor, and the second dissolving kettle is used to contain the precipitant solution required for preparing the ferromanganese carbonate precursor. The first dissolving kettle has a first discharge port, and the second dissolving kettle has a second discharge port. The tank reactor has a first feed port and a first overflow port. The first feed port of the tank reactor is connected to the first dissolving tank and the second dissolving tank through a first pipeline and a second pipeline respectively, so that the tank reactor can contain the metal salt solution and the precipitant solution and mix them to generate a first reaction solution by precipitation reaction. The first pipeline is provided with a first stop valve and a first metering pump to adjust the flow rate of the metal salt solution. The second pipeline is provided with a second stop valve and a second metering pump to adjust the flow rate of the precipitant solution. The tank reactor is also connected to a pH control device to monitor and adjust the pH value of the first reaction solution. The tubular reactor has a second feed port and a third discharge port. The second feed port of the tubular reactor is connected to the first overflow port of the tank reactor through a third pipeline, so that the tubular reactor can accommodate the first reaction liquid from the tank reactor and continue to precipitate it to form a second reaction liquid. The third discharge port of the tubular reactor is used to allow the second reaction liquid to flow out. The tubular reactor is also connected to one or more pH control devices to monitor and adjust the pH value of the second reaction liquid.

2. The continuous reaction system according to claim 1, wherein: The tubular reactor is a horizontal tubular reactor.

3. A method for preparing a ferromanganese carbonate precursor by the continuous reaction system according to claim 1 or 2, comprising at least the following steps: Connecting a tank reactor and a tubular reactor in series, wherein the tank reactor has a first feed port and a first overflow port, the first feed port of the tank reactor is communicated with a first dissolving material kettle and a second dissolving material kettle through a first pipeline and a second pipeline respectively, the first pipeline is provided with a first stop valve and a first metering pump, the second pipeline is provided with a second stop valve and a second metering pump, the tank reactor is also connected to a pH control device, the first dissolving material kettle has a first discharge port, the second dissolving material kettle has a second discharge port, the tubular reactor has a second feed port and a third discharge port, the second feed port of the tubular reactor is communicated with the first overflow port of the tank reactor through a third pipeline, and the tubular reactor is also connected to one or more pH control devices; Adding a metal salt solution required for preparing a ferromanganese carbonate precursor into the first dissolving kettle, and adding a precipitant solution required for preparing a ferromanganese carbonate precursor into the second dissolving kettle; The metal salt solution in the first dissolving kettle and the precipitant solution in the second dissolving kettle are respectively transported to the kettle reactor through the first pipeline and the second pipeline to mix them and then undergo precipitation reaction to generate a first reaction liquid; when the liquid level of the first reaction liquid is higher than the first overflow port of the kettle reactor, the first reaction liquid is transported to the tubular reactor, and then the first reaction liquid continues to precipitate in the tubular reactor to form a second reaction liquid, and the second reaction liquid flows out through the third discharge port of the tubular reactor; The second reaction liquid obtained from the third discharge port of the tubular reactor is subjected to washing and drying treatments to obtain a manganese iron carbonate precursor.

4. The method according to claim 3, wherein: A complexing agent is also added to the first dissolving kettle. Optionally, the complexing agent includes one or more of aminocarboxylates, hydroxycarboxylates and organic phosphonates. More optionally, the complexing agent includes one or more of sodium ethylenediaminetetramethylenephosphate, sodium ethylenediaminetetraacetate, sodium gluconate, and sodium citrate.

5. The method according to claim 3 or 4, wherein: The reaction temperature in the kettle reactor is less than or equal to the reaction temperature in the tubular reactor; Optionally, the reaction temperature in the autoclave reactor is 50-80° C.; and / or, Optionally, the reaction temperature in the tubular reactor is 50-80°C.

6. The method according to any one of claims 3 to 5, wherein: The volume of the kettle reactor is smaller than the volume of the tubular reactor. Optionally, the ratio of the volume of the autoclave reactor to the volume of the tubular reactor is 1:5-1:

7.

7. The method according to any one of claims 3 to 6, wherein: The residence time of the ferromanganese carbonate precursor in the autoclave reactor during the growth process is 0.5-4h; and / or, The residence time of the ferromanganese carbonate precursor in the tubular reactor during the growth process is 2.5-28 hours.

8. The method according to any one of claims 3 to 7, wherein: The concentration of the metal salt solution is 0.5-2 mol / L; and / or, The concentration of the precipitant solution is 0.5-2 mol / L; and / or, The molar ratio of the metal salt to the precipitant is 1:1-1:2; and / or, The flow rate of the metal salt solution is 0.5-4 L / min; and / or, The flow rate of the precipitant solution is 0.5-4 L / min; and / or, The flow rates of the metal salt solution and the precipitant solution are the same.

9. The method according to any one of claims 3 to 8, wherein: The method further comprises the steps of: During the reaction, a pH regulating liquid is added into the tank reactor through a pH control device connected to the tank reactor, so that the pH of the first reaction liquid in the tank reactor is 6-8, and can be 7-7.5; and / or, During the reaction, a pH regulating liquid is added into the tubular reactor through a pH control device connected to the tubular reactor, so that the pH of the second reaction liquid in the tubular reactor is 6-8, and can be 7-7.

5.

10. The method according to any one of claims 3 to 9, wherein: During the reaction, the first dissolving kettle, the second dissolving kettle, the kettle reactor and the tubular reactor are all placed under a protective gas atmosphere; and / or, During the reaction, the first dissolving kettle, the second dissolving kettle and the kettle reactor are all kept in a stirring state. Optionally, the stirring speed of the first dissolving kettle is 300-800 r / min; and / or, Optionally, the stirring speed of the second dissolving kettle is 300-800 r / min; and / or, Optionally, the stirring speed of the tank reactor is 300-800 r / min.

11. The method according to any one of claims 3 to 10, wherein: The metal salt required for preparing the ferromanganese carbonate precursor includes a water-soluble divalent iron salt, a water-soluble divalent manganese salt, and an optional divalent salt of a water-soluble doping element M, where M represents a doping element at the manganese position and / or iron position of the ferromanganese carbonate precursor, and optionally includes one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr; Optionally, the water-soluble divalent iron salt includes one or more of ferrous chloride, ferrous nitrate, ferrous sulfate, and ferrous acetate; and / or, Optionally, the water-soluble divalent manganese salt includes one or more of manganous chloride, manganous nitrate, manganous sulfate, and manganous acetate; and / or, Optionally, the divalent salt of the water-soluble doping element M includes one or more of hydrochloride, nitrate, sulfate and acetate of the doping element M.

12. The method according to any one of claims 3 to 11, wherein: The precipitating agent comprises a carbonate, optionally comprising one or more of ammonium bicarbonate, sodium bicarbonate, ammonium carbonate and sodium carbonate.

13. The method according to any one of claims 3 to 12, wherein: The protective gas includes nitrogen, an inert gas or a combination thereof.

14. A ferromanganese carbonate precursor prepared by the method according to any one of claims 3 to 13, having a chemical formula of Fe x Mn y M 1-x-y CO3, 0<x<1, optionally, 0.199≤x≤0.5; 0<y<1, optionally, 0.499≤y≤0.8; 0≤1-xy<1, optionally, 0<1-xy≤0.05; M represents the doping element at the manganese site and / or iron site of the ferromanganese carbonate precursor, and optionally includes one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr.

15. The ferromanganese carbonate precursor according to claim 14, wherein The volume distribution particle sizes Dv90 and Dv50 of the manganese ferrocarbonate precursor satisfy 1<Dv90 / Dv50≤1.

4.

16. A method for preparing lithium manganese iron phosphate, comprising at least the following steps: The ferromanganese carbonate precursor prepared by the method according to any one of claims 3 to 13 or the ferromanganese carbonate precursor according to any one of claims 14 to 15 is uniformly mixed with a lithium source, a phosphorus source, an optional source of a doping element N, an optional source of a doping element Q and an optional source of a doping element R to obtain a mixed raw material, in, N represents a doping element at the lithium site of the lithium iron manganese phosphate, optionally including one or more of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a doping element at the phosphorus site of the lithium iron manganese phosphate, optionally including one or more of B, S, Si and N; R represents a doping element at the oxygen site of the lithium iron manganese phosphate, optionally including one or more of S, F, Cl and Br; The obtained mixed raw material is subjected to sintering treatment, and the lithium manganese iron phosphate is obtained after sintering. Wherein, the lithium manganese iron phosphate has a chemical formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n , M represents a doping element at the manganese site and / or the iron site of the lithium manganese iron phosphate, and may optionally include one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr; N represents a doping element for the lithium site of the lithium iron manganese phosphate, and may optionally include one or more of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a doping element at the phosphorus position of the lithium manganese iron phosphate, and may optionally include one or more of B, S, Si and N; R represents the doping element of the oxygen position of the lithium manganese iron phosphate, and optionally includes one or more of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1, optionally, 0<b≤0.05; 0<x<1, optionally, 0.199≤x≤0.5; 0<y<1, optionally, 0.499≤y≤0.8; 0≤1-xy<1, optionally, 0<1-xy≤0.05; 0≤m≤0.1, optionally, 0<m≤0.05; 0≤n≤0.1, optionally, 0<n≤0.

05.

17. The method according to claim 16, wherein: A carbon source is also added to the mixed raw material.

18. Lithium manganese iron phosphate prepared by the method according to claim 16 or 17.

19. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein: The positive electrode film layer includes lithium manganese iron phosphate prepared by the method described in claim 16 or 17 or the lithium manganese iron phosphate described in claim 18.

20. A battery comprising the positive electrode sheet according to claim 19.

Citation Information

Patent Citations

  • Preparation method of large-particle precursor for lithium ion battery anode material

    CN108264097A

  • Narrow-distribution small-particle-size high-nickel ternary precursor prepared by continuous reactor system and method thereof

    CN115745017A

  • Manganese-iron-titanium phosphate positive electrode material as well as preparation method and application thereof

    CN115947329A

  • Manganese ammonium ferrous phosphate precursor as well as preparation method and application thereof

    CN115991464A

  • A system for continuous production of nickel-cobalt-manganese precursors

    CN209169292U