Medium-entropy rare earth tantalate ceramic as well as preparation method and application thereof

Through the preparation of medium-entropy rare earth tantalate ceramic materials, the lack of performance of existing thermal barrier coating materials at high temperatures is solved, and low thermal conductivity, high thermal expansion coefficient and high fracture toughness are achieved. It is suitable for hot end components of aircraft engines Surface coating.

CN119059813AActive Publication Date: 2024-12-03KUNMING UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411176985.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing thermal barrier coating materials have problems such as phase change, high thermal conductivity, small thermal expansion coefficient and low fracture toughness at high temperatures, which limit the temperature upper limit and performance of aircraft engines.

Method used

The medium-entropy rare earth tantalate ceramic material Y1-x/2Ta1-x/2MxO4 is prepared by ball milling and sintering processes to regulate the doping amount of Ti, Hf and Zr, reduce thermal conductivity, improve thermal expansion coefficient and fracture toughness.

Benefits of technology

Low thermal conductivity, excellent thermal insulation performance, high thermal expansion coefficient and high fracture toughness at high temperatures are achieved, reducing the expansion stress and resistance of external impact of the surface coating of the hot end components of the aircraft engine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059813A_ABST
    Figure CN119059813A_ABST
Patent Text Reader

Abstract

The invention discloses medium-entropy rare earth tantalate ceramic as well as a preparation method and application thereof. The chemical formula of the medium-entropy rare earth tantalate ceramic is Y < 1-x > / 2Ta < 1-x > / 2M < x > O < 4 >, wherein X is more than 0 and less than 0.8, M is Ti, Hf and Zr, and the molar content of each element in M is equal. The preparation method comprises the following steps: weighing corresponding Y2O3 powder, Ta2O5 powder, HfO2 powder, TiO2 powder and ZrO2 powder, adding a solvent, mixing, carrying out ball milling by adopting a planetary ball mill, sieving, compacting in a mold, and sintering. The medium-entropy rare earth tantalate ceramic provided by the invention is simple in raw material component, relatively low in heat conductivity at high temperature, good in heat insulation performance and relatively high in thermal expansion coefficient at high temperature, so that when the powder of the medium-entropy rare earth tantalate ceramic is used as a thermal barrier coating, the expansion stress between the powder and a base material (or a bonding layer) is reduced, and cracks are reduced. In addition, due to the excellent fracture toughness, the coating can well resist external impact during service, and the coating has wide application prospects in the aspect of aero-engine hot end component surface coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic coatings, and in particular relates to a medium-entropy rare earth tantalate ceramic and a preparation method and application thereof. Background Art

[0002] With the further development of the aerospace industry, the development direction of aircraft engines is gradually moving towards high flow ratio, high thrust-to-weight ratio and high inlet temperature. It is reported that the intake temperature of the most advanced aircraft engines has exceeded 1700℃, and it is expected that the temperature may exceed 2000℃ in the future. However, the effective operating temperature of aircraft engine turbine blades is much lower than the actual operating temperature of the combustion chamber, which greatly limits the development of aircraft engines. Thermal barrier coatings play an irreplaceable role in the development of temperature bearing capacity. The use of thermal barrier coatings can significantly increase the upper temperature limit of aircraft engines, which is comparable to the increase brought about by the development of high-temperature alloys in the past few decades.

[0003] YSZ, RE2Zr2O7 and RE3TaO7 are widely used thermal barrier coating materials. However, when the temperature is higher than 1200℃, YSZ will undergo phase change, which makes the use temperature of YSZ lower (≦1200℃), and the thermal conductivity of YSZ is relatively high; RE3TaO7 and RE2Zr2O7 have problems such as small thermal expansion coefficient and low fracture toughness. The performance can be improved by doping modification of RE and Ta positions, but it still cannot meet the requirements. This urgently requires the emergence of new materials that can replace the above-mentioned ceramic materials for thermal barrier coatings. Rare earth tantalate (YTaO4) has attracted attention due to its low thermal conductivity, ferroelastic phase transition, high temperature stability and other properties. However, the research on YTaO4 mainly focuses on theoretical calculations of its crystal structure and luminescence properties. In recent years, a large number of research and experimental conclusions by researchers have provided a theoretical basis for the application of YTaO4 in thermal barrier coatings.

[0004] In order to better apply YTaO4 in the field of thermal barrier coatings, it is necessary to further reduce thermal conductivity, improve thermal expansion coefficient, hardness, fracture toughness and other thermophysical and mechanical properties. Summary of the invention

[0005] The first object of the present invention is to provide a medium-entropy rare earth tantalate ceramic, and the second object of the present invention is to provide a method for preparing the medium-entropy rare earth tantalate ceramic.

[0006] The first object of the present invention is achieved by providing a medium entropy rare earth tantalate ceramic having a chemical formula of Y 1-x / 2Ta 1-x / 2 M x O4; wherein, 0<X<0.8, M is Ti, Hf, Zr, and the molar content of each element in M ​​is equal.

[0007] The second object of the present invention is achieved by the method for preparing the medium entropy rare earth tantalate ceramics according to the following steps: 1) Weigh the raw materials according to the ratio: Y2O3 powder, Ta2O5 powder, HfO2 powder, TiO2 powder and ZrO2 powder, add solvent and use planetary ball mill for ball milling, the ball milling time is 24-36h, the ball mill speed is 600-1000r / min; the solvent is ethanol or distilled water; 2) drying the powder obtained by ball milling in step 1), passing it through a 100-200 mesh sieve, pre-calcining it in a muffle furnace at 1000-1200° C. for 5-10 hours, and then passing it through a 300-600 mesh sieve; 3) The sieved powder obtained in step 2) is placed in a mold, compacted, and then sintered at 1500-1700° C. for 5-7 hours to obtain the target tantalate ceramic.

[0008] The medium-entropy rare earth tantalate ceramic is used in the surface coating of the hot end components of an aero-engine.

[0009] The entropy rare earth tantalate ceramics of the present invention include a chemical formula of Y 1-x / 2 Ta 1-x / 2 M x O4; where 0<X<0.8 (when X>0.8, a large amount of second phases will be generated, and these second phases gather at the grain boundaries, making the prepared tantalate material embrittled at the grain boundaries, resulting in reduced performance.) M is a mixture of three metal cations, Ti, Hf, and Zr, and different metal cations have the same molar content. Since the sum of the radii of the three metal cations of Ti, Hf, and Zr is approximately equal to twice the sum of the radii of a Y ion and a Ta ion, in order to maintain the electrical neutrality of the compound, the three metal cations of Ti, Hf, and Zr simultaneously replace the Y ions and Ta ions and enter the lattice of the tantalate. By regulating the content of the three metal cations of Ti, Hf, and Zr entering the lattice of the tantalate, the configuration entropy and lattice parameters a, b, and c of the lattice are further regulated, so that the phase structure of the tantalate changes, so that the tantalate material has better performance.

[0010] The beneficial effects of the present invention are as follows: the raw material composition of the medium-entropy rare earth tantalate ceramic provided by the present invention is simple, its thermal conductivity at high temperature is low, and it exhibits good thermal insulation performance. At the same time, the thermal expansion coefficient at high temperature is high, so that when its powder is used as a thermal barrier coating, the expansion stress with the base material (or bonding layer) is reduced, and cracking is reduced. In addition, its excellent fracture toughness enables it to resist external impact well during service, and has broad application prospects in the surface coating of the hot end components of aviation engines. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1The XRD patterns of the tantalate ceramics prepared in Examples 1 to 4 of the present invention; Figure 2 This is a SEM image of the tantalate ceramic prepared in Example 4 of the present invention; Figure 3 The thermal conductivity diagram of tantalate ceramics prepared in Examples 1 to 4 of the present invention and Comparative Example 1; Figure 4 This is a graph of thermal expansion coefficients of tantalate ceramics prepared in comparative example 1 of examples 1 to 4 of the present invention. DETAILED DESCRIPTION

[0012] The present invention is further described below, but the present invention is not limited in any way. Any changes made based on the present invention belong to the protection scope of the present invention.

[0013] The present invention discloses a medium entropy rare earth tantalate ceramic, whose chemical formula is Y 1-x / 2 Ta 1-x / 2 M x O4; wherein, 0<X<0.8, M is Ti, Hf, Zr, and the molar content of each element in M ​​is equal.

[0014] The thermal conductivity of the medium-entropy rare earth tantalate ceramic at 900°C is 1.23-1.42 W·m -1 ·K -1 , the thermal expansion coefficient at 1400°C is 9.8-10.4 × 10 -6 K -1 ; Its fracture toughness is 4.7-5.2MPam 0.5 .

[0015] The present invention also provides a method for preparing the medium-entropy rare earth tantalate ceramic, which is achieved by the following steps: 1) Weigh the raw materials according to the ratio: Y2O3 powder, Ta2O5 powder, HfO2 powder, TiO2 powder and ZrO2 powder, add solvent and use planetary ball mill for ball milling, the ball milling time is 24-36h, the ball mill speed is 600-1000r / min; the solvent is ethanol or distilled water; 2) drying the powder obtained by ball milling in step 1), passing it through a 100-200 mesh sieve, pre-calcining it in a muffle furnace at 1000-1200° C. for 5-10 hours, and then passing it through a 300-600 mesh sieve; 3) The sieved powder obtained in step 2) is placed in a mold, compacted, and then sintered at 1500-1700° C. for 5-7 hours to obtain the target tantalate ceramic.

[0016] In step 1), the molar ratio of the raw material to the solvent is 2-6:1.

[0017] In step 1), the purity of Y2O3 powder, Ta2O5 powder, HfO2 powder, TiO2 powder and ZrO2 powder is not less than 99.9%.

[0018] In step 2), the drying temperature is 100~150℃ and the drying time is 24~36h. In step 3), the holding pressure is 200-300 MPa, and the holding time is 2-4 min.

[0019] The present invention further provides an application of the medium-entropy rare earth tantalate ceramic, specifically an application in a surface coating of a hot end component of an aero-engine.

[0020] Examples 1-6 Examples 1-6 are to prepare medium entropy rare earth tantalate ceramics according to the following steps, and the specific parameters are shown in Table 1: 1) Weigh yttrium oxide Y2O3 powder, tantalum oxide Ta2O5 powder, hafnium oxide HfO2 powder, titanium oxide TiO2 powder and zirconium oxide ZrO2 powder according to the proportion, add solvent ethanol or distilled water to mix, the molar ratio of the above five powders (yttrium oxide Y2O3 powder, tantalum oxide Ta2O5 powder, hafnium oxide HfO2 powder, titanium oxide TiO2 powder and zirconium oxide ZrO2 powder) to the solvent is (2:1) to (6:1), and use a planetary ball mill to perform ball milling to obtain powder A. The ball milling time is 24 to 36 hours, the speed of the ball mill is 600 to 1000 r / min, and the purity of the raw materials yttrium oxide Y2O3 powder, tantalum oxide Ta2O5 powder, hafnium oxide HfO2 powder, titanium oxide TiO2 powder and zirconium oxide ZrO2 powder is not less than 99.9%.

[0021] 2) Dry the powder A obtained in step (1) and sieve it for the first time to obtain powder B. The drying temperature is 100-150° C., the drying time is 24-36 hours, and the mesh size of the first sieve is 100-200 meshes.

[0022] 3) Powder B obtained in step (2) is placed in a muffle furnace for pre-calcination, and then sieved for a second time to obtain powder C. The pre-calcination temperature is 1000-1200° C., the pre-calcination time is 5-10 hours, and the mesh size of the second sieving is 300-600 mesh.

[0023] 4) The powder C obtained in step (3) is placed in a mold and compacted to form a block C. The holding pressure is 200-300 MPa and the holding time is 2-4 min.

[0024] 5) Sintering the block C in step (4) to obtain a tantalate material, wherein the sintering temperature is 1500-1700° C. and the sintering time is 5-7 hours.

[0025] Tantalate ceramics with low thermal conductivity, high thermal expansion and high fracture toughness are prepared by the above method. In order to fully illustrate the tantalate ceramics with low thermal conductivity, high thermal expansion and high fracture toughness prepared by the above method, 6 groups of examples are first selected for illustration.

[0026] Table 1 Preparation parameters of medium entropy rare earth tantalate ceramics in Examples 1 to 6 of the present invention Comparative Example 1 The difference between this comparative example and Example 1 is that only yttrium oxide Y2O3 powder and tantalum oxide Ta2O5 powder are added to the raw material powder, that is, the content of hafnium oxide HfO2 powder, titanium oxide TiO2 powder and zirconium oxide ZrO2 powder is 0% mol, and the chemical formula of the prepared tantalate ceramic is YTaO4.

[0027] Comparative Example 2 The difference between this comparative example and Example 1 is that only yttrium oxide Y2O3 powder, tantalum oxide Ta2O5 powder and titanium oxide TiO2 powder are added to the raw material powder, that is, the content of hafnium oxide HfO2 powder and zirconium oxide ZrO2 powder is 0% mol, and the chemical formula of the prepared tantalate ceramic is Y 0.98 Ta 0.98 Ti 0.04 O4.

[0028] Comparative Example 3 The difference between this comparative example and Example 1 is that only yttrium oxide Y2O3 powder, tantalum oxide Ta2O5 powder and zirconium oxide ZrO2 powder are added to the raw material powder, that is, the content of titanium oxide TiO2 powder and hafnium oxide HfO2 powder is 0% mol, and the chemical formula of the prepared tantalate ceramic is Y 0.98 Ta 0.98 Zr 0.04 O4.

[0029] Comparative Example 4 The difference between this comparative example and Example 1 is that only yttrium oxide Y2O3 powder, tantalum oxide Ta2O5 powder and hafnium oxide HfO2 powder are added to the raw material powder, that is, the content of titanium oxide TiO2 powder and zirconium oxide ZrO2 powder is 0% mol, and the chemical formula of the prepared tantalate ceramic is Y 0.98 Ta 0.98 Hf 0.04 O4.

[0030] Comparative Example 5 The difference between this comparative example and Example 1 is that x=0.8, and the chemical formula is: Y 0.6 Ta 0.6 M 0.8 O4.

[0031] Test Example Structure and Performance Test of Tantalate Ceramics Prepared in Examples 1 to 6 1. XRD characterization The tantalate ceramics prepared in Examples 1 to 4 were tested using an X-ray diffractometer.

[0032] like Figure 1 As shown, the diffraction peaks of the XRD test results of Examples 1 to 3 correspond to the standard peaks of their standard PDF card #24-1415 one by one, and there is no second phase diffraction peak, indicating that the prepared ceramic is a single-phase ceramic, and HfO2, TiO2, and ZrO2 have entered the lattice of YTaO4, and its crystal structure is a monoclinic phase. The main phase of the ceramic prepared in Example 4 is the same as that of Examples 1 to 3, but a few diffraction peaks of the second phase appear, indicating that the phase structure of tantalate has been changed by equal doping of Ti, Zr, and Hf. The lattice parameters a, b, c and α, γ, and β of Examples 1 to 4 are shown in Table 2. By comparing the XRD diffraction peaks, it is found that the diffraction peaks have no obvious offset, which proves that Ti, Hf, and Zr atoms simultaneously replace Y and Ta atoms to maintain the electrical neutrality of the crystal structure, because the sum of the ionic radii of Ti, Hf, and Zr ions is approximately equal to twice the sum of the ionic radii of one Y and one Ta ion.

[0033] Table 2 Lattice parameters of tantalate ceramics prepared in Examples 1-4 2. SEM characterization from Figure 2 It can be seen that the tantalate ceramic prepared in Example 4 has no pores in its crystal structure, has uniform grain distribution and clear grain boundaries, and has good bonding between grains. The second phase exists in the grains (the black dots are the second phase), which can enhance the toughness of the ceramic.

[0034] The tantalate ceramics prepared in Comparative Examples 1 to 4 all have many small pores in their crystal structures, and they exist at the grain boundaries, making the block less dense, the grain boundaries blurred, and many fractures at the grain boundaries. In the tantalate ceramics prepared in Comparative Example 5, a large amount of second phases appear at the grain boundaries, making the grain boundaries embrittled and destroying the ceramic properties.

[0035] 3. Thermal conductivity detection The tantalate ceramic blocks obtained in Examples 1 to 4 and Comparative Example 1 were polished into φ6×2 mm circular slices, and their thermal conductivity was measured using a laser thermal conductivity meter.

[0036] Results: Figure 3 As shown, as the temperature continues to rise, the thermal conductivity of the ceramic blocks prepared in Examples 1 to 4 and Comparative Example 1 drops sharply, and the thermal conductivity is excellent at high temperatures. However, the thermal conductivity of the tantalate ceramics prepared in Examples 1 to 4 at high temperatures is significantly lower than that of Comparative Example 1.

[0037] 4. Thermal expansion detection The ceramic blocks obtained in Examples 1 to 4 and Comparative Example 1 were polished into cuboids of 10×3×1.5 mm, and their thermal expansion coefficients at 100 to 1400° C. were measured using a thermal expansion analyzer (TMA 402 F3).

[0038] Results: By Figure 4 It can be seen that the tantalate ceramics obtained in Examples 1 to 4 and Comparative Example 1 have better thermal expansion coefficients, so that less thermal stress is generated during use.

[0039] 5. Fracture toughness test The ceramic blocks obtained in Examples 1 to 6 and Comparative Examples 1 to 5 were polished, and the fracture toughness of the tantalate ceramics was calculated using the indentation method. The specific method is: the polished ceramic blocks were indented with a Vickers hardness tester at a certain load (F) to obtain the hardness (H), and each sample was performed 10 times; then the indentation diagonal length (a) and the crack length (c) along the diagonal extension of the crack were obtained from the scanning electron microscope image; the formula E is Young's modulus, and the fracture toughness is calculated (the average value of 10 times for each sample). The calculation results are shown in Table 3.

[0040] Results: From Table 3, it can be seen that the fracture toughness of the tantalate ceramics prepared in Examples 1-6 of the present invention is significantly higher than that of Comparative Examples 1-5, among which the average fracture toughness of the tantalate ceramics prepared in Example 4 is as high as 5.18 MPa. 0.5 However, in the chemical formula of the tantalate ceramic prepared in Comparative Example 5, since x=0.8, a large amount of second phases aggregate at the grain boundaries, resulting in a decrease in fracture toughness.

[0041] Table 3 Fracture toughness of tantalate ceramics prepared in Examples 1 to 6 and Comparative Examples 1 to 5 In summary, the tantalate ceramics prepared in Examples 1 to 6 of the present invention have distinct grains in their crystal structure, clear grain boundaries, and good bonding between grains. They have low thermal conductivity at high temperatures, showing good thermal insulation performance. At the same time, they have high thermal expansion coefficients at high temperatures, so that when their powders are used as thermal barrier coatings, the expansion stress between them and the base material (or bonding layer) is reduced, reducing cracking. In addition, their excellent fracture toughness enables them to resist external impacts well during service.

Claims

1. A medium-entropy rare earth tantalate ceramic, characterized in that: The chemical formula of the medium entropy rare earth tantalate ceramic is Y 1-x / 2Ta 1-x / 2 M x O4; wherein, 0<X<0.8, M is Ti, Hf, Zr, and the molar content of each element in M ​​is equal.

2. The medium entropy rare earth tantalate ceramic according to claim 1, characterized in that: The thermal conductivity of the medium-entropy rare earth tantalate ceramic at 900°C is 1.23-1.42 W·m -1 ·K -1 , the thermal expansion coefficient at 1400°C is 9.8-10.4 × 10 -6 K -1 ; Its fracture toughness is 4.7-5.2MPam 0.5 .

3. The method for preparing the medium-entropy rare earth tantalate ceramic according to claim 1, characterized in that: To do this, follow these steps: 1) Weigh the raw materials according to the ratio: Y2O3 powder, Ta2O5 powder, HfO2 powder, TiO2 powder and ZrO2 powder, add solvent and use planetary ball mill for ball milling, the ball milling time is 24-36h, the ball mill speed is 600-1000r / min; the solvent is ethanol or distilled water; 2) drying the powder obtained by ball milling in step 1), passing it through a 100-200 mesh sieve, pre-calcining it in a muffle furnace at 1000-1200° C. for 5-10 hours, and then passing it through a 300-600 mesh sieve; 3) The sieved powder obtained in step 2) is placed in a mold, compacted, and then sintered at 1500-1700° C. for 5-7 hours to obtain the target tantalate ceramic.

4. The method for preparing the medium-entropy rare earth tantalate ceramic according to claim 3, characterized in that: In step 1), the molar ratio of the raw material to the solvent is 2-6:

1.

5. The method for preparing the medium-entropy rare earth tantalate ceramic according to claim 3, characterized in that: In step 1), the purity of Y2O3 powder, Ta2O5 powder, HfO2 powder, TiO2 powder and ZrO2 powder is not less than 99.9%.

6. The method for preparing the medium-entropy rare earth tantalate ceramic according to claim 3, characterized in that: In step 2), the drying temperature is 100-150°C and the drying time is 24-36 hours.

7. The method for preparing the medium-entropy rare earth tantalate ceramic according to claim 3, characterized in that: In step 3), the holding pressure during the compaction process is 200-300 MPa, and the holding time is 2-4 min.

8. Use of the medium-entropy rare earth tantalate ceramics according to claim 1 in the surface coating of the hot end components of an aero-engine.

Citation Information

Patent Citations

  • Two-phase rare earth tantalate ceramic and preparation method thereof

    CN110002871A

  • Porous tantalite ceramic and preparation method thereof

    CN110002873A

  • High-entropy stable rare earth tantalate / niobate ceramic and preparation method thereof

    CN113264769A

  • High-entropy rare earth tantalate ceramic coating material and preparation method thereof