Garnet silicate orange fluorescent ceramic and preparation method thereof
By replacing Ca2+ to Sr2+ and Ba2+ in garnet silicate and introducing Sc3+, the preparation and thermal stability of red fluorescent ceramics are solved, and efficient and stable orange-red light emission is achieved, which is suitable for industrial production and high-brightness lighting needs.
Patent Information
- Application Number
- CN202411209819.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
Existing red fluorescent ceramics have difficulties in large-scale preparation and thermal stability, and traditional preparation methods are inefficient and have safety risks, making it difficult to meet the needs of industrial production.
By using Sr2+ and Ba2+ with larger radius in garnet silicates to replace Ca2+ and introducing Sc3+ to balance the lattice distortion, high-temperature solid phase reaction is used to prepare orange fluorescent ceramics, which improves its thermal stability and structural rigidity, and is suitable for large batches. Production.
It has achieved high luminous intensity and high thermal stability, with a peak emission wavelength of 565~590nm and a ceramic color temperature of 2800~3500K, which is suitable for high power, high brightness, and long-term luminescence applications.
Smart Images

Figure CN119059815A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fluorescent ceramics, and in particular to garnet silicate orange fluorescent ceramics and a preparation method thereof. Background Art
[0002] Light-emitting diode (LED) is a solid-state semiconductor device that can convert electrical energy into visible light. As the fourth generation of lighting sources, it has better energy saving, better environmental protection, higher luminous efficiency, faster startup speed and longer service life, so it is widely used in indoor and outdoor lighting, decorative lighting, automotive lighting and display lighting. Commercial LEDs usually use blue InGN LED chips to excite Y3Al5O 12 :Ce 3+ (YAG:Ce) yellow phosphor produces white light, but the emission spectrum of YAG:Ce mainly covers the yellow-green band, and there are problems such as missing red light band and cyan light valley effect. The white light obtained by exciting YAG:Ce faces the problem of poor color rendering performance (CRI ~ 60) and high color temperature (> 6000K). The above problems can be solved by exciting fluorescent conversion materials with more sufficient red light band.
[0003] At present, the packaging of white light LEDs is to disperse the phosphor in resin or silica gel. As the heat generated by the excitation source and the fluorescence conversion process continues to accumulate, the light-emitting device ages under long-term operation, resulting in a reduction in the life of the LED device and a decrease in efficiency. Fluorescent ceramics have become a very promising fluorescent conversion material in solid-state lighting due to their excellent thermal conductivity, low thermal quenching, high power density and high brightness. However, the technology of red fluorescent ceramics is still immature. The literature (Xin Liu, Heyu Zhou, Zewang Hu, Transparent Ce: GdYAG ceramic color converters for high-brightness white LEDs and LDs [J]. Optical Materials, 2019, 88: 97-102.) chooses to use Gd with a larger radius. 3+ Replace the Y with a smaller radius 3+ , the spectrum can be red-shifted from 528nm to 550nm, but with the Gd 3+ With the increase of the content, the thermal conductivity of GdYAG:Ce ceramics gradually decreased, and the thermal stability also decreased significantly. 4+[J].Optical Materials, 2020, 107:110140) used hot pressing to prepare K2SiF6 red fluorescent ceramics. This method can only prepare one piece of ceramic at a time, which is extremely inefficient and doped with Mn 4+ The chemical stability of K2SiF6 fluorescent ceramics is low, and hydrofluoric acid corrosion is required during treatment, which poses certain safety risks and is not conducive to industrial production. CN117049861A discloses a spark plasma (SPS) sintered CaAlSiN3:Eu 2+ Red ceramic, and then use organic resin to make CaAlSiN3:Eu 2+ Red ceramics are combined with YAG:Ce yellow ceramics. This method is used to prepare CaAlSiN3:Eu 2+ Red light ceramics have low efficiency and are prone to aging of the resin material when exposed to high-power light sources, affecting their luminous performance.
[0004] In the above patents and literature, there is a common problem that red light ceramics are difficult to prepare on a large scale or the thermal stability of ceramics is poor. Therefore, it is of great significance to explore new blue light-excitable orange-red fluorescent ceramics with excellent thermal stability and low cost. Summary of the invention
[0005] The purpose of the present invention is to provide a garnet silicate orange fluorescent ceramic and a preparation method thereof. 2+ , Ba 2+ Replace the smaller Ca in the matrix 2+ , with Sr 2+ Or Ba 2+ As the doping amount increases, the crystal lattice distortion also increases. When the doping amount is too high, the crystal structure collapses and a non-cubic phase is formed. Therefore, we choose to use Sc with a smaller radius. 3+ Replace Lu 3+ To balance this distortion. At the same time, due to the introduction of Sc 3+ , improving the structural rigidity and increasing the thermal stability of ceramics. The preparation process adopts high-temperature solid-phase reaction, which can be prepared in large quantities and is suitable for industrial production.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] In one aspect, the present invention provides a garnet silicate orange fluorescent ceramic, the chemical formula of which is (Lu 1-x-z Ce x Sc z )2Ca (1-y) (Sr,Ba) y Mg2Si3O 12 , where x is Ce 3+Occupy Lu 3+ The mole fraction of Sc 3+ Occupy Lu 3+ The mole fraction of Sr 2+ Or Ba 2+ Occupancy of Ca 2+ The mole fraction of the position, where 0.001≤x≤0.01, 0.4≤y≤0.8, 1 / 4y≤z≤1 / 2y.
[0008] On the other hand, the present invention also provides a method for preparing the above garnet silicate orange fluorescent ceramic, comprising the following steps:
[0009] (1) According to (Lu 1-x-z Ce x Sc z )2Ca (1-y) (Sr,Ba) y Mg2Si3O 12 Lu2O3, Ce2O3, Sc2O3, CaO, SrO, BaO, MgO, and SiO2 are accurately weighed in chemical dosage ratios of the elements as raw material powders, 0.1 to 0.5 wt% of Al2O3 as a sintering aid is added to the total mass of the raw material powders, and anhydrous ethanol is added as a solvent;
[0010] (2) placing the raw materials weighed in step (1) into a ball mill and performing planetary ball milling;
[0011] (3) placing the mixed slurry obtained by ball milling in step (2) in a drying oven to dry, and then sieving the dried mixed powder;
[0012] (4) placing the sieved powder in step (3) into a mold for dry pressing, and then performing cold isostatic pressing to obtain a green blank;
[0013] (5) The green blank obtained in step (4) is subjected to vacuum sintering, followed by annealing in air, and then double-sided polishing to obtain (Lu 1-x-z Ce x Sc z )2Ca (1-y) (Sr,Ba) y Mg2Si3O 12 Orange fluorescent ceramic.
[0014] Preferably, the mass ratio of the raw material powder to anhydrous ethanol in step (1) is 1:1 to 1:2.
[0015] Preferably, the ball milling speed in step (2) is 180-220 r / min, and the ball milling time is 12-20 h.
[0016] Preferably, the drying time in step (3) is 5 h to 10 h, and the drying temperature is 50° C. to 80° C.
[0017] Preferably, the mesh size of the sieve used in step (3) is 50 to 100 meshes, and the number of sieving is 1 to 3 times.
[0018] Preferably, the holding pressure of the cold isostatic pressing in step (4) is 150 to 200 MPa, and the holding time is 200 to 400 s.
[0019] Preferably, the vacuum sintering temperature in step (5) is 1300°C to 1500°C, the holding time is 8h to 16h, and the sintering vacuum degree is not less than 10 -3 Pa, the heating rate in the vacuum sintering stage is 1-10℃ / min, and the cooling rate after sintering is 1-10℃ / min,
[0020] Preferably, the annealing temperature in step (5) is 1150-1250° C., and the holding time is 10-15 h.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention selects Sr with a large radius 2+ , Ba 2+ Replacement of Ca in the matrix 2+ , and use a small radius Sc 3+ Replace Lu 3+ To balance the introduction of Sr 2+ , Ba 2+ The lattice distortion caused by the co-replacement of the above-mentioned ions of different sizes can form stable orange-red light emission, with a peak emission wavelength of 565-590nm and a ceramic color temperature of 2800-3500K.
[0023] 2. The fluorescent ceramic prepared by the present invention has a high luminous intensity, and the maximum luminous efficiency can reach 120lm / W.
[0024] 3. The present invention introduces Sc 3+ It also increases the structural rigidity of the ceramic crystal, making the fluorescent ceramic have high thermal stability. The luminous intensity at 150°C can reach about 87% of that at room temperature, making it suitable for high-power, high-brightness, and long-term luminescence. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the XRD pattern of the fluorescent ceramics prepared in Examples 1-7;
[0026] Figure 2 is an emission spectrum of the fluorescent ceramic prepared in Example 1 under 460nm blue light excitation;
[0027] Figure 3 is the emission spectrum of the fluorescent ceramic prepared in Example 5 under 460nm blue light excitation;
[0028] Figure 4 The electroluminescence spectrum of the fluorescent ceramic prepared in Example 3 and its color temperature and light efficiency data;
[0029] Figure 5 is a scanning electron microscope image of the fluorescent ceramic prepared in Example 3;
[0030] Figure 6 This is a graph showing the variation of the luminous intensity of the fluorescent ceramics prepared in Examples 1, 4, and 7 with temperature. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0032] To prepare 60 g of the target product, the raw material powders were weighed and the ingredients were shown in Table 1. The raw material powders used in the following examples were all commercially available products with a purity greater than or equal to 99.99%.
[0033] Table 1 Ingredients of Example
[0034] serial number 1# 2# 3# 4# 5# 6# 7# <![CDATA[Lu2O3]]> 27.9796g 26.9046g 27.8831g 27.1263g 20.6717g 28.6872g 23.9125g <![CDATA[CeO2]]> 0.0303g 0.2946g 0.1212g 0.1179g 0.1200g 0.1173g 0.1189g <![CDATA[Sc2O3]]> 2.4272g 2.3606g 2.4280g 2.3621g 4.8081g 1.7628g 3.5721g CaO 2.9609g 2.8796g 2.9618g 0.9605g 0.9776g 1.9114g 1.9367g SrO 3.6474g / 3.6485g 7.0990g / 5.2979g / BaO / 5.2489g / / 10.6912g / 7.9428g MgO 7.0936g 6.8988g 7.0958g 6.9032g 7.0259g 6.8690g 6.9597g <![CDATA[SiO2]]> 15.8624g 15.4267g 15.8672g 15.4365g 15.7110g 15.3600g 15.5629g
[0035] Embodiment 1: (Lu 0.799 Ce 0.001 Sc 0.2 )2Ca 0.6 Sr 0.4 Mg2Si3O 12
[0036] According to the mass shown in 1# in Table 1, weigh the raw materials of Lu2O3, Ce2O3, Sc2O3, CaO, SrO, MgO, and SiO2 powders, add 0.1%wt of Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 1:1, add grinding balls and put them into a planetary ball mill, the ball milling speed is 180r / min, and the ball milling time is 20h. The slurry after ball milling is placed in an oven at 80℃ and dried for 5h. The dried powder is passed through a 50-mesh screen 3 times and then dry pressed in a 20MPa steel mold, followed by cold isostatic pressing at 150MPa for 400s to obtain a green blank.
[0037] The obtained green billet was sintered in a high temperature vacuum sintering furnace, heated to 1300°C, and kept warm for 16 hours. The vacuum degree of the vacuum sintering furnace was 10 -3 pa, and anneal the sintered ceramic in air at 1150°C for 15 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0038] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0039] Figure 2 The emission spectrum of the sample prepared for this embodiment under 460nm blue light excitation can emit high-intensity broadband yellow-orange light near 565nm with a color temperature of 3500K.
[0040] Figure 6 This is a graph showing the luminescence intensity of the sample prepared in this embodiment as a function of temperature. At 150°C, the luminescence intensity is 87% of that at room temperature.
[0041] Embodiment 2: (Lu 0.79 Ce 0.01 Sc 0.2 )2Ca 0.6 Ba 0.4 Mg2Si3O 12
[0042] Weigh the raw materials of Lu2O3, Ce2O3, Sc2O3, CaO, BaO, MgO, and SiO2 powders according to the mass shown in 2# in Table 1, add 0.5%wt of Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 2:1, put into a planetary ball mill after adding grinding balls, the ball milling speed is 220r / min, and the ball milling time is 12h. The ball-milled slurry is placed in a 50℃ oven for drying for 10h, and the dried powder is passed through a 100-mesh sieve and dry-pressed in a 20MPa steel mold, followed by cold isostatic pressing at 200MPa for 200s to obtain a blank. The obtained blank is sintered in a high-temperature vacuum sintering furnace, heated to 1500℃, and kept warm for 8 hours. The vacuum degree of the vacuum sintering furnace is 10 -3 pa, and anneal the sintered ceramic in air at 1250°C for 10 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0043] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0044] When excited by 460nm blue light, the ceramic can emit high-intensity broadband orange light near 575nm with a color temperature of 3000K.
[0045] Embodiment 3: (Lu 0.796 Ce 0.004 Sc 0.2)2Ca 0.6 Sr 0.4 Mg2Si3O 12
[0046] Weigh Lu2O3, Ce2O3, Sc2O3, CaO, SrO, MgO, SiO2 powder raw materials according to the mass shown in 3# in Table 1, add 0.2%wt Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 1.2:1, add grinding balls and put them into a planetary ball mill, the ball milling speed is 200r / min, and the ball milling time is 15h. The ball-milled slurry is placed in a 60℃ oven and dried for 8h. The dried powder is passed through an 80-mesh sieve 3 times and then dry-pressed in a 20MPa steel mold, followed by cold isostatic pressing at 180MPa for 300s to obtain a blank. The obtained blank is sintered in a high-temperature vacuum sintering furnace, heated to 1400℃, and kept warm for 10 hours. The vacuum degree of the vacuum sintering furnace is 10 -3 pa, and anneal the sintered ceramic in air at 1200°C for 12 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0047] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0048] Figure 4 This is the electroluminescence spectrum diagram of this embodiment and its color temperature and light efficiency data. Under the excitation of 460nm blue light, the ceramic can emit high-intensity broadband orange light near 570nm, with a color temperature of 3100K and a light efficiency of 120lm / W.
[0049] Figure 5 This is the SEM picture of this embodiment at a sintering temperature of 1400°C, and the density reaches 99%.
[0050] Embodiment 4: (Lu 0.796 Ce 0.004 Sc 0.2 )2Ca 0.2 Sr 0.8 Mg2Si3O 12
[0051] Weigh Lu2O3, Ce2O3, Sc2O3, CaO, SrO, MgO, and SiO2 powder raw materials according to the mass shown in 4# in Table 1, add 0.2%wt Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 1.2:1, add grinding balls and put them into a planetary ball mill, the ball milling speed is 200r / min, and the ball milling time is 15h. The ball-milled slurry is placed in a 60℃ oven and dried for 8h. The dried powder is passed through an 80-mesh sieve 3 times and dry-pressed in a 20MPa steel mold, followed by cold isostatic pressing at 180MPa for 300s to obtain a blank. The obtained blank is sintered in a high-temperature vacuum sintering furnace, heated to 1400℃, and kept warm for 10 hours. The vacuum degree of the vacuum sintering furnace is 10 -3 pa, and anneal the sintered ceramic in air at 1200°C for 12 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0052] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0053] Figure 6 This is a graph showing the variation of the luminescence intensity of the sample prepared in this embodiment with temperature. At 150°C, the luminescence intensity is 80% of that at room temperature.
[0054] When excited by 460nm blue light, the ceramic can emit high-intensity broadband orange light near 585nm with a color temperature of 2900K.
[0055] Embodiment 5: 0.596 Ce 0.004 Sc 0.4 )2Ca 0.2 Ba 0.8 Mg2Si3O 12
[0056] Weigh the raw materials of Lu2O3, Ce2O3, Sc2O3, CaO, BaO, MgO, and SiO2 powders according to the mass shown in 5# in Table 1, add 0.2%wt of Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 1.2:1, add grinding balls and put into a planetary ball mill - ball mill, the ball mill speed is 200r / min, and the ball milling time is 15h. The ball-milled slurry is placed in a 60℃ oven and dried for 8h. The dried powder is passed through an 80-mesh sieve 3 times and then dry-pressed in a 20MPa steel mold, followed by cold isostatic pressing at 180MPa for 300s to obtain a blank. The obtained blank is sintered in a high-temperature vacuum sintering furnace, heated to 1400℃, and kept warm for 10 hours. The vacuum degree of the vacuum sintering furnace is 10-3 pa, and anneal the sintered ceramic in air at 1200°C for 12 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0057] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0058] Figure 3 The emission spectrum of the sample prepared for this embodiment under 460nm blue light excitation can emit high-intensity broadband orange light near 590nm with a color temperature of 2800K.
[0059] Embodiment 6: 0.846 Ce 0.004 Sc 0.15 )2Ca 0.4 Sr 0.6 Mg2Si3O 12
[0060] Weigh Lu2O3, Ce2O3, Sc2O3, CaO, SrO, MgO, SiO2 powder raw materials according to the mass shown in 6# in Table 1, add 0.2%wt Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 1.2:1, add grinding balls and put into planetary ball mill, the ball milling speed is 200r / min, and the ball milling time is 15h. The ball-milled slurry is placed in a 60℃ oven and dried for 8h. The dried powder is passed through an 80-mesh sieve 3 times and dry-pressed in a 20MPa steel mold, followed by cold isostatic pressing at 180MPa for 300s to obtain a blank. The obtained blank is sintered in a high-temperature vacuum sintering furnace, heated to 1400℃, and kept warm for 10 hours. The vacuum degree of the vacuum sintering furnace is 10 -3 pa, and anneal the sintered ceramic in air at 1200°C for 12 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0061] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0062] When excited by 460nm blue light, the ceramic can emit high-intensity broadband orange light near 578nm with a color temperature of 3050K.
[0063] Embodiment 7: (Lu 0.696 Ce 0.004Sc 0.3 )2Ca 0.4 Ba 0.6 Mg2Si3O 12
[0064] Weigh the raw materials of Lu2O3, Ce2O3, Sc2O3, CaO, BaO, MgO, and SiO2 powders according to the mass shown in 7# in Table 1, add 0.2%wt of Al2O3, add anhydrous ethanol after blending, the mass ratio of anhydrous ethanol to powder is 1.2:1, add grinding balls and put them into a planetary ball mill, the ball milling speed is 200r / min, and the ball milling time is 15h. The ball-milled slurry is placed in a 60℃ oven and dried for 8h. The dried powder is passed through an 80-mesh sieve 3 times and then dry-pressed in a 20MPa steel mold, followed by cold isostatic pressing at 180MPa for 300s to obtain a blank. The obtained blank is sintered in a high-temperature vacuum sintering furnace, heated to 1400℃, and kept warm for 10 hours. The vacuum degree of the vacuum sintering furnace is 10 -3 pa, and anneal the sintered ceramic in air at 1200°C for 12 hours. Finally, double-sided polishing is performed, and the diameter is about 15 mm and the thickness is 0.5 mm to obtain a dense fluorescent ceramic.
[0065] Figure 1 This is the XRD spectrum of the sample prepared in this example. The XRD test results show that the prepared ceramic sample is consistent with the standard card of LuAG (PDF#73-1368) and is a garnet phase.
[0066] Figure 6 This is a graph showing the luminescence intensity of the sample prepared in this embodiment as a function of temperature. At 150°C, the luminescence intensity is 75% of that at room temperature.
[0067] When excited by 460nm blue light, the ceramic can emit high-intensity broadband orange light near 583nm with a color temperature of 2960K.
[0068] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A garnet silicate orange fluorescent ceramic, characterized in that: The chemical formula of the fluorescent ceramic is (Lu 1-x- z Ce x Sc z )2Ca (1-y) (Sr,Ba) y Mg2Si3O 12 , where x is Ce 3+ Occupy Lu 3+ The mole fraction of Sc 3+ Occupy Lu 3+ The mole fraction of Sr 2+ Or Ba 2+ Occupancy of Ca 2+ The mole fraction of the position, where 0.001≤x≤0.01, 0.4≤y≤0.8, 1 / 4y≤z≤1 / 2y.
2. A method for preparing the garnet silicate orange fluorescent ceramic according to claim 1, characterized in that: The following steps are involved: (1) According to (Lu 1-x-z Ce x Sc z )2Ca (1-y) (Sr,Ba) y Mg2Si3O 12 Lu2O3, Ce2O3, Sc2O3, CaO, SrO, BaO, MgO, and SiO2 are accurately weighed as raw material powders according to the chemical dosage ratio of each element, 0.1 to 0.5 wt% of Al2O3 as a sintering aid is added to the total mass of the raw material powders, and anhydrous ethanol is added as a solvent; (2) placing the raw materials weighed in step (1) into a ball mill and performing planetary ball milling; (3) placing the mixed slurry obtained by ball milling in step (2) in a drying oven to dry, and then sieving the dried mixed powder; (4) placing the sieved powder in step (3) into a mold for dry pressing, and then performing cold isostatic pressing to obtain a green blank; (5) The green blank obtained in step (4) is subjected to vacuum sintering, followed by annealing in air, and then double-sided polishing to obtain (Lu 1-x-z Ce x Sc z )2Ca (1-y) (Sr,Ba) y Mg2Si3O 12 Orange fluorescent ceramic.
3. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The mass ratio of the raw material powder to anhydrous ethanol in step (1) is 1:1 to 1:
2.
4. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The ball milling speed in step (2) is 180-220 r / min, and the ball milling time is 12-20 h.
5. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The drying time in step (3) is 5 h to 10 h, and the drying temperature is 50° C. to 80° C.
6. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The mesh size of the sieve used in step (3) is 50 to 100 meshes, and the number of sieving is 1 to 3 times.
7. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The holding pressure of the cold isostatic pressing in step (4) is 150-200 MPa, and the holding time is 200-400 s.
8. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The vacuum sintering temperature in step (5) is 1300°C to 1500°C, the holding time is 8h to 16h, and the sintering vacuum degree is not less than 10 - 3 Pa, the heating rate in the vacuum sintering stage is 1-10°C / min, and the cooling rate after sintering is 1-10°C / min.
9. The method for preparing the garnet silicate orange fluorescent ceramic according to claim 2, characterized in that: The annealing temperature in step (5) is 1150-1250° C., and the holding time is 10-15 hours.
Citation Information
Patent Citations
Green phosphor for LED (Light-Emitting Diode) and preparation method of green phosphor
CN102618274A
Silicate fluorescent ceramic with full-spectrum emission effect and preparation method thereof
CN106518037A
Garnet-form aluminosilicate fluorescent powder, preparation method thereof and light-emitting device including same
CN107880885A
Color-adjustable silicate fluorescent powder for ultraviolet or near ultraviolet excited white light LED and preparation method of color-adjustable silicate fluorescent powder
CN108587621A
Fluorescent transparent ceramic capable of emitting blue-green light and preparation method thereof
CN110642624A