Preparation method of regenerated cellulose with controllable polymerization degree
By using KCl or MgCl2 to react with plant fibers and scrape the film in the Lyocell process, the problem of changing cellulose polymerization is solved, the precise regulation of cellulose polymerization is achieved, and the viscosity and fiber strength of the spinning liquid are improved. Controlled.
Patent Information
- Application Number
- CN202411163693.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the preparation process of cellulose in the Lyocell process, the degree of polymerization changes due to temperature and storage time, resulting in unsuitable viscosity of spinning liquid and insufficient fiber strength. It is difficult for the prior art to effectively regulate the degree of polymerization of cellulose.
KCl or MgCl2 is used as inorganic salt to react with plant fibers in NMMO solvent, and a thin film is made by scraping coating, soaking and drying in deionized water to regulate the polymerization degree of cellulose to achieve accurate cellulose within a certain range. control.
It realizes the precise regulation of cellulose polymerization, meets the requirements of liquid viscosity and fiber strength during spinning, and is more convenient, accurate and reliable than the raw material selection method.
Smart Images

Figure CN119060207A_ABST
Abstract
Description
Technical field:
[0001] The invention belongs to the technical field of regenerated fiber preparation, and in particular relates to a method for preparing regenerated cellulose which can effectively regulate the degree of polymerization of cellulose. Background technology:
[0002] The Lyocell process was launched and commercialized in the late 1980s. It uses renewable natural cellulose resources such as cotton linter and trees as the main raw materials, and a mild, efficient and pollution-free N-methylmorpholine-N-oxide (NMMO) solution as a new solvent to prepare regenerated cellulose fibers through dry-jet wet spinning. It has the characteristics of excellent product performance, environmentally friendly production process, energy saving, etc. It is a green process that is currently widely used.
[0003] Although the Lyocell process is relatively mature, there are still some aspects that need to be improved. One of the aspects that needs to be improved is that the degree of polymerization (DP) of the fiber will change due to various factors during the preparation process. For example, the fiber will be degraded due to high temperature (≥130°C) during the dissolution process. In addition, during the production process, the slurry usually needs to be stored for a long time (2 to 3 days) in order to continue spinning. Long-term dissolution will cause more serious degradation of cellulose. Since the diameter of the spinneret in Lyocell spinning is usually small, if the spinning solution is made of high-polymerization fiber (such as hemp fiber, mulberry branch fiber, etc.), the spinneret will be blocked due to excessive viscosity, and the spinning solution obtained by using low-polymerization fiber will result in lower strength of the prepared fiber. In contrast, it is undoubtedly a more reasonable, convenient and controllable way to obtain a spinning solution of suitable viscosity by regulating the degree of polymerization of the regenerated fiber during the preparation process through non-material selection. Summary of the invention:
[0004] The object of the present invention is to provide a method for preparing regenerated cellulose, which can effectively control the degree of polymerization of cellulose during the preparation process.
[0005] The technical solution of the present invention is specifically as follows:
[0006] A method for preparing regenerated cellulose with controllable degree of polymerization, characterized in that it comprises the following steps:
[0007] 1) Add plant fiber and inorganic salt to NMMO solvent in sequence, and stir to react for 1 hour under vacuum degree 0.1 MPa and 100°C;
[0008] 2) using the reacted solution as a casting solution, forming a thin film by doctor blade coating, and soaking the thin film in deionized water for at least 3 days, replacing the deionized water every 12 hours during the soaking process;
[0009] 3) completely drying the soaked film to obtain a regenerated cellulose film product;
[0010] The inorganic salt in step 1) is KCl or MgCl 2 ;in:
[0011] The KCl is used to increase the polymerization degree of the regenerated cellulose finally obtained, and the polymerization degree of the regenerated cellulose is positively correlated with the concentration of KCl in the NMMO solution, and the mass concentration of the KCl in the NMMO solution is not higher than 10%;
[0012] The MgCl 2 It is used to reduce the degree of polymerization of the regenerated cellulose obtained. The degree of polymerization of the regenerated cellulose is related to MgCl 2 The concentration of MgCl in NMMO solution is negatively correlated 2 The mass concentration in the NMMO solution is not higher than 3%.
[0013] Furthermore, when the inorganic salt in step 1) is KCl, its mass concentration in the NMMO solvent is 6-10%; when the inorganic salt is MgCl 2 When the mass concentration of the NMMO solvent is 1-3%.
[0014] Furthermore, the plant fiber in step 1) is hardwood fiber, and the amount of the plant fiber added to the NMMO solvent is 5 wt %; the NMMO solvent is a concentrated NMMO aqueous solution with a mass concentration of 86.7%.
[0015] Furthermore, the NMMO concentrated aqueous solution is obtained as follows: add an appropriate amount of propyl gallate antioxidant to an NMMO aqueous solution with a mass concentration of 50%, and concentrate by rotary evaporation at a vacuum degree of 0.1 MPa and 100° C. until the mass concentration of NMMO is 86.7%.
[0016] Furthermore, the specific method of forming the film by scraping in step 2) comprises the following steps:
[0017] a. Use a fully automatic coating machine for scraping, the coating machine glass plate temperature is 70 ~ 80 ℃, the scraping distance is 260mm, the scraping speed is 30mm / s, the casting liquid is poured on the glass plate of the coating machine, and the coating is automatically applied after constant temperature for 2min;
[0018] b. After coating, immerse the glass plate of the coating machine into a coagulation bath solution and perform coagulation bath at room temperature until a thin film is formed; the coagulation bath solution is deionized water.
[0019] Furthermore, in the step 1), the plant fiber and the inorganic salt are sequentially added to the NMMO solvent, and reacted for 1 hour under the conditions of a vacuum degree of 0.1 MPa, a 100°C water bath, and mechanical stirring at a speed of 60 rpm; in the step 2), the film is immersed in deionized water at 10°C; in the step 3), the film is dried at 25°C and 50% humidity.
[0020] The present invention uses two special inorganic salts to regulate the degree of polymerization in the process of preparing regenerated cellulose, so that the fiber degree of polymerization can be accurately controlled within a certain range, thereby meeting various requirements for the viscosity of the raw material liquid and the strength of the finished fiber in the subsequent spinning process; compared with the method of controlling the degree of polymerization through raw material selection, the method of regulating the degree of polymerization of cellulose in the present invention is more convenient, accurate and reliable. Description of the drawings:
[0021] Figure 1 Line graph showing the change of regenerated cellulose DP with KCl concentration in Example 1 of the present invention.
[0022] Figure 2 In Example 2 of the present invention, regenerated cellulose DP is mixed with MgCl 2 Line graph of concentration changes. Specific implementation method:
[0023] The technical scheme and effects of the present invention are further described below in conjunction with the embodiments and drawings.
[0024] Example 1
[0025] 1. Preparation of regenerated cellulose products:
[0026] 1) Add hardwood pulp foil and KCl to NMMO solvent in sequence, and react for 1 hour under the conditions of vacuum degree of 0.1 MPa, 100°C water bath, and mechanical stirring at a speed of 60 rpm;
[0027] Among them, the above-mentioned NMMO solvent is a concentrated NMMO aqueous solution with a mass concentration of 86.7%, which is obtained by adding an appropriate amount of propyl gallate antioxidant to a NMMO aqueous solution with a mass concentration of 50%, and then concentrating it by rotary evaporation at a vacuum degree of 0.1 MPa and 100°C; the addition amount of the above-mentioned hardwood pulp foil in the NMMO solvent is 5wt%; the mass concentration of KCl in the NMMO solvent is 6%.
[0028] 2) The solution after the reaction is used as a casting liquid, and a fully automatic coating machine is used for scraping. The temperature of the coating machine glass plate is 75°C, the scraping distance is 260mm, and the scraping speed is 30mm / s. The casting liquid is poured on the coating machine glass plate, and the film is automatically coated after the constant temperature is maintained for 2 minutes; after coating, the coating machine glass plate is immersed in deionized water, and a coagulation bath is performed at room temperature. After the solvent is fully exchanged, a thin film is formed; the film is soaked in 10°C deionized water for 3 days, and the deionized water is replaced every 12 hours during the soaking process;
[0029] 3) The soaked film is completely dried at 25° C. and 50% humidity to obtain a regenerated cellulose film product A.
[0030] In order to obtain regenerated cellulose membrane products with different DP in this example, the mass concentration of KCl in NMMO solvent in step 1) was adjusted to 7%, 8%, 9% and 10%, respectively, to obtain regenerated cellulose membrane products B, C, D and E, respectively.
[0031] 2. Determination of regenerated cellulose DP:
[0032] The regenerated cellulose film products A, B, C, D, and E obtained above were dried in an oven at 105° C. until absolutely dry, and the DP of each of the regenerated cellulose products was measured with reference to the method for measuring the intrinsic viscosity value in the copper ethylenediamine (CED) solution of pulp in GB / T1548-2016.
[0033] Weigh 0.35g of absolute dry sample of each product, accurate to ±0.5mg, and put it into a 50ml dissolution bottle. Weigh another portion as a parallel sample.
[0034] Use a pipette to take 25 ml of deionized water and add it to the dissolution bottle. Add 5 to 10 copper wires into the bottle and perform ultrasonic vibration until the regenerated cellulose in the dissolution bottle is evenly dispersed.
[0035] Then, 25 ml of 1 mol / L CED solution was added and stirred for 15 min. After the cellulose was dissolved, the constant temperature water bath was connected to the viscometer and the water bath temperature was adjusted to 25 °C within the range of (25 ± 0.1 °C).
[0036] Pipette the test liquid into the capillary viscometer to ensure that the solution flows out smoothly. Start timing when the concave page reaches the highest scale line and end timing when it reaches the lowest scale line. Record the time for the solution to flow out, accurate to (±0.2s). Test each solution twice. The measurement result error is within 0.5%. Calculate the average value as the outflow time.
[0037] First, calculate the relative viscosity according to the formula: η ratio =η / η 0 =h×t, where:
[0038] η——Viscosity of sample
[0039] η 0 ——Sample viscosity
[0040] h——Viscometer constant
[0041] t——solution outflow time
[0042] According to the relative viscosity η ratio The value of η×ρ can be obtained by looking up the value of GB / T1548-2016 Appendix table, where ρ is the density; η is obtained by calculation;
[0043] According to the formula: DP 0.905 =0.75η and the DP of cellulose was calculated.
[0044] The polymerization degrees of the regenerated cellulose film products A, B, C, D, and E obtained in Example 1 are measured and are shown in Table 1.
[0045] Example 1 Degree of polymerization of each regenerated cellulose product
[0046] Product A Product B Product C Product D Product E DP 478 500 510 520 530
[0047] It can be seen from Table 1 that as the mass concentration of KCl in NMMO solvent increases, the DP of regenerated cellulose membrane products also increases, and the two show a positive correlation within a certain range of KCl concentrations, such as Figure 1 As shown in the figure, regression analysis shows that the relationship between the two is consistent with the following regression equation:
[0048] Y=-1.4286X 2 +35.457X+318.23, R2=0.9872; where:
[0049] Y——Degree of polymerization of regenerated cellulose
[0050] X——mass concentration of KCl (wt%).
[0051] Example 2
[0052] 1. Preparation of regenerated cellulose products:
[0053] 1) Combine hardwood pulp foil and MgCl 2 Add them into NMMO solvent in sequence, and react for 1 h in a water bath at 100°C and vacuum degree of 0.1 MPa, with mechanical stirring at 60 rpm;
[0054] The NMMO solvent is a concentrated NMMO aqueous solution with a mass concentration of 86.7%, which is obtained by adding an appropriate amount of propyl gallate antioxidant to a NMMO aqueous solution with a mass concentration of 50%, and then concentrating it by rotary evaporation at a vacuum degree of 0.1 MPa and 100°C; the amount of the hardwood pulp foil added to the NMMO solvent is 5wt%; MgCl 2 The mass concentration in NMMO solvent is 1%.
[0055] 2) The solution after the reaction is used as a casting liquid, and a fully automatic coating machine is used for scraping. The temperature of the coating machine glass plate is 75°C, the scraping distance is 260mm, and the scraping speed is 30mm / s. The casting liquid is poured on the coating machine glass plate, and the film is automatically coated after the constant temperature is maintained for 2 minutes; after coating, the coating machine glass plate is immersed in deionized water, and a coagulation bath is performed at room temperature. After the solvent is fully exchanged, a thin film is formed; the film is soaked in 10°C deionized water for 3 days, and the deionized water is replaced every 12 hours during the soaking process;
[0056] 3) The soaked film is completely dried at 25° C. and 50% humidity to obtain a regenerated cellulose film product F.
[0057] In order to obtain regenerated cellulose membrane products with different DP in this example, MgCl 2 The mass concentrations in NMMO solvent were adjusted to 1.5%, 2%, 2.5% and 3%, respectively, and regenerated cellulose membrane products G, H, I and J were obtained accordingly.
[0058] 2. Determination of regenerated cellulose DP:
[0059] The DP of the regenerated cellulose film products F, G, H, I, and J obtained above was measured in the same manner as in Example 1.
[0060] The results are shown in Table 2 and Figure 2 As shown. 2 With the increase of NMMO solvent concentration, the DP of regenerated cellulose membrane products decreased. 2 There is a negative correlation within a certain concentration range.
[0061] Example 2 Degree of polymerization of each regenerated cellulose product
[0062] Product F Product G Product H Product I Product J DP 482 475 463 450 440
[0063] Regression analysis showed that the DP of regenerated cellulose increased with MgCl 2 The relationship between the concentration changes is consistent with the following regression equation:
[0064] Y=-2X 2-13.8X+498.6, R2=0.9947; where:
[0065] Y——Degree of polymerization of regenerated cellulose
[0066] X——MgCl 2 The mass concentration (wt%) of
Claims
1. A method for preparing regenerated cellulose with controllable degree of polymerization: Features The steps include: 1) Add plant fiber and inorganic salt to NMMO solvent in sequence, and stir to react for 1 hour under vacuum degree 0.1 MPa and 100°C; 2) using the reacted solution as a casting solution, forming a thin film by doctor blade coating, and soaking the thin film in deionized water for at least 3 days, replacing the deionized water every 12 hours during the soaking process; 3) completely drying the soaked film to obtain a regenerated cellulose film product; The inorganic salt in step 1) is KCl or MgCl 2 ;in: The KCl is used to increase the polymerization degree of the regenerated cellulose finally obtained, and the polymerization degree of the regenerated cellulose is positively correlated with the concentration of KCl in the NMMO solution, and the mass concentration of the KCl in the NMMO solution is not higher than 10%; The MgCl 2 It is used to reduce the degree of polymerization of the regenerated cellulose obtained. The degree of polymerization of the regenerated cellulose is related to MgCl 2 The concentration of MgCl in NMMO solution is negatively correlated 2 The mass concentration in the NMMO solution is not higher than 3%.
2. The method for preparing regenerated cellulose according to claim 1: Features: When the inorganic salt in step 1) is KCl, its mass concentration in the NMMO solvent is 6-10%; when the inorganic salt is MgCl 2 When the mass concentration of NMMO solvent is 1-3%.
3. The method for preparing regenerated cellulose according to claim 1 or 2, Features: The plant fiber in step 1) is hardwood fiber, and the amount of the plant fiber added to the NMMO solvent is 5 wt %; the NMMO solvent is a concentrated NMMO aqueous solution with a mass concentration of 86.7%.
4. The method for preparing regenerated cellulose according to claim 3, Features: The NMMO concentrated aqueous solution is obtained as follows: add an appropriate amount of propyl gallate antioxidant to an NMMO aqueous solution with a mass concentration of 50%, and concentrate by rotary evaporation at a vacuum degree of 0.1 MPa and 100° C. until the mass concentration of NMMO is 86.7%.
5. The method for preparing regenerated cellulose according to claim 3, Features: The specific method of forming the film by scraping in step 2) comprises the following steps: a. Use a fully automatic coating machine for scraping, the coating machine glass plate temperature is 70 ~ 80 ℃, the scraping distance is 260mm, the scraping speed is 30mm / s, the casting liquid is poured on the glass plate of the coating machine, and the coating is automatically applied after constant temperature for 2min; b. After coating, immerse the glass plate of the coating machine into deionized water and place it in a coagulation bath at room temperature until a thin film is formed.
6. The method for preparing regenerated cellulose according to claim 3, Features: In the step 1), the plant fiber and the inorganic salt are sequentially added to the NMMO solvent, and reacted for 1 hour under the conditions of a vacuum degree of 0.1 MPa, a 100° C. water bath, and mechanical stirring at a speed of 60 rpm; in the step 2), the film is immersed in deionized water at 10° C.; in the step 3), the film is dried at 25° C. and 50% humidity.
Citation Information
Patent Citations
Production method of regenerated cellulose nanofiltration membrane
CN105597551A
Preparation method of antibacterial cellulose flat nanofiltration membrane
CN106474944A
Composite thin membrane with multilayer composite structure and preparation method thereof
CN106739363A
Preparation method of regenerated cellulose based cross-linked modified nanofiltration membrane
CN107551832A
Preparation method of ion-doped cellulose gas separation membrane and cellulose gas separation membrane
CN108607372A
Cited By