Polyphenol phosphate ester chain-extended polyurethane foam material and preparation method thereof
Through the combination of polyphenol phosphate and prepolymers, high-strength, toughness and self-healing polyurethane foam materials are formed, which solves the problem of vulnerability of existing polyurethane foam materials under mechanical loads and harsh environments, and through Conjugation improves the stability of the material and achieves performance maintenance in extreme environments.
Patent Information
- Application Number
- CN202411236755.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-04
AI Technical Summary
Existing polyurethane foam materials are prone to damage under high mechanical loads and harsh environments, and the stability and application of plant extracts are limited, limiting their application efficiency in engineering materials.
Polyphenol phosphate as cross-linked foaming agent mixed with prepolymers, polytetrahydrofuran ether glycol, Tween 80, silicone oil and dibutyltin dilaurate, reacted under the protection of inert gas to form high strength, toughness and self-contained The polyurethane foam material uses the conjugation of phytic acid and tannin to improve material stability.
It significantly improves the mechanical strength and toughness of polyurethane foam materials, and can maintain stable performance in extreme environments, including high temperature, radiation, acid, alkali and high metal ion content environments, extending the service life of the material.
Smart Images

Figure CN119060285A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyphenol phosphate chain-extended polyurethane foam material and a preparation method thereof, belonging to the technical field of polyurethane. Background Art
[0002] Polyurethane elastomer is a material with a unique soft and hard phase separation microstructure. By changing the processing method, polyurethane elastomers with different morphologies and properties can be obtained, which have unique application value in many fields. Among them, flexible polyurethane foam (PUF) is usually synthesized by water foaming. In this process, the isocyanate group reacts with water to form a urea bond and release carbon dioxide gas. PUF is highly porous and has the advantages of low density, compression resistance, heat insulation, and damping capacity. Therefore, they are widely used in building materials, heat insulation, transportation industry, military equipment and other fields.
[0003] However, there are still many limitations to the current PUF. First, the mechanical properties of PUF, such as strength and toughness, are limited by its highly porous structure. Under large mechanical loads or deformations, irreversible damage may occur. This porous structure easily causes stress concentration, making PUF extremely susceptible to puncture stress. This significantly affects the application effect of PUF as an engineering material. Secondly, it is common for PUF to face complex and harsh environments in practice, including heat, radiation, salinity, etc. Long-term exposure to such harsh environments will lead to serious aging of the material structure, resulting in an irreversible and significant reduction in mechanical and other properties. The above bottlenecks significantly restrict the application efficiency of PUF. Therefore, there is an urgent need to develop PUFs with excellent mechanical properties, high self-healing efficiency, and durability to various environments.
[0004] Researchers are committed to finding natural substances to improve the performance of PUF materials. Plants are rich in a variety of organic compounds with unique microstructures. For example, organic phosphates such as phytic acid (PA) and polyphenols such as tannic acid. They have high water solubility, high functionality and central symmetric molecular structures, providing sufficient binding sites for the construction of functional polymers. Polyphenol groups and phosphate groups have a variety of physical and chemical bonding properties, such as covalent bonds, hydrogen bonds, ionic bonds, chelate bonds, etc. However, such plant extracts are easily oxidized, which highly limits the long-term stability in applications. Furthermore, such substances can easily chelate with metal ions, resulting in the inactivation of functional groups and the formation of large-scale metal organic aggregates. This limits their application scenarios in contact with metal elements. In addition, phytic acid and tannic acid are both nucleophiles with high steric hindrance effects. It is difficult for them to undergo electrophilic chemical reactions. This largely limits the design and synthesis principles of their derivatives. Therefore, the application of plant extracts in PUF is still very limited. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a polyphenol phosphate chain-extended polyurethane foam material and a preparation method thereof.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows.
[0007] A polyphenol phosphate chain-extended polyurethane foam material, with the total mass of raw materials for preparing the polyurethane foam material being 100%, the raw material components and their mass fractions are as follows: prepolymer: 42%-50%, polytetramethylene ether glycol (PTMEG): 45%-54.5%, Tween 80: 0.5%-1%, silicone oil: 0.5%-1%, dibutyltin dilaurate: 0.1%-0.2%, H2O solution of polyphenol phosphate: 2%-3%;
[0008] The prepolymer is a prepolymer having an -NCO value between 12 and 14 formed by reacting diisocyanate and polytetramethylene glycol under a protective gas atmosphere at 80 to 90° C. with stirring for 2 to 4 hours;
[0009] In the H2O solution of the polyphenol phosphate, the mass fraction of the polyphenol phosphate is 70% to 75%, and the mass fraction of H2O is 25% to 30%;
[0010] The structural formula of the polyphenol phosphate is:
[0011]
[0012] Among them, any one of R1, R2, and R3 is The other two groups are -H.
[0013] Preferably, the total mass of the raw materials for preparing the prepolymer is 100%, the mass fraction of the diisocyanate is 45% to 50%, and the mass fraction of the polytetramethylene ether diol is 50% to 55%.
[0014] Preferably, the molecular weight of the polytetramethylene ether glycol is 1000-2000.
[0015] Preferably, the polyphenol phosphate is prepared by the following method, which comprises the following steps:
[0016] (1) Under the protection of inert gas, dicyandiamide, urea and phytic acid are dissolved in dimethyl sulfoxide (DMSO) in a mass ratio of 2-3:4-6:20, and stirred at 90-130° C. to mix and dissolve, and the stirring rate is 100-200 r / min to obtain a mixture;
[0017] (2) Under a nitrogen environment, tannic acid is added to the mixture, and the mass ratio of tannic acid to phytic acid is 1:1.5-2.5; the mixture is reacted at 90-130° C. for 1-4 hours. After the reaction is completed, the mixture is centrifuged, washed, vacuum dried, and ground in a weakly polar organic solvent to obtain a polyphenol phosphate ester; more preferably, the weakly polar organic solvent is one or more of glycerol, ethyl acetate, ether, anhydrous ethanol, and anhydrous methanol.
[0018] Preferably, the tensile strength of the polyurethane foam material is 8.5-12.5 MP, and the elongation at break is 400%-600%.
[0019] A method for preparing a polyphenol phosphate chain-extended polyurethane foam material according to the present invention comprises the following steps:
[0020] The polyphenol phosphate is dissolved in H2O to obtain a H2O solution of the polyphenol phosphate; then the prepolymer, PTMEG, Tween 80, silicone oil, dibutyltin dilaurate and the H2O solution of the polyphenol phosphate are mixed, stirred at 1200-1500 r / min for 10-15s, poured into a mold, and cured to obtain a polyphenol phosphate chain-extended polyurethane foam material.
[0021] Beneficial Effects
[0022] The present invention provides a polyurethane foam material with chain extension of polyphenol phosphate, wherein a homogeneous solution of polyphenol phosphate and H2O is used as a cross-linking foaming agent, and is mixed with a prepolymer, PTMEG, Tween 80, silicone oil, and dibutyltin dilaurate to obtain a PUF material (TP-PUF) with high strength, strong toughness, self-healing, environmental protection and durability. Compared with the existing PUF, the mechanical strength of TP-PUF is significantly improved, which can reach more than 8MPa, close to the level of ordinary non-foamed polyurethane elastomers. The unique microstructure also enables TP-PUF to maintain stable performance in extreme environments (such as continuous high temperature, long-term ultraviolet (UV) radiation, acid, alkali and high-content metal ion environment).
[0023] The invention provides a polyurethane foam material with chain extension of polyphenol phosphate, wherein the polyphenol phosphate is obtained by esterifying phytic acid and tannic acid, and a highly hydrophilic composite is synthesized by a synergistic water absorption / dehydration technology; the structure and properties of the polyphenol substance are improved, a complex functionalized structure is constructed, and the functional integration of bio-based macromolecules is achieved through the complementary advantages and synergistic effect of the two molecules of phytic acid and tannic acid. In addition, through the conjugation of phytic acid and tannic acid, the stability of the polymer compound is improved and the influence of metal ions is reduced. The aqueous solution of polyphenol phosphate is used as a composite cross-linking agent, and hydrogen bonds form a more uniform cross-linking structure and interaction inside the material, and the homogeneous cross-linking agent is conducive to forming a more uniform pore structure.
[0024] The present invention provides a method for preparing a polyurethane foam material with chain extension of polyphenol phosphate, wherein a cross-linking agent polyphenol phosphate is dissolved in H2O to obtain a homogeneous cross-linking foaming agent, thereby achieving simultaneous foaming and cross-linking processes. The content of polyphenol phosphate and H2O is an important condition for regulating the physical properties of the material. By adjusting the content of the cross-linking agent polyphenol phosphate and H2O in the raw material, polyurethane foam materials with different strengths can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1-2 These are the mechanical strength test results of the polyurethane foam materials described in Examples 2-5.
[0026] Figure 3 These are the cyclic tensile test results of the polyurethane foam materials described in Example 5 and Comparative Example 1.
[0027] Figure 4-5 The mechanical properties test results of the polyurethane foam materials described in Example 5 and Comparative Example 1 at 100°C are shown.
[0028] Figure 6 The mechanical properties test results of the polyurethane foam materials described in Example 5 and Comparative Example 3 after being immersed in a metal ion solution for 72 hours. DETAILED DESCRIPTION
[0029] The present invention will be further described in detail below in conjunction with specific embodiments.
[0030] Example 1
[0031] 1.TP preparation:
[0032] (1) Dissolve 2.5 g of the catalyst dicyandiamide, 5 g of urea, and 20 g of TA in DMSO and add them to a three-necked flask. Install a water separator and a condenser. Install the reaction device in a constant temperature stirrer with a stirring rate of 100 r / min. Stir the raw materials until they are evenly mixed and completely dissolved. The reaction temperature is 90°C.
[0033] (2) After TA is dissolved, 20 ml of 70% PA aqueous solution is added and reacted for 2 h under nitrogen atmosphere. The solution after the reaction is poured into excess anhydrous ethanol to precipitate the product, and a solid is obtained after centrifugation.
[0034] (3) washing the product in step (2) with a solvent and then centrifuging to separate the solid, repeating the process three times to obtain a final solid product, drying it at 80° C. in a vacuum environment, and grinding it to obtain a polyphenol phosphate powder (TP).
[0035] 2.TP-PUF preparation:
[0036] (1) Prepolymer synthesis: According to the ratio of substance amount IPDI:PTMEG2000=6:1, react at 80°C for 2h to obtain a prepolymer.
[0037] (2) Foaming reaction: 2.0 g TP was dissolved in 0.8 g water. 45.5 g prepolymer, 50 g PTMEG2000, 2.8 g TP aqueous solution, 0.1 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at a speed of 1500 r / min for 15 seconds using a shear mixer, and then poured into a mold for molding. After standing for 2 hours, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material.
[0038] The structural formula of the polyphenol phosphate is:
[0039]
[0040] Among them, R1 is R2 and R3 are -H.
[0041] Example 2
[0042] 1.TP preparation:
[0043] (1) Dissolve 2.5 g of the catalyst dicyandiamide, 5 g of urea, and 20 g of TA in DMSO and add them to a three-necked flask. Install a water separator and a condenser. Install a water separator and a condenser. Install the reaction device in a constant temperature stirrer with a stirring rate of 200 r / min. Stir the raw materials until they are evenly mixed and completely dissolved. The reaction temperature is 130°C.
[0044] (2) After TA is dissolved, 20 ml of 70% PA aqueous solution is added and reacted for 4 h under nitrogen atmosphere. The solution after the reaction is poured into anhydrous ethanol to precipitate the product, and a solid is obtained after centrifugal separation.
[0045] (3) washing the product in step (2) with a solvent and then centrifuging to separate the solid, repeating the process three times to obtain a final solid product, drying it at 80° C. in a vacuum environment, and grinding it to obtain a polyphenol phosphate powder (TP).
[0046] 2.TP-PUF preparation:
[0047] (1) Prepolymer synthesis: According to the ratio of substance amount IPDI:PTMEG2000=6:1, the reaction was carried out at 80°C for 4 hours to obtain a prepolymer.
[0048] (2) Foaming reaction: 2.0 g TP was dissolved in 1 g water. 50 g prepolymer, 45.3 g PTMEG2000, 3 g TP aqueous solution, 0.1 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at a speed of 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material, which was recorded as T-P5-PUF-1.
[0049] Example 3
[0050] 1.TP preparation:
[0051] (1) Dissolve 2.5 g of the catalyst dicyandiamide, 5 g of urea, and 20 g of TA in DMSO and add them to a three-necked flask. Install a water separator and a condenser. Install a water separator and a condenser. Install the reaction device in a constant temperature stirrer with a stirring rate of 200 r / min. Stir the raw materials until they are evenly mixed and completely dissolved. The reaction temperature is 130°C.
[0052] (2) After TA is dissolved, 20 ml of 70% PA aqueous solution is added and reacted for 4 h under nitrogen atmosphere. The solution after the reaction is poured into anhydrous ethanol to precipitate the product, and a solid is obtained after centrifugal separation.
[0053] (3) washing the product in step (2) with a solvent and then centrifuging to separate the solid, repeating the process three times to obtain a final solid product, drying it at 80° C. in a vacuum environment, and grinding it to obtain a polyphenol phosphate powder (TP).
[0054] 2.TP-PUF preparation:
[0055] (1) Prepolymer synthesis: According to the molar ratio of TDI:PTMEG2000=6:1, the reaction was carried out at 80°C for 2h to obtain a prepolymer.
[0056] (2) Foaming reaction: 1.75 g TP was dissolved in 1 g water. 45.45 g prepolymer, 50 g PTMEG2000, 2.75 g TP aqueous solution, 0.2 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at a speed of 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material, which was recorded as T-P5-PUF-2.
[0057] Example 4
[0058] 1.TP preparation:
[0059] (1) Dissolve 2.5 g of the catalyst dicyandiamide, 5 g of urea, and 20 g of TA in DMSO and add them to a three-necked flask. Install a water separator and a condenser. Install a water separator and a condenser. Install the reaction device in a constant temperature stirrer with a stirring rate of 200 r / min. Stir the raw materials until they are evenly mixed and completely dissolved. The reaction temperature is 130°C.
[0060] (2) After TA is dissolved, 20 ml of 70% PA aqueous solution is added and reacted for 4 h under nitrogen atmosphere. The solution after the reaction is poured into anhydrous ethanol to precipitate the product, and a solid is obtained after centrifugal separation.
[0061] (3) washing the product in step (2) with a solvent and then centrifuging to separate the solid, repeating the process three times to obtain a final solid product, drying it at 80° C. in a vacuum environment, and grinding it to obtain a polyphenol phosphate powder (TP).
[0062] 2.TP-PUF preparation:
[0063] (1) Prepolymer synthesis: According to the molar ratio of HDI:PTMEG2000=6:1, the reaction was carried out at 80°C for 2h to obtain a prepolymer.
[0064] (2) Foaming reaction: 1.5 g TP was dissolved in 1 g water. 45.7 g prepolymer, 50 g PTMEG2000, 2.5 g TP aqueous solution, 0.2 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at a speed of 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material, which was recorded as T-P5-PUF-3.
[0065] Example 5
[0066] 1.TP preparation:
[0067] (1) Dissolve 2.5 g of the catalyst dicyandiamide, 5 g of urea, and 20 g of TA in DMSO and add them to a three-necked flask. Install a water separator and a condenser. Install a water separator and a condenser. Install the reaction device in a constant temperature stirrer with a stirring rate of 200 r / min. Stir the raw materials until they are evenly mixed and completely dissolved. The reaction temperature is 130°C.
[0068] (2) After TA is dissolved, 20 ml of 70% PA aqueous solution is added and reacted for 4 h under nitrogen atmosphere. The solution after the reaction is poured into anhydrous ethanol to precipitate the product, and a solid is obtained after centrifugal separation.
[0069] (3) washing the product in step (2) with a solvent and then centrifuging to separate the solid, repeating the process three times to obtain a final solid product, drying it at 80° C. in a vacuum environment, and grinding it to obtain a polyphenol phosphate powder (TP).
[0070] 2.TP-PUF preparation:
[0071] (1) Prepolymer synthesis: According to the molar ratio of MDI:PTMEG2000=6:1, the reaction was carried out at 80°C for 4 hours to obtain a prepolymer.
[0072] (2) Foaming reaction: 2 g of TP was dissolved in 1 g of water. 47.5 g of prepolymer, 48 g of PTMEG2000, 3 g of TP aqueous solution, 0.2 g of dibutyltin dilaurate, 0.8 g of Tween 80 and 0.5 g of silicone oil were mixed, and the mixture was rapidly stirred at a speed of 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material, which was recorded as T-P5-PUF-4.
[0073] Comparative Example 1
[0074] 2.BDO-PUF preparation:
[0075] (1) Prepolymer synthesis: According to the ratio of substance amount IPDI:PTMEG2000=6:1, react at 80°C for 2h to obtain a prepolymer.
[0076] (2) Foaming reaction: 2.0 g 1,4-butanediol (BDO) was dissolved in 0.8 g water. 45.5 g prepolymer, 50 g PTMEG2000, 2.8 g BDO aqueous solution, 0.1 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material. This was designated as BDO-PUF-1.
[0077] Comparative Example 2
[0078] 2.BDO-PUF preparation:
[0079] (1) Prepolymer synthesis: According to the ratio of substance amount IPDI:PTMEG2000=6:1, react at 80°C for 2h to obtain a prepolymer.
[0080] (2) Foaming reaction: 2.0 g 1,4-butanediol (BDO) was dissolved in 1 g water. 45.5 g prepolymer, 49.8 g PTMEG2000, 3 g BDO aqueous solution, 0.1 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material. This was designated as BDO-PUF-2.
[0081] Comparative Example 3
[0082] 2. TA-PUF preparation:
[0083] (1) Prepolymer synthesis: According to the ratio of substance amount IPDI:PTMEG2000=6:1, react at 80°C for 2h to obtain a prepolymer.
[0084] (2) Foaming reaction: 2.0 g TA was dissolved in 1 g water. 45.5 g prepolymer, 49.8 g PTMEG2000, 3 g TP aqueous solution, 0.1 g dibutyltin dilaurate, 0.6 g Tween 80 and 1 g silicone oil were mixed, and the mixture was rapidly stirred at 1500 r / min for 15 s using a shear mixer, and then poured into a mold for molding. After standing for 2 h, the mixture was taken out to obtain a polyphenol phosphate chain-extended polyurethane foam material. This was recorded as TA-PUF.
[0085] The polyurethane foam materials prepared in Examples 2-5 and Comparative Examples 1-2 were tested for mechanical strength. The results are as follows: Figure 1-2 As shown in the figure, the tensile properties of the PUF material with TP chain extension are significantly improved compared with the control group with BDO chain extension, and its tensile strength, elongation at break, and tensile toughness are increased to 190%, 200%, and 400%, respectively. The tensile strength can reach more than 8.5MPa, even close to the tensile strength of non-foamed polyurethane elastomer materials (about 10MPa).
[0086] The polyurethane foam material described in Example 5 was subjected to a cyclic tensile test. The results are as follows: Figure 3 When TP-PUF is stretched to 5 times its original length multiple times, the material can effectively absorb and dissipate external energy, avoid fatigue damage, and show good toughness and resilience.
[0087] The catechol structure in TP has a strong antioxidant effect, which inhibits the possible thermal oxidative aging of the material. The urethane bond formed by phenolic hydroxyl group and isocyanate is usually unstable and easily dissociates under the action of heating, thus affecting the thermal stability of the material. However, in this application, the conjugation effect of the phenolic hydroxyl group in TP greatly improves the structural stability. In addition, the phosphate group quenches the free radicals generated during the oxidation process and terminates further oxidation reactions. The test results are as follows Figure 4-5 As shown in the figure, after being placed in an oven at 100°C for 24 hours, the mechanical strength and elongation at break of BDO-PUF in Comparative Example 1 decreased by 26% and 11%, respectively. However, even after being placed in a high temperature environment at 100°C for 48 hours, the mechanical strength and elongation at break of TP-PUF did not decrease.
[0088] TA and PA have polyphenols and phosphate groups. 3+ In the solution of metal ions, a large complex precipitate will be formed. However, there is a conjugation effect between the TA and PA structures in TP, which improves the stability of the compound. Compared with TA, TP is less susceptible to metal ions. The stability test results of the material under different environments are as follows: Figure 6 As shown in the figure, the TA-PUF polyurethane foam material with TA chain extension is in 0.1 mol / L Fe 3+ After 72 hours of immersion in aqueous solution, the mechanical properties decreased by more than 30%, and the color of the material turned black significantly. This is because TA forms complexes with metal ions, forming large-sized stress concentration points and defects in the foam material, which deteriorates the mechanical properties of the material. Due to the conjugated stability of TP, TP-PUF is not stable in 0.1 mol / L Fe 3+ , Cu 2+ 、Al 3+ , Ga 2+ 、Zn 2+ The performance can be kept stable in the environment of aqueous solution of metal ions with strong chelating ability. The multi-level hydrogen bonds formed between TP and phenolic hydroxyl and phosphate groups, and the chemical bond cross-linking structure formed between TP and PTMEG enable TP-PUF to maintain its basic structure in organic solvents without being dissolved. It only swells slightly after long-term immersion, and the mechanical strength and elongation at break do not change significantly. It also maintains stable performance in alkaline environments.
[0089] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A polyurethane foam material with chain extension of polyphenol phosphate, Features: Taking the total mass of the raw materials for preparing the polyurethane foam material as 100%, the raw material components and their mass fractions are as follows: prepolymer: 42% to 50%, polytetramethylene glycol: 45% to 54.5%, Tween 80: 0.5% to 1%, silicone oil: 0.5% to 1%, dibutyltin dilaurate: 0.1% to 0.2%, H of polyphenol phosphate ester 2 O solution: 2% to 3%; The prepolymer is a prepolymer having an -NCO value between 12 and 14 formed by reacting diisocyanate and polytetramethylene glycol under a protective gas atmosphere at 80 to 90° C. with stirring for 2 to 4 hours; The H 2 In the O solution, the mass fraction of polyphenol phosphate is 70% to 75%, and the H 2 The mass fraction of O is 25% to 30%; The structural formula of the polyphenol phosphate is: Among them, R 1 , R 2 , R 3 Any group in The other two groups are -H.
2. The polyurethane foam material of claim 1 wherein the polyphenol phosphate chain is extended. Features: The total mass of the raw materials for preparing the prepolymer is 100%, the mass fraction of the diisocyanate is 45% to 50%, and the mass fraction of the polytetramethylene ether diol is 50% to 55%.
3. The polyurethane foam material of claim 1 wherein the polyphenol phosphate chain is extended. Features: The molecular weight of the polytetramethylene ether glycol is 1000-2000.
4. The polyurethane foam material of claim 1 wherein the polyphenol phosphate chain is extended. Features: The polyphenol phosphate is prepared by the following method, which comprises the following steps: (1) Under the protection of inert gas, dicyandiamide, urea and phytic acid are dissolved in dimethyl sulfoxide in a mass ratio of 2-3:4-6:20, and stirred at 90-130° C. to mix and dissolve, and the stirring rate is 100-200 r / min to obtain a mixture; (2) Under a nitrogen environment, tannic acid is added to the mixture, and the mass ratio of tannic acid to phytic acid is 1:1.5-2.5; the mixture is reacted at 90-130° C. for 1-4 hours. After the reaction is completed, the mixture is centrifuged in a weakly polar organic solvent, washed, vacuum dried, and ground to obtain a polyphenol phosphate.
5. A polyphenol phosphate chain-extended polyurethane foam material as claimed in claim 4, Features: The weakly polar organic solvent is one or more of glycerol, ethyl acetate, ethyl ether, anhydrous ethanol and anhydrous methanol.
6. A polyurethane foam material with chain extension of polyphenol phosphate according to any one of claims 1 to 5, Features: The tensile strength of the polyurethane foam material is 8.5-12.5 MP, and the elongation at break is 400%-600%.
7. A method for preparing a polyurethane foam material chain-extended by polyphenol phosphate as claimed in any one of claims 1 to 6, Features: The method steps include: Dissolve polyphenol phosphates in H 2 O to obtain polyphenol phosphate esters 2 O solution; then prepolymer, polytetramethylene glycol, Tween 80, silicone oil, dibutyltin dilaurate and polyphenol phosphate H 2 The mixture is mixed with a polyphenol phosphate chain-extended polyurethane foam material, stirred at 1200-1500 r / min for 10-15 seconds, poured into a mold, and cured to obtain a polyphenol phosphate chain-extended polyurethane foam material.
Citation Information
Patent Citations
Low-density high-strength polyurethane foam as well as preparation method and application thereof
CN113248681A
Functionalized carbon nanotube / polyurethane composite material and preparation method thereof
CN116217878A
Polyphenol phosphate ester and preparation method thereof
CN117327114A
Process for producing soft polyurethane foam, process for producing conductive soft polyurethane foam, conductive roll and process for producing the same
WO2005061571A1