Ionic polymer oxygen-absorbing composite material as well as preparation method and application thereof

The ion polymer oxygen-absorbing composite material addresses solvent resistance issues by forming a zwitterionic polymer with a dynamic cross-linked network, enhancing transparency and mechanical properties for effective QR code scanning and oxygen absorption.

CN119060485AActive Publication Date: 2024-12-03四川大学青岛研究院 +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411176130.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing oxygen absorbents in beer and beverage packaging have poor solvent resistance, leading to transparency issues that affect QR code scanning due to their linear molecular chain structure.

Method used

A method for preparing an ion polymer oxygen-absorbing composite material using methacrylic acid, dimethylaminoethyl methacrylate, and styrene to form a zwitterionic polymer with a dynamic cross-linked network, combined with hydrogenated styrene-butadiene block copolymer and an oxygen scavenger, ensuring excellent transparency and mechanical properties.

Benefits of technology

The composite material maintains transparency and enhances solvent resistance, elasticity, and tensile strength, improving QR code scanning success rates and oxygen absorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060485A_ABST
    Figure CN119060485A_ABST
Patent Text Reader

Abstract

The invention discloses an ionic polymer oxygen-absorbing composite material as well as a preparation method and application thereof, and relates to the technical field of high polymer materials. The preparation method of the ionic polymer oxygen absorption composite material comprises the following steps: providing methacrylic acid, dimethylaminoethyl methacrylate and styrene, mixing and reacting to obtain an ionic polymer; and mixing the ionic polymer with the hydrogenated styrene-butadiene block copolymer, white oil and an oxygen scavenger, and reacting to obtain the ionic polymer oxygen absorption composite material. The ionic polymer oxygen uptake composite material provided by the invention has excellent oxygen uptake, transparency and strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to an ion polymer oxygen-absorbing composite material and a preparation method and application thereof. Background Art

[0002] Thermoplastic elastomers TPE / TPR are a type of elastomer that has the elasticity of rubber at room temperature and can be plasticized and molded at high temperatures. Thermoplastic elastomers are selected as the substrate of oxygen-absorbing gaskets for beer and beverage packaging, such as SBS, SEBS and SEPS, due to their high elasticity, excellent durability and easy processing. Nowadays, more and more beer or beverage products need to scan the QR code printed on the bottle cap through the oxygen-absorbing gasket.

[0003] However, in the related art, ordinary oxygen absorbents have poor solvent resistance due to their linear molecular chain structure. After being soaked and swollen in beer or beverages for a long time, they will gradually change from transparent to translucent or opaque, affecting the scanning of the QR code on the bottle cap. Summary of the invention

[0004] In view of this, the present application provides an ion polymer oxygen absorbing composite material and a preparation method and application thereof.

[0005] The embodiment of the present application is implemented as follows: a method for preparing an ion polymer oxygen absorbing composite material comprises the following steps:

[0006] Providing methacrylic acid, dimethylaminoethyl methacrylate and styrene, mixing and reacting them to obtain an ionomer;

[0007] The ion polymer is mixed with hydrogenated styrene-butadiene block copolymer, white oil and oxygen scavenger to react and obtain the ion polymer oxygen absorbing composite material.

[0008] Optionally, in some embodiments of the present application, the molar ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is (0.2-0.4): (0.2-0.4): (0.2-0.6); and / or

[0009] The method for preparing the ionic polymer further comprises adding a solvent; and / or

[0010] The method for preparing the ionic polymer further comprises adding a catalyst.

[0011] Optionally, in some embodiments of the present application, the solvent is selected from one or more of ethyl acetate, tetrahydrofuran, chlorobenzene, diethylene glycol monobutyl ether, trimethoxybutanol, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, acetophenone, N,N-dimethylformamide, pyrrole, butyric acid, and cresol; and / or

[0012] The mass ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene to the solvent is 10:(15-25); and / or

[0013] The catalyst is selected from one or more of azobisisobutyronitrile, dicumyl peroxide, and potassium persulfate; and / or

[0014] The mass ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene to the mass ratio of the catalyst is (99.7-99.9): (0.1-0.3).

[0015] Optionally, in some embodiments of the present application, the reaction of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is carried out in an inert atmosphere; and / or

[0016] The reaction of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is carried out under stirring; the stirring speed is 40 rpm to 80 rpm; and / or

[0017] The reaction temperature of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is 60° C. to 80° C., and the reaction time is 6 h to 10 h.

[0018] Optionally, in some embodiments of the present application, the mixing of the ionomer, the hydrogenated styrene-butadiene block copolymer, the white oil, and the oxygen scavenger comprises:

[0019] The white oil and the oxygen scavenger are mixed and ground to obtain a premixed material;

[0020] The premix material is mixed with the ionomer and the hydrogenated styrene-butadiene block copolymer.

[0021] Optionally, in some embodiments of the present application, the mass ratio of the oxygen scavenger to the white oil is 1:(4-20); and / or

[0022] The grinding further comprises adding grinding media; the grinding media comprises grinding balls, and the average particle size of the grinding balls is 0.25 mm to 0.85 mm; and / or

[0023] The grinding speed is 3000 rpm to 3500 rpm; and / or

[0024] The grinding time is 10 min to 15 min.

[0025] Optionally, in some embodiments of the present application, the oxygen scavenger includes one or more of sodium sulfite, bishydroxymethyl ether, and metal powder; and / or

[0026] The mass ratio of the ion polymer, the hydrogenated styrene-butadiene block copolymer, the white oil and the oxygen scavenger is (25-50):(40-50):(10-30):(1-5).

[0027] Optionally, in some embodiments of the present application, the reaction of the ionomer and the hydrogenated styrene-butadiene block copolymer, the white oil, and the oxygen scavenger comprises extrusion molding, wherein:

[0028] The extrusion molding temperature is 180°C to 220°C; and / or

[0029] The rotation speed of the extrusion molding is 200 rpm / min to 500 rpm / min; and / or

[0030] The feeding speed of the extrusion molding is 100r / min to 200r / min.

[0031] Correspondingly, an embodiment of the present application further provides an ion polymer oxygen absorbing composite material, which is prepared by any of the preparation methods described above.

[0032] Correspondingly, an embodiment of the present application further provides a sealing gasket, the material of which includes the composite material prepared by any of the preparation methods described above, or includes the composite material described above.

[0033] The preparation method of the ionic polymer oxygen-absorbing composite material provided by the present application adopts methacrylic acid as an anion unit and dimethylaminoethyl methacrylate as a cationic unit to prepare the zwitterionic polymer through random copolymerization. The side chain volume of the structural unit is large and the molecular chain cannot be arranged regularly, thereby ensuring its transparency. Styrene is used as a comonomer to improve the compatibility of the ionic polymer and SEBS, thereby ensuring that the prepared oxygen-absorbing composite material has both excellent transparency and mechanical properties. The composite material is prepared by using ionic polymer, SEBS, white oil and oxygen scavenger as raw materials. The ionic polymer has a large number of side chain structures, and the side chains form a dynamic cross-linked network that can be dissociated by heating and cross-linked by cooling through ionic bonds. This unique structure makes the ionic polymer have excellent solvent resistance, elasticity and tensile strength. Then, the flexibility and mechanical toughness of the oxygen-absorbing composite material are adjusted by blending an appropriate amount of SEBS to meet the sealing requirements of different products. The preparation method provided by the present application is simple to operate, the raw materials are easily available, and a composite material with excellent transparency, strength and toughness can be efficiently prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0035] Figure 1 This is a flow chart of a method for preparing an ionic polymer oxygen-absorbing composite material provided in an embodiment of the present application. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0037] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0038] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0039] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple, respectively.

[0040] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0041] The structural formula and molecular weight of some chemical reagents used in this application are described as follows:

[0042] Methacrylic acid (AA): Molecular weight = 86.09;

[0043] Dimethylaminoethyl methacrylate (DMAEMA): Molecular weight = 157.21;

[0044] Styrene: Molecular weight = 104.15.

[0045] The technical solution of this application is as follows:

[0046] First, see Figure 1 The present invention provides a method for preparing an ion polymer oxygen absorbing composite material, comprising the following steps:

[0047] S11, providing methacrylic acid (AA), dimethylaminoethyl methacrylate (DMAEMA), and styrene, mixing, and reacting to obtain an ionomer;

[0048] S12, mixing the ionomer with hydrogenated styrene-butadiene block copolymer (SEBS), white oil and oxygen scavenger, and reacting them to obtain an ionomer oxygen-absorbing composite material.

[0049] The preparation method of the ionic polymer oxygen-absorbing composite material provided by the present application adopts methacrylic acid as an anion unit and dimethylaminoethyl methacrylate as a cationic unit to prepare the zwitterionic polymer through random copolymerization. The side chain volume of the structural unit is large and the molecular chain cannot be arranged regularly, thereby ensuring its transparency. Styrene is used as a comonomer to improve the compatibility of the ionic polymer and SEBS, thereby ensuring that the prepared oxygen-absorbing composite material has both excellent transparency and mechanical properties. The composite material is prepared by using ionic polymer, SEBS, white oil and oxygen scavenger as raw materials. The ionic polymer has a large number of side chain structures, and the side chains form a dynamic cross-linked network that can be dissociated by heating and cross-linked by cooling through ionic bonds. This unique structure makes the ionic polymer have excellent solvent resistance, elasticity and tensile strength. Then, the flexibility and mechanical toughness of the oxygen-absorbing composite material are adjusted by blending an appropriate amount of SEBS to meet the sealing requirements of different products. The preparation method provided by the present application is simple to operate, the raw materials are easily available, and a composite material with excellent transparency, strength and toughness can be efficiently prepared.

[0050] In the S11:

[0051] In some embodiments, the molar ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is (0.2-0.4):(0.2-0.4):(0.2-0.6), for example, 0.2:0.2:0.6, 0.3:0.3:0.4, 0.4:0.4:0.2, etc. Within the molar ratio range, the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene are conducive to fully reacting to form an ionic polymer.

[0052] In some embodiments, the method for preparing the ionic polymer further comprises adding a solvent. In other words, the reaction of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is carried out in a solution.

[0053] In some embodiments, the mass ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene to the solvent is 10:(15-25), for example, 10:18, 10:20, 10:22 or any range between two ratios, etc. Within the mass ratio range, the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene are uniformly dissolved and dispersed.

[0054] In some embodiments, the solvent is selected from one or more of ethyl acetate, tetrahydrofuran, chlorobenzene, diethylene glycol monobutyl ether, trimethoxybutanol, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, acetophenone, N,N-dimethylformamide, pyrrole, butyric acid, and cresol.

[0055] In some embodiments, the method for preparing the ionic polymer further comprises adding a catalyst.

[0056] In some embodiments, the mass ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene to the mass ratio of the catalyst is (99.7-99.9):(0.1-0.3), for example, 99.7:0.3, 99.8:0.2, 99.9:0.1 or any range between two ratios, etc. Within the mass ratio range, the copolymerization reaction of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is promoted.

[0057] In some embodiments, the catalyst is selected from one or more of azobisisobutyronitrile, dicumyl peroxide, and potassium persulfate.

[0058] In some embodiments, the reaction of the methacrylic acid, the dimethylaminoethyl methacrylate, and the styrene is performed under an inert atmosphere.

[0059] Furthermore, the inert gas in the inert atmosphere includes one or more of nitrogen, helium, neon, argon, krypton, and xenon.

[0060] In some embodiments, the reaction of the methacrylic acid, the dimethylaminoethyl methacrylate, and the styrene is performed under stirring.

[0061] Further, the stirring speed is 40 rpm to 80 rpm, for example, 45 rpm, 50 rpm, 55 rpm, 60 rpm, 65 rpm, 70 rpm, 75 rpm or any range between two values, etc. At the stirring speed, the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene are mixed evenly.

[0062] In some embodiments, the reaction temperature of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is 60°C to 80°C, for example, 65°C, 70°C, 75°C or any range between two values, etc.; the reaction time is 6h to 10h, for example, 7h, 8h, 9h or any range between two values, etc. Thus, under the reaction conditions, the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene are conducive to fully reacting to form an ionic polymer.

[0063] In some embodiments, after the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene react, precipitation, filtration, washing and drying are further included.

[0064] In some embodiments, the structural formula of the ionic polymer is as shown below:

[0065] Among them, 0.2≤x≤0.4, 0.2≤y≤0.4, 0.2≤z≤0.6.

[0066] It should be noted that x, y, and z represent molar numbers.

[0067] In S12:

[0068] It is understood that SEBS can be purchased commercially, such as G1641HU from Kraton Performance Polymers.

[0069] In some embodiments, the mass ratio of the ionomer, the hydrogenated styrene-butadiene block copolymer, the white oil and the oxygen scavenger is (25-50): (40-50): (10-30): (1-5), for example, 25:50:20:5, 35:45:16:4, 40:40:18:2, 49:40:10:1, etc. Within the mass ratio range, the ionomer, the hydrogenated styrene-butadiene block copolymer, the white oil and the oxygen scavenger are conducive to fully reacting to form the ionomer oxygen-absorbing composite material, thereby improving the transparency, strength and toughness of the composite material.

[0070] In some embodiments, the mixing of the ionomer with the hydrogenated styrene-butadiene block copolymer, the white oil, and the oxygen scavenger comprises:

[0071] S121, mixing the white oil and the oxygen scavenger, and grinding to obtain a premixed material;

[0072] S122, mixing the premixed material, the ionomer and the hydrogenated styrene-butadiene block copolymer.

[0073] In some embodiments, the oxygen scavenger includes one or more of sodium sulfite, bishydroxymethyl ether, and metal powder.

[0074] In some embodiments, the mass ratio of the oxygen scavenger to the white oil is 1:(4-20), 1:5, 1:8, 1:10, 1:12, 1:15, 1:18 or a range between any two ratios, etc. Within the mass ratio range, the oxygen scavenger and the white oil are facilitated to be fully mixed and grinding is promoted.

[0075] In some embodiments, the grinding further comprises adding grinding media.

[0076] Furthermore, the grinding medium includes grinding balls, and the average particle size of the grinding balls is 0.25 mm to 0.85 mm, for example, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm or a range between any two values.

[0077] In some embodiments, the grinding speed is 3000 rpm to 3500 rpm, for example, 3100 rpm, 3200 rpm, 3300 rpm, 3400 rpm or any range between two values, etc.; the grinding time is 10 min to 15 min, for example, 11 min, 12 min, 13 min, 14 min or any range between two ratios, etc. Thus, under the grinding conditions, it is beneficial to fully mix the oxygen scavenger and the white oil.

[0078] It is understood that the grinding can be achieved using conventional equipment in the art, such as a horizontal bead mill.

[0079] In some embodiments, the reaction of the ionomer with the hydrogenated styrene-butadiene block copolymer, the white oil, and the oxygen scavenger comprises extrusion molding.

[0080] In some embodiments, the extrusion molding temperature is 180°C to 220°C, for example, it can be 190°C, 200°C, 210°C or a range between any two values, etc.; the extrusion molding speed is 200rpm / min to 500rpm / min, for example, it can be 250r / min, 300r / min, 350r / min, 400r / min, 450r / min or a range between any two values, etc.; the extrusion molding feeding speed is 100r / min to 200r / min, for example, it can be 120r / min, 140r / min, 150r / min, 160r / min, 180r / min or a range between any two values, etc.

[0081] In this way, under the extrusion molding conditions, it is beneficial to the molding and granulation of the ion polymer oxygen absorbing composite material.

[0082] It is understood that the extrusion molding can be achieved using conventional equipment in the art, such as a twin-screw extruder.

[0083] In a second aspect, an embodiment of the present application further provides an ion polymer oxygen absorbing composite material obtained by the above-mentioned preparation method.

[0084] In a third aspect, the present application also provides an application of the ionic polymer oxygen-absorbing composite material prepared by the above preparation method.

[0085] Specifically, a sealing gasket is provided, wherein the material of the sealing gasket comprises the ion polymer oxygen absorbing composite material prepared by the above preparation method.

[0086] In some embodiments, the sealing gasket can be obtained by extruding the ionic polymer oxygen-absorbing composite material through a molding machine.

[0087] Furthermore, the extrusion includes segmented heating, and the temperatures of the segmented heating are 90°C to 95°C, 100°C to 105°C, 105°C to 110°C, 110°C to 115°C, and 115°C to 120°C, respectively.

[0088] The extrusion motor speed is 1000 r / min to 1500 r / min, for example, it can be 1100 r / min, 1200 r / min, 1300 r / min, 1400 r / min or a range between any two values.

[0089] The feeding speed of the extrusion is 80 r / min to 100 r / min, for example, it can be 82 r / min, 85 r / min, 88 r / min, 90 r / min, 92 r / min, 95 r / min, 98 r / min or a range between any two values.

[0090] A bottle cap comprises a bottle cap body and a sealing gasket located inside the bottle cap body, wherein the material of the sealing gasket comprises the ion polymer oxygen absorbing composite material prepared by the above preparation method.

[0091] In some embodiments, the bottle cap body may be made of chrome-plated steel plate.

[0092] The bottle cap can be used for packaging beer, beverages and the like.

[0093] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0094] Example 1

[0095] This embodiment provides an ion polymer oxygen absorbing composite material, and the preparation method thereof is as follows:

[0096] Weigh 0.3 mol of methacrylic acid, 0.3 mol of dimethylaminoethyl methacrylate, 0.4 mol of styrene, 200 g of ethyl acetate and 0.1 g of azobisisobutyronitrile, add them into a 500 mL three-necked flask, seal the three-necked flask, replace the air in the reactor with nitrogen, start stirring, and set the stirring speed to 60 rpm; heat to 70°C, and react at a constant temperature for 8 hours. After the reaction is completed, pour the reaction solution into excess n-hexane for precipitation, filter, rinse with ethanol to remove unreacted monomers, and dry to obtain an ionic polymer;

[0097] Sodium sulfite and white oil were added into the material hopper of DMQ-07 horizontal bead mill at a mass ratio of 5:20, the power was turned on, the coolant was turned on, the speed was set to 3000 rpm, and grinding balls with an average particle size of 0.35 mm were selected. After cyclic grinding for 10 minutes, a premixed material was obtained;

[0098] Calculated by the mass percentage of each component, 35 parts of ionomer, 45 parts of SEBS (G1641 HU, purchased from Kraton High Performance Polymers Co., Ltd.), and 25 parts of premixed materials (20 parts of white oil and 5 parts of sodium sulfite) were uniformly mixed, and then extruded using a twin-screw extruder at an extrusion temperature of 200°C, an extrusion speed of 300 r / min, and a feeding speed of 120 r / min to obtain an ionomer oxygen-absorbing composite material.

[0099] Example 2

[0100] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ionomer oxygen absorbing composite material contains 35 parts of ionomer, 45 parts of SEBS, and 20 parts of premixed materials (16 parts of white oil and 4 parts of sodium sulfite).

[0101] Example 3

[0102] This embodiment is substantially the same as the embodiment 1, except that, in this embodiment, the ionomer oxygen absorbing composite material comprises 40 parts of ionomer, 40 parts of SEBS, and 20 parts of premixed materials (18 parts of white oil and 2 parts of sodium sulfite).

[0103] Example 4

[0104] This embodiment is substantially the same as the embodiment 1, except that, in this embodiment, the ionomer oxygen absorbing composite material contains 49 parts of ionomer, 40 parts of SEBS, and 11 parts of premixed materials (10 parts of white oil and 1 part of sodium sulfite).

[0105] Comparative Example

[0106] This comparative example is substantially the same as Example 3, except that the ionomer is replaced by polypropylene in this comparative example.

[0107] The ion polymer oxygen absorption composite materials of Examples 1 to 4 and the composite materials of the comparative example were added into the silo of the DMS-250K molding machine, pressed into a sealing gasket and bonded and compounded into the inside of the bottle cap body to obtain a crown cap product for subsequent transparency and oxygen absorption performance tests. The specific processing parameters are as follows: the temperatures of the first to fifth zones of the molding machine are: 90℃~95℃, 100℃~105℃, 105℃~110℃, 110℃~115℃, 115℃~120℃ respectively; the extrusion motor speed is 1000r / min, the feeding speed is 80r / min, the bottle cap is made of chrome-plated steel plate SPCC-BA, and the average sealing gasket weight is 220mg.

[0108] The mechanical properties of the ionomer oxygen absorbing composite materials of Examples 1 to 4 and the composite materials of the comparative example were tested. The test results are shown in Table 1.

[0109] Among them, the mechanical properties test is carried out according to the standard ASTM D638.

[0110] Table 1

[0111]

[0112] It can be seen from Table 1 that the tensile strength of the ionomer oxygen absorbing composite materials provided in Examples 1 to 4 is much higher than that of the composite materials in the comparative example.

[0113] The transparency performance of the ionomer oxygen absorbing composite material of Example 3 and the composite material of the comparative example was tested. The test results are shown in Table 2.

[0114] The test method of transparency performance includes: after preparing the ion polymer oxygen absorbing composite material or composite material into the sealing gasket of the crown cap, the crown cap is pressed on the beer bottle containing beer by a capping machine, 12 groups of samples are set for each experiment, and then inverted for 30 days, the bottle cap is removed, and the QR code on the bottle cap is scanned with a mobile phone to record the scanning result. S1 is the ion polymer oxygen absorbing material obtained in Example 3, and S2 is the ordinary oxygen absorbing material obtained in the comparative example. Among them, Y represents that it can be scanned, and N represents that it cannot be scanned.

[0115] Table 2

[0116] Sample 1 Sample 2 <![CDATA[Sample 3]]> Sample 4 <![CDATA[Sample 5]]> <![CDATA[Sample 6]]> <![CDATA[Sample 7]]> <![CDATA[Sample 8]]> <![CDATA[Sample 9]]> <![CDATA[Sample 10]]> Sample 11 Sample 12 S1 Y Y Y Y Y Y Y Y Y Y Y Y S2 Y Y N N N N N N N N N N

[0117] For the convenience of comparison, the data are sorted, and the data that cannot be scanned in the actual test are interspersed. It can be seen from Table 2 that the QR code scanning of Example 3 is 100%, and its transparency performance is not greatly affected during the 30-day inversion process. The QR codes of all 12 groups of samples can be scanned, and the QR code scanning success rate is greatly improved compared with 16.7% of the comparative example, which proves that the transparency performance of the ion polymer oxygen absorbing composite material of Example 3 is greatly improved compared with the composite material of the comparative example, and can meet the customer's requirements for transparent oxygen absorbing composite materials.

[0118] The oxygen absorption performance of the ionic polymer oxygen absorption composite materials of Examples 1 to 4 and the composite materials of the comparative example was tested. The test results are shown in Table 3.

[0119] Among them, the test methods for oxygen absorption performance include: using (GEN III 5250i, OxySense, Texas, USA) fluorescent residual oxygen analyzer is used to track the test by inserting the oxygen sensor chip of the instrument Pre-paste it on the inside of the container lid, pour 400mL of deionized water into the container, press the sample into a thin sheet with a thickness of 0.2mm in advance, take 1g and put it into the deionized water in the container, seal it, and purge the chamber with 99.999% high-purity oxygen for 5min. After the purge is completed, close the lid and valve. At this time, the container containing the sample to be tested has become an oxygen-rich closed chamber. Place the fluorescent signal reading pen in the groove for measuring dissolved oxygen, and its test point corresponds to the oxygen sensor sheet. The fluorescent signal reading pen tracks and measures the change data of dissolved oxygen content in the deionized water solution in the closed chamber with time. The fluorescence method for measuring oxygen content is greatly affected by temperature. In order to eliminate the test fluctuations caused by temperature, the equipment and the closed chamber are placed in a constant temperature and humidity chamber. The test temperature conditions are 23±2℃, the relative humidity is 50±3%, and the detection period is 7 days. Each sample is tested three times on average and the average value is taken.

[0120] Table 3

[0121]

[0122] It can be seen from Table 3 that the oxygen absorption performance of the ionic polymer oxygen-absorbing composite materials provided by Examples 1 to 4 is much higher than that of the composite materials in the comparative example.

[0123] In summary, the ionic polymer oxygen-absorbing composite material provided in the present application has significantly improved strength and toughness on the basis of excellent oxygen-absorbing performance.

[0124] The technical solutions provided by the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing an ion polymer oxygen absorbing composite material, characterized in that: The steps include: Providing methacrylic acid, dimethylaminoethyl methacrylate and styrene, mixing and reacting them to obtain an ionomer; The ion polymer is mixed with hydrogenated styrene-butadiene block copolymer, white oil and oxygen scavenger to react and obtain the ion polymer oxygen absorbing composite material.

2. The preparation method according to claim 1, characterized in that The molar ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is (0.2-0.4):(0.2-0.4):(0.2-0.6); and / or The method for preparing the ionic polymer further comprises adding a solvent; and / or The method for preparing the ionic polymer further comprises adding a catalyst.

3. The preparation method according to claim 2, characterized in that: The solvent is selected from one or more of ethyl acetate, tetrahydrofuran, chlorobenzene, diethylene glycol monobutyl ether, trimethoxybutanol, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether, methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, dimethyl sulfoxide, acetone, acetophenone, N,N-dimethylformamide, pyrrole, butyric acid, and cresol; and / or The mass ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene to the solvent is 10:(15-25); and / or The catalyst is selected from one or more of azobisisobutyronitrile, dicumyl peroxide, and potassium persulfate; and / or The mass ratio of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene to the mass ratio of the catalyst is (99.7-99.9):(0.1-0.3).

4. The preparation method according to claim 3, characterized in that: The reaction of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is carried out in an inert atmosphere; and / or The reaction of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is carried out under stirring; the stirring speed is 40 rpm to 80 rpm; and / or The reaction temperature of the methacrylic acid, the dimethylaminoethyl methacrylate and the styrene is 60° C. to 80° C., and the reaction time is 6 h to 10 h.

5. The preparation method according to claim 1, characterized in that: The mixing of the ionomer, the hydrogenated styrene-butadiene block copolymer, the white oil, and the oxygen scavenger comprises: The white oil and the oxygen scavenger are mixed and ground to obtain a premixed material; The premix material is mixed with the ionomer and the hydrogenated styrene-butadiene block copolymer.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the oxygen scavenger to the white oil is 1:(4-20); and / or The grinding further comprises adding grinding media; the grinding media comprises grinding balls, and the average particle size of the grinding balls is 0.25 mm to 0.85 mm; and / or The grinding speed is 3000 rpm to 3500 rpm; and / or The grinding time is 10 min to 15 min.

7. The preparation method according to claim 1, characterized in that: The oxygen scavenger includes one or more of sodium sulfite, bishydroxymethyl ether, and metal powder; and / or The masses of the ion polymer, the hydrogenated styrene-butadiene block copolymer, the white oil and the oxygen scavenger are (25-50): (40-50): (10-30): (1-5).

8. The preparation method according to claim 1, characterized in that: The reaction of the ionomer with the hydrogenated styrene-butadiene block copolymer, the white oil and the oxygen scavenger comprises extrusion molding, wherein: The extrusion molding temperature is 180°C to 220°C; and / or The rotation speed of the extrusion molding is 200 rpm / min to 500 rpm / min; and / or The feeding speed of the extrusion molding is 100r / min to 200r / min.

9. An ion polymer oxygen absorbing composite material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 8.

10. A sealing gasket, characterized in that: The material of the sealing gasket includes the composite material prepared by the preparation method according to any one of claims 1 to 8, or includes the composite material according to claim 9.

Citation Information

Patent Citations

  • Metal crown lid internal gasket sealing material with oxygen absorbing function

    CN102977452A

  • Compositions containing polyanion, ethoxylated cationic polymer and phyllosilicates for improved oxygen barrier coatings

    CN107849387A

  • Oxygen absorption material for manufacturing sealing gaskets and manufacturing method thereof

    CN110564039A

  • Thermoplastic elastomer material and preparation method thereof

    CN111269581A

  • Transparent elastomer sealing material with oxygen inhalation function

    CN113402808A