Low-precipitation low-climbing polyurethane protective film and preparation method thereof

By adopting a three-layer structure with low precipitation and low climbing polyurethane protective film, combined with high cohesive antistatic polyurethane adhesive and antistatic particles, the problem of difficulty in precipitation and peeling of protective film under high temperature and high humidity conditions is solved, and a good result is achieved. Aging resistance and low peeling force, suitable for the production of folding screen mobile phones.

CN119060652AInactive Publication Date: 2024-12-03ZHEJIANG AOBEI OPTICAL FILM IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411267040.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the production process of folding screen mobile phones, the protective film is prone to precipitation under high temperature and high humidity conditions, resulting in difficulty in attenuation of the performance of the back patch and peeling, and the peeling force is significantly increased, affecting process flow and product quality.

Method used

Low precipitation low-climbing polyurethane protective film adopts a three-layer structure, including silicone release film layer, high-cohesion antistatic polyurethane adhesive layer and high-permeability polyester film layer. High-cohesion antistatic polyurethane adhesive contains antistatic particles , antistatic particles and polyurethane adhesives are prepared through specific preparation methods to ensure that they are not easy to precipitate under high temperature and high humidity conditions and reduce peeling force.

Benefits of technology

Under high temperature and high humidity conditions, the performance attenuation of the back patch is reduced, the peeling force does not increase significantly, and the aging resistance is good, ensuring the protection effect of carbon fiber board and titanium material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005037439590000041
    Figure BDA0005037439590000041
  • Figure BDA0005037439590000051
    Figure BDA0005037439590000051
  • Figure BDA0005037439590000081
    Figure BDA0005037439590000081
Patent Text Reader

Abstract

The invention provides a low-precipitation low-climbing polyurethane protective film and a preparation method thereof. Comprising the following steps: adding polyether polyol, diisocyanate and a solvent into a reaction kettle for prepolymerization reaction, heating, adding an organic tin additive, cooling, and adding a chain extender for continuous reaction; the composite polyurethane resin is obtained; and uniformly mixing the composite polyurethane resin, a curing agent, a retarder, antistatic particles, a surfactant and a solvent to obtain the high-cohesion antistatic polyurethane adhesive. The preparation method comprises the following steps: uniformly coating a PET base material layer with a high-cohesion antistatic polyurethane adhesive, leveling, volatilizing a solvent, drying, laminating a release film, and curing to obtain the low-precipitation low-climbing polyurethane protective film. The high-cohesion antistatic polyurethane adhesive contains antistatic particles, so that the antistatic particles are not easy to separate out under high-temperature and high-humidity conditions when being protected by a carbon fiber plate and a titanium material for a folding screen bonding process, and the dyne value of a back bonding object is slightly attenuated; and during stripping, the stripping force does not obviously climb, and the aging resistance is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of release films, and in particular to a low-precipitation and low-climbing polyurethane protective film and a preparation method thereof. Background Art

[0002] At present, folding screen mobile phones are constantly developing towards being lighter, thinner and higher quality. New material carbon fiber is used in the design and production of folding screen structural parts. As one of the most important materials for the support plate of the folding screen of mobile phones, the 3C industry has an increasing demand for carbon fiber board materials; many high-end models use titanium alloy frames and titanium metal 3D printed hinge shaft covers, and the penetration rate of titanium metal in consumer electronics is expected to gradually increase. Whether it is a carbon fiber board or titanium material, a protective film is required for process protection during the manufacturing process, and there are high requirements for low precipitation and low climb of the protective film. However, after a long period of bonding between the protective film and the adhered object, two problems often occur: 1. The relative peeling force climb increases significantly, so that it is difficult to peel off in the final link or process flow; the back sticker is damaged and the surface is contaminated due to the precipitation of the protective film. Therefore, it is urgent to develop a low precipitation and low climb polyurethane protective film to solve the above problems. Summary of the invention

[0003] Technical problem to be solved: In view of the above technical problems, the purpose of the present invention is to provide a low-precipitation and low-climbing polyurethane protective film and a preparation method thereof. The high-cohesion antistatic polyurethane adhesive used contains antistatic particles. When protecting carbon fiber plates and titanium materials used in the folding screen process, it is not easy to precipitate under high temperature and high humidity conditions, and the dyne value of the back sticker is rarely attenuated; when peeling, the peeling force has no obvious climb, and the aging resistance is good.

[0004] Technical solution: A low precipitation and low climbing polyurethane protective film, the protective film has a three-layer structure, which includes a release film layer, a high cohesion pressure-sensitive adhesive layer and a PET substrate layer from top to bottom; The release film layer is an organic silicon release film, the residual bonding rate is greater than 85%, and the surface silicon content is 0.1-0.2g / m 2 , peeling force 10-20gf / 25mm; The high cohesion pressure-sensitive adhesive layer is formed by coating with a high cohesion antistatic polyurethane adhesive; The PET substrate layer is a high-transmittance polyester film with an apparent light transmittance of ≥90%, a haze of <3%, and a corona surface dyne value of ≥52dyn / cm. Furthermore, the high cohesive antistatic polyurethane adhesive comprises, by weight: Composite polyurethane resin 40-70 parts Curing agent 2-10 parts Retardant 1-5 parts Antistatic particles 0.5-4 parts Surfactant 0.05-1 part 90-150 parts of solvent. Furthermore, the composite polyurethane resin has a viscosity of 2000-5000 CPS. Furthermore, the curing agent is one of hexamethylene diisocyanate dimer, hexamethylene diisocyanate trimer, toluene diisocyanate trimer, and amino resin, or a combination in any weight ratio. Furthermore, the retarder is one of diethyl sulfate and triethylenediamine or a combination in any weight ratio. Furthermore, the antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize the nano-molybdenum powder and the fermentation medium separately and mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 4-7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 800-1200°C under inert atmosphere, heating rate is 5°C / min, carbonization time is 4-5h; S4: Screening carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100 μm. Furthermore, the particle size of the nano-molybdenum powder is 50-100 nm. Furthermore, the surfactant is one of fluorinated acrylate copolymers, fluorinated additives, polyester-modified hydroxyl-functional polydimethylsiloxane and silicone leveling agents, or a combination in any weight ratio; the solvent is one of ethyl acetate, butyl acetate and phenylmethane, or a combination in any weight ratio. Furthermore, the preparation method of the high cohesion antistatic polyurethane adhesive is as follows: (1) adding polyether polyol, diisocyanate and solvent into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) heating the mixture to 50-60°C, adding an organic tin additive, and continuing to heat the mixture by the reaction heat for 2 hours; (3) The temperature is lowered to 60°C, a chain extender is added, and the reaction is continued for 2 hours. The temperature does not exceed 70°C, and an organic tin additive is added; (4) heating to 80° C. and reacting at this temperature for 3 h to obtain a composite polyurethane resin; (5) Take the composite polyurethane resin, curing agent, retarder, antistatic particles, surfactant and solvent, mix them for 30-50 minutes at room temperature of 20-26° C. and humidity of 40-60% until the mixture is uniform, and obtain a high cohesive antistatic polyurethane adhesive. Furthermore, the polyether polyol is any one or a combination of at least two of a plurality of polyether triols and polyether diols having different relative molecular masses. Furthermore, the diisocyanate is any one of isophorone diisocyanate and dicyclohexylmethane diisocyanate with different hard segment contents or a combination in any weight ratio. Furthermore, the solvent is one of ethyl acetate and butyl acetate or a combination in any weight ratio. Further, the organic tin additive is one of dibutyltin dilaurate and stannous octoate or a combination thereof in any weight ratio. Further, the chain extender is one of trimethylolpropane, dimethylolbutyric acid and 1,4-butanediol or a combination thereof in any weight ratio. The preparation method of the above-mentioned low-precipitation and low-climbing polyurethane protective film includes the following steps: uniformly coating the high cohesion antistatic polyurethane adhesive on the PET substrate layer, leveling, solvent volatilization, drying, laminating the release film, and aging at a temperature of 45-50°C for 72 hours to obtain a low-precipitation and low-climbing polyurethane protective film. Beneficial effects: 1. The high cohesive antistatic polyurethane adhesive used in the present invention contains antistatic particles. When the carbon fiber plate and titanium material used in the folding screen process are protected, it is not easy to precipitate under high temperature and high humidity conditions, and the dyne value of the back sticker is rarely attenuated; when peeling, the peeling force does not increase significantly, and the aging resistance is good. 2. The antistatic particles of the present invention are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder. After carbonization, the bacterial cellulose microspheres form conductive carbon nanoclusters, which make it more likely that the carbon nanoclusters will contact each other, so that they themselves have a certain electrical conductivity. After being doped with nano-molybdenum powder, the electrical conductivity is enhanced, the antistatic effect is improved, the electrostatic adsorption is small, and the relative peeling force is reduced; at the same time, the carbonized bacterial cellulose microspheres have a three-dimensional continuous structure and an interconnected fiber network, with a high specific surface area and a porous structure. During the long-term bonding process between the protective film and the carbon fiber plate / titanium material at room temperature, a large number of active sites are provided for adsorbing the excess Si-H overflowing from the release film, thereby reducing the contact between Si-H and the carbon fiber plate / titanium material and reducing the increase in the peeling force. 3. The protective film of the present invention can be peeled off after being attached to the carbon fiber plate / titanium material for a long time at room temperature, and there is no residual glue pollution on the carbon fiber plate / titanium material. DETAILED DESCRIPTION The present invention proposes a low precipitation and low climbing polyurethane protective film and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention will be further described in detail with reference to the following examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Example 1 The antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize nano-molybdenum powder with a particle size of 50-100 nm and fermentation medium, mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 800°C under an inert atmosphere, heating rate of 5°C / min, carbonization time of 5h; S4: screen carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100μm. Example 2 The antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize nano-molybdenum powder with a particle size of 50-100 nm and fermentation medium, mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 900°C under an inert atmosphere, heating rate of 5°C / min, carbonization time of 5h; S4: screen carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100μm. Example 3 The antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize nano-molybdenum powder with a particle size of 50-100 nm and fermentation medium, mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 1000°C under inert atmosphere, heating rate is 5°C / min, carbonization time is 5h; S4: Screening carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100 μm. Example 4 The antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize nano-molybdenum powder with a particle size of 50-100 nm and fermentation medium, mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 1100°C under inert atmosphere, heating rate is 5°C / min, carbonization time is 4h; S4: Screening carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100 μm. Example 5 The antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize nano-molybdenum powder with a particle size of 50-100 nm and fermentation medium, mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 1200°C under inert atmosphere, heating rate is 5°C / min, carbonization time is 4h; S4: Screening carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100 μm. The electrical conductivity and porosity of carbonized bacterial cellulose microspheres doped with nano-molybdenum powder were determined. After comparing the conductivity and porosity, the carbonized bacterial cellulose microspheres doped with nano-molybdenum powder prepared in Example 4 were selected for subsequent experiments. Example 6 A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 60 parts of composite polyurethane resin, 8 parts of hexamethylene diisocyanate dimer, 4 parts of diethyl sulfate, 0.5 parts of antistatic particles, 0.6 parts of fluorinated acrylate copolymer and 30 parts of ethyl acetate were mixed for 40 minutes at room temperature of 25° C. and humidity of 54% until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. Example 7 A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 60 parts of composite polyurethane resin, 8 parts of hexamethylene diisocyanate dimer, 4 parts of diethyl sulfate, 1.5 parts of antistatic particles, 0.6 parts of fluorinated acrylate copolymer and 30 parts of ethyl acetate were mixed for 40 minutes at room temperature of 25° C. and humidity of 54% until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. Example 8 A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 60 parts of composite polyurethane resin, 8 parts of hexamethylene diisocyanate dimer, 4 parts of diethyl sulfate, 3.0 parts of antistatic particles, 0.6 parts of fluorinated acrylate copolymer and 30 parts of ethyl acetate were mixed for 40 minutes at room temperature of 25° C. and humidity of 54% until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. Example 9 A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 60 parts of composite polyurethane resin, 8 parts of hexamethylene diisocyanate dimer, 4 parts of diethyl sulfate, 4.0 parts of antistatic particles, 0.6 parts of fluorinated acrylate copolymer and 30 parts of ethyl acetate were mixed for 40 minutes at room temperature of 25° C. and humidity of 54% until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. Example 10 A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 40 parts of composite polyurethane resin, 2 parts of hexamethylene diisocyanate dimer, 1 part of diethyl sulfate, 3.0 parts of antistatic particles, 0.05 parts of fluorinated acrylate copolymer and 90 parts of ethyl acetate were mixed for 40 minutes at room temperature of 25° C. and humidity of 54% until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. Embodiment 11 A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 70 parts of composite polyurethane resin, 10 parts of hexamethylene diisocyanate dimer, 5 parts of diethyl sulfate, 3.0 parts of antistatic particles, 1 part of fluorinated acrylate copolymer and 150 parts of ethyl acetate were mixed for 40 minutes at room temperature of 25° C. and humidity of 54% until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. Comparative Example 1 The difference between this comparative example and Example 8 is that conventional antistatic particles-carbon nanotubes are added, as follows: A method for preparing a low precipitation and low climb polyurethane protective film comprises the following steps: (1) adding 35 parts of polyether triol, 25 parts of polyether diol, 20 parts of isophorone diisocyanate and 20 parts of ethyl acetate into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) The mixture was heated to 60°C, 1 part of dibutyltin dilaurate was added, and the temperature was continued to rise by the reaction heat for 2 hours; (3) When the temperature drops to 60°C, trimethylolpropane is added and the reaction is continued for 2 hours. When the temperature does not exceed 70°C, dibutyltin dilaurate is added; (4) heating to 80° C. and reacting at a constant temperature for 3 h to obtain a composite polyurethane resin with a viscosity of 3078 CPS; (5) 60 parts of composite polyurethane resin, 8 parts of hexamethylene diisocyanate dimer, 4 parts of diethyl sulfate, 3.0 parts of carbon nanotubes, 0.6 parts of fluorinated acrylate copolymer and 30 parts of ethyl acetate were mixed at room temperature of 25° C. and humidity of 54% for 40 minutes until the mixture was uniform, thereby obtaining a high cohesive antistatic polyurethane adhesive; (6) The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at 50° C. for 72 hours, a low precipitation and low climb polyurethane protective film is obtained; the release film layer is a silicone release film, with a residual bonding rate of 86% and a surface silicon content of 0.16 g / m 2 , peel force 10.4gf / 25mm; the PET substrate layer is a high-transmittance polyester film with an apparent transmittance of 92.3%, a haze of 2.6%, and a corona surface dyne value of 53dyn / cm. The embodiments of the present invention were applied to carbon fiber plate / titanium material, and the dyne value and peeling force thereof were measured. Test method: In a constant temperature and humidity environment of 23±2℃ and 55±10%, cut the protective film into 25mm wide * 200mm long strips, wipe the back sticker with alcohol, tear off the release film of the protective film and stick it on the back sticker, and roll it back and forth three times at a constant speed with a 2KG roller; leave it for 30 minutes, adjust the peeling angle to 180°, set the speed to 300mm / min, fold the free end of the sample 180°, clamp the end of each strip on the tensile fixture of the tensile testing machine (Iandra testing machine), peel it at a speed of 300mm / min, test 5 sets of data, and take the average value. Table 2

Claims

1. A low precipitation and low climbing polyurethane protective film, characterized in that: The protective film has a three-layer structure, which includes a release film layer, a high cohesion pressure-sensitive adhesive layer and a PET substrate layer from top to bottom; The release film layer is an organic silicon release film, the residual bonding rate is greater than 85%, and the surface silicon content is 0.1-0.2g / m 2 , peeling force 10-20gf / 25mm; The high cohesion pressure-sensitive adhesive layer is formed by coating with a high cohesion antistatic polyurethane adhesive; The PET substrate layer is a high-transmittance polyester film with an apparent light transmittance of ≥90%, a haze of <3%, and a corona surface dyne value of ≥52dyn / cm.

2. The low precipitation and low climbing polyurethane protective film according to claim 1, characterized in that: The high cohesive antistatic polyurethane adhesive comprises, by weight: Composite polyurethane resin 40-70 parts Curing agent 2-10 parts Retardant 1-5 parts Antistatic particles 0.5-4 parts Surfactant 0.05-1 part 90-150 parts of solvent.

3. The low precipitation and low climbing polyurethane protective film according to claim 2, characterized in that: The viscosity of the composite polyurethane resin is 2000-5000 CPS.

4. The low precipitation and low climbing polyurethane protective film according to claim 2, characterized in that: The curing agent is one of hexamethylene diisocyanate dimer, hexamethylene diisocyanate trimer, toluene diisocyanate trimer and amino resin, or a combination in any weight ratio.

5. The low precipitation and low climbing polyurethane protective film according to claim 2, characterized in that: The retarder is one of diethyl sulfate and triethylenediamine or a combination in any weight ratio.

6. The low precipitation and low climbing polyurethane protective film according to claim 2, characterized in that: The antistatic particles are carbonized bacterial cellulose microspheres doped with nano-molybdenum powder, and the preparation method is as follows: S1: Sterilize the nano-molybdenum powder and the fermentation medium separately and mix them, inoculate Acetobacter xylinum at an inoculation rate of 6%, and culture them in a constant temperature box at 30°C for 4-7 days to obtain conductive bacterial cellulose microspheres; S2: Wash with deionized water and 0.5 mol / L sodium hydroxide solution until neutral; S3: After drying, place in a tube furnace, heat to 800-1200°C under inert atmosphere, heating rate is 5°C / min, carbonization time is 4-5h; S4: Screening carbonized bacterial cellulose microspheres doped with nano-molybdenum powder with a particle size of 10-100 μm.

7. The low precipitation and low climbing polyurethane protective film according to claim 6, characterized in that: The particle size of the nano molybdenum powder is 50-100nm.

8. The low precipitation and low climbing polyurethane protective film according to claim 2, characterized in that: The surfactant is one of fluorine-containing acrylic copolymer, fluorine additive, polyester-modified hydroxyl-functional polydimethylsiloxane and silicone leveling agent or a combination in any weight ratio; the solvent is one of ethyl acetate, butyl acetate and phenylmethane or a combination in any weight ratio.

9. The low precipitation and low climbing polyurethane protective film according to claim 2, characterized in that: The preparation method of the high cohesion antistatic polyurethane adhesive is as follows: (1) adding polyether polyol, diisocyanate and solvent into a reaction kettle, blending them uniformly under nitrogen protection, and performing a prepolymerization reaction to obtain a mixture; (2) heating the mixture to 50-60°C, adding an organic tin additive, and continuing to heat the mixture by the reaction heat for 2 hours; (3) The temperature is lowered to 60°C, a chain extender is added, and the reaction is continued for 2 hours. The temperature does not exceed 70°C, and an organic tin additive is added; (4) heating to 80° C. and reacting at this temperature for 3 h to obtain a composite polyurethane resin; (5) Take the composite polyurethane resin, curing agent, retarder, antistatic particles, surfactant and solvent, mix them for 30-50 minutes at room temperature of 20-26° C. and humidity of 40-60% until the mixture is uniform, and obtain a high cohesive antistatic polyurethane adhesive.

10. The method for preparing a low precipitation and low climb polyurethane protective film according to any one of claims 1 to 9, characterized in that: The following steps are involved: The high cohesive antistatic polyurethane adhesive is evenly coated on the PET substrate layer, and after leveling, solvent volatilization, drying, laminating with a release film, and aging at a temperature of 45-50°C for 72 hours, a low precipitation and low climb polyurethane protective film is obtained.

Citation Information

Patent Citations

  • Preparation method of bacterial cellulose based carbon nanofibers

    CN103820883A

  • High-dyne-value antistatic polyurethane protective film and preparation method thereof

    CN113429896A

  • PU (polyurethane) protective film as well as preparation method and application thereof

    CN117363246A

  • Adhesive for electrostatic protection film, and electrostatic protection film having ultralow film tearing voltage