Operation method for controlling inclusion of molten steel through high-alkalinity refining slag
By preparing and adding a specific composition of slag mixing agent, the problem of controlling inclusions in the steelmaking process is solved, which significantly reduces the inclusion content in the molten steel and improves the purity and performance of the steel.
Patent Information
- Application Number
- CN202411307501.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
During the steelmaking process, it is difficult for the prior art to effectively control and reduce the inclusion content in the molten steel. Especially under the requirements of extreme purity, the chemical composition and physical characteristics of high-alkaline refining slag are not yet fully mature.
Prepare slag agent, including Fe 1-2%, SiO2 1-3%, S 0.005-0.02%, H2O 1-2%, MgO 0.3-1%, Al 45-60%, CaO 15-20%, Al2O3 3 -7% and Na2O 2-3%, and a slag mixing agent was added to the surface of the molten steel during RH refining. The top slag characteristics of the molten steel were adjusted to reduce the inclusion content by using slag of less than 10mm particle size.
By changing the composition and ratio of the slag mixer, the top slag characteristics of the molten steel are significantly improved, the inclusion content in the molten steel is reduced, and the purity and performance of the steel are improved.
Smart Images

Figure CN119061236A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metallurgy, and specifically relates to a deep inclusion removal technology in the technical field of steelmaking, and more specifically relates to an operating method for controlling inclusions in molten steel by using high-basicity refined slag. Background Art
[0002] In steel production, improving the purity of molten steel is the key to improving the quality of steel. Inclusions in molten steel can seriously affect the mechanical properties and processing properties of steel. Therefore, developing effective technologies to control and reduce the inclusion content in molten steel has always been a hot topic in metallurgical science research. At present, domestic and foreign steelmaking technologies mainly reduce the generation of inclusions and improve removal efficiency by adjusting the physical and chemical conditions during the smelting process. These methods include optimizing smelting parameters, improving steelmaking equipment, and using additives. However, although a variety of technologies have been proposed and applied, there is still a need for effective control technologies for specific steel grades under extreme purity requirements.
[0003] In the steelmaking process, high basicity refined slag effectively reduces the inclusion content in molten steel through the following mechanisms: Reaction between slag and metal: High basicity refined slag can react chemically with oxides in molten steel to change the chemical composition of inclusions. For example, aluminum oxide (Al 2 O 3 ) can react with calcium (Ca) in the slag to form calcium aluminate (CaO-Al 2 O 3 ) which have lower melting points and are easier to remove during the steelmaking process. Improve the morphology of inclusions: Through the reaction between slag and metal, the originally hard and brittle oxide inclusions can be transformed into spherical or ellipsoidal shapes. Inclusions in this shape are more likely to float to the slag surface when the molten steel flows, and thus be removed. This helps to reduce the number of inclusions in the steel and improve the purity of the steel. Adjusting the distribution of inclusions: High basicity refined slag can adjust the distribution of inclusions in steel, so that they are concentrated near the slag-liquid interface, which is convenient for removal in subsequent refining steps. In addition, the optimized slag-liquid interface properties also help reduce the re-adsorption of inclusions and secondary contamination. Control the number of inclusions: The basicity of refined slag has a significant effect on the number of inclusions in steel. Properly increasing the basicity of refined slag can reduce the number density of inclusions in steel, thereby reducing the content of non-metallic inclusions in steel. Through the above mechanism, high basicity refined slag plays an important role in the steelmaking process, helping to produce purer and higher performance steel. In actual production, controlling the chemical composition and physical properties of refined slag and rationally operating the steelmaking process are the keys to achieving efficient inclusion removal.
[0004] Therefore, it is desirable to design an operating method for controlling inclusions in molten steel using high basicity refined slag. Summary of the invention
[0005] In view of this, and in view of the deficiencies in the prior art, an object of the present invention is to provide an operating method for controlling inclusions in molten steel using high basicity refined slag.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions, which are specifically described as follows: According to aspects of the present invention, there is provided a method for controlling inclusions in molten steel using high basicity refined slag, comprising the following steps: Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by mass: Fe 1-2%, SiO 2 1-3%, S0.005-0.02%, H 2 O 1-2%, MgO 0.3-1%, Al 45-60%, CaO 15-20%, Al 2 O 3 5-7% and Na 2 O 2-3%; During RH refining, slag conditioning agents are added to the surface of molten steel.
[0007] In one embodiment of the present invention, the slag conditioning agent further comprises slag with a particle size of less than 10 mm.
[0008] In one embodiment of the present invention, the mass percentage of slag with a particle size less than 10 mm is 1-3%.
[0009] In one embodiment of the present invention, the slag conditioning agent does not include slag with a particle size greater than 50 mm.
[0010] In one embodiment of the present invention, the mass percentages of the components in the slag conditioning agent are as follows: Fe 1%, SiO 2 3%, S 0.005%, H 2 O 2%, MgO 0.3%, Al 45%, CaO 20%, Al 2 O 3 5%, Na 2 O 3% and slag with particle size less than 10mm 1%.
[0011] In one embodiment of the present invention, the mass percentages of the components in the slag conditioning agent are as follows: Fe 1.5%, SiO 2 2.8%, S 0.01%, H 2 O 1.5%, MgO 0.5%, Al 50.2%, CaO 16.3%, Al 2 O 35.9%, Na 2 O 2.7% and slag with particle size less than 10mm 2%.
[0012] In one embodiment of the present invention, the mass percentages of the components in the slag conditioning agent are as follows: Fe 2%, SiO 2 1%, S 0.02%, H 2 O 1%, MgO 1%, Al 60%, CaO 15%, Al 2 O 3 7%, Na 2 O 2% and slag material with particle size less than 10mm 3%.
[0013] In one embodiment of the present invention, the RH refining process includes a vacuum breaking step, and 400-450 kg of slag conditioning agent is added to the surface of the molten steel within 5 minutes after the vacuum breaking step.
[0014] In one embodiment of the present invention, the method further comprises: before adding the slag conditioning agent, stirring the molten steel with an inert gas.
[0015] In one embodiment of the present invention, the method further comprises: adding slag conditioning agent and active lime according to the converter endpoint control state after steel tapping.
[0016] By adopting the above technical solution, the present invention has the following advantages compared with the prior art: The present invention can achieve the maximum effect of improving the top slag characteristics of molten steel by changing various effective components of the slag conditioning agent and their proportions, thereby reducing inclusions in the molten steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0018] The above and / or additional aspects and advantages of the present invention will be more obvious and easily understood in the description of the embodiments in conjunction with the accompanying drawings, in which: Figure 1 A schematic flow chart of an operating method for controlling inclusions in molten steel using high basicity refined slag provided by the present invention is shown. DETAILED DESCRIPTION
[0019] It should be understood that the embodiments of the present invention shown in the exemplary embodiments are only illustrative. Although only a few embodiments are described in detail in the present invention, it is easy for those skilled in the art to appreciate that multiple modifications are feasible without actually departing from the teaching of the subject matter of the present invention. Accordingly, all such modifications should be included within the scope of the present invention. Without departing from the gist of the present invention, other replacements, modifications, changes and deletions may be made to the design, operating conditions and parameters of the following exemplary embodiments.
[0020] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0021] Figure 1 The schematic diagram of the process of controlling inclusions in molten steel using high basicity refined slag provided by the present invention is shown. Figure 1 As shown, the present invention provides an operating method for controlling inclusions in molten steel by high basicity refined slag, comprising the following steps: S101: Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by mass: Fe 1-2%, SiO 2 1-3%, S0.005-0.02%, H 2 O 1-2%, MgO 0.3-1%, Al 45-60%, CaO 15-20%, Al 2 O 3 5-7% and Na 2 O 2-3%; S102: Add slag conditioning agent to the surface of molten steel during RH refining.
[0022] Through the above technical scheme of the present invention, the present invention can achieve the maximum effect of improving the top slag characteristics of molten steel by changing the various effective components and the proportions of the slag conditioning agent, thereby reducing inclusions in the molten steel.
[0023] In a preferred embodiment of the above-mentioned operating method, the slag conditioning agent further includes slag with a particle size of less than 10 mm, and the mass percentage of the slag with a particle size of less than 10 mm is 1-3%.
[0024] In a preferred embodiment of the above operation method, the slag conditioning agent does not include slag with a particle size greater than 50 mm.
[0025] In the preferred embodiment of the above operation method, the mass percentages of the components in the slag conditioning agent are as follows: Fe 1%, SiO 2 3%, S 0.005%, H 2 O 2%, MgO 0.3%, Al 45%, CaO 20%, Al 2 O 35%, Na 2 O 3% and slag with particle size less than 10mm 1%.
[0026] In the preferred embodiment of the above operation method, the mass percentages of the components in the slag conditioning agent are as follows: Fe1.5%, SiO 2 2.8%, S 0.01%, H 2 O 1.5%, MgO 0.5%, Al 50.2%, CaO 16.3%, Al 2 O 3 5.9%, Na 2 O 2.7% and slag with particle size less than 10mm 2%.
[0027] In the preferred embodiment of the above operation method, the mass percentages of the components in the slag conditioning agent are as follows: Fe 2%, SiO 2 1%, S 0.02%, H 2 O 1%, MgO 1%, Al 60%, CaO 15%, Al 2 O 3 7%, Na 2 O 2% and slag material with particle size less than 10mm 3%.
[0028] In a preferred embodiment of the above operation method, the RH refining process includes a vacuum breaking step, and 400-450 kg of slag conditioning agent is added to the surface of the molten steel within 5 minutes after the vacuum breaking step. For example, preferably, the slag conditioning agent can be added to the surface of the molten steel immediately, within 1 minute or within 2 minutes after the vacuum breaking step.
[0029] In a preferred embodiment of the above operating method, the method further comprises: before adding the slag conditioning agent, stirring the molten steel with an inert gas.
[0030] In a preferred embodiment of the above operation method, the method further comprises: adding slag adjusting agent and active lime according to the converter endpoint control state after steel tapping, wherein the amount of slag adjusting agent in this step is adjusted or determined according to actual conditions, and the amount of active lime is fixed.
[0031] The scheme of the present invention will be explained below in conjunction with embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. Where specific techniques or conditions are not specified in the embodiments, conventional techniques in the art are followed.
[0032] An operating method for controlling inclusions in molten steel by high basicity refined slag provided in an embodiment of the present invention comprises the following specific steps: Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by mass: Fe 1-2%, SiO 21-3%, S0.005-0.02%, H 2 O 1-2%, MgO 0.3-1%, Al 45-60%, CaO 15-20%, Al 2 O 3 5-7% and Na 2 O 2-3% and slag with a particle size of less than 10mm 1-3%; in the RH refining process, the molten steel is stirred with inert gas and vacuum broken, and 400-500kg of the prepared slag adjusting agent is added to the surface of the molten steel within 5 minutes after the vacuum breaking step to maximize the control of inclusions in the molten steel.
[0033] Example 1 Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by mass: Fe 1%, SiO 2 3%, S 0.005%, H 2 O 2%, MgO 0.3%, Al 45%, CaO 20%, Al 2 O 3 5%, Na 2 O 3% and slag with particle size less than 10mm 1%, as shown in the following table.
[0034]
[0035] Then, during the RH refining process, argon gas was used to stir the molten steel, vacuum breaking was performed, and 410 kg of the prepared slag conditioning agent was added to the surface of the molten steel within 1 minute after the vacuum breaking step to maximize the control of inclusions in the molten steel.
[0036] Through the above Example 1, according to the inclusion rating standard GB / T10561-2005, it was evaluated that the rating of Class A inclusions in the finished steel was controlled within 1.5, and the ratings of Class B inclusions, Class C inclusions, and Class D inclusions were all controlled within 1.0.
[0037] Example 2 Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by mass: Fe 1.5%, SiO 2 2.8%, S0.01%, H 2 O 1.5%, MgO 0.5%, Al 50.2%, CaO 16.3%, Al 2 O 3 5.9%, Na 2 O 2.7% and slag with particle size less than 10mm 2%, as shown in the following table.
[0038]
[0039] Then, during the RH refining process, argon gas was used to stir the molten steel, vacuum breaking was performed, and 400 kg of the prepared slag conditioning agent was added to the surface of the molten steel immediately after the vacuum breaking step to maximize the control of inclusions in the molten steel.
[0040] Through the above Example 2, according to the inclusion rating standard GB / T10561-2005, it was evaluated that the ratings of Class A inclusions, Class B inclusions, Class C inclusions, and Class D inclusions in the finished steel were all controlled within Class 1.0.
[0041] Example 3 Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by mass: Fe 2%, SiO 2 1%, S 0.02%, H 2 O1%, MgO 1%, Al 60%, CaO 15%, Al 2 O 3 7%, Na 2 O 2% and slag material with particle size less than 10mm 3%, as shown in the following table.
[0042]
[0043] Then, during the RH refining process, argon gas was used to stir the molten steel, vacuum breaking was performed, and 450 kg of the prepared slag conditioning agent was added to the surface of the molten steel within 2 minutes after the vacuum breaking step to maximize the control of inclusions in the molten steel.
[0044] Through the above Example 3, according to the inclusion rating standard GB / T10561-2005, it was evaluated that the rating of Class A inclusions in the finished steel was within 1.0 level, the rating of Class B inclusions and Class C inclusions were within 1.5 level, and the rating of Class D inclusions were all controlled within 1.0 level.
[0045] Comparative Example Prepare a slag conditioning agent, wherein the slag conditioning agent includes the following components in percentage by weight: CaO 80%, Al 2 O 3 15%, B 2 O 3 8%, MgO 1%, and the remainder are impurities. As shown in the following table.
[0046]
[0047] Then, during the RH refining process, argon gas was used to stir the molten steel, vacuum breaking was performed, and 400 kg of the prepared slag conditioning agent was added to the surface of the molten steel immediately after the vacuum breaking step to maximize the control of inclusions in the molten steel.
[0048] Through the above comparative examples, according to the inclusion rating standard GB / T10561-2005, it was evaluated that the ratings of Class A inclusions, Class B inclusions, Class C inclusions, and Class D inclusions in the finished steel were all controlled within Grade 2.0.
[0049] It can be seen from the comparison of the above Examples 1-3 with the comparative example that the present invention can achieve the maximum effect of improving the top slag characteristics of molten steel by changing the various effective components and their proportions of the slag conditioning agent, thereby reducing inclusions in the molten steel.
[0050] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0051] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for controlling inclusions in molten steel using high basicity refined slag, characterized in that: The following steps are involved: A slag conditioning agent is prepared, wherein the slag conditioning agent comprises the following components in percentage by mass: Fe 1-2%, SiO2 1-3%, S0.005-0.02%, H2O 1-2%, MgO 0.3-1%, Al 45-60%, CaO 15-20%, Al2O3 5-7% and Na2O 2-3%; The slag conditioning agent is added to the surface of molten steel during RH refining.
2. The method for controlling inclusions in molten steel by using high basicity refined slag according to claim 1, characterized in that: The slag conditioning agent also includes slag with a particle size of less than 10 mm.
3. The method for controlling inclusions in molten steel by using high basicity refined slag according to claim 2, characterized in that: The mass percentage of the slag with a particle size less than 10 mm is 1-3%.
4. The method for controlling inclusions in molten steel by using high basicity refined slag according to claim 1, characterized in that: The slag adjusting agent does not include slag with a particle size greater than 50 mm.
5. The method for controlling inclusions in molten steel with high basicity refined slag according to claim 3, characterized in that: The mass percentages of the components in the slag conditioning agent are as follows: Fe 1%, SiO2 3%, S 0.005%, H2O 2%, MgO 0.3%, Al45%, CaO 20%, Al2O3 5%, Na2O 3% and 1% slag with a particle size of less than 10 mm.
6. The method for controlling inclusions in molten steel with high basicity refined slag according to claim 3, characterized in that: The mass percentages of the components in the slag conditioning agent are as follows: Fe 1.5%, SiO2 2.8%, S 0.01%, H2O 1.5%, MgO 0.5%, Al 50.2%, CaO 16.3%, Al2O3 5.9%, Na2O 2.7% and slag with a particle size of less than 10 mm 2%.
7. The method for controlling inclusions in molten steel with high basicity refined slag according to claim 3, characterized in that: The mass percentages of the components in the slag conditioning agent are as follows: Fe 2%, SiO2 1%, S 0.02%, H2O 1%, MgO 1%, Al 60%, CaO 15%, Al2O3 7%, Na2O 2% and 3% of slag material with a particle size of less than 10 mm.
8. The method for controlling inclusions in molten steel by using high basicity refined slag according to claim 1, characterized in that: The RH refining process includes a vacuum breaking step, and within 5 minutes after the vacuum breaking step, 400-450 kg of slag conditioning agent is added to the surface of the molten steel.
9. The method for controlling inclusions in molten steel by using high basicity refined slag according to claim 1, characterized in that: The method further comprises: before adding the slag adjusting agent, stirring the molten steel with an inert gas.
10. The method for controlling inclusions in molten steel by using high basicity refined slag according to claim 1, characterized in that: The method further comprises: adding slag adjusting agent and active lime according to the converter endpoint control state after steel tapping.