Pipeline crack stress internal detection method based on strong and weak magnetism

By combining the advantages of leakage magnetic and metal magnetic memory detection in oil and gas pipelines, mathematical models and finite element methods under strong and weak magnetic fields are used to solve the problem that the existing technology is difficult to detect pipeline crack stress, and the stress on pipeline cracks is achieved Accurate detection and effective extraction.

CN119066900APending Publication Date: 2024-12-03LIAONING UNIVERSITY OF PETROLEUM AND CHEMICAL TECHNOLOGY
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202311214660.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to accurately detect stress at pipeline cracks in oil and gas pipelines. Magnetic leakage detection can only detect macroscopic volume defects. The metal magnetic memory detection signal is weak and is easily disturbed by external interference, making it difficult to effectively detect stress at pipeline cracks.

Method used

Using a stress detection method at the pipeline cracks based on strong and weak magnets, the magnetic signal characteristics are calculated under strong and weak magnetic fields through mathematical models, and the stress signal is extracted by using the finite element equation, combining the advantages of leakage magnetic and metal magnetic memory detection to achieve the pipeline cracks. All-round detection of stress.

Benefits of technology

It realizes accurate detection of stress at pipeline cracks, improves detection efficiency and anti-interference ability, can effectively extract stress signals and eliminate crack size information, and completes effective internal detection of pipeline crack surface stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the field of long oil and gas pipeline internal detection, and particularly relates to a strong and weak magnetism-based pipeline crack stress internal detection method. The invention provides a pipeline crack stress internal detection method based on strong and weak magnetism. The method comprises the following steps: 1) calculating strong and weak magnetic crack stress detection characteristics; step 2), extracting stress signals at the cracks under strong and weak magnetism; the method further comprises an analytical calculation part of the model for strong and weak magnetic stress detection characteristic research, and a finite element simulation modeling and calculation analysis part of the model for engineering calculation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of long-distance oil and gas pipeline internal detection, and in particular relates to a pipeline crack stress internal detection method based on strong and weak magnetism. Background Art

[0002] During the construction process, oil and gas pipelines will be affected by welding, high temperature and high pressure, resulting in cracks on the surface. These cracks will expand under the action of stress, causing disasters such as pipeline explosions. Pipeline in-line detection is currently recognized internationally as the most accurate and efficient means of pipeline safety maintenance. Therefore, accurate in-line detection of stress at pipeline cracks is extremely important for pipeline safety assessment. However, due to the complex magnetic field distribution of stress at pipeline cracks and the many factors affecting working parameters, it is difficult for existing in-line detection technologies to effectively detect them. For example, for magnetic leakage, a mainstream detection technology in the field of international pipeline in-line detection, it uses a strong saturated magnetic field for excitation, which can only detect formed macroscopic volume defects, but cannot effectively detect pipeline stress. As an emerging stress detection technology, metal magnetic memory uses the geomagnetic field for excitation to detect pipeline stress, but because its signal is weak and easily disturbed by the external environment, it is also difficult to accurately detect stress at pipeline cracks. To this end, we comprehensively integrate the advantages of magnetic leakage detection and metal magnetic memory detection to form strong and weak magnetic detection, and then propose a pipeline in-line detection method for all-round detection of stress at pipeline cracks. Summary of the invention

[0003] In order to realize comprehensive detection of stress at pipeline cracks during internal pipeline inspection, based on the advantages of magnetic flux leakage detection and metal magnetic memory detection, we use mathematical models to perform strong and weak magnetic crack stress detection and stress signal extraction calculation at the crack under dual magnetic field excitation of strong and weak magnetic fields, in order to design a method for internal stress detection at pipeline cracks based on strong and weak magnetic fields.

[0004] Step 1): Calculation of strong and weak magnetic crack stress detection characteristics

[0005] The essence of pipeline strong and weak magnetic stress internal detection is to use the magnetic signals generated at pipeline cracks under strong and weak excitation magnetic fields to detect different crack stress intensities. To this end, the purpose of mathematical model calculation is to calculate the magnetic signal characteristics of cracks under two changing parameters: external magnetic field and stress.

[0006] First, assume that there is a crack on the pipe surface, and the crack size is: D X *D Y *D Z, with the crack center as the origin, establish a three-dimensional Cartesian coordinate system. In a pipeline pressure environment, an excitation magnetic field with an external magnetic field of H0 is added to the pipeline. At this time, the pipeline pressure and the external magnetic field will cause the crack to accumulate positive and negative magnetic charges, and then generate a magnetic signal with an intensity of H at the crack. Set the magnetic charge surface element to dy m dz m , the magnetic signal intensity generated by this surface element at any point P(X, Y, Z) in the detection space is:

[0007]

[0008] Where r0 is the distance from the surface element to point P, μ0 is the vacuum magnetic permeability, and ρ is the magnetic charge density, which can be expressed as:

[0009]

[0010] Where M is the material magnetization intensity. Integrate equation (1) and substitute equation (2) to obtain the magnetic signal intensity generated by the crack at point P:

[0011]

[0012]

[0013] Where H x is the tangential magnetic signal intensity, H z is the normal magnetic signal intensity. It can be seen from formulas (3) and (4) that the magnetic signal generated by pipeline cracks is related to the magnetization intensity, crack size and detection point position.

[0014] In order to further study the crack stress detection characteristics of strong and weak magnetism, the magnetic space coefficient f(x, z) related to the crack size and the detection point position is defined, that is, H = M × f(x, z). The magnetic space coefficient f(x, z) can be expressed as:

[0015]

[0016] From the equation H = M × f (x, z), we know that in strong and weak magnetic detection, the two changing parameters of external magnetic field and stress that we want to study are both reflected by the magnetization intensity M. For this reason, the changing characteristics of the pipeline magnetization intensity under different external magnetic fields and stresses are clarified, that is, the crack stress detection characteristics of strong and weak magnetism are clarified. The magnetization intensity of the in-service pipeline can be expressed as:

[0017] M=cM an +(1-c)M irr (6)

[0018] Where c is the reversible component coefficient, M irr is the irreversible magnetization caused by the pinning point, M anis the hysteresis-free magnetization. The asymptotic principle in JA theory can further give the energy consumption E caused by the pinning point. pin The equation is:

[0019]

[0020] Therefore, based on the law of conservation of energy, the hysteresis-free magnetization intensity M can be calculated according to formula (7): an Further solving:

[0021]

[0022] Where k is the pinning coefficient of the material, δ=±1 is the directional coefficient, and H e is the equivalent magnetic field, which can be expressed as:

[0023]

[0024] Where F is the system energy value, α is the molecular field parameter, σ is the stress value, and λ is the hysteresis expansion coefficient, which can be expressed as:

[0025] λ=γ1M 2 +2γ2M 4 (10)

[0026] In formula (10), γ1 and γ2 are stress determining parameters, which can be obtained by Taylor series expansion:

[0027]

[0028] Derivative of equation (6) with respect to the external magnetic field H0 and solve it together with equations (8), (9) and (10) to obtain:

[0029]

[0030] Formula (12) is the magnetization intensity equation of the pipeline under the external magnetic field. Combining formula (3), (4), and (12), it can be seen that under the action of the external excitation magnetic field, the magnetization intensity and magnetic signal of the crack will further increase with the increase of the excitation magnetic field, thereby making the detection efficiency of the crack magnetic signal higher and the anti-interference ability stronger.

[0031] When stress exists at the crack of the pipeline, the stress will increase the energy at the crack. At this time, the pipeline material will rotate the magnetic domain according to the principle of minimum energy, thereby balancing the increase in energy and generating magnetization intensity. At this time, the magnetization intensity of the crack under stress can be expressed as:

[0032]

[0033] Where ξ is the energy-related coefficient per unit volume, W is the stress energy, and the stress energy of the pipeline crack under stress can be expressed as:

[0034]

[0035] In formula (14), υ is Poisson's ratio, E is elastic modulus, and σ r is the composite stress value of the crack, which can be expressed as:

[0036]

[0037] In the formula, σ1, σ2, and σ3 are the three main direction stresses of the pipeline crack.

[0038] Solving equations (13), (14) with equations (8), (9), and (10) yields:

[0039]

[0040] Formula (16) is the magnetization intensity equation of the pipeline under stress. From formulas (3), (4), and (16), it can be seen that the magnetization intensity and magnetic signal of the crack will also increase further with the increase of stress, thereby realizing stress detection of pipeline cracks.

[0041] Combining equations (12) and (16), we can see that the magnetic signal at the crack will effectively detect stress, and the external excitation magnetic field will also increase the detection effect. However, at this time, no matter what the intensity of the single excitation magnetic field is, the magnetic signal at the crack is a mixed signal generated by stress and the external magnetic field, that is, the detection signal contains dual information of stress and crack size. Therefore, only by using strong and weak excitation magnetic fields can the stress signal extraction at the crack be completed, and the effective detection of stress at the pipeline crack can be achieved.

[0042] Step 2): Extract stress signals at cracks under strong and weak magnetic fields

[0043] Here, we extract stress signals and realize stress detection at pipeline cracks by calculating the finite element equations of pipeline crack magnetic signals under strong and weak excitation. In the finite element method, the solution to pipeline crack magnetic signals is actually the solution of Maxwell's equations under the corresponding boundary conditions. In order to realize the calculation of crack magnetic signals under the finite element equation, we first assume that the normal pipeline material is uniform and isotropic, that is, it is assumed that the magnetic permeability at each point in the pipeline is the same, and the magnetic properties manifested in all directions are the same. At this time, under Maxwell's equations, in the pipeline wall where the medium magnetic permeability is μ, the current density The stable magnetic field formed With magnetic induction The relationship between them is:

[0044]

[0045]

[0046]

[0047] However, in actual engineering calculations, since the curl of the magnetic field intensity vector is not zero, it is impossible to use the scalar magnetic potential for analytical solution in a relatively stable magnetization region. Therefore, we use the vector magnetic potential To calculate the corresponding finite element magnetic signal in the magnetic field. and magnetic induction intensity The relationship between them is:

[0048]

[0049] Solving equations (17), (18), (19), and (20) together, we can obtain:

[0050]

[0051] In solving the finite element method, we generally do not directly give the solution of equation (21), but through an energy functional equivalent to it, by solving the extreme value of this energy functional at each point of the material, we can solve the magnetic signal generated by the pipeline under the external magnetic field and stress. Since equation (21) is a vector magnetic potential equation, it satisfies the Poisson equation and belongs to a generalized equation. Therefore, combining it with the boundary conditions constitutes a boundary value problem. From the above, we can see that: in the cylindrical coordinate system (r, θ, z), the boundary conditions of the vector magnetic potential can be written as:

[0052]

[0053] Solving in equation (22), the region is Ω, and the corresponding boundary condition is Γ. In solving electromagnetic field problems, the functional F(A) has the energy dimension, so it is also called the energy functional. The minimum value of the energy functional can be expressed as:

[0054]

[0055] Discretize the region Ω into E triangular units, the three vertices of the unit are (i, j, m), and select the unit displacement function:

[0056] A(r,z)=a1+a2r+a3z (24)

[0057] In solving the energy functional, the total energy is the sum of the individual energy functionals:

[0058] F(A) e =F(A) e′ +F(A) e″ (25)

[0059] In formula (25):

[0060]

[0061]

[0062] In formula (26) and formula (27), Γ e / Γ2 belongs to the unit boundary Γ e , but it does not belong to the edge of Γ2, and S is the surface integral region. The surface integral of formula (26) and the line integral of formula (27) can be discretized in the operational equations.

[0063] The linear interpolation function F(A) e′ The expression is:

[0064]

[0065] Formula (28) is the energy expression of the discretized unit e. Taking the first-order partial derivative of the potential function A (k = i, j, m, l = i, j, m) of each vertex in the unit, we get:

[0066]

[0067] In formula (29):

[0068]

[0069] By further taking the extreme value of F(A) in equation (29), we can obtain the finite element linear equations of the crack magnetic signal at n nodes:

[0070]

[0071] In formula (31):

[0072]

[0073]

[0074] In formula (31), A lk , K lk , R lkThe matrices are the magnetic potential matrix, coefficient matrix and excitation matrix of the finite element equations of the crack magnetic signal, respectively. The magnetic potential matrix contains the stress information of the crack, and the coefficient matrix contains the crack size information. Further solving the Vandermonde determinant of equation (31) under strong and weak dual excitation magnetic fields can make use of the characteristics that the strong and weak excitation detection systems will simultaneously detect the same crack in strong and weak magnetic detection. On the basis of retaining the magnetic potential matrix, the coefficient matrix is ​​eliminated, thereby eliminating the crack size information of the detection signal and retaining the stress information, completing the stress information extraction of the strong and weak detection signals, and realizing the effective detection of stress at the pipeline crack.

[0075] As a preferred solution, the present invention also includes an analytical calculation part of the model used for the study of strong and weak magnetic stress detection characteristics, and a finite element simulation modeling and calculation analysis part of the model used for engineering calculations.

[0076] As a preferred solution, the analytical calculation part uses Matlab software to perform analytical calculation and analysis of the model; the finite element simulation part uses ANAYS software for simulation modeling and calculation analysis.

[0077] As a preferred solution, in the analytical calculation part, the external magnetic field change parameter is set to 20K / AM -1 —-20K / AM -1 , stress variation parameters are 0MPa-100MPa (interval 20MPa).

[0078] As a preferred solution, in the analytical calculation part, the parameters of equations (12) and (16) are set as μ0=4*pi*(1e-7), δ=±1, Ms=1.71e6, a=1000, α=0.001, c=0.1, r1=7×10-18A. -2 m 2 ,r′1=-1×10-25A -2 ·m 2 ·Pa -1 ,r2=-3.3×10-30A -4 ·m 4 ,r′2=2.1×10-38A -4 ·m 4 ·Pa -1 , and further analytically calculated the pipeline crack hysteresis loop and magnetization curve, and conducted an analytical study on the pipeline strong and weak magnetic crack stress detection characteristics.

[0079] As a preferred solution, the finite element simulation modeling and calculation analysis part uses finite element simulation software to establish a magnetic mechanical model of a cracked pipeline. The crack is set at the center of the pipeline surface, and displacement constraints are applied to both sides of the pipeline model to simulate the pipeline operation condition. Internal pressure is applied to the pipeline, and an excitation magnetic field is added. The internal pressure of the pipeline causes severe stress concentration at the pipeline defect. As the internal pressure of the pipeline increases, the stress at the pipeline crack also increases.

[0080] As a preferred solution, the finite element simulation modeling and calculation analysis part sets the pipeline to be X70 steel, with an elastic modulus of 2*10 6 N / m -2 , Poisson's ratio PRXY is 0.3 and the magnetic permeability is 280H / m.

[0081] As a preferred solution, the finite element simulation modeling and calculation analysis part sets the pipeline length to 4000mm, the wall thickness to 16.5mm, and the pipeline diameter to 1100mm.

[0082] As a preferred solution, the present invention also includes hysteresis loop experiments of experimental specimens under different stresses, and magnetic signal detection characteristic experiments under different external magnetic fields and stresses, so as to verify the correctness of the calculations of various theoretical models.

[0083] As a preferred solution, the experimental specimen is a cracked X70 pipe cut specimen, the specimen size is 400mm*40mm*16.6mm, and the crack size is 30mm*1.5mm*2mm.

[0084] As a preferred solution, the hysteresis loop experimental system: the excitation coil is evenly wound on the U-shaped magnetic core, and it is fixed on the specimen together with the receiving coil. The excitation coil and the receiving coil are respectively connected to the excitation and receiving terminals of the magnetic properties analyzer (MATS-2010SD) to provide magnetization information for the experiment. The specimen is fixed on the electro-hydraulic servo universal tensile machine (WAW-2000) to provide tensile force for the specimen.

[0085] As a preferred solution, the magnetic signal detection characteristic experimental system: fix the specimen on the WAW-2000 tensile machine to provide stress for it, paste the strain gauge on the specimen, and detect the stress in real time. The excitation coil is installed on the side of the specimen, and a magnetic probe is installed inside it, which can excite and scan the specimen driven by a forklift. The sampling frequency of the magnetic probe is 1.5KHz, and the magnetic field detection accuracy is 1nT. The strain gauge is DH3818 model, the sampling rate is 200 times / second, and the A / D resolution is 14 bits.

[0086] The invention has beneficial effects.

[0087] The present invention combines the two effective in-pipeline detection methods, namely magnetic flux leakage detection and metal magnetic memory detection, and proposes an in-pipeline detection method for detecting surface stress of pipeline cracks under strong and weak dual excitation magnetic fields. We establish and calculate the pipeline crack magnetic signal equations under different stresses and external magnetic fields to clarify the strong and weak magnetic stress detection characteristics of pipeline cracks, and use the crack magnetic signal under a strong excitation magnetic field to detect the crack size, and the crack magnetic signal under a weak magnetic excitation magnetic field to detect the stress. We further perform finite element mixed operations on the two groups of strong and weak crack magnetic signals, use the characteristics that strong and weak magnetic signals can simultaneously detect the same group of cracks, and use the magnetic potential matrix under the finite element equation to complete the pipeline crack stress signal extraction, thereby achieving accurate and effective internal detection of pipeline crack surface stress. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods. The protection scope of the present invention is not limited to the following description.

[0089] Figure 1 Hysteresis loop and magnetization curve of pipeline crack.

[0090] Figure 2 Simulation model diagram.

[0091] Figure 3 a Excitation characteristics diagram of tangential magnetic signal of pipeline crack.

[0092] Figure 3 b Excitation characteristics diagram of normal magnetic signal of pipeline crack.

[0093] Figure 4 a Pipeline crack tangential magnetic signal stress detection characteristics diagram.

[0094] Figure 4 b Stress detection characteristics diagram of normal magnetic signal of pipeline crack.

[0095] Figure 5 a Characteristic diagram of the crack tangential magnetic signal changing with stress under strong excitation.

[0096] Figure 5 b Characteristic diagram of the crack normal magnetic signal changing with stress under strong excitation.

[0097] Figure 6 a Characteristic diagram of crack tangential magnetic signal changing with stress under weak excitation.

[0098] Figure 6 b Characteristic diagram of the crack normal magnetic signal changing with stress under weak excitation.

[0099] Figure 7 Relationship diagram of crack stress and magnetic potential matrix.

[0100] Figure 8a Characteristic diagram of the crack tangential magnetic signal changing with crack size under strong excitation.

[0101] Figure 8 b Characteristic diagram of the change of crack normal magnetic signal with crack size under strong excitation.

[0102] Fig. 9 a Characteristic diagram of the crack tangential magnetic signal changing with crack size under weak excitation.

[0103] Fig. 9 b Characteristic diagram of the change of crack normal magnetic signal with crack size under weak excitation.

[0104] Fig.10 Relationship diagram between crack size and magnetic potential matrix.

[0105] Fig.11 Magnified image of the experimental specimen and crack.

[0106] Fig.12 Hysteresis loop experimental system.

[0107] Fig.13 Magnetic signal detection characteristics experimental system.

[0108] Fig.14 Hysteresis loop diagram of the specimen under different stresses.

[0109] Fig.15 Stress detection characteristic diagram of experimental specimen.

[0110] Fig.16 a Tangential excitation characteristics diagram of the experimental specimen.

[0111] Fig.16 b Normal excitation characteristics diagram of the experimental specimen.

[0112] Fig.17 a Tangential magnetic potential matrix characteristic diagram.

[0113] Fig.17 b Normal magnetic potential matrix characteristic diagram.

[0114] Fig.18 The strong and weak magnetic stress internal detection of pipelines is shown in the figure.

[0115] Fig.19 a Pure crack strong magnetic detection signal.

[0116] Fig.19 b Pure crack weak magnetic detection signal.

[0117] Fig. 20 aContains strong magnetic detection signal of stress crack.

[0118] Fig. 20 b Contains weak magnetic detection signal of stress crack.

[0119] Fig.21 a Strong magnetic detection signal of pure stress concentration.

[0120] Fig.21 b Weak magnetic detection signal of pure stress concentration.

[0122] Fig. 22 Pipeline excavation verification site

[0123] Fig.23 Magnetic memory stress detection signal diagram DETAILED DESCRIPTION

[0124] The present invention comprises the following steps:

[0125] Step 1): Calculation of strong and weak magnetic crack stress detection characteristics

[0126] The essence of pipeline strong and weak magnetic stress internal detection is to use the magnetic signals generated at pipeline cracks under strong and weak excitation magnetic fields to detect different crack stress intensities. To this end, the purpose of mathematical model calculation is to calculate the magnetic signal characteristics of cracks under two changing parameters: external magnetic field and stress.

[0127] First, assume that there is a crack on the pipe surface, and the crack size is: D X *D Y *D Z , with the crack center as the origin, establish a three-dimensional Cartesian coordinate system. In a pipeline pressure environment, an excitation magnetic field with an external magnetic field of H0 is added to the pipeline. At this time, the pipeline pressure and the external magnetic field will cause the crack to accumulate positive and negative magnetic charges, and then generate a magnetic signal with an intensity of H at the crack. Set the magnetic charge surface element to dy m dz m , the magnetic signal intensity generated by this surface element at any point P(X, Y, Z) in the detection space is:

[0128]

[0129] Where r0 is the distance from the surface element to point P, μ0 is the vacuum magnetic permeability, and ρ is the magnetic charge density, which can be expressed as:

[0130]

[0131] Where M is the material magnetization intensity. Integrate equation (1) and substitute equation (2) to obtain the magnetic signal intensity generated by the crack at point P:

[0132]

[0133]

[0134] Where H x is the tangential magnetic signal intensity, Hz is the normal magnetic signal intensity. It can be seen from formulas (3) and (4) that the magnetic signal generated by pipeline cracks is related to the magnetization intensity, crack size and detection point position.

[0135] In order to further study the crack stress detection characteristics of strong and weak magnetism, the magnetic space coefficient f(x, z) related to the crack size and the detection point position is defined, that is, H = M × f(x, z). The magnetic space coefficient f(x, z) can be expressed as:

[0136]

[0137] From the equation H = M × f (x, z), we know that in strong and weak magnetic detection, the two changing parameters of external magnetic field and stress that we want to study are both reflected by the magnetization intensity M. For this reason, the changing characteristics of the pipeline magnetization intensity under different external magnetic fields and stresses are clarified, that is, the crack stress detection characteristics of strong and weak magnetism are clarified. The magnetization intensity of the in-service pipeline can be expressed as:

[0138] M=cM an +(1-c)M irr (6)

[0139] Where c is the reversible component coefficient, M irr is the irreversible magnetization caused by the pinning point, M an is the hysteresis-free magnetization. The asymptotic principle in JA theory can further give the energy consumption E caused by the pinning point. pin The equation is:

[0140]

[0141] Therefore, based on the law of conservation of energy, the hysteresis-free magnetization intensity M can be calculated according to formula (7): an Further solving:

[0142]

[0143] Where k is the pinning coefficient of the material, δ=±1 is the directional coefficient, and H e is the equivalent magnetic field, which can be expressed as:

[0144]

[0145] Where F is the system energy value, α is the molecular field parameter, σ is the stress value, and λ is the hysteresis expansion coefficient, which can be expressed as:

[0146] λ=γ1M 2 +2γ2M 4 (10)

[0147] In formula (10), γ1 and γ2 are stress determining parameters, which can be obtained by Taylor series expansion:

[0148]

[0149] Derivative of equation (6) with respect to the external magnetic field H0 and solve it together with equations (8), (9) and (10) to obtain:

[0150]

[0151] Formula (12) is the magnetization intensity equation of the pipeline under the external magnetic field. Combining formula (3), (4), and (12), it can be seen that under the action of the external excitation magnetic field, the magnetization intensity and magnetic signal of the crack will further increase with the increase of the excitation magnetic field, thereby making the detection efficiency of the crack magnetic signal higher and the anti-interference ability stronger.

[0152] When stress exists at the crack of the pipeline, the stress will increase the energy at the crack. At this time, the pipeline material will rotate the magnetic domain according to the principle of minimum energy, thereby balancing the increase in energy and generating magnetization intensity. At this time, the magnetization intensity of the crack under stress can be expressed as:

[0153]

[0154] Where ξ is the energy-related coefficient per unit volume, W is the stress energy, and the stress energy of the pipeline crack under stress can be expressed as:

[0155]

[0156] In formula (14), υ is Poisson's ratio, E is elastic modulus, and σ r is the composite stress value of the crack, which can be expressed as:

[0157]

[0158] Among them, σ1, σ2, and σ3 are the three main direction stresses of pipeline cracks.

[0159] Solving equations (13), (14) with equations (8), (9), and (10) yields:

[0160]

[0161] Formula (16) is the magnetization intensity equation of the pipeline under stress. From formulas (3), (4), and (16), it can be seen that the magnetization intensity and magnetic signal of the crack will also increase further with the increase of stress, thereby realizing stress detection of pipeline cracks.

[0162] Combining equations (12) and (16), we can see that the magnetic signal at the crack will effectively detect stress, and the external excitation magnetic field will also increase the detection effect. However, at this time, no matter what the intensity of the single excitation magnetic field is, the magnetic signal at the crack is a mixed signal generated by stress and the external magnetic field, that is, the detection signal contains dual information of stress and crack size. Therefore, only by using strong and weak excitation magnetic fields can the stress signal extraction at the crack be completed, and the effective detection of stress at the pipeline crack can be achieved.

[0163] Step 2): Extract stress signals at cracks under strong and weak magnetic fields

[0164] Here, we extract stress signals and realize stress detection at pipeline cracks by calculating the finite element equations of pipeline crack magnetic signals under strong and weak excitation. In the finite element method, the solution to pipeline crack magnetic signals is actually the solution of Maxwell's equations under the corresponding boundary conditions. In order to realize the calculation of crack magnetic signals under the finite element equation, we first assume that the normal pipeline material is uniform and isotropic, that is, it is assumed that the magnetic permeability at each point in the pipeline is the same, and the magnetic properties manifested in all directions are the same. At this time, under Maxwell's equations, in the pipeline wall where the medium magnetic permeability is μ, the current density The stable magnetic field formed With magnetic induction The relationship between them is:

[0165]

[0166]

[0167]

[0168] However, in actual engineering calculations, since the curl of the magnetic field intensity vector is not zero, it is impossible to use the scalar magnetic potential for analytical solution in a relatively stable magnetization region. Therefore, we use the vector magnetic potential To calculate the corresponding finite element magnetic signal in the magnetic field. and magnetic induction intensity The relationship between them is:

[0169]

[0170] Solving equations (17), (18), (19), and (20) together, we can obtain:

[0171]

[0172] In solving the finite element method, we generally do not directly give the solution of equation (21), but through an energy functional equivalent to it, by solving the extreme value of this energy functional at each point of the material, we can solve the magnetic signal generated by the pipeline under the external magnetic field and stress. Since equation (21) is a vector magnetic potential equation, it satisfies the Poisson equation and belongs to a generalized equation. Therefore, combining it with the boundary conditions constitutes a boundary value problem. From the above, we can see that: in the cylindrical coordinate system (r, θ, z), the boundary conditions of the vector magnetic potential can be written as:

[0173]

[0174] Solving in equation (22), the region is Ω, and the corresponding boundary condition is Γ. In solving electromagnetic field problems, the functional F(A) has the energy dimension, so it is also called the energy functional. The minimum value of the energy functional can be expressed as:

[0175]

[0176] Discretize the region Ω into E triangular units, the three vertices of the unit are (i, j, m), and select the unit displacement function:

[0177] A(r,z)=a1+a2r+a3z (24)

[0178] In solving the energy functional, the total energy is the sum of the individual energy functionals:

[0179] F(A) e =F(A) e′ +F(A) e″ (25)

[0180] In formula (25):

[0181]

[0182]

[0183] In formula (26) and formula (27), Γ e / Γ2 belongs to the unit boundary Γ e , but it does not belong to the edge of Γ2, and S is the surface integral region. The surface integral of formula (26) and the line integral of formula (27) can be discretized in the operational equations.

[0184] The linear interpolation function F(A) e′ The expression is:

[0185]

[0186] Formula (28) is the energy expression of the discretized unit e. Taking the first-order partial derivative of the potential function A (k = i, j, m, l = i, j, m) of each vertex in the unit, we get:

[0187]

[0188] In formula (29):

[0189]

[0190] By further taking the extreme value of F(A) in equation (29), we can obtain the finite element linear equations of the crack magnetic signal at n nodes:

[0191]

[0192] In formula (31):

[0193]

[0194] In formula (31), A lk , K lk , R lk The matrices are the magnetic potential matrix, coefficient matrix and excitation matrix of the finite element equations of the crack magnetic signal, respectively. The magnetic potential matrix contains the stress information of the crack, and the coefficient matrix contains the crack size information. Further solving the Vandermonde determinant of equation (31) under strong and weak dual excitation magnetic fields can make use of the characteristics that the strong and weak excitation detection systems will simultaneously detect the same crack in strong and weak magnetic detection. On the basis of retaining the magnetic potential matrix, the coefficient matrix is ​​eliminated, thereby eliminating the crack size information of the detection signal and retaining the stress information, completing the stress information extraction of the strong and weak detection signals, and realizing the effective detection of stress at the pipeline crack.

[0195] The present invention also includes an analytical calculation part of the model used for the research of strong and weak magnetic stress detection characteristics, and a finite element simulation modeling and calculation analysis part of the model used for engineering calculations.

[0196] The analytical calculation part uses Matlab software to perform analytical calculation and analysis of the model; the finite element simulation part uses ANAYS software to perform simulation modeling and calculation analysis.

[0197] In the analytical calculation part, the external magnetic field change parameter is set to 20K / AM -1 —-20K / AM -1 , stress variation parameters are 0MPa-100MPa (interval 20MPa).

[0198] In the analytical calculation part, the parameters of equation (12) and equation (16) are set as μ0=4*pi*(1e-7), δ=±1, Ms=1.71e6, a=1000, α=0.001, c=0.1, r1=7×10-18A. -2 m 2 ,r′1=-1×10-25A -2 ·m 2 ·Pa -1 ,r2=-3.3×10-30A -4 ·m 4 ,r′2=2.1×10-38A -4 ·m 4 ·Pa -1 , and further analytical calculations are performed as Figure 1 The pipeline crack hysteresis loop and magnetization curve shown are used to analyze and study the stress detection characteristics of pipeline strong and weak magnetic cracks.

[0199] like Figure 1 As shown in the figure: With the increase of stress value, the hysteresis loop and magnetization curve decrease, and the decrease amplitude increases first and then decreases with the increase of external magnetic field, and overlaps again when magnetic saturation is reached. It can be seen that the stress information in the crack magnetic signal under strong excitation is covered, which is pure crack size information. The crack magnetic signal under weak excitation can detect crack stress, but it is a mixture of crack size and stress information.

[0200] The finite element simulation modeling and calculation analysis part uses finite element simulation software to establish a magnetic mechanical model of the cracked pipe. Figure 2 It can be seen that the crack is set at the center of the pipeline surface, and displacement constraints are applied to both sides of the pipeline model to simulate the pipeline operation condition. Internal pressure is applied to the pipeline, and an excitation magnetic field is added. The internal pressure of the pipeline causes severe stress concentration at the pipeline defect. As the internal pressure of the pipeline increases, the stress at the pipeline crack also increases.

[0201] In all the finite element simulation modeling and calculation analysis parts, the pipeline is set to be X70 steel, with an elastic modulus of 2*10 6 N / m -2 , Poisson's ratio PRXY is 0.3 and the magnetic permeability is 280H / m.

[0202] In the finite element simulation modeling and calculation analysis part, the pipeline length is set to 4000mm, the wall thickness is 16.5mm, and the pipeline diameter is 1100mm.

[0203] The specific calculation and analysis steps of the finite element simulation model of the present invention are:

[0204] 1) Calculation of pipeline crack excitation characteristics and stress detection characteristics

[0205] a. Calculation of excitation characteristics of crack magnetic signal

[0206] Fixed model parameters: pipeline internal pressure 10Mpa, crack size: 30mm*1mm*2mm (length*width*depth), lift-off value 3mm; variable model parameters: excitation magnetic field 50nμT-75μT; scanning path: along the X axis +30mm--30mm. Figure 3 As shown, the excitation characteristic diagram of the pipeline crack magnetic signal is calculated.

[0207] Depend on Figure 3 It can be seen that the magnetic signal of the crack under the excitation magnetic field has a peak value in the tangent line and a peak-to-peak value in the normal direction and passes through the zero point. As the external magnetic field increases, the intensity of the magnetic signal increases, but the peak point and the zero point do not fluctuate.

[0208] b. Calculation of stress detection characteristics of crack magnetic signal

[0209] Fixed model parameters: excitation magnetic field 50nμT (geomagnetic field), crack size: 30mm*1mm*2mm, lift-off value 3mm; variable model parameters: pipeline internal pressure 5MPa-30MPa; scanning path: +30mm--30mm along the X axis. Figure 4 As shown in the figure, the stress detection characteristic diagram of pipeline crack magnetic signal is calculated.

[0210] Depend on Figure 4 It can be seen that the magnetic signal of the crack under stress has a peak value on the tangent line and a peak-to-peak value and passes through the zero point in the normal direction, indicating that the signal characteristics generated by the external field and stress are the same. As the internal pressure of the pipeline, that is, the crack stress, increases, the intensity of the magnetic signal increases, but the peak point and the zero point do not fluctuate.

[0211] 2) Extraction of stress signals at cracks under strong and weak magnetic fields

[0212] a. Influence of crack stress on magnetic potential matrix

[0213] Fixed model parameters: crack size 30mm*1mm*2mm, lift-off value 3mm; variable model parameters: pipeline internal pressure 5MPa-20MPa; scanning path: along the X axis +30mm--30mm. At this time, under 75μT and 60μT as strong and weak excitation magnetic fields, the following are calculated respectively: Figure 5 , Figure 6 The characteristic diagram of crack magnetic signal changing with stress under strong and weak excitation, and the magnetic potential matrix under strong and weak magnetization are extracted at the same time, as shown in the following figure: Figure 7 The crack stress influence on the magnetic potential matrix is ​​shown.

[0214] Depend on Figure 5 , 67 It can be seen that the crack magnetic signal increases with the increase of pipeline internal pressure (crack stress) under strong and weak excitation, and the magnetic potential moment decreases with the increase of pipeline internal pressure, which shows that the magnetic potential matrix can effectively detect crack stress.

[0215] b. Effect of crack size on magnetic potential matrix

[0216] Fixed model parameters: pipeline internal pressure value is 10Mpa, lift-off value is 3mm; variable model parameters: crack size No. 1 30mm*0.5mm*1mm, No. 2 30mm*0.5mm*2mm, No. 3 30mm*1mm*2mm, No. 4 30mm*1mm*3mm; scanning path: along the X axis +30mm--30mm. At this time, under 75μT and 60μT as strong and weak excitation magnetic fields, the following are calculated respectively: Figure 8 , Fig. 9 The crack magnetic signal under strong and weak excitation changes with the crack size characteristic diagram, and the magnetic potential matrix under strong and weak magnetization is extracted at the same time, and the following is obtained: Fig.10 The diagram shows the effect of crack size on the magnetic potential matrix.

[0217] Depend on Figure 8 , 9 , 10 It can be seen that the crack magnetic signal increases with the size of the defect under strong and weak excitation, but its magnetic potential matrix does not change, which means that the magnetic potential matrix can eliminate the influence of crack size while detecting crack stress.

[0218] The present invention also includes hysteresis loop experiments of experimental specimens under different stresses, and magnetic signal detection characteristic experiments under different external magnetic fields and stresses, so as to verify the correctness of various theoretical model calculations.

[0219] Depend on Fig.11 It can be seen that the experimental specimen is a cracked X70 pipe specimen with a specimen size of 400mm*40mm*16.6mm and a crack size of 30mm*1.5mm*2mm.

[0220] Depend on Fig.12 It can be seen that the hysteresis loop experimental system: the excitation coil is evenly wound on the U-shaped magnetic core, and it is fixed on the specimen together with the receiving coil. The excitation coil and the receiving coil are respectively connected to the excitation and receiving terminals of the magnetic properties analyzer (MATS-2010SD) to provide magnetization information for the experiment. The specimen is fixed on the electro-hydraulic servo universal tensile machine (WAW-2000) to provide tensile force for the specimen.

[0221] Depend on Fig.13It can be seen that the magnetic signal detection characteristic experimental system: the specimen is fixed on the WAW-2000 tensile machine to provide stress for it, and a strain gauge is attached to the specimen to detect the stress in real time. The excitation coil is installed on the side of the specimen, and a magnetic probe is installed inside it, which can excite and scan the specimen when driven by a forklift. The sampling frequency of the magnetic probe is 1.5KHz, and the magnetic field detection accuracy is 1nT. The strain gauge is DH3818 model, the sampling rate is 200 times / second, and the A / D resolution is 14 bits.

[0222] The specific steps of the experiment described in the present invention are:

[0223] 1) Hysteresis loop experiment under different stresses: Using the hysteresis loop experiment system, stress is applied to the specimen, strain gauges are attached to the surface of the specimen to test the stress value, and the hysteresis loop under different stresses is measured at the same time. Fig.14 The hysteresis loop diagram of the specimen under different stresses is shown. Fig.14 It can be seen that with the increase of stress, the hysteresis loop decreases, and its decrease amplitude increases first and then decreases. In the saturation magnetization stage, the hysteresis loops under different stresses overlap, and its stress detection characteristics disappear.

[0224] 2): Stress detection characteristics and excitation characteristics experiment: Using the magnetic signal detection characteristics experimental system, the specimen is tested at a fixed point when the excitation magnetic field is the earth's magnetic field and the tension is 10NK-80KN. The specimen is scanned when the excitation magnetic field is 0A-10A and the tension is 15KN. Thus, the following are obtained respectively: Fig.15 , 16 The stress detection characteristic diagram and excitation characteristic diagram of the experimental specimen are shown in Fig.15 , 16 It can be seen that the crack magnetic signal has a peak value in the tangential component and a peak-to-peak value in the normal component, and crosses the zero point. With the increase of stress and external magnetic field, the intensity of the crack magnetic signal increases.

[0225] 3): Stress signal extraction characteristic experiment: Use the magnetic signal detection characteristic experimental system, and add external magnetic field and stress to the specimen at the same time when the excitation magnetic field is 0A-10A and the tension is 10NK-80KN. The detection signal under 10A excitation is the crack magnetic signal under strong excitation, and the detection signal under other excitations is the crack magnetic signal under weak excitation. Based on the magnetization characteristic equation of the magnetic potential of ferromagnetic materials in the static magnetic space ( A, M, and H are respectively the magnetic potential, magnetization intensity, and magnetic signal intensity under strong and weak magnetic fields. The magnetic potential calculation is performed using the signals under strong and weak excitation to complete the stress signal extraction. Fig.17 As shown. Fig.17It can be seen that when the weak excitation intensity is 5A and 2A, the calculation results do not change with the change of tension. This is because the strong external magnetic field covers the stress signal. When the weak excitation intensity is reduced to 1.5A, 1A, and 0.5A, the stress signal gradually appears, and the calculation results begin to decrease with the increase of stress, thereby completing the stress signal extraction.

[0226] In order to increase the engineering practicability of the method, the present invention also conducts engineering experiments and excavation verification of pipeline strong and weak magnetic stress internal detection.

[0227] Depend on Fig.18 It can be seen that this is the launch site for the strong and weak magnetic stress internal detection of pipelines. Its running path is from Manas to Urumqi, with an operating length of 210km. The detector running speed is 2.62m / s. The diameter of the detected pipeline is 1219mm and the wall thickness is 18.37mm. During the detection process, 12145 circumferential welds, 62 elbows, 16 tees and 3 flanges were found. 2463 defects were detected, which can be divided into: pure crack detection signals (strong magnetic detection has signals, weak magnetic detection has no signals), stress crack detection signals (strong magnetic detection has signals, weak magnetic detection has signals), pure stress concentration detection signals (strong magnetic detection has no signals, weak magnetic detection has signals), and their representative signals are shown in the figure below. Fig.19 , 20 , as shown in Figure 21.

[0228] Depend on Fig. 22 It can be seen that the present invention further conducts excavation verification on crack stress damage of some pipelines, and uses a magnetic memory detector to measure the excavation crack stress. The figure shows the excavation site. Fig.23 It is the magnetic memory detection data.

[0229] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solution described in the examples of the present invention. Ordinary technicians in the field should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for detecting internal stress at pipeline cracks based on strong and weak magnetism, comprising the following steps: Step 1): Calculation of strong and weak magnetic crack stress detection characteristics The essence of pipeline strong and weak magnetic stress internal detection is to use the magnetic signals generated at pipeline cracks under strong and weak excitation magnetic fields to detect different crack stress intensities. To this end, the purpose of mathematical model calculation is to calculate the magnetic signal characteristics of cracks under two changing parameters: external magnetic field and stress. First, assume that there is a crack on the pipe surface, and the crack size is: D X *D Y *D Z , with the crack center as the origin, establish a three-dimensional Cartesian coordinate system. In a pipeline pressure environment, an excitation magnetic field with an external magnetic field of H0 is added to the pipeline. At this time, the pipeline pressure and the external magnetic field will cause the crack to accumulate positive and negative magnetic charges, and then generate a magnetic signal with an intensity of H at the crack. Set the magnetic charge surface element to dy m dz m , the magnetic signal intensity generated by this surface microelement at any point P(X, Y, Z) in the detection space is: Where r0 is the distance from the surface element to point P, μ0 is the vacuum magnetic permeability, and ρ is the magnetic charge density, which can be expressed as: Where M is the material magnetization intensity. Integrate equation (1) and substitute equation (2) to obtain the magnetic signal intensity generated by the crack at point P: Where H x is the tangential magnetic signal intensity, H z is the normal magnetic signal intensity. It can be seen from formulas (3) and (4) that the magnetic signal generated by pipeline cracks is related to the magnetization intensity, crack size and detection point position. In order to further study the crack stress detection characteristics of strong and weak magnetism, the magnetic space coefficient f(x, z) related to the crack size and the detection point position is defined, that is, H = M × f(x, z). The magnetic space coefficient f(x, z) can be expressed as: From the equation H = M × f (x, z), we know that in strong and weak magnetic detection, the two changing parameters of external magnetic field and stress that we want to study are both reflected by the magnetization intensity M. For this reason, the changing characteristics of the pipeline magnetization intensity under different external magnetic fields and stresses are clarified, that is, the crack stress detection characteristics of strong and weak magnetism are clarified. The magnetization intensity of the in-service pipeline can be expressed as: M=cM an +(1-c)Mirr (6) Where c is the reversible component coefficient, M irr is the irreversible magnetization caused by the pinning point, M an is the hysteresis-free magnetization. The asymptotic principle in JA theory can further give the energy consumption E caused by the pinning point. pin The equation is: Therefore, based on the law of conservation of energy, the hysteresis-free magnetization intensity M can be calculated according to formula (7): an Further solving: Where k is the pinning coefficient of the material, δ=±1 is the directional coefficient, and H e is the equivalent magnetic field, which can be expressed as: Where F is the system energy value, α is the molecular field parameter, σ is the stress value, and λ is the hysteresis expansion coefficient, which can be expressed as: λ=γ1M 2 +2γ2M 4 (10) In formula (10), γ1 and γ2 are stress determining parameters, which can be obtained by Taylor series expansion: Derivative of equation (6) with respect to the external magnetic field H0 and solve it together with equations (8), (9) and (10) to obtain: Formula (12) is the magnetization intensity equation of the pipeline under the external magnetic field. Combining formula (3), (4), and (12), it can be seen that under the action of the external excitation magnetic field, the magnetization intensity and magnetic signal of the crack will further increase with the increase of the excitation magnetic field, thereby making the detection efficiency of the crack magnetic signal higher and the anti-interference ability stronger. When stress exists at the crack of the pipeline, the stress will increase the energy at the crack. At this time, the pipeline material will rotate the magnetic domain according to the principle of minimum energy, thereby balancing the increase in energy and generating magnetization intensity. At this time, the magnetization intensity of the crack under stress can be expressed as: Where ξ is the energy-related coefficient per unit volume, W is the stress energy, and the stress energy of the pipeline crack under stress can be expressed as: In formula (14), υ is Poisson's ratio, E is elastic modulus, σ r is the composite stress value of the crack, which can be expressed as: In the formula, σ1, σ2, and σ3 are the three main direction stresses of the pipeline crack. Solving equations (13), (14) with equations (8), (9), and (10) yields: Formula (16) is the magnetization intensity equation of the pipeline under stress. From formulas (3), (4), and (16), it can be seen that the magnetization intensity and magnetic signal of the crack will also increase further with the increase of stress, thereby realizing stress detection of pipeline cracks. Combining equations (12) and (16), we can see that the magnetic signal at the crack will effectively detect stress, and the external excitation magnetic field will also increase the detection effect. However, at this time, no matter what the intensity of the single excitation magnetic field is, the magnetic signal at the crack is a mixed signal generated by stress and the external magnetic field, that is, the detection signal contains dual information of stress and crack size. Therefore, only by using strong and weak excitation magnetic fields can the stress signal extraction at the crack be completed, and the effective detection of stress at the pipeline crack can be achieved. Step 2): Extract stress signals at cracks under strong and weak magnetic fields Here, we extract stress signals and realize stress detection at pipeline cracks by calculating the finite element equations of pipeline crack magnetic signals under strong and weak excitation. In the finite element method, the solution to pipeline crack magnetic signals is actually the solution of Maxwell's equations under the corresponding boundary conditions. In order to realize the calculation of crack magnetic signals under the finite element equation, we first assume that the normal pipeline material is uniform and isotropic, that is, it is assumed that the magnetic permeability at each point in the pipeline is the same, and the magnetic properties manifested in all directions are the same. At this time, under Maxwell's equations, in the pipeline wall where the medium magnetic permeability is μ, the current density The stable magnetic field formed With magnetic induction The relationship between them is: However, in actual engineering calculations, since the curl of the magnetic field intensity vector is not zero, it is impossible to use the scalar magnetic potential for analytical solution in a relatively stable magnetization region. Therefore, we use the vector magnetic potential To calculate the corresponding finite element magnetic signal in the magnetic field. and magnetic induction intensity The relationship between them is: Solving equations (17), (18), (19), and (20) together, we can obtain: In solving the finite element method, we generally do not directly give the solution of equation (21), but through an energy functional equivalent to it, by solving the extreme value of this energy functional at each point of the material, we can solve the magnetic signal generated by the pipeline under the external magnetic field and stress. Since equation (21) is a vector magnetic potential equation, it satisfies the Poisson equation and belongs to a generalized equation. Therefore, combining it with the boundary conditions constitutes a boundary value problem. From the above, we can see that: in the cylindrical coordinate system (r, θ, z), the boundary conditions of the vector magnetic potential can be written as: Solving in equation (22), the region is Ω, and the corresponding boundary condition is Γ. In solving electromagnetic field problems, the functional F(A) has the energy dimension, so it is also called the energy functional. The minimum value of the energy functional can be expressed as: Discretize the region Ω into E triangular units, the three vertices of the unit are (i, j, m), and select the unit displacement function: A(r,z)=a1+a2r+a3z (24) In solving the energy functional, the total energy is the sum of the individual energy functionals: F(A) e =F(A) e′ +F(A) e″ (25) In formula (25): In formula (26) and formula (27), Γ e / Γ2 belongs to the unit boundary Γ e , but it does not belong to the edge of Γ2, and S is the surface integral region. The surface integral of formula (26) and the line integral of formula (27) can be discretized in the operational equations. The linear interpolation function F(A) e′ The expression is: Formula (28) is the energy expression of the discretized unit e. Taking the first-order partial derivative of the potential function A (k = i, j, m, l = i, j, m) of each vertex in the unit, we get: In formula (29): By further taking the extreme value of F(A) in equation (29), we can obtain the linear equations of the finite element of the crack magnetic signal at n nodes: In formula (31): In formula (31), A lk , K lk , R lk The matrices are the magnetic potential matrix, coefficient matrix and excitation matrix of the finite element equations of the crack magnetic signal, respectively. The magnetic potential matrix contains the stress information of the crack, and the coefficient matrix contains the crack size information. Further solving the Vandermonde determinant of equation (31) under strong and weak dual excitation magnetic fields can make use of the characteristics that the strong and weak excitation detection systems will simultaneously detect the same crack in strong and weak magnetic detection. On the basis of retaining the magnetic potential matrix, the coefficient matrix is ​​eliminated, thereby eliminating the crack size information of the detection signal and retaining the stress information, completing the stress information extraction of the strong and weak detection signals, and realizing the effective detection of stress at the pipeline crack. The present invention also includes an analytical calculation part for studying the strong and weak magnetic stress detection characteristics using the model of the present invention, and a finite element simulation modeling and calculation analysis part for engineering calculations using the model.

2. According to claim 1, a method for detecting internal stress at pipeline cracks based on strong and weak magnetism, characterized in that The analytical calculation part uses Matlab software to perform analytical calculation and analysis of the model; the finite element simulation part uses ANAYS software to perform simulation modeling and calculation analysis.

3. According to claim 1, a method for detecting internal stress at a pipeline crack based on strong and weak magnetism, characterized in that In the analytical calculation part, the external magnetic field change parameter is set to 20K / AM -1 —-20K / AM -1 , stress variation parameters are 0MPa-100MPa (interval 20MPa).

4. According to claim 1, a method for detecting internal stress at pipeline cracks based on strong and weak magnetism is characterized in that In the analytical calculation part, the parameters of equation (12) and equation (16) are set as μ0=4*pi*(1e-7), δ=±1, Ms=1.71e6, a=1000, α=0.001, c=0.1, r1=7×10-18A. -2 m 2 ,r′1=-1×10-25A -2 ·m 2 ·Pa -1 ,r2=-3.3×10-30A -4 ·m 4 ,r′2=2.1×10-38A -4 ·m 4 ·Pa -1 , and further analytically calculated the pipeline crack hysteresis loop and magnetization curve, and conducted an analytical study on the pipeline strong and weak magnetic crack stress detection characteristics.

5. According to claim 1, a method for detecting internal stress of pipeline defects based on dual magnetic fields is characterized in that In the finite element simulation modeling and calculation analysis part, the magnetic mechanical model of the cracked pipeline is established using finite element simulation software. The crack is set at the center of the pipeline surface, and displacement constraints are applied to both sides of the pipeline model to simulate the pipeline operation condition. Internal pressure is applied to the pipeline, and an excitation magnetic field is added. The internal pressure of the pipeline causes severe stress concentration at the pipeline defect. As the internal pressure of the pipeline increases, the stress at the pipeline crack also increases.

6. According to claim 1, a method for detecting internal stress at pipeline cracks based on strong and weak magnetism is characterized in that In the finite element simulation modeling and calculation analysis part, the pipeline is set to be X70 steel, with an elastic modulus of 2*10 6 N / m -2 , Poisson's ratio PRXY is 0.3 and the magnetic permeability is 280H / m.

7. According to claim 1, a method for detecting internal stress at pipeline cracks based on strong and weak magnetism, characterized in that The finite element simulation modeling and calculation analysis part sets the pipeline length to 4000 mm, the wall thickness to 16.5 mm, and the pipeline diameter to 1100 mm.

Citation Information

Cited By

  • Stress detection method for pipeline

    CN119394476A

  • Mixed source magnetic memory remote sensing rail transit engineering structure health detection method and device

    CN120009386A