Magnetic core and magnetic component
Optimizing the area ratio and skewness of soft magnetic powder distribution in magnetic cores improves magnetic permeability and DC superposition characteristics by controlling particle size and resin binder usage, addressing local magnetic saturation issues.
Patent Information
- Application Number
- CN202410679349.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-03
AI Technical Summary
Increasing the filling rate of soft magnetic powder in magnetic cores leads to increased contact points between magnetic particles, causing local magnetic saturation and deteriorating DC superposition characteristics in magnetic components.
A magnetic core with an average area ratio of soft magnetic powder between 75% and 90% and a skewness of the area ratio distribution between 0.01 and 0.05 in absolute value, achieved by controlling the particle size distribution and using a resin binder to maintain optimal contact points and reduce local magnetic saturation.
The solution enhances both magnetic permeability and DC superposition characteristics by optimizing the area ratio and skewness of the soft magnetic powder distribution, allowing for higher DC superposition rated currents and reduced filling factors.
Smart Images

Figure CN119069225A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a magnetic core containing soft magnetic powder and a magnetic component having the magnetic core. Background Art
[0002] Magnetic components such as inductors, transformers, and choke coils are widely used in power circuits of various electronic devices. In order to improve magnetic properties, attempts have been made to increase the filling rate of soft magnetic powder contained in the magnetic core of magnetic components. For example, Patent Document 1 discloses that by using two types of metal magnetic powders with different particle sizes as soft magnetic powders, the filling rate of the soft magnetic powder in the magnetic core can be increased, and magnetic properties such as magnetic permeability can be improved.
[0003] However, when the filling rate of the soft magnetic powder in the magnetic core is increased, the number of contact points between magnetic particles may increase, causing local magnetic saturation and deteriorating the DC superposition characteristics.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2011-192729 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] An object of the embodiments illustrated in the present disclosure is to provide a magnetic core and a magnetic component having excellent DC superposition characteristics.
[0009] Technical means to solve technical problems
[0010] In order to achieve the above object, the magnetic core of the present invention comprises soft magnetic powder, wherein the average area ratio of the soft magnetic powder in any cross section of the magnetic core is 75% or more and 90% or less, and the skewness of the area ratio distribution of the soft magnetic powder in the cross section is 0.01 or more in absolute value, wherein the skewness of the area ratio distribution is obtained by setting the maximum particle size of the soft magnetic powder in the cross section to D MAX , the area demarcated by dividing the above cross section with equally spaced grids is (2D MAX ) 2 The area ratio of the soft magnetic powder is calculated in each square area and determined.
[0011] Since the magnetic core has the above characteristics, it can have both high magnetic permeability and excellent DC superposition characteristics.
[0012] It is preferable that the skewness of the area ratio distribution is 0.05 or more in absolute value.
[0013] A magnetic component according to the present invention includes the above-mentioned magnetic core and a coil. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic cross-sectional view showing a magnetic core according to one embodiment of the present invention.
[0015] Figure 2 This is an example of the particle size distribution of soft magnetic powder.
[0016] Figure 3A It is a schematic diagram showing the method of measuring the area ratio of the soft magnetic powder.
[0017] Figure 3B It is a schematic diagram showing the method of measuring the area ratio of the soft magnetic powder.
[0018] Figure 4 This is a graph illustrating the area ratio distribution of the soft magnetic powder.
[0019] Figure 5 To include Figure 1 Schematic cross-sectional view of an example of a magnetic component of the magnetic core shown.
[0020] Fig. 6A The graph is a graph showing the relationship between the average area ratio (filling rate) of the soft magnetic powder and the DC superposition rated current (Isat).
[0021] Figure 6B The graph is a graph showing the relationship between the average area ratio (filling rate) of the soft magnetic powder and the initial magnetic permeability (μi).
[0022] Figure 6C This is a graph showing the relationship between initial magnetic permeability and DC superposition rated current.
[0023] Figure 7 This is a graph showing the relationship between initial magnetic permeability and DC superposition rated current.
[0024] Figure 8 This is a graph showing the relationship between initial magnetic permeability and DC superposition rated current.
[0025] Fig. 9 The graph is a graph showing the relationship between the absolute value of the skewness and the DC superposition rated current.
[0026] Explanation of symbols:
[0027] 2: Magnetic core
[0028] 1: Soft magnetic powder
[0029] 10: Metal particles
[0030] 10a: Large particles
[0031] 10b: Small particles
[0032] 10c: Medium grain
[0033] 3: Resin
[0034] 20: Square area
[0035] 100: Magnetic parts
[0036] 5: Coil
[0037] 5a, 5b: End
[0038] 6, 8: External electrodes DETAILED DESCRIPTION
[0039] The embodiments of the present disclosure are described below with reference to the accompanying drawings. The embodiments of the present disclosure described below are examples for explaining the present disclosure, and the components of the embodiments, such as numerical values, shapes, materials, and manufacturing processes, may be changed or modified within the scope that does not cause technical problems.
[0040] The magnetic core 2 of this embodiment is a composite magnetic body including a soft magnetic powder 1 and a resin 3. The soft magnetic powder 1 contains metal particles 10 made of a soft magnetic metal. Figure 1 As shown, the metal particles 10 of the soft magnetic powder 1 are dispersed in the resin 3, and the metal particles 10 are bonded via the resin 3, thereby forming the magnetic core 2 into a predetermined shape. The outer dimensions and shape of the magnetic core 2 are not particularly limited. In addition to the soft magnetic powder 1 and the resin 3, the magnetic core 2 may also contain voids and a modifier.
[0041] The composition and structure of the metal particles 10 are not particularly limited. For example, the metal particles 10 may have a crystalline structure, a nanocrystalline structure, or an amorphous structure. Examples of soft magnetic metals having a crystalline structure include pure iron, pure cobalt, Fe-Ni alloys, Fe-Si alloys, Fe-Si-Cr alloys, Fe-Si-Al alloys, Fe-Si-Al-Ni alloys, Fe-Ni-Si-Co alloys, Fe-Co alloys, Fe-Co-V alloys, Fe-Co-Si alloys, and Fe-Co-Si-Al alloys. As soft magnetic metals having a nanocrystalline structure or an amorphous structure, there can be mentioned Fe-Si-B alloys, Fe-Si-BC alloys, Fe-Si-BC-Cr alloys, Fe-Nb-B alloys, Fe-Nb-BP alloys, Fe-Nb-B-Si alloys, Fe-Co-PC alloys, Fe-Co-B alloys, Fe-Co-B-Si alloys, Fe-Si-B-Nb-Cu alloys, Fe-Si-B-Nb-P alloys, Fe-Co-BP-Si alloys, Fe-Co-BP-Si-Cr alloys, etc.
[0042] The composition of the metal particles 10 can be analyzed using, for example, an EDX device (energy dispersive X-ray analyzer) or an EPMA (electron probe microanalyzer). In addition, the composition of the metal particles 10 can also be analyzed using a 3DAP (three-dimensional atom probe). When using 3DAP, a small area (e.g., an area of Φ20nm×100nm) can be set inside the metal particle 10 of the measurement object to measure the average composition, and the composition of the particle body can be determined by excluding the influence of the resin component contained in the magnetic core 2 or the oxidation of the particle surface.
[0043] In addition, the structure of the metal particles 10 can be analyzed using XRD (X-ray diffraction) or electron diffraction. In the present embodiment, "amorphous structure" refers to a structure with an amorphous degree of more than 85%, or a structure in which no spots caused by crystallization can be detected in electron diffraction. Amorphous structures include structures that are substantially composed of amorphous or structures composed of heterogeneous amorphous. In the case of a structure composed of heterogeneous amorphous, the average particle size (average crystallite size) of the crystals present in the amorphous is preferably greater than 0.1nm and less than 10nm. In addition, in the present embodiment, "nanocrystalline structure" refers to a structure with an amorphous degree of less than 85% and an average crystallite size of less than 100nm (preferably 3nm to 50nm), while "crystalline structure" refers to a structure with an amorphous degree of less than 85% and an average crystallite size of more than 100nm.
[0044] When the structure of the metal particle 10 is analyzed by XRD, the degree of amorphization can be expressed by the ratio of the amorphous scattering integrated intensity to the crystalline scattering integrated intensity and the total of the amorphous scattering integrated intensity. In addition, the amorphous part and the crystallized part inside the metal particle 10 can be identified by using an electron microscope, and the degree of amorphization can be obtained based on the area ratio of the amorphous part in the metal particle 10.
[0045] The particle size of the metal particles 10 is not particularly limited. For example, the metal particles 10 may have an average particle size of 1 μm or more and 100 μm or less. The particle size of the metal particles 10 may be measured and calculated by image analysis of the cross section of the magnetic core 2. The “particle size” shown in this embodiment refers to the equivalent circular diameter of the metal particles 10 observed in the cross section of the magnetic core 2. The equivalent circular diameter of each metal particle 10 is calculated by (4α / π) when the area of each metal particle 10 in the cross section of the magnetic core 2 is set to α. 1 / 2 The particle size distribution of the soft magnetic powder 1 is preferably determined by measuring and calculating the equivalent circle diameters of at least 100 metal particles 10 in the cross section of the magnetic core 2, and the average particle size of the metal particles 10 can also be determined by calculating the arithmetic mean of the measured equivalent circle diameters.
[0046] The shape of the metal particles 10 is not limited, but the average circularity of the metal particles 10 is preferably 0.80 or more, more preferably 0.90 or more. The circularity of each metal particle 10 is calculated by 2(πα) when the area of each metal particle 10 on the cross section of the magnetic core 2 is α and the perimeter of each metal particle 10 is L. 1 / 2 The average circularity is preferably calculated by measuring the circularity of at least 100 metal particles 10 .
[0047] In the soft magnetic powder 1, an insulating film is preferably formed to cover the surface of the particles. The insulating film can be formed on each metal particle 10 constituting the soft magnetic powder 1, and the soft magnetic powder 1 can also include metal particles 10 with an insulating film and metal particles 10 without an insulating film. The material of the insulating film is not particularly limited. For example, the insulating film can be made into a film (oxide film) formed by oxidation of the particle surface, or a film containing an inorganic material such as BN, SiO2, MgO, Al2O3, phosphate, silicate, borosilicate, bismuthate or various glasses, preferably a film containing oxide glass.
[0048] Examples of oxide glass include silicate (SiO2) glass, phosphate (P2O5) glass, bismuth (Bi2O3) glass, and borosilicate (B2O3-SiO2) glass. More specifically, examples of silicate glass include SiO2 (Si-O glass), soda-lime glass (Si-Na-Ca-O glass), Si-Ba-Mn-O glass, and Si-Mn-Ca-Na-O glass. Examples of phosphate glass include P2O5 (PO glass), P-Zn-Al-O glass, and P-Zn-Al-RO glass ("R" is one or more elements selected from alkali metals). Examples of bismuth glass include Bi-Zn-B-Si-O glass and Bi-Zn-B-Si-Al-O glass. In addition, examples of borosilicate glass include Ba-Zn-B-Si-Al-O glass.
[0049] The insulating film may have a structure in which two or more films are stacked. The average thickness of the insulating film is preferably from 1 nm to 100 nm, and more preferably from 5 nm to 50 nm.
[0050] Although the soft magnetic powder 1 may be composed of a single powder, it is preferably composed of two or more particle groups having different particle compositions and / or particle sizes. Figure 3B As shown, the soft magnetic powder 1 preferably includes, as the metal particles 10 , large particles 10 a and small particles 10 b having a smaller particle size than the large particles 10 a .
[0051] In the case where the soft magnetic powder 1 contains large particles 10a and small particles 10b, the average particle size of the large particles 10a is preferably 5 μm to 40 μm, more preferably 10 μm to 35 μm. On the other hand, the average particle size of the small particles 10b is preferably 2 μm or less, more preferably 0.2 μm or more and less than 2 μm. In addition, the large particles 10a may have a crystalline structure, a nanocrystalline structure or an amorphous structure, and from the perspective of reducing coercive force, it is preferred to have a nanocrystalline structure or an amorphous structure. On the other hand, the small particles 10b are preferably soft magnetic metals with a crystalline structure having a high saturation magnetic flux density, such as pure iron, pure cobalt, Fe-Ni alloy, Fe-Si alloy or Fe-Co alloy.
[0052] In addition, the content ratio of the large particles 10a and the small particles 10b contained in the magnetic core 2 is not particularly limited. For example, in the cross section of the magnetic core 2, the ratio of the total area of the large particles 10a to the total area of the metal particles 10 is preferably 50% to 90%, and more preferably 60% to 80%. The ratio of the total area of the small particles 10b to the total area of the metal particles 10 is preferably 5% to 50%, and more preferably 5% to 30%.
[0053] In the soft magnetic powder 1, as metal particles 10, medium particles 10c may be included in addition to large particles 10a and small particles 10b. The average particle size of the medium particles 10c is not particularly limited but is preferably, for example, 3 μm or more and 5 μm or less. The medium particles 10c may have a crystalline structure, a nanocrystalline structure or an amorphous structure, and preferably have a nanocrystalline structure or an amorphous structure from the perspective of achieving low coercive force. The content of the medium particles 10c is not particularly limited, but it is preferably, for example, that the total area of the medium particles 10c relative to the total area of the metal particles 10 is 5% to 30%.
[0054] As described above, in the case where the soft magnetic powder 1 includes two or more particle groups, the soft magnetic powder 1 may also include a particle group without an insulating coating, but preferably the large particles 10a, the medium particles 10c, and the small particles 10b each have an insulating coating. In this case, each particle group may have an insulating coating of the same material or an insulating coating of different materials. In addition, the average circularity of each particle group is not particularly limited, but preferably the large particles 10a, the medium particles 10c, and the small particles 10b each have an average circularity of 0.80 or more.
[0055] The large particles 10a, the medium particles 10c, and the small particles 10b can be identified by classifying the metal particles 10 contained in the cross section of the magnetic core 2 based on the composition through surface analysis using an EDX device or EPMA. In addition, the large particles 10a, the medium particles 10c, and the small particles 10b can also be identified based on the particle size distribution of the soft magnetic powder 1. For example, Figure 2 is an example of the particle size distribution of the soft magnetic powder 1. Figure 2 In the case of the particle size distribution shown, the "particle group belonging to peak 1 located on the maximum particle size side (particle group in the range of LP1 to EP1)" can be specified as large particles 10a, the "particle group belonging to peak 2 located on the minimum particle size side (particle group in the range of EP2 to LP2)" can be specified as small particles 10b, and the "particle group belonging to peak 3 located between peak 1 and peak 2 (particle group in the range of LP2 to LP1)" can be specified as medium particles 10c.
[0056] The resin 3 is an insulating binder material that fixes the soft magnetic powder 1 in a predetermined dispersed state. The material of the resin 3 is not particularly limited. For example, the resin 3 may contain a thermoplastic resin, but preferably contains a thermosetting resin such as an epoxy resin, a phenolic resin or a silicone resin, and more preferably contains an epoxy resin.
[0057] The filling rate of the soft magnetic powder 1 in the magnetic core 2 is represented by the area ratio of the soft magnetic powder 1 in the cross section of the magnetic core 2. The "area ratio of the soft magnetic powder 1" refers to the ratio of the total area of the metal particles 10 contained in the cross section of the magnetic core 2 to the area of the cross section. In the present embodiment, the area ratio distribution of the soft magnetic powder 1 in the magnetic core 2 is determined by dividing any cross section of the magnetic core 2 into a plurality of analysis areas and measuring the area ratio of the soft magnetic powder 1 in each analysis area. Figure 3A and Figure 3B , the method for determining the area ratio distribution is explained in detail.
[0058] First, an arbitrary cross section of the magnetic core 2 is observed with a SEM (scanning electron microscope), and the equivalent circle diameter of the metal particles 10 contained in the cross section is measured and calculated. Then, the maximum value of the equivalent circle diameter obtained by measurement is set as the maximum particle size D of the soft magnetic powder 1. MAX (Unit: μm). Then, Figure 3A As shown in the figure, any cross section under observation is divided into equally spaced grids G. The equally spaced grids G are imaginary partitions composed of vertical and horizontal lines arranged at constant intervals. Figure 3A In the figure, the dotted lines represent the equally spaced grids G. The grid width of the equally spaced grids G is set to the maximum particle size D MAX That is, any cross section of the core 2 is divided into grids G with equal spacing and a side length of 2D. MAX With (2D MAX ) 2 The square region 20 divided by the equally spaced grids G is an analysis unit of the area ratio. It should be noted that the number of vertical lines and the number of horizontal lines in the equally spaced grids G may be different, but are preferably equal.
[0059] Figure 3B This is a schematic diagram showing an example of a square region 20. After dividing any cross section of the magnetic core 2, the area ratio x of the soft magnetic powder 1 in each square region 20 is measured. i The area ratio x of the soft magnetic powder 1 in each square region 20 is i (Unit: %) is the area of each square region 20 is set to A i (i.e. A i =(2D MAX ) 2 ), the total area of the metal particles 10 contained in each square region 20 is set to α i When α i Relative to A i The ratio (α i / A i ) indicates. Measurement area ratio x i The number of square regions 20 is set to at least 30, preferably 100 or more. In the above method, the area ratio x of the soft magnetic powder 1 in each square region 20 is measured. i , thereby being able to determine the area ratio distribution of the soft magnetic powder 1 in the magnetic core 2. It should be noted that the above analysis can be implemented using image analysis software.
[0060] In the magnetic core 2 of the present embodiment, the area ratio x i The average value (hereinafter referred to as the average area ratio x A ) is 75% or more and 90% or less. The average area ratio x A Equivalent to the average filling rate of the soft magnetic powder 1 in the magnetic core 2. Average area ratio x A Through α i / A i The total value of is divided by the number of samples (i.e. the number of square areas 20) and can also be calculated by α i The total value of divided by A i Calculated based on the total value of .
[0061] In the magnetic core 2, the skewness S of the area ratio distribution of the soft magnetic powder 1 is k (dimensionless quantity) in absolute value above 0.01 (i.e. |0.01|≤S k ). Among them, the skewness S k It is an index that indicates the bilateral symmetry of the area ratio distribution, and is a statistic that indicates that the area ratio distribution deviates from the normal distribution to a certain extent. Specifically, the skewness S of the area ratio distribution is k It is calculated by the following formula (1).
[0062]
[0063] In the above formula (1), x i is the area ratio of the soft magnetic powder 1 in each square region 20, x A is the average area ratio of the soft magnetic powder 1, σ is the standard deviation of the area ratio, and n is the number of samples (ie, the number of square regions 20).
[0064] Figure 4 The following is a graph showing the area ratio distribution of soft magnetic powder 1. The horizontal axis of the graph is the area ratio (i.e., filling rate), and the vertical axis is the frequency. Along the horizontal axis, the right side of the graph is called the high filling side, and the left side of the graph is called the low filling side. Figure 4 In the graph of FIG. 1 , three distribution curves are shown as the area ratio distribution of the soft magnetic powder 1. The average area ratio x in each distribution curve is A Both are 80%. Figure 4 Among the three distribution curves shown, the distribution curve represented by the solid line is a normal distribution. The normal distribution has a shape that is symmetrical around the maximum value. When the area ratio of the soft magnetic powder 1 follows the normal distribution, the skewness S k is 0.
[0065] Figure 4 The distribution curve represented by the single dot-dashed line is the skewness S k An example of an area ratio distribution showing negative values. k When a negative value is displayed, the area ratio is distributed more widely on the low filling rate side than on the high filling rate side, based on the maximum value. In other words, when the hem of the low filling rate side in the area ratio distribution is longer than the hem of the high filling rate side, the skewness S k Negative values are displayed. A ≤90% of the core 2, by setting the skewness S k Controlled below -0.01, and -0.01<S k Compared with the case of <0.01, the DC superposition characteristics can be further improved.
[0066] On the other hand, the distribution curve represented by the dotted line is the skewness S k An example of an area ratio distribution showing positive values. k When a positive value is displayed, the area ratio is distributed more widely on the high filling rate side than on the low filling rate side, based on the maximum value. In other words, when the bottom hem of the high filling rate side in the area ratio distribution is longer than the bottom hem of the low filling rate side, the skewness S k Displays positive value. A ≤90% of the core 2, by setting the skewness S k Set above 0.01, and the skewness S kWhen designing the magnetic core, the average filling rate of the soft magnetic powder is set so that the desired magnetic permeability can be obtained. In the magnetic core 2 of the present embodiment, the skewness S is set to 0. k Controlled above 0.01, and -0.01<S k Compared with the case of <0.01, the average area ratio x required to achieve the required magnetic permeability can be reduced. A (Average filling rate) That is, since a high magnetic permeability can be obtained at a low filling rate, contact between the metal particles 10 can be suppressed, and local magnetic saturation can be suppressed. As a result, the DC superposition characteristics can be improved.
[0067] As mentioned above, the skewness S k It can be either negative or positive. k The absolute value of S is controlled to be above 0.01, which can improve the DC superposition characteristics. From the perspective of further improving the DC superposition characteristics, the skewness S k The absolute value of is preferably 0.05 or more, more preferably 0.10 or more. k The upper limit of the absolute value of is not necessarily limited, but preferably, for example, the skewness S k The absolute value of is less than 10.00, and more preferably less than 5.00. In addition, from the viewpoint of better combining high magnetic permeability and good DC superposition characteristics, the skewness S is preferably k Displays negative values (e.g., above -10.00 and below -0.01).
[0068] An example of a method for manufacturing the magnetic core 2 according to the present embodiment will be described below.
[0069] First, prepare a soft magnetic powder 1. There is no particular limitation on the method for producing the soft magnetic powder 1, as long as an appropriate production method is used according to the desired particle composition. For example, the soft magnetic powder can be produced by an atomization method such as a water atomization method or a gas atomization method. Alternatively, the soft magnetic powder can be produced by a CVD method using at least one of evaporation, reduction, and thermal decomposition of a metal salt. In addition, a soft magnetic metal strip can be prepared by a single-roll method, etc., and the soft magnetic metal strip can be crushed to produce the soft magnetic powder. In addition, the soft magnetic powder can also be produced by an electrolytic method or a carbonyl method.
[0070] When manufacturing the soft magnetic powder of amorphous structure or nanocrystalline structure, in the above-mentioned powder manufacturing method, preferably adopt gas atomization method or single roller method. In addition, the soft magnetic powder of nanocrystalline structure can also be manufactured by implementing the heat treatment for controlling the crystal structure of the soft magnetic powder of amorphous structure made by gas atomization method or single roller method.
[0071] When manufacturing a soft magnetic powder 1 containing two or more particle groups, raw material powders of each particle group are prepared. For example, in the case of manufacturing a soft magnetic powder 1 containing large particles 10a and small particles 10b, a large particle size powder composed of large particles 10a and a small particle size powder composed of small particles 10b can be manufactured respectively, and the large particle size powder and the small particle size powder can be mixed in a desired ratio. In addition, when manufacturing a soft magnetic powder 1 containing large particles 10a, medium particles 10c and small particles 10b, large particle size powder, small particle size powder and medium particle size powder composed of medium particles 10c can also be prepared, and these powders can be mixed in a desired ratio. The ratio of large particle size powder, medium particle size powder and small particle size powder is not particularly limited. For example, relative to 100wt% of the soft magnetic powder, the ratio of large particle size powder is preferably 50wt% or more and 90wt% or less, and more preferably 60wt% or more and 80wt% or less. In addition, the ratio of medium particle size powder and the ratio of small particle size powder are preferably 5wt% or more and 30wt% or less, respectively.
[0072] In the case where an insulating film is formed on the surface of the particles in the soft magnetic powder 1, the soft magnetic powder 1 can be subjected to a coating forming treatment. The method of the coating forming treatment is not particularly limited, and an appropriate coating forming treatment can be selected according to the type of insulating film to be formed. As the coating forming treatment, heat treatment, phosphate treatment, surface treatment by a mechanochemical method, mechanical alloying technology, silane coupling treatment or hydrothermal synthesis can be exemplified. It should be noted that in the case of mixing two or more powders such as large particle size powder, medium particle size powder and small particle size powder to manufacture the soft magnetic powder 1, the coating forming treatment can be performed on the mixed soft magnetic powder 1, or the coating forming treatment can be performed on each powder before mixing.
[0073] Next, the soft magnetic powder 1 is used to manufacture particles as the raw material of the magnetic core 2. First, a resin raw material such as a thermosetting resin and a curing agent is added to an organic solvent such as acetone or ethanol to prepare a resin solution. Then, the soft magnetic powder 1 is added to the resin solution and kneaded. At this time, in the kneading of the soft magnetic powder 1 and the resin solution, various kneading machines such as a kneader, a planetary mixer, a rotation-revolution mixer or a twin-screw extruder can be used, and a modifier, a preservative, a dispersant, a non-magnetic powder, etc. can be added to the kneaded material. After kneading, the particles are obtained by volatilizing the organic solvent.
[0074] The mixing ratio of the soft magnetic powder 1 and the resin raw material in the above-mentioned kneading process is not particularly limited, but for example, the soft magnetic powder 1 and the resin raw material are preferably weighed in such a manner that the content of the resin 3 after curing becomes 1 part by weight or more and 5 parts by weight or less relative to 100 parts by weight of the soft magnetic powder. In addition, when two or more raw material powders such as large particle size powder, medium particle size powder and small particle size powder are used, these raw material powders may be mixed in advance and the resulting mixed powder may be added to the resin solution, or the raw material powders may be added to the resin solution without being mixed, and the raw material powders may be mixed in the kneading process.
[0075] The size and shape of the particles are not particularly limited, but preferably, for example, the particles have a particle shape of 0.02 mm to 0.5 mm, and the average particle size of the particles is 0.05 mm to 0.2 mm. In order to control the size of the particles within the above range, it is preferred to perform sieving and grading after the kneading process. The conditions for sieving and grading are not particularly limited. For example, by using a plurality of sieves with an aperture of 20 μm to 500 μm to grade the particles after the kneading process, the particle size distribution of the particles can be controlled within the range of 0.02 mm to 0.50 mm, and the peak of the particle size distribution can be increased. In this embodiment, the particles after sieving and grading are referred to as primary particles.
[0076] If only primary particles are used as raw materials to manufacture magnetic cores, the area ratio distribution of the soft magnetic powder in the magnetic core follows a normal distribution, and the skewness S of the area ratio distribution is k Approximately 0 (specifically -0.01<S k The skewness of the area ratio distribution of the soft magnetic powder 1 can be determined by the specific gravity of the particles (unit: g / cm 3 ) distribution. The specific gravity of each particle is related to the content of soft magnetic powder in each particle. The content of soft magnetic powder in particles with a large specific gravity is high, and the content of soft magnetic powder in particles with a small specific gravity is low. For example, when particles with a larger specific gravity are removed from raw material particles, thereby increasing the proportion of particles with a smaller specific gravity, the skewness of the area ratio distribution can be controlled below -0.01; on the other hand, when particles with a smaller specific gravity are removed from raw material particles, thereby increasing the proportion of particles with a larger specific gravity, the skewness of the area ratio distribution can be controlled above 0.01. Therefore, in this embodiment, in order to control the skewness of the area ratio distribution to a desired value, secondary particles that have been further subjected to air flow classification after screening and classification are prepared.
[0077] The manufacturing conditions of the secondary particles are not necessarily limited. For example, the particles can be classified by using a fine sieve with a mesh size of 20 μm to 100 μm to screen out small particles. Then, the sieved particles are further subjected to air flow classification to remove particles with a large specific gravity and screen out secondary particles with a small specific gravity. By using such secondary particles with a small specific gravity, the skewness S can be reduced. k On the other hand, in order to control the skewness S k Controlled above 0.01, secondary particles with a larger specific gravity can also be screened out. For example, a coarse sieve with a mesh size of 200 μm to 500 μm is used to classify the particles. Then, the screened and classified particles are further subjected to airflow classification to screen out secondary particles with a larger specific gravity.
[0078] Skewness S of the area ratio distribution k It can be controlled by the conditions of sieving and airflow classification. In addition, it is preferred to mix the secondary particles after the above classification process with the primary particles that have not been subjected to airflow classification. According to the mixing ratio of the primary particles and the secondary particles, the skewness S can be controlled with higher accuracy. k .
[0079] Next, the secondary particles or the mixed particles of the primary particles and the secondary particles are filled into a mold and compression molded to produce a powder compact. The molding pressure at this time is not particularly limited and can be set to, for example, 9.8 MPa or more. 3 MPa or less (0.1t / cm 2 Above 12t / cm 2 The average area ratio x of the soft magnetic powder 1 in the magnetic core 2 is A (i.e., average filling rate) can be controlled by the content of resin 3 (mixing ratio of resin raw materials) or by the molding pressure. When a thermosetting resin is used as resin 3, the molded powder body is heated at 100°C to 200°C for 1 to 5 hours to cure the thermosetting resin. Through the above process, a film having Figure 1 A cross section of the magnetic core 2 is shown.
[0080] The magnetic core 2 of this embodiment can be applied to various magnetic components such as inductors, transformers, and choke coils. For example, Figure 5 The magnetic component 100 shown is an example of a magnetic component having a magnetic core 2 .
[0081] The magnetic component 100 has a body composed of a magnetic core 2 and a coil 5, and the coil 5 is buried inside the magnetic core 2. The coil 5 has a structure in which a conductor is wound in a spiral shape, and the number of turns and the winding method of the conductor are not particularly limited. The shape and size of the conductor constituting the coil 5 are not particularly limited, and the surface of the conductor is preferably covered with an insulating film. It should be noted that the coil 5 is not limited to Figure 5 In the structure shown, the magnetic component 100 may also include a flexible substrate printed with a coil pattern as the coil.
[0082] Ends 5a and 5b of the conductor constituting the coil 5 are led out to the end surface of the core 2. A pair of external electrodes 6 and 8 are formed on the end surface of the core 2 and are electrically connected to the ends 5a and 5b of the coil 5, respectively.
[0083] in, Figure 5 1 shows a cross section of the magnetic component 100 along the coil axis. The coil axis refers to a central axis that passes through the center of the area surrounded by the inner circumference of the coil 5. It should be noted that Figure 5 The X-axis, Y-axis, and Z-axis shown are perpendicular to each other, and the Z-axis is roughly parallel to the coil axis. In the magnetic core 2 of the magnetic component 100, the main surface located above the Z-axis of the two main surfaces perpendicular to the coil axis is called "upper surface 2s1", and the main surface located below the Z-axis is called "lower surface 2s2". In addition, the height of the magnetic core 2 in the Z-axis direction is set to T.
[0084] When determining the area ratio distribution of the soft magnetic powder 1 in the cross section of the magnetic component 100, there is no particular limitation on the position of acquiring the cross-sectional image, that is, the position of the region where the area ratio is analyzed using the equally spaced grid G. For example, it is preferably as follows Figure 5 As shown, the cross section of the magnetic core 2 after cutting along the coil axis is analyzed. In addition, it is preferred that Figure 5 As shown, the cross section of the magnetic core 2 along the coil axis is divided into a central portion 2α and an outer portion 2β, and the area ratio of the soft magnetic powder 1 is measured.
[0085] Specifically, Figure 5The cross section shown is divided into three equal parts along the coil axis and is divided into three regions. The central region of the three regions is called the "central portion 2α", and the region outside the central portion 2α is called the "outer portion 2β". "Divided into three equal parts along the coil axis" means that an imaginary line perpendicular to the coil axis as represented by a single-dot chain line is drawn at a position 1 / 3T deep from the upper surface 2s1 of the magnetic core 2 and at a position 1 / 3T deep from the lower surface 2s2 to divide the cross section of the magnetic core 2. The analysis region of the area ratio preferably includes at least a portion of the central portion 2α. In addition, it is more preferable to set an analysis region formed by an equally spaced grid G in both the central portion 2α and the outer portion 2β, and combine the analysis results in the central portion 2α with the analysis results in the outer portion 2β to determine the area ratio distribution and the average area ratio x. A and skewness S k .
[0086] When the area ratio distribution of the soft magnetic powder 1 is determined separately in the central portion 2α and the outer portion 2β, it is preferred that at least one of the area ratio distribution in the central portion 2α and the area ratio distribution in the outer portion 2β satisfies |0.01|≤S k More preferably, the area ratio distribution in the central portion 2α satisfies |0.01|≤S k It is further preferred that both the area ratio distribution in the central portion 2α and the area ratio distribution in the outer portion 2β satisfy |0.01|≤S k The skewness S in the central portion 2α and the outer portion 2β k The values of may be consistent or inconsistent. In addition, the average area ratio x in the central portion 2α and the outer portion 2β is A The (average fill rate) values may or may not be consistent.
[0087] It should be noted that in the analysis of the area ratio distribution, the cross section of the core 2 can also be divided into a middle core region surrounded by the inner circumference of the coil 5 and an outer region that is a region outside the middle core region. In this case, it is also preferred to set an analysis region formed by equally spaced grids G in both the middle core region and the outer region, and combine the analysis results of the middle core region with the analysis results of the outer region to determine the area ratio distribution and the average area ratio x. A and skewness S k In addition, when the area ratio distribution of the soft magnetic powder 1 is determined in the middle core region and the outer region, it is preferred that at least one of the area ratio distribution in the middle core region and the area ratio distribution in the outer region satisfies |0.01|≤S k , more preferably the area ratio distribution in the middle core region satisfies |0.01|≤S kIt is further preferred that both the area ratio distribution in the middle core region and the area ratio distribution in the outer region satisfy |0.01|≤S k The skewness S in the middle core region and the outer region k The values of may be consistent or inconsistent. In addition, the average area ratio x between the middle core region and the outer region is A The (average fill rate) values may or may not be consistent.
[0088] When determining the area ratio distribution of the soft magnetic powder 1 in the cross section of the magnetic core 2 in which the coil 5 is buried as in the magnetic component 100 , the square region 20 reflected by the coil 5 is not within the analysis target.
[0089] Figure 5 The use of the magnetic component 100 shown is not particularly limited. For example, the magnetic component 100 can be suitably used as a power inductor used in a power supply circuit. Figure 5 For example, a magnetic component may be formed by winding a conductive wire on the surface of a magnetic core 2 having a predetermined shape.
[0090] (Summary of Implementation Methods)
[0091] In the magnetic core 2 of the present embodiment, the average area ratio x of the soft magnetic powder 1 in the cross section of the magnetic core 2 is A The skewness S of the area ratio distribution of the soft magnetic powder 1 is 75% or more and 90% or less. k The absolute value is above 0.01.
[0092] The magnetic core 2 has the above-mentioned characteristics, and thus can improve the DC superposition characteristics compared with the conventional magnetic core. k Set to below -0.01, so that the area ratio distribution follows the normal distribution of the core (satisfying -0.01<S k Compared with the core with skewness S<0.01), the DC superposition rated current can be increased, and excellent DC superposition characteristics can be obtained. k By setting the ratio to 0.01 or more, a higher magnetic permeability can be obtained than in a core whose area ratio distribution follows a normal distribution, and the filling factor required to achieve the desired magnetic permeability can be reduced. As a result, the DC superposition characteristics can be improved compared to the conventional ones.
[0093] Although the embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and various modifications can be made within the scope not departing from the gist of the present invention.
[0094] For example, a plurality of magnetic cores 2 may be combined to manufacture a magnetic component. In addition, the manufacturing method of the magnetic core 2 is not limited to the manufacturing method shown in the above embodiment, and the magnetic core 2 may also be manufactured by two-step compression. For example, in the two-step compression manufacturing method, the magnetic core 2 may be obtained by pre-compressing secondary particles or mixed particles to form a plurality of preformed molded bodies, and then combining these preformed molded bodies and performing formal compression.
[0095] Example
[0096] The present disclosure will be described below based on more specific embodiments, but the present disclosure is not limited to these embodiments.
[0097] (Experiment 1)
[0098] Sample A6 to Sample A15
[0099] Magnetic cores of Samples A6 to A15 shown in Table 1 were manufactured according to the following operation procedures.
[0100] First, large particles and small particles were prepared as raw material powders of soft magnetic powder. Specifically, large particles with an amorphous structure were prepared by a quenching gas atomization method. The average composition of the large particles was 57.5 at% Fe, 24.6 at% Co, 11 at% B, 3 at% P, 3 at% Si, and 1 at% Cr, and the average particle size of the large particles was 25 μm. In addition, an insulating film having a composition of P-Zn-Na-Al-O was formed by subjecting the large particles to a coating formation treatment using a mechanochemical method. The average thickness of the insulating film was 20 nm. On the other hand, as small particles, Fe powder with a crystalline structure having an average particle size of 1 μm was prepared.
[0101] Next, epoxy resin and imide resin as a curing agent were prepared as resin raw materials, and these resin raw materials were added to acetone to obtain a resin solution. Then, the resin solution, large particles and small particles were kneaded, and the resulting kneaded product was dried under specified conditions to volatilize the acetone, thereby obtaining particles. In this kneading process, the proportion of large particles was set to 80wt%, and the proportion of small particles was set to 20wt% relative to the total of 100wt% of large particles and small particles. In addition, the soft magnetic powder (large particles and small particles) and the resin raw materials were weighed so that the content of the resin component after curing became 2.5 weight parts relative to 100 weight parts of the soft magnetic powder.
[0102] Next, the particles after the kneading process were classified using a sieve with a mesh size of 20 μm to 500 μm to obtain primary particles. In addition, in samples A6 to A10, the particles after the kneading process were classified using a sieve with a mesh size of 20 μm to 100 μm. Then, the sieved and classified particles were further subjected to airflow classification to screen out secondary particles with a smaller specific gravity. In samples A6 to A10, the primary particles that were not subjected to airflow classification and the secondary particles after airflow classification were separated so that the skewness S of the area ratio distribution was 1 / 2. k The mixture was mixed at a ratio of -0.50 to obtain mixed particles.
[0103] On the other hand, in samples A11 to A15, the particles after the kneading process were classified using a sieve with a mesh size of 200 μm to 500 μm. Then, the sieved and classified particles were further subjected to airflow classification to screen out secondary particles with a larger specific gravity. In samples A11 to A15, the primary particles that were not subjected to airflow classification and the secondary particles after airflow classification were separated so that the skewness S of the area ratio distribution was 1:1. k The mixture was mixed at a ratio of 0.50 to obtain mixed particles.
[0104] Next, the mixed particles were filled into a mold and pressurized to obtain a ring-shaped powder compact. The molding pressure at this time was set to 9.8 MPa or more. 3 MPa or less, and the average area ratio x of the soft magnetic powder in each sample was set by using the molding pressure. A The average filling rate was controlled to the value shown in Table 1. The powder compact was then heated at 180°C for 60 minutes to cure the epoxy resin in the powder compact, thereby obtaining a toroidal (outer diameter 11 mm, inner diameter 6.5 mm, thickness 2.5 mm) magnetic core.
[0105] Sample A1 to Sample A5
[0106] In samples A1 to A5, the same soft magnetic powder and resin raw materials as samples A6 to A15 were used, and primary particles were manufactured under the same conditions as samples A6 to A15. However, in samples A1 to A5, only primary particles that have not been subjected to air flow classification were used to manufacture the magnetic core instead of mixed particles. That is, in samples A1 to A5, only primary particles were filled into the mold, and after obtaining the powder compact, the epoxy resin in the powder compact was cured to obtain a ring-shaped (outer diameter 11mm, inner diameter 6.5mm, thickness 2.5mm) magnetic core. Samples A1 to A5 set the molding pressure to 9.8MPa or more like samples A6 to A15.1.2×10 3 MPa or less, using this molding pressure, the average area ratio x A(Average filling rate) is controlled to the value shown in Table 1.
[0107] In each sample of Experiment 1, the produced magnetic core was evaluated as follows.
[0108] Cross-sectional analysis of magnetic core
[0109] The random cross-section of the magnetic core was observed using SEM, and the area ratio distribution of the soft magnetic powder was analyzed using image analysis software (Nano System Co., Ltd., Nano Hunter NS2K-Pro). Specifically, the equivalent circle diameter of each metal particle contained in the random cross-section of the magnetic core was measured first, and the maximum particle size D of the soft magnetic powder was determined. MAX Next, use the grid width as the maximum particle size D MAX The arbitrary cross section of the core is divided into 100 square regions by using a grid of equal spacing twice the size of the grid. Then, the measured area is calculated as (2D MAX ) 2 The total area of the metal particles contained in each square area is calculated to calculate the area ratio x of the soft magnetic powder in each square area. i Based on the measurement results, the average area ratio x of the soft magnetic powder in the magnetic core was calculated. A and the skewness S of the area ratio distribution k .
[0110] In the magnetic cores of Samples A1 to A5 using primary particles, the area ratio distribution of the soft magnetic powder follows a normal distribution, and the skewness S of the area ratio distribution is k On the other hand, in the magnetic cores of Samples A6 to A10 using mixed particles of primary particles and secondary particles with a smaller specific gravity, the skewness S of the area ratio distribution of the soft magnetic powder is k In addition, in the magnetic cores of samples A11 to A15 using mixed particles of primary particles and secondary particles with a larger specific gravity, the skewness S of the area ratio distribution of the soft magnetic powder is k is 0.50.
[0111] Core performance evaluation
[0112] Copper wire (UEW wire) with polyurethane insulation coating was wound on the toroidal core. Then, the core inductance L0 at 1 MHz was measured using an LCR meter (4284A manufactured by Agilent Technologies Inc.), and the initial magnetic permeability μi (dimensionless) of the core was calculated based on the inductance L0. In Experiment 1, an initial magnetic permeability μi of 20 or more was judged as good.
[0113] In addition, a DC current was applied to the core wound with the UEW wire at a constant rate of increase from 0 A, and the change in inductance at this time was measured and calculated. Then, the value of the DC current when the inductance L when the DC current was applied decreased by 10% relative to the inductance L0 at 0 A (i.e., the DC current value when L / L0=90%) was determined as the DC superposition rated current Isat (unit: A).
[0114] Table 1 shows the evaluation results of each sample in Experiment 1.
[0115]
Table 1
[0116]
[0117] As shown in Table 1, the average area ratio x of the soft magnetic powder A For samples with a value of 75% or more (samples A2 to A5, samples A7 to A10, samples A12 to A15), μi is 20 or more, which ensures high magnetic permeability. A The trend of decreasing with the increase of skewness S k The embodiment (samples A7 to A10) with a skewness S of -0.50 k In the embodiments (samples A12 to A15) with a value of 0.50, not only a high magnetic permeability is ensured, but also a specific skewness S k The comparative examples (samples A2 to A5) with a value of 0.00 have better DC superposition characteristics. Figure 6A to Figure 6B The effect of improving the DC superposition characteristics will be described in detail.
[0118] Fig. 6A is the average area ratio x of the soft magnetic powder in the magnetic core A A graph showing the relationship between (average fill rate) and Isat. Fig. 6A The horizontal axis is the average area ratio x A , the vertical axis is Isat, and a curve chart of the evaluation results of samples A1 to A15 shown in Table 1 is drawn. Fig. 6A As shown, in the skewness S k In the example with a value of -0.50, Isat higher than that of the comparative example was obtained, and the DC superposition characteristic was improved.
[0119] on the other hand, Figure 6B is the average area ratio x of the soft magnetic powder in the magnetic core A (average filling rate) versus μi. Figure 6B The horizontal axis is the average area ratio x AThe vertical axis is μi, and a graph of the evaluation results of samples A1 to A15 shown in Table 1 is plotted. A In the range of 75% to 90%, the skewness S k The μi in the example of 0.50 is improved compared with the comparative example.
[0120] In designing a magnetic core used in a magnetic component, the magnetic permeability for obtaining the desired inductance is first determined, and the average filling rate of the soft magnetic powder required to achieve the magnetic permeability is set. The DC superposition characteristic is the performance exhibited as a result of the set average filling rate. k In the embodiment where the skewness S is 0.50, a higher magnetic permeability than the comparative example can be obtained, so the average filling rate required to obtain the desired magnetic permeability can be reduced. k In the comparative example where μi=30, the average filling rate of the soft magnetic powder needs to be set at about 85%, but the skewness S k In the embodiment where μi=0.50, μi=30 can be achieved with an average filling rate of about 76%. In this way, since the average filling rate can be reduced, the skewness S k In the example where the value is 0.50, the DC superposition characteristics at a predetermined magnetic permeability can be further improved compared to the comparative example.
[0121] Figure 6C As a graph showing the relationship between μi and Isat, a graph showing the evaluation results of each sample shown in Table 1 is plotted. Figure 6C It can be seen that: in the skewness S k In the comparative example with skewness S = 0.00, Isat is about 9.4A when μi = 30. k In the embodiment where μi=0.50, Isat is about 10.7A when μi=30, which can improve the DC superposition characteristics compared with the comparative example. Figure 6C The closer the curve is to the upper right corner of the graph, the better the magnetic properties are. Figure 6C From the curve graph shown, we can see that the skewness S k Example of -0.50 and skewness S k The embodiment with a value of 0.50 can have both high magnetic permeability and excellent DC superposition characteristics.
[0122] (Experiment 2)
[0123] In Experiment 2, in order to study in more detail the effect of skewness S k In order to improve the DC superposition characteristics, the magnetic cores shown in Tables 2 and 3 were manufactured. It should be noted that in Experiment 2, as shown in Tables 2 and 3, for each specified skewness S k, four magnetic cores with different average area ratios were prepared.
[0124] Sample B1 to Sample B28
[0125] Specifically, in Samples B1 to B28 shown in Table 2, the same soft magnetic powder and resin raw materials as those in Experiment 1 were used to produce primary particles under the same conditions as those in Experiment 1. In addition, the particles after the kneading process were classified using a sieve with a mesh size of 20 μm to 100 μm, and the sieved and classified particles were further subjected to air flow classification, thereby screening out secondary particles with a smaller specific gravity.
[0126] In all samples B1 to B24 shown in Table 2, the toroidal cores were made of mixed particles obtained by mixing primary particles and secondary particles with a smaller specific gravity. In this process, the mixing ratio of the primary particles and the secondary particles was set so that the skewness S in the area ratio distribution of the soft magnetic powder was 0.0447 W / cm2. k The values are shown in Table 2. In Samples B25 to B28 shown in Table 2, the toroidal cores were manufactured using only the secondary particles having a small specific gravity.
[0127] As described above, in samples B1 to B28, although the mixing ratio of primary particles to secondary particles is set to a ratio different from that of samples A6 to A10 in Experiment 1, other conditions such as the specifications of large particles and small particles, the ratio of large particles to small particles, the ratio of soft magnetic powder to resin, and the size of the annular magnetic core are the same as those in Experiment 1. It should be noted that, in samples B1 to B28, the average area ratio x is set by the molding pressure when manufacturing the magnetic core, as in Experiment 1. A (Average filling rate) was controlled to the value shown in Table 2.
[0128] Sample C1 to Sample C28
[0129] In samples C1 to C28 shown in Table 3, the same soft magnetic powder and resin raw materials as those in Experiment 1 were used to produce primary particles under the same conditions as those in Experiment 1. In addition, the particles after the kneading process were classified using a sieve with a mesh size of 200 μm to 500 μm, and the sieved and classified particles were further subjected to air flow classification to screen out secondary particles with a larger specific gravity.
[0130] In all samples C1 to C24, the toroidal core was manufactured using mixed particles obtained by mixing primary particles and secondary particles with a larger specific gravity. In this process, the mixing ratio of the primary particles and the secondary particles was set so that the skewness S in the area ratio distribution of the soft magnetic powder was k The values are shown in Table 3. In Samples C25 to C28 shown in Table 3, the toroidal cores were manufactured using only the secondary particles having a large specific gravity.
[0131] As described above, in samples C1 to C28, although the mixing ratio of primary particles to secondary particles was set to a different ratio from that of samples A11 to A15 of experiment 1, other conditions such as the specifications of large particles and small particles, the ratio of large particles to small particles, the ratio of soft magnetic powder to resin, and the size of the annular magnetic core were the same as those of experiment 1. It should be noted that, in samples C1 to C28, the average area ratio x was set by the molding pressure during the manufacture of the magnetic core, as in experiment 1. A (Average filling rate) is controlled to the value shown in Table 3.
[0132] For each sample in Experiment 2, the average area ratio x was measured in the same manner as in Experiment 1. A , skewness S k , μi and Isat. The evaluation results of each sample are shown in Tables 2 and 3. Table 2 shows the skewness S k The evaluation results of the embodiments after setting the skewness S to -0.01 or less are shown in Table 3. k The evaluation results of the examples after setting the value to 0.01 or more. Figure 7 To show the relationship between μi and Isat, some of the evaluation results shown in Table 2 (skewness S k =0.00, -0.01, -0.05, -0.10, -0.50). Figure 8 To show the relationship between μi and Isat, some evaluation results (skewness S k =0.00, 0.01, 0.05, 0.10, 0.50).
[0133] In addition, in Experiment 2, according to the skewness S k The evaluation results of the four samples under the above conditions are used to calculate the skewness S of each sample. k Specifically, the skewness S is set to 30. k The evaluation results of the following four samples are shown in Figure 7 and Figure 8 The curves are drawn in the graph showing the relationship between μi and Isat shown in FIG. 1 and the fitting straight line based on the four curves is obtained by the least square method. Then, the Isat when μi is set to 30 is calculated using the fitting straight line. Tables 2 and 3 show the slope (unit: A) and intercept (unit: A) of the fitting straight line, and Isat (unit: A) when μi=30.
[0134] Fig. 9 is the absolute value of the skewness (|S k |) and Isat when μi=30. Fig. 9The horizontal axis is the logarithmic axis representing the absolute value of the skewness, and the vertical axis is the axis representing Isat when μi=30. The embodiment shown in Table 2 (i.e., S k The evaluation results of the embodiments shown in Table 3 (i.e., 0.01≤S k The evaluation results of the embodiment of the present invention are shown by hollow marks and dotted lines. Fig. 9 The double-dotted line shows the skewness S k The Isat curve is when μi is set to 30 and is not correlated with the horizontal axis of the graph.
[0135] In addition, when μi is set to 30, the skewness S k The skewness S of each k The improvement rate of Isat under skewness S (unit: %). k When the value is 0.00 and μi is set to 30, Isat is “I STD ”, with each skewness S k When μi is set to 30, Isat is Skew ”, thus based on the calculation formula “I Skew / I STD (%)" calculated the skewness S k The improvement rate of Isat is judged to be good when it is 105% or more, and particularly good when it is 110% or more.
[0136] [Table 2]
[0137]
[0138] [Table 3]
[0139]
[0140] From the evaluation results shown in Table 2, it can be seen that the skewness S of the area ratio distribution of the soft magnetic powder in the magnetic core is k By setting it to -0.01 or less, the DC superposition characteristics can be improved. Figure 7 The curve diagram shows that: by k By setting the skewness S to less than -0.01, the curve showing the relationship between μi and Isat tends to move to the upper right of the graph compared with the curve of the comparative example. k By setting it to -0.01 or less, it is possible to improve the DC superposition characteristics while ensuring high magnetic permeability.
[0141] In addition, according to Fig. 9The curves shown by the black mark and solid line in the figure can prove that: when -0.50≤S k ≤-0.01, as S k The decrease of Isat has a tendency to further increase; at -10.00≤S k In the range of ≤-0.50, Isat tends to remain at a high level. Figure 7 and Fig. 9 The results show that when S k When ≤-0.01, skewness S k It is preferably -0.05 or less, more preferably -0.10 or less, and further preferably -0.50 or less. k When ≤-0.01, the skewness S k The lower limit of is not particularly limited, but may be, for example, -10.00.
[0142] From the evaluation results shown in Table 3, it can be seen that the skewness S of the area ratio distribution of the soft magnetic powder in the magnetic core is k is set to 0.01 or more, thereby increasing the magnetic permeability. Figure 8 In the curve diagram, it can be confirmed that by k By setting the skewness S to 0.01 or more, the curve showing the relationship between μi and Isat tends to move to the upper right of the graph compared with the curve of the comparative example. k By setting it to 0.01 or more, the DC superposition characteristics can be improved while maintaining high magnetic permeability.
[0143] In addition, according to Fig. 9 The hollow mark and the dotted curve in the figure can confirm that: when 0.01≤S k ≤1.00, there is a k The trend of Isat further increasing is that when 1.00≤S k In the range of ≤10.00, high Isat can also be obtained. Figure 8 and Fig. 9 The results show that when 0.01≤S k When the skewness S k It is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.50 or more. k In the case of k The upper limit of is not particularly limited but may be, for example, 10.00.
[0144] As described above, the evaluation results of Experiment 2 confirm that, in a magnetic core in which the average area ratio of the soft magnetic powder is set to 75% or more and 90% or less, the skewness S kThe absolute value of is controlled above 0.01, thereby ensuring high magnetic permeability while improving the DC superposition characteristics.
[0145] (Experiment 3)
[0146] In Experiment 3, the conditions related to the insulating coating of large particles were changed, and 15 types of magnetic cores shown in Table 4 were manufactured. Specifically, in Samples D1 to D3, large particles without insulating coating were used; in Samples D4 to D9, the average thickness of the insulating coating in the large particles was changed; in Samples D10 to D15, the composition of the insulating coating in the large particles was changed. Other specifications related to the soft magnetic powder (composition of large particles, average particle size of large particles, specifications of small particles, ratio of large particles to small particles, etc.) were the same as those in Experiment 1, and magnetic cores were manufactured under the same conditions as in Experiment 1.
[0147] In Experiment 3, according to the relevant conditions of the insulation coating of large particles, the skewness S k Comparative example with skewness S of 0.00 k For the embodiment of -0.50, the skewness S k In each comparative example, only one particle was used to reduce the skewness S k is controlled at 0.00, and the skewness S in each embodiment k The mixing ratio of primary particles and secondary particles was controlled in the same manner as in Experiment 1. In Experiment 3, the molding pressure in each sample was set so that the corresponding comparative example and the embodiment would show the same degree of magnetic permeability, and the Isat improvement rate in each embodiment was calculated based on the Isat in the comparative example.
[0148] Table 4 shows the evaluation results of Experiment 3.
[0149] [Table 4]
[0150]
[0151] The evaluation results of samples D1 to D3 show that, regardless of whether or not there is an insulating film, the skewness S k Furthermore, the evaluation results of samples D4 to D15 show that even when the composition or thickness of the insulating film is changed, the DC superposition characteristics can be improved based on the skewness S k Improvement of DC superposition characteristics is achieved.
[0152] (Experiment 4)
[0153] Sample E1 to Sample E15
[0154] In samples E1 to E15, magnetic cores were manufactured by mixing large particles and small particles in the ratio shown in Table 5. The specifications (particle composition, average particle size, coating composition, and average coating thickness) of the large particles and small particles used in samples E1 to E15 were the same as those in Experiment 1, and the manufacturing conditions other than the ratio of large particles to small particles were the same as those in Experiment 1.
[0155] Sample F1 to Sample F12
[0156] In samples F1 to F12, the small particles were changed to the composition shown in Table 6 to produce magnetic cores. The average particle size of the small particles in samples F1 to F12 was 1 μm. In addition, in samples F1 to F12, the ratio of large particles was set to 80 wt %, and the ratio of small particles was set to 20 wt %. The experimental conditions other than the above were the same as those in Experiment 1.
[0157] In Experiment 4, according to the changed manufacturing conditions (ratio of large particles to small particles (Table 5), composition of small particles (Table 6)), the skewness S k Comparative example with skewness S of 0.00 k The embodiment of -0.50 and the skewness S k In Experiment 4, the molding pressure in each sample was set so that the corresponding comparative example and the embodiment showed the same degree of magnetic permeability, and the Isat improvement rate in each embodiment was calculated based on the Isat in the comparative example.
[0158] [Table 5]
[0159]
[0160] [Table 6]
[0161]
[0162] The evaluation results shown in Table 5 show that even when the ratio of large particles to small particles is changed, the skewness S k It is also possible to improve the DC superposition characteristics. It is also known that from the viewpoint of improving the magnetic permeability, it is preferable to set the ratio of large particles to 60 wt % or more.
[0163] The evaluation results shown in Table 6 show that even when the small particle composition is changed, the skewness S k It is also possible to improve the DC superposition characteristics.
[0164] (Experiment 5)
[0165] In Experiment 5, 15 types of magnetic cores were manufactured using soft magnetic powder containing large particles, medium particles and small particles. The specifications of the large particles and small particles used in each sample of Experiment 5 (particle composition, average particle size, coating composition and average coating thickness) are the same as those in Experiment 1. When manufacturing the primary particles, medium particles having the composition shown in Table 7 are added while adding large particles and small particles. The average particle size of the medium particles used in samples G1 to G15 is 5μm. In addition, the ratio of large particles in samples G1 to G15 is set to 80wt%, the ratio of medium particles is set to 10wt%, and the ratio of small particles is set to 10wt%. The experimental conditions other than the above are the same as those in Experiment 1.
[0166] In Experiment 5, different skewness values S and k Comparative example with skewness S of 0.00 k Example of -0.50 and skewness S k In Experiment 5, the molding pressure of each sample was set so that the corresponding comparative example and the embodiment showed the same degree of magnetic permeability, and the Isat improvement rate of each embodiment was calculated based on the Isat in the comparative example.
[0167] [Table 7]
[0168]
[0169] From the evaluation results shown in Table 7, it can be seen that even when the soft magnetic powder consists of three types of particle groups, the skewness S k It is also possible to improve the DC superposition characteristics.
[0170] (Experiment 6)
[0171] In Experiment 6, the composition of the large particles was changed to produce the magnetic cores shown in Tables 8 to 10. In Samples H1 to H9 in Table 8, large particles with an amorphous structure were used; in Samples I1 to I9 in Table 9, large particles with a nanocrystalline structure were used; and in Samples J1 to J12 in Table 10, large particles with a crystalline structure were used. The average particle size of the large particles used in each example in Experiment 6 was 25 μm, and an insulating coating with an average thickness of 20 nm and the same composition as in Experiment 1 was formed on the large particles in each sample.
[0172] In Experiment 6, the skewness S was produced according to the composition of the large particles. k Comparative example with skewness S of 0.00 k Example of -0.50 and skewness S kIn Experiment 6, the molding pressure in each sample was set so that the corresponding comparative example and the embodiment showed the same degree of magnetic permeability, and the improvement rate of Isat in each embodiment was calculated based on the Isat in the comparative example.
[0173] [Table 8]
[0174]
[0175] [Table 9]
[0176]
[0177] [Table 10]
[0178]
[0179] From the evaluation results shown in Tables 8 to 10 of Experiment 6, it can be seen that regardless of the composition of the large particles, the skewness S k Both can improve the DC superposition characteristics.
Claims
1. A magnetic core, wherein: The magnetic core comprises soft magnetic powder, The average area ratio of the soft magnetic powder in any cross section of the magnetic core is 75% or more and 90% or less, The skewness of the area ratio distribution of the soft magnetic powder in the cross section is greater than or equal to 0.01 in absolute value, wherein the skewness of the area ratio distribution is obtained by setting the maximum particle size of the soft magnetic powder in the cross section to D MAX When the cross section is divided into equal-spaced grids, the area demarcated is (2D MAX ) 2 The area ratio of the soft magnetic powder is calculated in each square area.
2. The magnetic core according to claim 1, wherein: The skewness of the area ratio distribution is greater than or equal to 0.05 in absolute value.
3. A magnetic component, wherein: A magnetic core and a coil as claimed in claim 1 or 2.