Positive electrode active material, preparation method thereof, positive electrode plate comprising positive electrode active material, battery and electric device

By graded doping M1 and M2 elements in the ternary positive electrode material particles to form a core-shell structure, the problem of structural changes in the high-nickel ternary positive electrode material during the charge and discharge cycle is solved, and the energy density and circulation performance of the battery are improved. .

CN119069656AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202310630845.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The existing high-nickel ternary cathode materials have cation mixed discharge during the charging and discharging cycle, resulting in structural changes, cracking and powdering, limiting the energy density, rate performance and circulation performance of the battery.

Method used

Using ternary positive electrode material particles with core-shell structure, the core part and M2 (such as Zr, Nb, Ta, W, Mo, Ti, Ir) are doped in the core part by doping elements M1 (such as Na, Mg, K, Ca) and M2 (such as Zr, Nb, Ta, W, Mo, Ti, Ir) are The hierarchical doping of the shell portion regulates the diffusion kinetics and structural stability of lithium ion, and reduces charge state differences and stress.

Benefits of technology

It significantly improves the battery's energy density, rate performance and cycle performance, and extends the battery's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069656A_ABST
    Figure CN119069656A_ABST
Patent Text Reader

Abstract

The invention provides a positive active material, a preparation method thereof, a positive pole piece containing the positive active material, a battery and an electric device. The positive electrode active material comprises ternary positive electrode material particles with a core-shell structure, the ternary positive electrode material particles comprise a doping element M1 and a doping element M2, and based on the total molar weight of transition metal elements in the ternary positive electrode material particles, the molar ratio of the Ni element in the ternary positive electrode material particles is greater than or equal to 0.6; wherein the ion radius rM1 of M1 and the lithium ion radius rLi meet the condition that rM1-rLi is less than or equal to 80pm, and M1 is distributed in the core part of the ternary positive electrode material particle; m2 comprises one or more of Zr, Nb, Ta, W, Mo, Ti and Ir, and M2 is distributed at the shell part of the ternary positive electrode material particle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a positive electrode active material and a preparation method thereof, a positive electrode sheet containing the same, a battery and an electrical device. Background Art

[0002] Secondary batteries rely on active ions to be reciprocated between the positive and negative electrodes for charging and discharging. Secondary batteries represented by lithium-ion batteries have outstanding features such as high energy density, long cycle life, no pollution, and no memory effect. Therefore, as a clean energy source, secondary batteries have gradually spread from electronic products to large-scale devices such as electric vehicles to adapt to the sustainable development strategy of the environment and energy. As a result, higher requirements are also placed on the energy density of secondary batteries. Summary of the invention

[0003] In order to achieve the above-mentioned objectives, the present application provides a positive electrode active material, which can improve the energy density, rate performance and cycle performance of the battery containing it; the present application also provides a method for preparing the positive electrode active material, a positive electrode sheet containing the positive electrode active material, a battery and an electrical device.

[0004] In a first aspect, the present invention provides a positive electrode active material, including a ternary positive electrode material particle having a core-shell structure. The ternary positive electrode material particle contains a doping element M 1 And doping element M 2 , and based on the total molar amount of transition metal elements in the ternary positive electrode material particles, the molar ratio of Ni element in the ternary positive electrode material particles is greater than or equal to 0.6; wherein, M 1 The ionic radius r M1 and the radius of lithium ions r Li Satisfy: |r M1 -r Li |≤80pm, and M 1 Distributed in the core of the ternary cathode material particles; M 2 Includes one or more of Zr, Nb, Ta, W, Mo, Ti, and Ir, and M 2 Distributed in the shell of the ternary positive electrode material particles.

[0005] It is not intended to be limited to any theory or explanation. In the embodiments of the present application, the above M 1 The ion radius of the element is close to that of the lithium ion, and can be doped into the lithium site of the high-nickel ternary cathode material particles, thereby helping to widen the interlayer spacing of the lithium layer in the crystal of the high-nickel ternary cathode material particles, improve the lithium ion diffusion kinetics in the core of the high-nickel ternary cathode material particles, and reduce the energy barrier for the migration of lithium ions in the core. 2The element is mainly doped into the transition metal site of the shell of the high-nickel ternary positive electrode material particles, thereby improving the structural stability of the surface layer of the high-nickel ternary positive electrode material particles and inhibiting the structural change of the surface layer of the high-nickel ternary positive electrode material particles during excessive lithium removal or lithium insertion. 1 Elements and M 2 The graded doping of elements reduces the difference in charge state inside the high-nickel ternary cathode material particles during the charge-discharge cycle. This can improve the structural stability of the high-nickel ternary cathode material particles, reduce the stress inside the high-nickel ternary cathode material particles, and thus improve the capacity and cycle stability of the high-nickel ternary cathode material.

[0006] Therefore, the positive electrode active material of the embodiment of the present application is applied to a secondary battery, which can effectively improve the energy density, rate performance and cycle performance of the battery.

[0007] In any embodiment of the present application, M 1 Including one or more of Na, Mg, K, Ca. M selected from the above types 1 The difference between the ion radius of the element and the lithium ion radius is small, so it can be smoothly doped into the lithium position of the high-nickel ternary cathode material particles, widening the interlayer spacing of the lithium layer in the crystal of the high-nickel ternary cathode material particles. This helps to further reduce the difference in charge state inside the high-nickel ternary cathode material particles during the charge and discharge cycle.

[0008] In any embodiment of the present application, the ternary positive electrode material particles have the general formula [Li 1+a M 1 b ][Ni x Co y Mn z M 2 c ]O2, where 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0.05≤a+b≤0.1, 0 <b≤0.05,0<c≤0.1,x+y+z+c=1。

[0009] Optionally, 0.01≤b≤0.03, 0 <c≤0.08。

[0010] The nickel-cobalt-manganese ternary material with the above general formula is applied to secondary batteries, which can significantly improve the energy density and cycle performance of the batteries.

[0011] In any embodiment of the present application, the radius R of the core portion and the thickness D of the shell portion satisfy: 0.1≤R / D≤0.9, optionally, 0.4≤R / D≤0.7. When R / D satisfies the above relationship, the unit cell parameter c of different regions inside the high-nickel ternary positive electrode material particles can be adjusted within a suitable range, thereby reducing the charge state difference and stress accumulation inside the high-nickel ternary positive electrode material particles. Thus, the rate performance and cycle performance of the battery can be further improved.

[0012] In any embodiment of the present application, the unit cell parameter c of the positive electrode active material is Optional As a result, the charge state difference and stress accumulation inside the high-nickel ternary positive electrode material particles can be reduced, thereby further improving the battery's rate performance and cycle performance.

[0013] In any embodiment of the present application, the volume distribution particle size span SPAN of the positive electrode active material is SPAN=(Dv90-Dv10) / Dv50, then SPAN≥1.1, optionally, SPAN≥1.2. Thus, the positive electrode active material can be allowed to have a higher powder compaction density, thereby increasing the volume energy density of the positive electrode active material, and further increasing the energy density of the battery.

[0014] In any embodiment of the present application, the volume distribution particle size Dv90 of the positive electrode active material is 15 μm-25 μm, and can be optionally 18 μm-22 μm.

[0015] In any embodiment of the present application, the volume distribution particle size Dv50 of the positive electrode active material is 6 μm-14 μm, and can be 8 μm-12 μm.

[0016] In any embodiment of the present application, the volume distribution particle size Dv10 of the positive electrode active material is 1 μm-5 μm, and can be 2 μm-4 μm.

[0017] As a result, the positive electrode active material can have a higher powder compaction density, thereby increasing the volume energy density of the positive electrode active material and further increasing the energy density of the battery.

[0018] In any embodiment of the present application, the powder compaction density of the positive electrode active material under 5 tons of pressure is greater than or equal to 3.5g / cc, and can be 3.5g / cc-3.7g / cc. Therefore, the positive electrode active material of the embodiment of the present application is applied to secondary batteries, which can further improve the energy density of the battery.

[0019] In a second aspect, the present invention provides a method for preparing a positive electrode active material, comprising: providing a precursor solution, the precursor solution comprising a nickel salt, a cobalt salt, a manganese salt and a 1A mixed solution of salts, wherein M 1 The ionic radius r M1 and the radius of lithium ions r Li Satisfy: |r M1 -r Li |≤80pm; preparing a seed slurry, comprising mixing a precursor solution with a first precipitant and a first complexing agent to uniformly mix the nickel salt, the cobalt salt, the manganese salt and the M-containing 1 The salt of M is coprecipitated in the presence of a first precipitant and a first complexing agent to obtain 1 The precursor seed slurry of the ternary positive electrode material is prepared, including uniformly mixing the seed slurry with the nickel-cobalt-manganese mixed metal solution, the second precipitant and the second complexing agent, and reacting to obtain the ternary positive electrode material precursor; the positive electrode active material is prepared, including mixing the ternary positive electrode material precursor with the lithium source, M 2 After the source is mixed evenly, calcination is performed to obtain the positive electrode active material, M 2 Includes one or more of Zr, Nb, Ta, W, Mo, Ti, and Ir.

[0020] The positive electrode active material includes a ternary positive electrode material particle having a core-shell structure, wherein the ternary positive electrode material particle contains a doping element M 1 And doping element M 2 , based on the total molar amount of transition metal elements in the ternary positive electrode material particles, the molar ratio of Ni element in the ternary positive electrode material particles is greater than or equal to 0.6; wherein, M 1 Distributed in the core of the ternary cathode material particles, and M 2 Distributed in the shell of the ternary positive electrode material particles.

[0021] Without intending to be limited by any theory or explanation, the above-mentioned high-nickel ternary positive electrode material particles can be prepared according to the method of the embodiment of the present application. In the above-mentioned high-nickel ternary positive electrode material particles, M 1 Doping the element into the lithium site of the high-nickel ternary cathode material particles helps to widen the interlayer spacing of the lithium layer in the high-nickel ternary cathode material particle crystals, thereby improving the lithium ion diffusion kinetics in the core of the high-nickel ternary cathode material particles and reducing the energy barrier for lithium ion migration in the core; M 2 The element is mainly doped into the transition metal site of the shell of the high-nickel ternary positive electrode material particles, thereby improving the structural stability of the surface layer of the high-nickel ternary positive electrode material particles and inhibiting the structural changes of the surface layer of the high-nickel ternary positive electrode material particles during excessive lithium removal or lithium insertion. 1 Elements and M 2The graded doping of elements reduces the difference in charge state inside the high-nickel ternary cathode material particles during the charge-discharge cycle. This can improve the structural stability of the high-nickel ternary cathode material particles, reduce the stress inside the high-nickel ternary cathode material particles, and thus improve the capacity and cycle stability of the high-nickel ternary cathode material.

[0022] In any embodiment of the present application, M 1 Salts including those containing M 1 One or more of sulfates, nitrates, carbonates, oxalates, and chlorides of the element. 1 The salt can be coprecipitated to make M 1 Elements are evenly distributed in the M-containing 1 Thus, it is beneficial for M 1 The elements are smoothly doped into the lithium sites in the core of the ternary cathode material particles during the calcination process, thereby facilitating a greater lithium ion diffusion rate inside the high-nickel ternary cathode material particles.

[0023] In any embodiment of the present application, the first precipitant and the second precipitant each independently include one or more of sodium hydroxide, sodium carbonate, potassium carbonate, and potassium hydroxide.

[0024] In any embodiment of the present application, the first complexing agent and the second complexing agent each independently include one or more of ammonia water, ammonium chloride, ammonium sulfate, urea, citric acid, and ethylenediaminetetraacetic acid (EDTA).

[0025] In any embodiment of the present application, the pH of the coprecipitation reaction is 11.5-14, and the reaction temperature of the coprecipitation reaction is 50°C-80°C.

[0026] By adjusting at least one of the precipitant, complexing agent, pH of the coprecipitation reaction, and reaction temperature to meet the above conditions, the M-containing 1 The composition and structure of the precursor seed. Thus, it is possible to allow the M-containing 1 The precursor seed crystals have a higher nickel content and a suitable particle size, which is beneficial to improving the theoretical gram capacity of the high-nickel ternary positive electrode material particles and the structural stability of the core.

[0027] In any embodiment of the present application, M 1 Volume distribution particle size Dv of the precursor seed 1 50 is 1μm-5μm.

[0028] When containing M 1 Volume distribution particle size Dv of the precursor seed 1When 50 satisfies the given range, the core of the high-nickel ternary positive electrode material particle can have an appropriate radius. This is conducive to further reducing the charge state difference inside the high-nickel ternary positive electrode material particle and improving the cycle performance and rate performance of the battery.

[0029] In any embodiment of the present application, M 2 Sources include M 2 One or more of the sulfates, carbonates, oxides, hydroxides, nitrates, silicates, acetates, and oxalates of the elements. 2 During the calcination process, the elements are smoothly doped into the transition metal sites on the surface of the high-nickel ternary positive electrode material particles, which is beneficial to improving the structural stability of the surface of the high-nickel ternary positive electrode material particles.

[0030] In any embodiment of the present application, in the step of preparing a ternary cathode material precursor, the pH of the reaction is 10-12, and the reaction temperature is 30°C-60°C.

[0031] By controlling the steps of preparing the ternary cathode material precursor, the pH and temperature of the reaction are within the above-mentioned suitable range, which is conducive to the uniform coprecipitation of nickel ions, cobalt ions, and manganese ions in the M-containing 1 The surface of the precursor seed crystal is formed, and a structurally complete ternary positive electrode material precursor is obtained.

[0032] In any embodiment of the present application, the volume distribution particle size Dv of the ternary cathode material precursor is 2 50 is 5μm-15μm.

[0033] Therefore, it is beneficial to M 2 The elements are smoothly doped into the surface layer of the high-nickel ternary positive electrode material particles during the calcination process, so that the shell of the high-nickel ternary positive electrode material particles has an appropriate thickness, which is conducive to further reducing the charge state difference inside the high-nickel ternary positive electrode material particles and improving the battery's cycle performance and rate performance.

[0034] In any embodiment of the present application, the lithium source includes one or more of LiOH·H2O, Li2CO3, Li2SO4, LiNO3, LiC2O4, and CH3COOLi.

[0035] Optionally, the molar amount of Li element contained in the lithium source is n Li Can satisfy 1.0≤n Li / n Me ≤1.2, where n Me It represents the total molar amount of Ni, Co and Mn elements in the ternary positive electrode material precursor.

[0036] In this way, the structure of the ternary positive electrode material particles can be regulated to prepare high-nickel ternary positive electrode material particles with excellent electrochemical performance.

[0037] In any embodiment of the present application, the ternary cathode material precursor is mixed with a lithium source, M 2 After the source is evenly mixed, calcination is performed to obtain the positive electrode active material, including: mixing the ternary positive electrode material precursor with the lithium source, M 2 After the source is evenly mixed, it is calcined at 500℃-700℃ for 8h-12h, and then calcined at 600℃-900℃ for 4h-8h to obtain the positive electrode active material, and the calcination atmosphere is an oxygen-containing atmosphere. 1 Elements and M 2 The graded doping of elements inside the high nickel ternary cathode material particles makes M 1 Elements are distributed in the core of high nickel ternary material particles, M 2 The elements are distributed in the shell of the high-nickel ternary material particles, which helps to improve the battery's cycle performance and rate performance.

[0038] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector, the positive electrode film layer comprising the positive electrode active material of the first aspect, or the positive electrode active material prepared according to the method of the second aspect.

[0039] A fourth aspect of an embodiment of the present application provides a battery, comprising the positive electrode plate of the third aspect.

[0040] A fifth aspect of an embodiment of the present application provides an electrical device, comprising the battery of the fourth aspect.

[0041] The electric device of the embodiment of the present application comprises the battery of the fourth aspect, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a schematic diagram of the structure of ternary positive electrode material particles in one embodiment of the present application.

[0043] Figure 2 It is a schematic diagram of an implementation of a battery cell of the present application.

[0044] Figure 3 yes Figure 2 An exploded view of an embodiment of a battery cell of the present application is shown.

[0045] Figure 4 It is a schematic diagram of an embodiment of a battery module of the present application.

[0046] Figure 5 It is a schematic diagram of an embodiment of the battery pack of the present application.

[0047] Figure 6 yes Figure 5 An exploded view of an embodiment of a battery pack of the present application is shown.

[0048] Figure 7 It is a schematic diagram of an implementation of an electrical device of the present application, and the electrical device may include a battery pack or a battery module according to an embodiment of the present application as a power source.

[0049] 10 ternary positive electrode material particles; 11 core; 12 shell; 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0050] Hereinafter, the embodiments of the positive electrode active material and its preparation method, the positive electrode sheet, the battery and the electric device containing the positive electrode active material of the present application are specifically disclosed with appropriate reference to the drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0051] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0052] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0053] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0054] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0055] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0056] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0057] Unless otherwise specified, the ratio parameters involved in this application are compared in the same unit. For example, the thickness ratio of A to B is 1.2:1, and the thickness units of A and B are the same.

[0058] With the application and promotion of secondary batteries in various electronic products and new energy vehicles and other industries, higher requirements are placed on the energy density of secondary batteries.

[0059] Increasing the battery's charge cutoff voltage is considered an effective method to increase the battery's energy density. Currently, the cathode materials of commercial high-capacity lithium-ion batteries mainly include ternary cathode materials (such as nickel-cobalt-manganese ternary cathode materials or nickel-cobalt-aluminum ternary cathode materials).

[0060] According to research, the use of high-nickel ternary positive electrode materials, that is, ternary positive electrode materials in which the molar ratio of Ni elements in transition metal elements is greater than or equal to 0.6, can further improve the energy density of the battery. However, during the charge and discharge cycle, the high-nickel ternary positive electrode material will experience a more serious cation mixing phenomenon, causing the high-nickel ternary positive electrode material to undergo an irreversible phase change. In particular, during the high-voltage charge and discharge cycle, the crystal structure changes inside the high-nickel ternary positive electrode material particles intensify, causing the high-nickel ternary positive electrode material particles to crack, pulverize, and deactivate, thereby not only limiting the capacity of the high-nickel ternary positive electrode material, but also deteriorating the rate performance and cycle performance of the battery.

[0061] In view of this, an embodiment of the present application provides a positive electrode active material, which can improve the energy density, rate performance and cycle performance of a battery containing the same; the present application also provides a method for preparing a positive electrode active material, a positive electrode sheet containing the positive electrode active material, a battery and an electrical device.

[0062] Positive electrode active material

[0063] In a first aspect, an embodiment of the present application provides a positive electrode active material, which includes ternary positive electrode material particles having a core-shell structure.

[0064] The ternary cathode material particles contain doping elements M 1 And doping element M 2 , and based on the total molar amount of transition metal elements in the ternary positive electrode material particles, the molar ratio of Ni element in the ternary positive electrode material particles is greater than or equal to 0.6. 1 The ionic radius r M1 and the radius of lithium ions r Li Satisfy: |r M1 -r Li |≤80pm, and M 1 Distributed in the core of the ternary cathode material particles. 2 Includes one or more of Zr, Nb, Ta, W, Mo, Ti, and Ir, and M 2 Distributed in the shell of the ternary positive electrode material particles.

[0065] The "core-shell" structure mentioned above has a well-known meaning in the art. Figure 1 Schematic diagram of ternary positive electrode material particles according to an embodiment of the present application is shown. Figure 1 As shown, the ternary positive electrode material particle 10 may include a core portion 11 and a shell portion 12. The core portion 11 is located in the central region of the ternary positive electrode material particle 10. 1 The shell 12 is located in the outer peripheral area of ​​the core 11, and the doping element M 2The core-shell structure can be determined by equipment and methods known in the art. For example, the EDS element surface distribution diagram of the cross section of the ternary positive electrode material particle can be measured by an EDS spectrometer; the EDS element surface distribution diagram of the cross section of the ternary positive electrode material particle is processed, and a circle is drawn with the geometric center of the cross section of the ternary positive electrode material particle as the center, and the radius of the circle is adjusted so that the area of ​​the circle is M 1 The pixel points corresponding to the element occupy 90% of the entire cross section. The area below this radius is the core, and the rest is the shell.

[0066] The above mentioned “M 1 The core portion distributed in the ternary cathode material particles has a well-known meaning in the art, which may represent M 1 The elements are mainly distributed in the core of the ternary cathode material particles. That is, in the EDS element surface distribution map of the cross section of the ternary cathode material particles, more than 10 core test areas and more than 10 shell test areas are randomly selected. 1 The average molar concentration c1 of the element is related to the M 2 The average molar concentration c2 of the element satisfies: [(c1-c2) / c2]×100%≥90%.

[0067] The above mentioned “M 2 The “shell part” distributed in the ternary cathode material particles can represent M 2 The elements are mainly distributed in the shell of the ternary cathode material particles. That is, in the EDS element surface distribution diagram of the cross section of the ternary cathode material particles, more than 10 shell test areas and more than 10 core test areas are randomly selected. 2 The average molar concentration c3 of the element is related to the M 2 The average molar concentration c4 of the element satisfies: [(c3-c4) / c4]×100%≥90%.

[0068] Research has found that due to the limitation of lithium ion diffusion kinetics, there are serious differences in charge state inside the high-nickel ternary positive electrode material particles. The charge state of the surface layer of the high-nickel ternary positive electrode material particles is higher than that of the central area, which leads to uneven changes in the unit cell volume and stress generation, and then leads to structural changes in the high-nickel ternary positive electrode material particles. The relevant technology involves doping the ternary positive electrode material particles so that the doping elements are evenly distributed in the crystal structure of the ternary positive electrode material particles. Although the relevant technology can improve the structural stability of the ternary positive electrode material particles to a certain extent, it is difficult to improve the charge state difference caused by the difference in lithium ion diffusion kinetics during the charge and discharge cycle. Therefore, the improvement of the cycle performance of the ternary positive electrode material particles is very limited.

[0069] It is not intended to be limited to any theory or explanation. In the embodiments of the present application, the above M 1 The ion radius of the element is close to that of the lithium ion, and can be doped into the lithium site of the high-nickel ternary cathode material particles, thereby helping to widen the interlayer spacing of the lithium layer in the crystal of the high-nickel ternary cathode material particles, improve the lithium ion diffusion kinetics in the core of the high-nickel ternary cathode material particles, and reduce the energy barrier for the migration of lithium ions in the core. 2 The element is mainly doped into the transition metal site of the shell of the high-nickel ternary positive electrode material particles, thereby improving the structural stability of the surface layer of the high-nickel ternary positive electrode material particles and inhibiting the structural change of the surface layer of the high-nickel ternary positive electrode material particles during excessive lithium removal or lithium insertion. 1 Elements and M 2 The graded doping of elements reduces the difference in charge state inside the high-nickel ternary cathode material particles during the charge-discharge cycle. This can improve the structural stability of the high-nickel ternary cathode material particles, reduce the stress inside the high-nickel ternary cathode material particles, and thus improve the capacity and cycle stability of the high-nickel ternary cathode material.

[0070] Therefore, the positive electrode active material of the embodiment of the present application is applied to a secondary battery, which can effectively improve the energy density, rate performance and cycle performance of the battery.

[0071] In some embodiments, M 1 It may include one or more of Na, Mg, K, and Ca.

[0072] Without intending to be bound by any theory or explanation, the M selected from the above types 1 The difference between the ion radius of the element and the lithium ion radius is small, and it can be smoothly doped into the lithium position of the high-nickel ternary positive electrode material particles, widening the interlayer spacing of the lithium layer in the crystal of the high-nickel ternary positive electrode material particles, thereby further improving the lithium ion diffusion kinetics in the core of the high-nickel ternary positive electrode material particles and reducing the energy barrier for the migration of lithium ions in the core. As a result, it helps to further reduce the difference in charge state inside the high-nickel ternary positive electrode material particles during the charge and discharge cycle. Therefore, the positive active material of the embodiment of the present application is applied to secondary batteries, which can further improve the energy density, rate performance and cycle performance of the battery.

[0073] In some embodiments, the ternary cathode material particles may have the general formula [Li 1+a M 1 b ][Ni x Co y Mn z M 2 c]O2, where 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0.05≤a+b≤0.1, 0 <b≤0.05,0<c≤0.1,x+y+z+c=1。

[0074] Optionally, in some embodiments, 0.01≤b≤0.03, 0 <c≤0.08。

[0075] Optionally, in some embodiments, x may be greater than or equal to 0.8, for example, may be 0.8, 0.9, 0.95, and so on.

[0076] Without intending to be bound by any theory or explanation, the nickel-cobalt-manganese ternary material having the above general formula has a higher nickel content and thus has a higher theoretical gram capacity. Further, the nickel-cobalt-manganese ternary material having the above general formula also has a suitable M 1 Element doping amount and appropriate M 2 The amount of element doping can thus have a higher structural stability. Therefore, the nickel-cobalt-manganese ternary material with the above general formula is applied to secondary batteries, which can significantly improve the energy density and cycle performance of the battery.

[0077] In some embodiments, the radius R of the core and the thickness D of the shell may satisfy: 0.1≤R / D≤0.9. For example, R / D may be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or a range formed by any two of the above values.

[0078] Optionally, in some embodiments, the radius R of the core and the thickness D of the shell may also satisfy: 0.4≤R / D≤0.7. For example, R / D may be 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, or a range formed by any two of the above values.

[0079] By adjusting the radius of the core and the thickness of the shell in the high-nickel ternary positive electrode material particles, the unit cell parameter c of different regions inside the high-nickel ternary positive electrode material particles can be adjusted. When R / D satisfies the above relationship, the unit cell parameter c of different regions inside the high-nickel ternary positive electrode material particles can be adjusted within a suitable range, so that the high-nickel ternary positive electrode material particles have a higher lithium ion migration rate, thereby reducing the charge state difference and stress accumulation inside the high-nickel ternary positive electrode material particles. In this way, the rate performance and cycle performance of the battery can be further improved.

[0080] In some embodiments, the unit cell parameter c of the positive electrode active material may be

[0081] Optionally, in some embodiments, the unit cell parameter c of the positive electrode active material may also be

[0082] Without intending to be limited by any theory or explanation, when the unit cell parameter c of the positive electrode active material is within the above-mentioned suitable range, the internal lithium ion migration rate of the high-nickel ternary positive electrode material particles can be made higher, thereby reducing the charge state difference and stress accumulation inside the high-nickel ternary positive electrode material particles. Thus, the rate performance and cycle performance of the battery can be further improved.

[0083] The unit cell parameter c of the positive electrode active material has a well-known meaning in the art and can be measured by equipment and methods known in the art, for example, by X-ray powder diffraction.

[0084] In some embodiments, the volume distribution particle size span of the positive electrode active material SPAN = (Dv90-Dv10) / Dv50. For example, SPAN can be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, or a range consisting of any two of the above values.

[0085] Optionally, in some embodiments, SPAN ≥ 1.2, for example, SPAN can be 1.2-2.0, 1.3-2.0, 1.4-2.0, 1.5-2.0, 1.6-2.0, 1.7-2.0, 1.8-2.0, 1.9-2.0, 1.2-1.9, 1.3-1.8, 1.4-1.7, 1.5-1.6, etc.

[0086] It is not intended to be limited by any theory or explanation. When the positive electrode active material has the above-mentioned larger volume distribution particle size span SPAN value, it means that the positive electrode active material has a wider particle size distribution. Thus, the positive electrode active material can be allowed to have a higher powder compaction density, thereby improving the volume energy density of the positive electrode active material. Therefore, the positive electrode active material of the embodiment of the present application is applied to a secondary battery, which can further improve the energy density of the battery.

[0087] In some embodiments, the volume distribution particle size Dv90 of the positive electrode active material may be 15 μm-25 μm. For example, Dv90 may be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, or a range consisting of any two of the above values.

[0088] Optionally, in some embodiments, the volume distribution particle size D of the positive electrode active material is vDv90 may also be 18 μm-22 μm. For example, Dv90 may be 18 μm, 18.5 μm, 19 μm, 19.5 μm, 20 μm, 20.5 μm, 21 μm, 21.5 μm, 22 μm, or a range consisting of any two of the above values.

[0089] In some embodiments, the volume distribution particle size Dv50 of the positive electrode active material may be 6 μm-14 μm. For example, Dv50 may be 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, or a range consisting of any two of the above values.

[0090] Alternatively, in some embodiments, the volume distribution particle size Dv50 of the positive electrode active material may also be 8 μm-12 μm. For example, Dv50 may be 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, or a range consisting of any two of the above values.

[0091] In some embodiments, the volume distribution particle size Dv10 of the positive electrode active material may be 1 μm-5 μm. For example, Dv10 may be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, or a range consisting of any two of the above values.

[0092] Optionally, in some embodiments, the volume distribution particle size D of the positive electrode active material is v Dv10 may also be 2 μm-4 μm. For example, Dv10 may be 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm, 3.2 μm, 3.5 μm, 3.8 μm, 4 μm, or a range consisting of any two of the above values.

[0093] Without intending to be limited by any theory or explanation, when one or more of the volume distribution particle sizes Dv90, Dv50, and Dv10 of the positive electrode active material meet the given range, the positive electrode active material can be allowed to have a wider particle size distribution. Thus, the positive electrode active material can be allowed to have a higher powder compaction density, thereby increasing the volume energy density of the positive electrode active material, and further increasing the energy density of the battery.

[0094] The volume distribution particle size of the positive electrode active material has a well-known meaning in the art and can be measured by equipment and methods known in the art. Among them, the volume distribution particle size Dv50 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 50%; the volume distribution particle size Dv10 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 10%; the volume distribution particle size Dv90 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 90%. The volume distribution particle sizes Dv50, Dv10, and Dv90 of the positive electrode active material can all be measured by laser diffraction particle size analysis. For example, refer to the standard GB / T19077-2016 and use a laser particle size analyzer (such as Malvern Master Size 3000) for measurement.

[0095] In some embodiments, the powder compaction density of the positive electrode active material under 5 tons of pressure is greater than or equal to 3.5g / cc, and can be selected as 3.5g / cc-3.7g / cc. When the powder compaction density of the positive electrode active material under 5 tons of pressure meets the given range, the positive electrode active material can have a higher volume energy density. Therefore, the positive electrode active material of the embodiment of the present application is applied to a secondary battery, which can further improve the energy density of the battery.

[0096] The powder compaction density of the positive electrode active material under a pressure of 5 tons has a meaning well known in the art and can be measured by equipment and methods known in the art. As an example, the compaction density of the positive electrode active material under a pressure of 5 tons (i.e., under a pressure of 5T) can be determined with reference to GB / T 24533-2009. Specifically, a certain amount of positive electrode active material powder can be placed in a special compaction mold, and then the mold can be placed on a compaction density instrument. A pressure of 5T is applied, and the thickness of the powder under a pressure of 5T (the thickness after pressure relief) is read on the equipment, and the powder compaction density ρ of the positive electrode active material is calculated by ρ=m / v.

[0097] Preparation method

[0098] In a second aspect, an embodiment of the present application provides a method for preparing a positive electrode active material, comprising the following steps S10 to S40.

[0099] S10, providing a precursor solution, the precursor solution comprising a nickel salt, a cobalt salt, a manganese salt and a 1 A mixed solution of salts, wherein M 1 The ionic radius r M1 and the radius of lithium ions r Li Satisfy: |r M1 -r Li |≤80pm.

[0100] In step S10, providing a precursor solution may include mixing a nickel salt solution, a cobalt salt solution, a manganese salt solution and a solution containing M1 The salt solution is mixed to obtain a mixed solution; it may also include nickel salt, cobalt salt, manganese salt and M 1 The salts are mixed and dissolved in deionized water to obtain a mixed solution, which is not limited here.

[0101] Nickel salts, cobalt salts, manganese salts and M-containing 1 The salt may be selected from soluble nickel salts, cobalt salts, manganese salts and M-containing salts known in the art. 1 Examples of soluble nickel salts may include one or more of sulfates, nitrates, acetates, carbonates, oxalates, citrates, chlorides, etc. containing nickel. Examples of soluble cobalt salts may include one or more of sulfates, nitrates, acetates, carbonates, oxalates, citrates, chlorides, etc. containing cobalt. Examples of soluble manganese salts may include one or more of sulfates, nitrates, acetates, carbonates, oxalates, citrates, chlorides, etc. containing manganese. Those skilled in the art may select according to actual needs, which is not limited here. Nickel salts, cobalt salts, manganese salts and M-containing 1 The ratio of the salt can be adjusted according to actual needs. For example, the ratio of the salt can be adjusted according to the Ni element, Co element, Mn element and Mn element in the ternary positive electrode material particles to be prepared. 1 The molar ratio of the elements is adjusted to prepare the nickel salt, cobalt salt, manganese salt and M-containing 1 The concentration of the precursor solution is not specifically limited and can be adjusted by a person skilled in the art as needed. As an example, in the precursor solution, Ni, Co, Mn and 1 The total concentration of the elements may be 0.1 mol / L to 10 mol / L.

[0102] S20, preparing a seed slurry, including mixing the precursor solution with the first precipitant and the first complexing agent to uniformly mix the nickel salt, the cobalt salt, the manganese salt and the M-containing 1 The salt of M is coprecipitated in the presence of a first precipitant and a first complexing agent to obtain 1 Precursor seed slurry.

[0103] In step S20, examples of the first precipitant and the first complexing agent may include one or more precipitants and complexing agents known in the art, and those skilled in the art may select them according to actual needs, and are not limited here. In one embodiment, 10L-50L of pure water may be added to a 100L reactor, and a certain amount of the first precipitant solution may be added under stirring to a concentration of 0.2mol / L to 0.6mol / L, optionally 0.3mol / L to 0.5mol / L; the precursor solution, the first precipitant solution, and the first complexing agent solution are added to the reactor at a certain rate, and the pH of the solution in the reactor and the concentration of the complexing agent are kept substantially unchanged, so that the nickel salt, the cobalt salt, the manganese salt, and the M-containing 1 The salt of M is coprecipitated in the presence of a first precipitant and a first complexing agent, and then centrifuged, washed, filtered, and dried to obtain a 1 The concentration of the first precipitant solution may be 0.1 mol / L to 20 mol / L; the concentration of the first complexing agent solution may be 0.1 mol / L to 10 mol / L.

[0104] S30, preparing a ternary cathode material precursor, including uniformly mixing and reacting the seed slurry with a nickel-cobalt-manganese mixed metal solution, a second precipitant and a second complexing agent to obtain a ternary cathode material precursor.

[0105] In step S30, the second precipitant and the second complexing agent may be of the same type as the first precipitant and the first complexing agent, or may be different. Examples of the second precipitant and the second complexing agent may include one or more precipitants and complexing agents known in the art, and those skilled in the art may select them according to actual needs, which are not limited here. The nickel-cobalt-manganese mixed metal solution may be a solution including nickel ions, cobalt ions and manganese ions, for example, it may be a mixed solution of nickel salt, cobalt salt and manganese salt. The ratio of nickel ions, cobalt ions and manganese ions can be adjusted according to actual needs, for example, according to the Ni element, Co element, Mn element and Mn element in the ternary positive electrode material particles to be prepared. 1 The molar ratio of the elements is used to adjust the ratio of nickel ions, cobalt ions and manganese ions in preparing the nickel-cobalt-manganese mixed metal solution.

[0106] In some embodiments, step S30 may include: treating part of the M-containing 1 The precursor seed slurry is used as the base liquid, and the pH is adjusted to a certain value; then the nickel-cobalt-manganese mixed metal solution, the second precipitant solution and the second complexing agent solution and the remaining M-containing 1The precursor seed slurry is added to the reactor at a certain flow rate, and the concentration and pH of the second complexing agent in the reactor are kept unchanged. After the reaction is completed, a ternary cathode material precursor is obtained. As an example, 10L-50L of pure water and 1kg-20kg of M-containing 1 The precursor seed slurry is used as the base liquid, and a certain amount of the second precipitant solution is added under stirring to a concentration of 0.2mol / L to 0.6mol / L, optionally 0.3mol / L to 0.5mol / L; the nickel-cobalt-manganese mixed metal solution, the second precipitant solution, the second complexing agent solution and the remaining M-containing 1 The precursor seed slurry is added into the reactor at a certain rate. The concentration of the second precipitant solution can be 0.1 mol / L to 20 mol / L; the concentration of the second complexing agent solution can be 0.1 mol / L to 10 mol / L.

[0107] S40, preparing a positive electrode active material, including mixing a ternary positive electrode material precursor with a lithium source, M 2 After the source is mixed evenly, calcination is performed to obtain the positive electrode active material, M 2 Includes one or more of Zr, Nb, Ta, W, Mo, Ti, and Ir.

[0108] In step S40, the ternary cathode material precursor is mixed with a lithium source, M 2 After the source is mixed evenly, during the calcination process, M 1 The element can be doped into the lithium site of the ternary cathode material particles in the central region, thereby being distributed in the core of the ternary cathode material particles. 2 The elements can penetrate from the surface of the ternary cathode material precursor to the inside, and thus be distributed in the shell of the ternary cathode material particles.

[0109] The positive electrode active material prepared according to steps S10 to S40 includes ternary positive electrode material particles having a core-shell structure, wherein the ternary positive electrode material particles contain a doping element M 1 And doping element M 2 , based on the total molar amount of transition metal elements in the ternary positive electrode material particles, the molar ratio of Ni element in the ternary positive electrode material particles is greater than or equal to 0.6. 1 Distributed in the core of the ternary cathode material particles, and M 2 Distributed in the shell of the ternary positive electrode material particles.

[0110] Without intending to be limited by any theory or explanation, the above-mentioned high-nickel ternary positive electrode material particles can be prepared according to the method of the embodiment of the present application. In the above-mentioned high-nickel ternary positive electrode material particles, M 1Doping the element into the lithium site of the high-nickel ternary cathode material particles helps to widen the interlayer spacing of the lithium layer in the high-nickel ternary cathode material particle crystals, thereby improving the lithium ion diffusion kinetics in the core of the high-nickel ternary cathode material particles and reducing the energy barrier for lithium ion migration in the core; M 2 The element is mainly doped into the transition metal site of the shell of the high-nickel ternary positive electrode material particles, thereby improving the structural stability of the surface layer of the high-nickel ternary positive electrode material particles and inhibiting the structural changes of the surface layer of the high-nickel ternary positive electrode material particles during excessive lithium removal or lithium insertion. 1 Elements and M 2 The graded doping of elements reduces the difference in charge state inside the high-nickel ternary cathode material particles during the charge-discharge cycle. This can improve the structural stability of the high-nickel ternary cathode material particles, reduce the stress inside the high-nickel ternary cathode material particles, and thus improve the capacity and cycle stability of the high-nickel ternary cathode material.

[0111] Therefore, the positive electrode active material prepared according to the method of the embodiment of the present application is applied to a secondary battery, which can effectively improve the energy density, rate performance and cycle performance of the battery.

[0112] In some embodiments, the 1 The salt may include M 1 One or more of the sulfates, nitrates, carbonates, oxalates and chlorides of the element.

[0113] Without intending to be bound by any theory or explanation, the above-mentioned types of M 1 The salt can be coprecipitated to make M 1 Elements are evenly distributed in the M-containing 1 Thus, it is beneficial for M 1 The elements are smoothly doped into the lithium sites in the core of the ternary cathode material particles during the calcination process, which is conducive to a larger lithium ion diffusion rate inside the high-nickel ternary cathode material particles. Therefore, the positive electrode active material prepared in the embodiment of the present application is applied to secondary batteries, which can reduce the difference in charge state inside the high-nickel ternary cathode material particles during the charge and discharge cycle, thereby further improving the energy density, rate performance and cycle performance of the battery.

[0114] In some embodiments, the first precipitant and the second precipitant may each independently include one or more of sodium hydroxide, sodium carbonate, potassium carbonate, and potassium hydroxide.

[0115] In some embodiments, the first complexing agent and the second complexing agent may each independently include one or more of ammonia, ammonium chloride, ammonium sulfate, urea, citric acid, and ethylenediaminetetraacetic acid (EDTA).

[0116] In some embodiments, the pH of the coprecipitation reaction may be 11.5-14, and may be 12-13. The reaction temperature of the coprecipitation reaction may be 50°C-80°C.

[0117] Without intending to be limited by any theory or explanation, when at least one of the precipitant, the complexing agent, the pH of the coprecipitation reaction, and the reaction temperature satisfies the above conditions, the M-containing 1 The composition and structure of the precursor seed. Thus, it is possible to allow the M-containing 1 The precursor seed crystals have a higher nickel content and a suitable particle size, which is beneficial to improving the theoretical gram capacity of the high-nickel ternary positive electrode material particles and the structural stability of the core.

[0118] In some embodiments, the 1 Volume distribution particle size Dv of the precursor seed 1 50 can be 1 μm-5 μm.

[0119] Without intending to be bound by any theory or explanation, 1 Volume distribution particle size Dv of the precursor seed 1 When 50 satisfies the given range, the structure of the high-nickel ternary positive electrode material particles can be adjusted so that the core of the high-nickel ternary positive electrode material particles has an appropriate radius. This is conducive to further reducing the difference in the state of charge inside the high-nickel ternary positive electrode material particles, thereby improving the structural stability of the positive electrode active material, and further improving the cycle performance and rate performance of the battery.

[0120] In some embodiments, M 2 The source may include 2 One or more of the sulfates, carbonates, oxides, hydroxides, nitrates, silicates, acetates and oxalates of an element.

[0121] Without intending to be bound by any theory or interpretation, 2 When the source is selected from the above substances, it is beneficial to M 2 During the calcination process, the elements are smoothly doped into the transition metal sites on the surface of the high-nickel ternary cathode material particles, which is beneficial to improving the structural stability of the surface of the high-nickel ternary cathode material particles and inhibiting the structural changes of the surface of the high-nickel ternary cathode material particles during excessive lithium removal or lithium insertion. This is beneficial to further improve the rate performance and cycle performance of the battery.

[0122] In some embodiments, in the step of preparing a ternary cathode material precursor, the reaction pH may be 10-12, and the reaction temperature may be 30°C-60°C.

[0123] By controlling the steps of preparing the ternary cathode material precursor, the pH and temperature of the reaction are within the above-mentioned suitable range, which is conducive to the uniform coprecipitation of nickel ions, cobalt ions, and manganese ions in the M-containing 1 The surface of the precursor seed crystal is formed, and a structurally complete ternary positive electrode material precursor is obtained.

[0124] In some embodiments, the volume distribution particle size Dv of the ternary cathode material precursor is 2 50 can be 5μm-15μm.

[0125] Without intending to be bound by any theory or explanation, by controlling the volume distribution particle size Dv of the ternary cathode material precursor 2 50 is within the above suitable range, which is beneficial to M 2 The elements are smoothly doped into the surface layer of the high-nickel ternary positive electrode material particles during the calcination process. As a result, the shell of the high-nickel ternary positive electrode material particles can have a suitable thickness, which is conducive to further reducing the difference in the state of charge inside the high-nickel ternary positive electrode material particles, thereby helping to improve the structural stability of the positive electrode active material, and further improve the cycle performance and rate performance of the battery.

[0126] In some embodiments, the lithium source may include one or more of LiOH·H2O, Li2CO3, Li2SO4, LiNO3, LiC2O4, and CH3COOLi. The molar amount of Li element contained in the lithium source is n Li Can satisfy 1.0≤n Li / n Me ≤1.2, where n Me It represents the total molar amount of Ni, Co and Mn in the ternary cathode material precursor. Thus, the structure of the ternary cathode material particles can be regulated to prepare high-nickel ternary cathode material particles with excellent electrochemical performance.

[0127] In some embodiments, the ternary cathode material precursor is mixed with a lithium source, M 2 After the source is evenly mixed, calcination is performed to obtain the positive electrode active material, which may specifically include: mixing the ternary positive electrode material precursor with the lithium source, M 2 After the sources are uniformly mixed, they are calcined at 500°C-700°C for 8h-12h, and then calcined at 600°C-900°C for 4h-8h to obtain the positive electrode active material. The calcination atmosphere is an oxygen-containing atmosphere, for example, it can include but is not limited to air or oxygen atmosphere.

[0128] Without intending to be bound by any theory or explanation, this embodiment adopts a step-by-step calcination process of first low temperature and then high temperature to reduce M 1 Ion and M 2 The risk of high temperature ion diffusion of ions is reduced. 1 Elements and M2 The graded doping of elements inside the high nickel ternary cathode material particles makes M 1 Elements are distributed in the core of high nickel ternary material particles, M 2 The elements are distributed in the shell of the high-nickel ternary material particles, which helps to improve the battery's cycle performance and rate performance.

[0129] Positive electrode

[0130] The third aspect of the embodiment of the present application provides a positive electrode plate, which includes a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector. The positive electrode film layer includes the positive electrode active material of the first aspect, or the positive electrode active material prepared according to the method of the second aspect.

[0131] The positive electrode plate of the embodiment of the present application includes the positive electrode active material of the first aspect, or the positive electrode active material prepared according to the method of the second aspect, and is applied to a secondary battery, so that the secondary battery can have high energy density, good rate performance and cycle performance.

[0132] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent includes at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0133] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. The present application has no particular restrictions on the type of positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0134] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base and a metal material layer formed on at least one surface of the polymer material base. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0135] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, optional conductive agent, optional binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.

[0136] Battery

[0137] The battery mentioned in the embodiments of the present application may include one or more battery cells to provide a single physical module with higher voltage and capacity. When there are multiple battery cells, the multiple battery cells are connected in series, in parallel or in mixed connection through a busbar component.

[0138] Typically, a battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode, a negative electrode, and a separator. During the charge and discharge process of the battery cell, active ions (such as lithium ions) are embedded and removed back and forth between the positive electrode and the negative electrode. The separator is arranged between the positive electrode and the negative electrode, which can prevent the positive and negative electrodes from short-circuiting and allow active ions to pass through. The electrolyte plays the role of conducting active ions between the positive electrode plate and the negative electrode plate.

[0139] [Positive electrode]

[0140] In the battery cell of the embodiment of the present application, the positive electrode sheet of the electrode assembly may include the positive electrode sheet of the third aspect. The implementation of the positive electrode sheet has been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery cell of the embodiment of the present application can achieve the beneficial effects of any of the above implementations of the positive electrode sheet of the embodiment of the present application.

[0141] [Negative electrode]

[0142] The negative electrode sheet may include a negative electrode current collector and a negative electrode film layer disposed on at least one side of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0143] The negative electrode active material may adopt the negative electrode active material for secondary batteries known in the art. As an example, the negative electrode active material may include but is not limited to at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate. The silicon-based material may include at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite and silicon alloy material. The tin-based material may include at least one of elemental tin, tin oxide and tin alloy material.

[0144] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent. As an example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0145] In some embodiments, the negative electrode film layer may further include a negative electrode binder. The present application has no particular restrictions on the type of the negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, aqueous acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0146] In some embodiments, the negative electrode film layer may further include other additives. As an example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC-Na), a PTC thermistor material, and the like.

[0147] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0148] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional conductive agent, optional binder, and other optional auxiliary agents in a solvent and stirring them evenly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0149] The negative electrode plate does not exclude other additional functional layers besides the negative electrode film layer. For example, in some embodiments, the negative electrode plate also includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In some embodiments, the negative electrode plate of the present application also includes a protective layer covering the surface of the negative electrode film layer.

[0150] [Isolation film]

[0151] The separator is disposed between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The embodiment of the present application has no particular limitation on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0152] In some embodiments, the material of the isolation membrane can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different, without special restrictions.

[0153] [Electrolytes]

[0154] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present application embodiment has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid or gel.

[0155] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0156] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0157] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0158] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0159] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly by a winding process or a lamination process.

[0160] In some embodiments, the battery cell further includes a housing for accommodating the electrode assembly and the electrolyte. The housing of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The housing of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0161] The embodiment of the present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square or any other shape. Figure 2 The battery cell 5 is a square structure as an example.

[0162] In some embodiments, reference Figure 3 , the shell may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0163] The preparation method of the battery cell of the embodiment of the present application is well known. In some embodiments, the electrode assembly can be placed in a housing, and after drying, an electrolyte can be injected, and the battery cell can be obtained through vacuum packaging, standing, forming, shaping and other processes.

[0164] In some embodiments, the battery mentioned in the embodiments of the present application refers to a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the embodiments of the present application can be a battery module or a battery pack. The battery generally includes a box for encapsulating one or more battery cells. The box can prevent liquid or other foreign matter from affecting the charging or discharging of the battery cells.

[0165] In some embodiments, there may be multiple battery cells in the battery, and the multiple battery cells may be connected in series, in parallel, or in a hybrid connection. A hybrid connection means that the multiple battery cells are both connected in series and in parallel. The multiple battery cells may be directly connected in series, in parallel, or in a hybrid connection, and then the whole formed by the multiple battery cells is accommodated in the box; of course, multiple battery cells may be first connected in series, in parallel, or in a hybrid connection to form a battery module, and then the multiple battery modules are connected in series, in parallel, or in a hybrid connection to form a whole, and then accommodated in the box.

[0166] Figure 4 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 4As shown, there are multiple battery cells 5, and the multiple battery cells 5 are first connected in series, in parallel, or in mixed connection to form a battery module 4. The multiple battery cells 5 in the battery module 4 can be electrically connected through a busbar component to realize the series connection, parallel connection, or mixed connection of the multiple battery cells 5 in the battery module 4. In the battery module 4, the multiple battery cells 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. Further, the multiple battery cells 5 can be fixed by fasteners.

[0167] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0168] Figure 5 and Figure 6 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 5 and Figure 6 As shown, the battery pack 1 may include a box body and a plurality of battery modules 4 disposed in the box body. The plurality of battery modules 4 in the battery pack 1 may be electrically connected through a busbar component to achieve series connection, parallel connection, or mixed connection of the plurality of battery modules 4 in the battery pack 1. The box body includes an upper box body 2 and a lower box body 3, wherein the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0169] Electrical devices

[0170] The embodiment of the present application also provides an electric device, the electric device includes a battery cell provided in the embodiment of the present application, and the battery cell is used to provide electrical energy. The battery cell can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0171] As the electrical device, a battery cell, a battery module including a plurality of battery cells, or a battery pack may be selected according to its usage requirements.

[0172] Figure 7 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the power consumption device for high power and high energy density, a battery pack or a battery module can be used.

[0173] As another example, the power-consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and a battery cell may be used as a power source.

[0174] Example

[0175] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0176] Example 1

[0177] Preparation of positive electrode active materials

[0178] (1) nickel sulfate hexahydrate, cobalt sulfate heptahydrate, manganese sulfate monohydrate, and M 1 The salt NaCl is mixed and dissolved in pure water to obtain a precursor solution with a total concentration of 2 mol / L of nickel, cobalt, manganese and M1 elements.

[0179] (2) Add 20 L of pure water to a 100 L reactor, start stirring, maintain the temperature at 50 ° C, add an appropriate amount of the first precipitant solution (4 mol / L NaOH solution), and adjust the pH of the solution in the reactor to 10-13.

[0180] (3) Under stirring conditions, the precursor solution, the first precipitant solution (4 mol / L NaOH solution), and the first complexing agent solution (2 mol / L ammonia solution) are added to the reactor at a certain rate to make the nickel salt, cobalt salt, manganese salt and M-containing 1 The salt undergoes a coprecipitation reaction in the presence of the precipitant and the complexing agent, and the ammonia concentration and pH in the reactor are kept constant during the reaction. After centrifugation, washing, filtering and drying, a M-containing 1 The precursor seed slurry contains M 1 Volume distribution particle size Dv of the precursor seed 1 50 is 3.8μm.

[0181] (4) Add 20 L of pure water to a 100 L reactor, followed by 10 kg of M-containing 1 The precursor seed slurry was stirred, the temperature was maintained at 40° C., an appropriate amount of the second precipitant solution (4 mol / L NaOH solution) was added, and the pH of the solution in the reactor was adjusted to 10-12.

[0182] (5) Under stirring conditions, add M-containing 1The precursor seed slurry, the second precipitant solution (1 mol / L NaOH solution), the second complexing agent solution (2 mol / L ammonia water) and the nickel-cobalt-manganese mixed metal solution (2 mol / L nickel-cobalt-manganese sulfate mixed solution) are prepared. During the reaction, the ammonia concentration and pH in the reactor are kept unchanged. After a period of reaction, the precursor is centrifuged, washed, filtered and dried to obtain a ternary cathode material precursor. The chemical formula of the ternary cathode material precursor is [Na 0.02 Ni 0.9 Co 0.06 Mn 0.02 ](OH)2, and the volume distribution particle size Dv of the ternary cathode material precursor 2 50 is 11.4μm.

[0183] (6) The ternary cathode material precursor is mixed with lithium source Li2CO3, M 2 After the source Zr(SO4)2 is fully mixed, it is calcined at 600℃ for 10h in air atmosphere and then calcined at 800℃ for 6h to obtain the positive electrode active material. Among them, the ratio w1 of the molar amount of Li element in the lithium source to the total molar amount of Ni element, Co element and Mn element in the ternary positive electrode material precursor is 1.04:0.98. 2 Source M 2 The ratio w2 of the molar amount of the element to the total molar amount of Ni, Co and Mn in the ternary positive electrode material precursor is 0.02:0.98.

[0184] Preparation of positive electrode

[0185] The positive electrode active material [Li 1.04 Na 0.02 ][Ni 0.9 Co 0.06 Mn 0.02 Zr 0.02 ]O2, conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in a proper amount of solvent N-methylpyrrolidone (NMP) in a mass ratio of 98:1:1 to obtain positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through processes such as drying, cold pressing, slitting, and cutting.

[0186] Preparation of negative electrode

[0187] The negative electrode active material artificial graphite, the conductive agent carbon black (Super P), the binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) are mixed uniformly in a proper amount of solvent deionized water at a mass ratio of 97:1:1:1 to obtain a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained through the processes of drying, cold pressing, slitting and cutting.

[0188] Preparation of isolation membrane

[0189] Polypropylene film is used as the isolation film.

[0190] Preparation of electrolyte

[0191] LiPF6 was dissolved in a solvent prepared by mixing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a ratio of 1:1:1 by volume to obtain an electrolyte solution with a LiPF6 concentration of 1 mol / L.

[0192] Preparation of secondary batteries

[0193] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained.

[0194] Example 2-18

[0195] Based on the preparation process of the positive electrode active material in Example 1, the content of M 1 Salt, M 2 Source, w1 to w2, Dv P 50 and Dv 2 50, prepare a positive electrode active material with a preset composition and structure to obtain the positive electrode active material of Examples 2 to 18. The preparation of the positive electrode sheet, the negative electrode sheet, the separator, the electrolyte and the secondary battery of Examples 2 to 18 is the same as that of Example 1.

[0196] Example 2-4 is based on Example 1, respectively containing M 1 The salt was replaced with equimolar amounts of MaCl2, KCl, and CaCl2.

[0197] Example 5-8 Based on Example 1, the M-containing 2 Source replaced with equal M 2 Molar amounts of niobium pentoxide (Nb2O5), tantalum pentoxide (Ta2O5), tungsten oxide (WO3), molybdenum oxide (MoO3), and titanium dioxide (TiO2).

[0198] Example 10 Based on Example 1, Dv 1 50 and Dv 2 50 is adjusted to 1.20μm and 13.2μm.

[0199] Example 11 Based on Example 1, Dv 1 50 and Dv 250 is adjusted to 2.43μm and 10.53μm.

[0200] Example 12 Based on Example 1, Dv 1 50 and Dv 2 50 is adjusted to 3.25μm and 9.75μm.

[0201] Example 13 Based on Example 1, Dv 1 50 and Dv 2 50 is adjusted to 3.78μm and 9.18μm.

[0202] Example 14 Based on Example 1, Dv 1 50 and Dv 2 50 is adjusted to 4.05μm and 8.55μm.

[0203] In Example 15, the chemical formula of the ternary cathode material precursor is [Na 0.01 Ni 0.6 Co 0.2 Mn 0.15 ](OH)2, w1 is 1.05:0.95, w2 is 0.05:0.95.

[0204] In Example 16, the chemical formula of the ternary cathode material precursor is [Na 0.01 Ni 0.77 Co 0.12 Mn 0.08 ](OH)2, w1 is 1.06:0.97, w2 is 0.03:0.97.

[0205] In Example 17, the chemical formula of the ternary cathode material precursor is [Na 0.005 Ni 0.82 Co 0.1 Mn 0.06 ](OH)2, w1 is 1.05:0.98, w2 is 0.02:0.98.

[0206] In Example 18, the chemical formula of the ternary cathode material precursor is [Na 0.015 Ni 0.92 Co 0.05 Mn 0.02 ](OH)2, w1 is 1.04:0.99, w2 is 0.01:0.99.

[0207] The secondary batteries of Comparative Examples 1-5 are similar to those of Example 1, except that conventional nickel-cobalt-manganese ternary positive electrode material particles are used as positive electrode active materials in Comparative Examples 1-5.

[0208] The chemical formula, core radius R, shell thickness D and unit cell parameter c of the positive electrode active materials of Examples 1-18 and Comparative Examples 1-5 were characterized, and the characterization results are shown in Table 1. The chemical formula of the positive electrode active material is characterized by the following steps: the positive electrode active material is dissolved in aqua regia, and element analysis is performed by inductively coupled plasma emission spectrometry (ICP, Ametek, model: SPECTROARCOSICP-OES) to obtain the ratio of each element, and the chemical formula of the positive electrode active material is determined by the ratio of each element. The core radius R, the shell thickness D and the unit cell parameter c can be determined according to the method described in the specification of this application.

[0209] Test Section

[0210] Normal temperature cycle performance test

[0211] At 25°C, charge the secondary battery to 4.25V at 0.5C constant current, then charge to a cut-off current of 0.05C at 4.25V constant voltage, leave for 10 minutes, then discharge to 2.8V at 0.5C constant current, leave for 5 minutes. This is a charge and discharge cycle. Record the discharge capacity at this time as C0. Repeat this charge and discharge cycle process for the same secondary battery, and record the discharge capacity C1 at the 300th cycle. The battery cycle capacity retention rate P 300 =C1 / C0×100%.

[0212] The test results are shown in Table 1.

[0213]

[0214]

[0215] From the test results in Table 1, it can be seen that the positive electrode active material of the embodiment of the present application has a specific structure and element composition. Therefore, the positive electrode active material can have a higher structural stability and can be applied to secondary batteries to effectively improve the cycle performance of the battery.

[0216] In contrast, the positive electrode active materials of Comparative Examples 1-5 do not have a core-shell structure, and there is no M in the positive electrode active material particles. 1 Elements and M 2 The graded doping of elements seriously deteriorates the cycle performance of the battery as the nickel content in the positive electrode active material increases. Therefore, the cycle performance of the secondary battery of Comparative Examples 1-5 is far inferior to that of Examples 1-18.

[0217] For some compounds given but not listed in the embodiments, since their chemical properties and reaction properties when participating in electrochemical reactions are similar to those of the compounds listed in the embodiments, they are all suitable for the technical scheme of the present invention and are therefore not listed one by one here.

[0218] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A positive electrode active material, characterized in that: It includes ternary positive electrode material particles having a core-shell structure, The ternary positive electrode material particles contain doping elements M 1 And doping element M 2 , and based on the total molar amount of transition metal elements in the ternary positive electrode material particles, the molar amount of Ni element in the ternary positive electrode material particles accounts for greater than or equal to 0.6; Among them, M 1 The ionic radius r M1 and the radius of lithium ions r Li Satisfy: |r M1 -r Li |≤80pm, and M 1 Distributed in the core of the ternary positive electrode material particles; M 2 Includes one or more of Zr, Nb, Ta, W, Mo, Ti, and Ir, and M 2 Distributed in the shell of the ternary positive electrode material particles.

2. The positive electrode active material according to claim 1, characterized in that The M 1 Includes one or more of Na, Mg, K, and Ca.

3. The positive electrode active material according to claim 1 or 2, characterized in that: The ternary positive electrode material particles have the general formula [Li 1+a M 1 b ][Ni x Co y Mn z M 2 c ]O2, where 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0.05≤a+b≤0.1, 0 <b≤0.05,0<c≤0.1,x+y+z+c=1; Optionally, 0.01≤b≤0.03, 0 <c≤0.08。 4. The positive electrode active material according to any one of claims 1 to 3, characterized in that The radius R of the core portion and the thickness D of the shell portion satisfy: 0.1≤R / D≤0.9, optionally, 0.4≤R / D≤0.

7.

5. The positive electrode active material according to any one of claims 1 to 4, characterized in that The unit cell parameter c of the positive electrode active material is Optional 6. The positive electrode active material according to any one of claims 1 to 5, characterized in that The volume distribution particle size span SPAN of the positive electrode active material is SPAN=(Dv90-Dv10) / Dv50, then SPAN≥1.1, optionally, SPAN≥1.

2.

7. The positive electrode active material according to any one of claims 1 to 6, characterized in that The volume distribution particle size Dv90 of the positive electrode active material is 15 μm-25 μm, and can be 18 μm-22 μm; and / or The volume distribution particle size Dv50 of the positive electrode active material is 6 μm-14 μm, and can be 8 μm-12 μm; and / or The volume distribution particle size Dv10 of the positive electrode active material is 1 μm-5 μm, and can be optionally 2 μm-4 μm.

8. The positive electrode active material according to any one of claims 1 to 7, characterized in that The powder compaction density of the positive electrode active material under a pressure of 5 tons is greater than or equal to 3.5 g / cc, and can be optionally 3.5 g / cc-3.7 g / cc.

9. A method for preparing a positive electrode active material, characterized in that: include: Provide a precursor solution, the precursor solution comprising a nickel salt, a cobalt salt, a manganese salt and a 1 A mixed solution of salts, wherein M 1 The ionic radius r M1 and the radius of lithium ions r Li Satisfy: |r M1 -r Li |≤80pm; The seed slurry is prepared, including mixing the precursor solution with a first precipitant and a first complexing agent to uniformly mix the nickel salt, the cobalt salt, the manganese salt and the M-containing 1 The salt undergoes a coprecipitation reaction in the presence of the first precipitant and the first complexing agent to obtain a compound containing M 1 A precursor seed slurry; Preparing a ternary cathode material precursor, comprising uniformly mixing and reacting the seed slurry with a nickel-cobalt-manganese mixed metal solution, a second precipitant and a second complexing agent to obtain a ternary cathode material precursor; The positive electrode active material is prepared by mixing the ternary positive electrode material precursor with a lithium source, M 2 After the source is mixed evenly, calcination is performed to obtain the positive electrode active material. 2 Including one or more of Zr, Nb, Ta, W, Mo, Ti, Ir, The positive electrode active material comprises a ternary positive electrode material particle having a core-shell structure, wherein the ternary positive electrode material particle contains a doping element M 1 And doping element M 2 , based on the total molar amount of transition metal elements in the ternary positive electrode material particles, the molar ratio of Ni element in the ternary positive electrode material particles is greater than or equal to 0.6; wherein, M 1 Distributed in the core of the ternary positive electrode material particles, and M 2 Distributed in the shell of the ternary positive electrode material particles.

10. The method according to claim 9, characterized in that The M-containing 1 Salts including those containing M 1 One or more of the sulfates, nitrates, carbonates, oxalates and chlorides of the element.

11. The method according to claim 9 or 10, characterized in that: The first precipitant and the second precipitant each independently include one or more of sodium hydroxide, sodium carbonate, potassium carbonate, potassium hydroxide; and / or The first complexing agent and the second complexing agent each independently include one or more of ammonia water, ammonium chloride, ammonium sulfate, urea, citric acid, and ethylenediaminetetraacetic acid (EDTA); and / or The pH of the coprecipitation reaction is 11.5-14, and the reaction temperature of the coprecipitation reaction is 50° C.-80° C.; and / or The M-containing 1 Volume distribution particle size Dv of the precursor seed 1 50 is 1μm-5μm.

12. The method according to any one of claims 9 to 11, characterized in that: The M 2 Sources include M 2 One or more of the sulfates, carbonates, oxides, hydroxides, nitrates, silicates, acetates and oxalates of an element.

13. The method according to any one of claims 9 to 12, characterized in that: In the step of preparing the ternary cathode material precursor, the reaction pH is 10-12, and the reaction temperature is 30° C.-60° C.; and / or Volume distribution particle size Dv of ternary cathode material precursor 2 50 is 5μm-15μm.

14. The method according to any one of claims 9 to 13, characterized in that: The lithium source includes one or more of LiOH·H2O, Li2CO3, Li2SO4, LiNO3, LiC2O4, and CH3COOLi; Optionally, the molar amount of Li element contained in the lithium source is n Li Can satisfy 1.0≤n Li / n Me ≤1.2, where n Me It represents the total molar amount of Ni, Co and Mn in the ternary positive electrode material precursor.

15. The method according to any one of claims 9 to 14, characterized in that: The ternary cathode material precursor is mixed with a lithium source, M 2 After the sources are uniformly mixed, calcination is performed to obtain the positive electrode active material, including: The ternary cathode material precursor is mixed with a lithium source, M 2 After the sources are uniformly mixed, they are calcined at 500° C.-700° C. for 8 h-12 h, and then calcined at 600° C.-900° C. for 4 h-8 h to obtain a positive electrode active material, wherein the calcination atmosphere is an oxygen-containing atmosphere.

16. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector, wherein the positive electrode film layer comprises the positive electrode active material according to any one of claims 1 to 8, or the positive electrode active material prepared by the method according to any one of claims 9 to 15.

17. A battery comprising the positive electrode sheet according to claim 16.

18. An electrical device comprising the battery according to claim 17.

Citation Information

Patent Citations

  • Positive electrode active material and preparation method thereof, positive electrode plate and lithium ion secondary battery

    CN112447950A

  • Positive electrode active material, positive electrode plate and lithium ion secondary battery

    CN112447967A

  • Positive electrode active material for lithium secondary battery, method for manufacturing same, and lithium secondary battery including same

    CN112514115A

  • Positive electrode active material for lithium secondary battery and preparation method therefor

    CN113169329A

  • Ternary positive electrode active material and lithium ion battery containing same

    CN115692704A

Cited By

  • Gradient-doped lithium ion battery high-nickel positive electrode material as well as preparation method and application thereof

    CN121355248A

  • Gradient-doped lithium-ion battery high-nickel cathode material, preparation method and application thereof

    CN121355248B

  • Positive electrode material, positive electrode sheet and secondary battery

    WO2026138645A1