Silicon-carbon composite material, preparation method thereof, negative plate and lithium ion battery
By using silicon-carbon composite materials in lithium-ion batteries, a silicon-carbon composite layer with reduced silicon element content is formed through vapor deposition, which solves the problems of poor conductivity and high volume expansion of silicon negative electrode materials, and improves the energy density and circulation of the battery performance.
Patent Information
- Application Number
- CN202310634929.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The existing silicon negative electrode materials have poor conductivity, high volume expansion rate and poor circulation performance, which is difficult to meet the needs of new energy vehicles for the energy density, cycle life and safety performance of power batteries.
Using silicon-carbon composite materials, by vapor deposition on a carbon matrix, the gas flow rate of the silicon source decreases with time and the gas flow rate of the carbon source increases with time, forming a silicon-carbon composite layer with decreasing silicon element content from the inside to the outside. Improve conductivity and strength and reduce expansion rate.
A silicon-carbon composite material with good conductivity has a low expansion rate and high specific capacity. As the negative electrode active substance of lithium-ion battery, it significantly improves the energy density and circulation performance of the battery.
Smart Images

Figure BDA0004261445760000181 
Figure BDA0004261445760000191 
Figure BDA0004261445760000201
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a silicon-carbon composite material and a preparation method thereof, a negative electrode sheet and a lithium ion battery. Background Art
[0002] The rapid development of the new energy vehicle industry has put forward higher requirements on the performance indicators of supporting power batteries, such as energy density, cycle life and safety performance. At present, most of the negative electrode materials of power batteries use graphite materials, which are difficult to meet market demand. As an emerging negative electrode material, silicon material has become the most promising negative electrode material because of its advantages such as high theoretical capacity (4200mAh / g), low lithium insertion platform and abundant resources. However, silicon materials will have a large-scale volume expansion (about 300%) during the lithium insertion process, resulting in structural pulverization of silicon materials and instability of the solid electrolyte interface (SEI), which ultimately leads to a decrease in lithium insertion capacity. In addition, the low conductivity of silicon will also affect its electrochemical performance.
[0003] Therefore, there is an urgent need to develop a silicon negative electrode material with good conductivity, low volume expansion rate and good cycle performance. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of poor conductivity, high volume expansion rate and poor cycle performance of silicon negative electrode materials in the prior art, and to provide a silicon-carbon composite material and a preparation method thereof, a negative electrode sheet and a lithium ion battery.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a silicon-carbon composite material, wherein the silicon-carbon composite material comprises a carbon matrix and a silicon-carbon composite layer coated on the carbon matrix;
[0006] Wherein, the content of silicon element in the silicon-carbon composite layer decreases from the inside to the outside.
[0007] A second aspect of the present invention provides a method for preparing a silicon-carbon composite material, wherein the method comprises: vapor depositing a silicon source and a carbon source on a carbon substrate, wherein the gas flow rate of the silicon source decreases over time, and the gas flow rate of the carbon source increases over time, so as to form a silicon-carbon composite layer in which the content of silicon element decreases from the inside to the outside, thereby obtaining a silicon-carbon composite material.
[0008] The third aspect of the present invention provides a silicon-carbon composite material obtained by the preparation method described in the second aspect.
[0009] A fourth aspect of the present invention provides a negative electrode sheet, comprising the silicon-carbon composite material provided by the present invention.
[0010] A fifth aspect of the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the negative electrode sheet provided by the present invention.
[0011] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0012] In the silicon-carbon composite material provided by the present invention, the carbon matrix provides attachment points for the deposition of silicon atoms and carbon atoms. At the same time, the carbon matrix and the carbon in the silicon-carbon composite layer build an internal conductive network for the silicon-carbon composite material, thereby increasing the conductivity of the silicon-carbon composite material.
[0013] In the silicon-carbon composite material provided by the present invention, silicon elements are distributed decreasingly from the inside to the outside in the silicon-carbon composite layer, that is, silicon elements are distributed decreasingly in the composite layer along the direction away from the matrix, which can increase the strength of the silicon-carbon composite layer and slowly release the influence of silicon lithium insertion reaction expansion on the overall particle structure of the silicon-carbon composite material.
[0014] Therefore, the silicon-carbon composite material provided by the present invention has good conductivity, low expansion rate and high specific capacity. When it is used as the negative electrode active material of a lithium ion battery, the lithium ion battery can have excellent energy density and cycle performance. DETAILED DESCRIPTION
[0015] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0016] A first aspect of the present invention provides a silicon-carbon composite material, the silicon-carbon composite material comprising a carbon matrix and a silicon-carbon composite layer coated on the carbon matrix;
[0017] Wherein, the content of silicon element in the silicon-carbon composite layer decreases from the inside to the outside.
[0018] In the present invention, the carbon matrix provides attachment points for the deposition of silicon atoms and carbon atoms. At the same time, the carbon matrix and the carbon in the silicon-carbon composite layer build an internal conductive network for the silicon-carbon composite material, thereby increasing the conductivity of the silicon-carbon composite material. The silicon element is distributed decreasingly from the inside to the outside in the silicon-carbon composite layer, that is, the silicon element is distributed decreasingly in the composite layer in a direction away from the matrix, thereby increasing the intensity of the lithium insertion reaction of the silicon-carbon composite layer, thereby slowing down the effect of silicon expansion on the overall particle structure of the silicon-carbon composite material.
[0019] In this silicon content decreasing distribution from the inside to the outside, the silicon element is mainly concentrated on the side of the silicon-carbon composite layer close to the carbon matrix, that is, from the side of the silicon-carbon composite layer close to the carbon matrix to the side far away from the carbon matrix, the silicon element content is distributed decreasingly, which effectively reduces its lithium insertion expansion rate by binding most of the silicon elements on the inside, thereby increasing the cycle performance of the silicon-carbon composite material.
[0020] In the present invention, "the silicon content in the silicon-carbon composite layer decreases from the inside to the outside" can be determined by measuring the silicon content at different locations of the silicon-carbon composite layer from the inside to the outside. The silicon-carbon composite layer is divided into five equal parts from the side close to the carbon substrate to the outside, and five points A, B, C, D and E are taken in sequence at the division points. Based on the total weight of the silicon-carbon composite layer, the silicon content at point A is 56-91wt%, the content at point B is 53-71wt%, the content at point C is 48-51wt%, the content at point D is 31-47wt%, and the content at point E is 11-46wt%.
[0021] The silicon-carbon composite material provided by the present invention has good electrical conductivity, low expansion rate and high specific capacity. When it is used as the negative electrode active material of a lithium ion battery, the lithium ion battery can have excellent energy density and cycle performance.
[0022] According to some embodiments of the present invention, the carbon matrix is selected from at least one of carbon nanotubes, graphene, carbon black and porous carbon. The types of the carbon matrix can be used alone or in combination, and those skilled in the art can select according to actual needs.
[0023] It is understandable that the carbon matrix can be carbon nanotubes, which can provide an internal one-dimensional conductive network for the silicon-carbon composite material; the carbon matrix can be graphene, which can provide an internal two-dimensional conductive network for the silicon-carbon composite material; the carbon matrix can be carbon black, which can provide an internal dispersed zero-dimensional conductive network for the silicon-carbon composite material; the carbon matrix can be porous carbon, and the high specific surface area and rich pore structure of porous carbon can provide rich sites and a three-dimensional conductive network for the deposition of silicon sources and carbon sources. The carbon matrix can also be a structure in which carbon nanotubes, graphene, carbon black and porous carbon are mixed in any proportion. It is understandable that the length of the carbon nanotubes is 10-200nm, and the maximum width of the graphene sheet diameter is 50-200nm.
[0024] According to some preferred embodiments of the present invention, the carbon matrix is porous carbon, and the average particle size (D 50) is 2-8μm, preferably 4-6μm. If the average particle size of the porous carbon is too small, silicon is easily deposited on the surface of the porous carbon during the silicon deposition process, resulting in silicon-rich porous carbon surface, which is not conducive to the dispersion of silicon elements, and there are many side reactions on the surface of the material, resulting in serious performance degradation. If the size of the porous carbon is too large, the deposition process of the silicon-carbon composite layer takes a long time. In addition, it will also cause the silicon-carbon composite particles to be too large, and the lithium insertion path is long, which is not conducive to the utilization of the silicon-carbon composite material.
[0025] According to some preferred embodiments of the present invention, the silicon in the silicon-carbon composite layer includes amorphous silicon and optional silicon grains. Amorphous silicon is isotropic, and when amorphous silicon undergoes lithium insertion reaction, the stress generated is small, the structure is relatively stable, and the volume expansion rate is low.
[0026] According to some preferred embodiments of the present invention, the silicon-carbon composite layer further comprises silicon grains, and the average grain size (D 50 ) is less than 8nm, preferably less than 3nm. In the present invention, if the size of silicon grains is too large, it will lead to serious expansion of silicon embedded with lithium, increase the expansion of negative electrode sheets, and poor cycle performance.
[0027] According to some preferred embodiments of the present invention, based on the total amount of the silicon-carbon composite material, the total content of amorphous silicon and optional silicon grains in the silicon-carbon composite layer is 20-40wt%, for example, 20wt%, 23wt%, 25wt%, 30wt%, 35wt%, 37wt%, 40wt%, and any value within the range of any two of the above values, preferably 25-35wt%.
[0028] The content of carbon element in the silicon-carbon composite layer increases from the inside to the outside.
[0029] According to some embodiments of the present invention, the carbon in the silicon-carbon composite layer is amorphous carbon. The carbon lattice in amorphous carbon is disordered, which helps to alleviate the lattice change caused by lithium ion embedding and ensure the structural stability of the carbon.
[0030] According to some preferred embodiments of the present invention, based on the total amount of the silicon-carbon composite material, the content of amorphous carbon in the silicon-carbon composite layer is 20-40wt%, for example, 20wt%, 23wt%, 25wt%, 30wt%, 35wt%, 37wt%, 40wt%, and any value within the range of any two of the above values, preferably 25-35wt%.
[0031] Both silicon and carbon can be used as carriers for lithium ion storage, providing energy density for lithium ion batteries. Among them, silicon has a higher theoretical specific capacity, but its conductivity and cycle stability are poor; carbon has a lower specific capacity than silicon, but its conductivity and cycle stability are good. In addition, the presence of carbon can effectively alleviate the problem of silicon being easily oxidized. The present invention further optimizes the specific capacity and cycle stability of the silicon-carbon composite material by controlling the content of silicon (amorphous silicon and optional silicon grains) and the content of carbon (amorphous carbon) within a suitable range.
[0032] According to some preferred embodiments of the present invention, the silicon-carbon composite material further includes a carbon coating layer coated outside the silicon-carbon composite layer, which can prevent silicon from being exposed on the surface of the material, resulting in poor performance.
[0033] According to some preferred embodiments of the present invention, the thickness of the carbon coating layer is 5-100nm, for example, 5nm, 10nm, 30nm, 50nm, 80nm, 100nm, and any value within the range of any two of the above values, preferably 10-30nm. In the present invention, if the thickness of the carbon coating layer is too small, there will be a risk of uneven coating and incomplete coating; if the thickness of the carbon coating layer is too large and the preparation reaction time is too long, it will increase the size of the silicon grains and increase the risk of side reactions in the carbon layer.
[0034] According to some preferred embodiments of the present invention, the average particle size (D 50 ) is 3-15 μm, for example, 3 μm, 5 μm, 7 μm, 9 μm, 11 μm, 13 μm, 15 μm, and any value within the range of any two of the above values, preferably 5-10 μm. In the present invention, the average particle size (D 50 ) is too small, the material specific surface area is high, there are more surface side reactions, and the cycle performance is poor; if the average particle size is too large, the diffusion distance of lithium ions in the silicon-carbon composite material will increase, some silicon will not be fully reacted, and the utilization rate will be low; at the same time, the silicon-carbon composite material within this particle size range can also increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the battery.
[0035] In the present invention, the content of silicon in the silicon-carbon composite layer outside the carbon matrix is distributed decreasingly from the inside to the outside, so that the performance of the lithium-ion battery can be stable during the cycle and storage process. The selection of amorphous silicon and amorphous carbon can reduce the material expansion rate and improve the cycle performance. By controlling the content of amorphous silicon and optional silicon grains and the content of amorphous carbon, a silicon-carbon composite material with better performance can be obtained.
[0036] A second aspect of the present invention provides a method for preparing a silicon-carbon composite material, wherein the method comprises: vapor depositing a silicon source and a carbon source on a carbon substrate, wherein the gas flow rate of the silicon source decreases over time, and the gas flow rate of the carbon source increases over time, so as to form a silicon-carbon composite layer in which the content of silicon element decreases from the inside to the outside, thereby obtaining a silicon-carbon composite material.
[0037] In the present invention, the method is simple, fast, and easy to operate, and can obtain a silicon-carbon composite material with good structural stability, while also making the distribution state of the silicon element inside the silicon-carbon composite layer controllable.
[0038] The present invention utilizes silicon source and carbon source to form a silicon-carbon composite layer on the surface of a carbon matrix through chemical reaction. In this process, the silicon source and carbon source diffuse to the surface of the carbon matrix, and are deposited, cracked (or cracked first and then deposited) and atoms are rearranged on the surface of the carbon matrix to generate corresponding silicon nuclei and carbon nuclei. The nuclei grow and connect with each other to form an amorphous structure.
[0039] According to some preferred embodiments of the present invention, the gas flow rate of the silicon source decreases uniformly over time, and the gas flow rate of the carbon source increases uniformly over time. This can make the distribution of silicon and carbon elements in the silicon-carbon composite layer more uniform, and can form a silicon-carbon composite layer in which the content of silicon and carbon elements is uniformly distributed from the inside to the outside.
[0040] Furthermore, the gas flow rate of the silicon source decreases uniformly over time at a rate of change of 0.056-0.333 sccm / min, and the gas flow rate of the carbon source increases uniformly over time at a rate of change of 0.056-0.333 sccm / min.
[0041] The gas flow rate of the silicon source and the carbon source determines the probability of contact with the carbon matrix, and further determines the number of deposition nucleation sites. The greater the gas flow rate, the greater the probability of contact with the carbon matrix, the more corresponding deposition nucleation sites are generated, and the more corresponding silicon or carbon elements are generated. It can be understood that when the gas flow rate of the silicon source is greater than the gas flow rate of the carbon source, the greater the possibility of the silicon source diffusing to the surface of the carbon matrix, the more silicon deposition nucleation sites are formed on the surface of the carbon matrix, and the more silicon content is generated.
[0042] Therefore, the key point of the present invention is to control the gas flow rate of the silicon source and the carbon source to increase the probability of contacting with the carbon matrix or itself after cracking, and regulate their distribution state.
[0043] For example, monosilane as a silicon source decomposes into silicon atoms, and ethylene as a carbon source decomposes into carbon atoms. After the silicon atoms and carbon atoms are deposited on the carbon substrate, a silicon-carbon composite layer is formed in which the contents of silicon and carbon elements are independently distributed from the inside to the outside.
[0044] According to some preferred embodiments of the present invention, the ratio of the gas flow rates of the silicon source and the carbon source changes from 8-17:1 to 1:8-17 evenly over time. Within this ratio range, it is favorable for the silicon content to be distributed decreasingly from the inside to the outside, so as to achieve the aforementioned situation of measuring the silicon content at different locations of the silicon-carbon composite layer from the inside to the outside (see the aforementioned five-equal-division measurement). If the ratio of the gas flow rates of the silicon source and the carbon source is too small, the decreasing distribution trend of the silicon content from the inside to the outside is not obvious, and the difference between the silicon content inside and outside is small, the effect cannot be achieved, and the performance is poor; if the ratio of the gas flow rates of the silicon source and the carbon source is too large, the decreasing distribution trend of the silicon content from the inside to the outside is more obvious, and the difference between the silicon content inside and outside is larger, resulting in uneven distribution of lithium-embedded stress in the material and unstable material structure.
[0045] According to some embodiments of the present invention, the silicon source is selected from at least one of monosilane, disilane, trisilane, silicon chloride, silicon trichloride, hexachlorodisilane and dichlorosilane.
[0046] According to some preferred embodiments of the present invention, the carbon source is selected from at least one of acetylene, methane, ethane, ethylene, carbon monoxide and carbon dioxide.
[0047] According to some preferred embodiments of the present invention, the temperature of the vapor deposition is 300-700° C., for example, 300° C., 400° C., 500° C., 600° C., 700° C., and any value within the range of any two of the above values, preferably 400-600° C. In the present invention, if the temperature of the vapor deposition is too high, the silicon grains will grow and the crystallinity will increase, which is not conducive to the cycle performance of the silicon-carbon material; if the temperature of the vapor deposition is too low, the carbon source cracking efficiency will be low, resulting in poor product quality.
[0048] According to some preferred embodiments of the present invention, the gas flow rates of the silicon source and the carbon source are independently 1-90sccm, such as 1sccm, 5sccm, 10sccm, 25sccm, 40sccm, 50sccm, 60sccm, 75sccm, 80sccm, 85sccm, 90sccm, and any value within the range of any two of the above values, preferably 5-85sccm. In the present invention, if the gas flow rates of the silicon source and the carbon source are too small, the deposition rate will be slow and the reaction time will be too long; if the gas flow rates of the silicon source and the carbon source are too large, the gas will be carried away by the gas flow before it has time to contact the carbon matrix, thereby resulting in insufficient atomic deposition after gas cracking.
[0049] According to some preferred embodiments of the present invention, the ventilation time of the silicon source and the carbon source is 250-500 min, for example, 250 min, 280 min, 320 min, 350 min, 380 min, 410 min, 450 min, 475 min, 500 min, and any value within the range of any two of the above values, preferably 300-400 min. In the present invention, if the ventilation time of the silicon source and the carbon source is too short, the particles generated after deposition are too small; if the ventilation time of the silicon source and the carbon source is too long, the particles generated after deposition are too large.
[0050] According to some preferred embodiments of the present invention, the silicon source and the carbon source are introduced together with the carrier gas. According to some preferred embodiments of the present invention, the ratio of the flow rate of the carrier gas to the gas flow rate of the silicon source or the carbon source is 4-5.5:1, such as 4:1, 4.2:1, 4.5:1, 4.8:1, 5:1, 5.2:1, 5.5:1, and any value within the range of any two of the above values, preferably 4-5:1. In the present invention, if the flow rate of the carrier gas is too small, it will lead to a slow deposition rate and a long reaction time; if the flow rate of the carrier gas is too large, it will lead to a low gas cracking efficiency and insufficient atomic deposition after cracking.
[0051] According to some embodiments of the present invention, a silicon source and a carbon source are vapor-deposited on a carbon substrate, and then vapor-phase carbon coating is performed to form a carbon coating layer.
[0052] According to some preferred embodiments of the present invention, the gas-phase carbon-coated carbon source is selected from at least one of methane, ethylene, acetylene, propane and propylene.
[0053] According to some preferred embodiments of the present invention, the temperature of the gas-phase carbon coating is 600-1200°C, such as 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, and any value within the range of any two of the above values, preferably 800-1000°C; the time is 50-500min, such as 50min, 100min, 150min, 200min, 250min, 300min, 350min, 400min, 450min, 500min, and any value within the range of any two of the above values, preferably 100-400min. In the present invention, if the temperature of the gas-phase carbon coating is too low, the carbon source cannot be completely cracked at too low a temperature; if the temperature of the gas-phase carbon coating is too high, the silicon grains will grow and the crystallinity will increase. If the gas phase carbon coating time is too short, the carbon content will be low and there will be a risk of incomplete coating; if the gas phase carbon coating time is too long, the thickness of the coated carbon layer will increase and the side reactions will increase.
[0054] According to some preferred embodiments of the present invention, the gas flow rate of the carbon source coated with gas phase carbon is 5-60sccm, for example, 5sccm, 10sccm, 15sccm, 20sccm, 25sccm, 30sccm, 35sccm, 40sccm, 45sccm, 50sccm, 55sccm, 60sccm, and any value within the range of any two of the above values, preferably 10-50sccm. In the present invention, if the gas flow rate of the carbon source is too small, the carbon content may be low, there may be a risk of incomplete coating or the coating time may be too long; if the gas flow rate of the carbon source is too large, the carbon atoms after the cracking of the carbon source may not be effectively deposited, the synthesis efficiency may be low, and the raw materials may be wasted.
[0055] According to some embodiments of the present invention, the carbon matrix is selected from at least one of carbon nanotubes, graphene, carbon black and porous carbon, preferably porous carbon.
[0056] According to some preferred embodiments of the present invention, the silicon in the silicon-carbon composite layer includes amorphous silicon and optional silicon grains.
[0057] According to some preferred embodiments of the present invention, the average particle size (D 50 ) is less than 8 nm, preferably less than 3 nm.
[0058] According to some preferred embodiments of the present invention, the carbon in the silicon-carbon composite layer is amorphous carbon.
[0059] According to some preferred embodiments of the present invention, the thickness of the carbon coating layer is 5-100 nm, preferably 10-30 nm.
[0060] According to some preferred embodiments of the present invention, the average particle size of the silicon-carbon composite material is 3-15 μm, preferably 5-10 μm.
[0061] According to some preferred embodiments of the present invention, the average particle size (D 50 ) is 2-8μm, preferably 4-6μm.
[0062] According to some preferred embodiments of the present invention, the content of amorphous silicon and optional silicon grains in the silicon-carbon composite layer is 20-40 wt %, preferably 25-35 wt %, based on the total amount of the silicon-carbon composite material.
[0063] According to some preferred embodiments of the present invention, based on the total amount of the silicon-carbon composite material, the content of amorphous carbon in the silicon-carbon composite layer is 20-40 wt %, preferably 25-35 wt %.
[0064] The present invention can obtain a silicon-carbon composite material comprising a carbon matrix and a silicon-carbon composite layer through the above-mentioned preparation method. The content of silicon element in the silicon-carbon composite layer is distributed decreasingly from the inside to the outside, which can make the structure of the lithium-ion battery stable during the cycle and storage process, and obtain excellent charge and discharge performance and cycle performance.
[0065] According to a particularly preferred embodiment of the present invention, a method for preparing a silicon-carbon composite material comprises first vapor-depositing a silicon source and a carbon source on a carbon substrate, wherein the gas flow rate of the silicon source decreases uniformly over time, and the gas flow rate of the carbon source increases uniformly over time, so as to form a silicon-carbon composite layer in which the content of silicon element decreases from the inside to the outside, and then vapor-phase carbon coating is performed to form a carbon coating layer to obtain a silicon-carbon composite material;
[0066] The ratio of the gas flow rates of the silicon source and the carbon source changes evenly from 8-17:1 to 1:8-17 over time;
[0067] The silicon source is selected from at least one of monosilane, disilane, trisilane, silicon chloride, silicon trichloride, hexachlorodisilane and dichlorosilane; the carbon source is selected from at least one of acetylene, methane, ethane, ethylene, carbon monoxide and carbon dioxide;
[0068] The temperature of the vapor deposition is 400-600°C;
[0069] The gas flow rates of the silicon source and the carbon source are independently 5-85 sccm; the ventilation time of the silicon source and the carbon source is 300-400 min;
[0070] The silicon source and the carbon source are introduced together with the carrier gas; the ratio of the flow rate of the carrier to the flow rate of the silicon source or the carbon source gas is 4-5.5:1;
[0071] The carbon source of the gas-phase carbon coating is selected from at least one of methane, ethylene, acetylene, propane and propylene; the temperature of the gas-phase carbon coating is 800-1000°C; the time is 100-400min; the gas flow rate of the carbon source of the gas-phase carbon coating is 10-50sccm.
[0072] The third aspect of the present invention provides a silicon-carbon composite material obtained by the preparation method described in the second aspect.
[0073] A fourth aspect of the present invention provides a negative electrode sheet, comprising the silicon-carbon composite material provided by the present invention.
[0074] A fifth aspect of the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the negative electrode sheet provided by the present invention.
[0075] In a preferred embodiment of the present invention, the coulombic efficiency of the lithium ion battery is 82.5-91.5%, the expansion rate after 50 cycles is 25-55%, and the capacity retention rate after 100 cycles is 30-70%.
[0076] In other preferred embodiments of the present invention, the coulombic efficiency of the lithium ion battery is 85.5-89.5%, the expansion rate after 50 cycles is 28-48%, and the capacity retention rate after 100 cycles is 45-65%.
[0077] In a more preferred embodiment of the present invention, the coulombic efficiency of the lithium ion battery is 88.5-89.5%, the expansion rate after 50 cycles is 28-31%, and the capacity retention rate after 100 cycles is 60-65%.
[0078] Using the silicon-carbon composite material of the present invention as the negative electrode active material of a lithium-ion battery can enable the lithium-ion battery to obtain excellent charge-discharge performance and cycle performance.
[0079] The present invention will be described in detail below through examples.
[0080] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.
[0081] Among them, the test methods for various parameters in silicon-carbon composite materials are as follows:
[0082] The size of silicon grains: According to the refined XRD pattern of the silicon-carbon composite material, the size of silicon grains is calculated using the Scherrer formula, which is: D = Kγ / (Bcosθ), where K is the Scherrer constant, D is the grain size, B is the half-peak width of the diffraction peak of the measured sample, θ is the Bragg angle, and γ is the X-ray wavelength.
[0083] The method for determining the carbon content and silicon content in the silicon-carbon composite layer is as follows: the content of the carbon matrix is weighed and determined before deposition; the silicon-carbon composite material before carbon coating is oxidized by oxygen at high temperature in a combustion furnace, and carbon dioxide is produced after carbon oxidation. The carbon content is determined by a carbon detection device. The carbon content determined by the device is the sum of the carbon content in the carbon matrix and the silicon-carbon composite layer. The carbon content in the silicon-carbon composite layer is calculated by subtracting the carbon content of the carbon matrix from the carbon content determined by the device. The silicon-carbon composite material is composed of silicon, carbon and oxygen elements, wherein the oxygen content is extremely trace (≤2wt%). For simplicity, the oxygen content is ignored, and the silicon content is obtained by subtracting the carbon content from the total amount of the silicon-carbon composite material.
[0084] Carbon coating thickness: The coating of the silicon-carbon composite material was observed using a transmission electron microscope (TEM), and the coating thickness was calculated based on the magnification and scale.
[0085] Particle size: Samples were treated before testing and ultrasonically dispersed in anhydrous ethanol for 5 minutes at an ultrasonic frequency of 59kHz and a power of 45W. The test was carried out in industrial ethanol as the dispersion medium. The irradiation path / volume of the laser particle size analyzer was 25cm / 200mL. The average particle size of the silicon-carbon composite material, i.e., D50, was tested.
[0086] Test button battery performance, the test method is as follows:
[0087] Charge and discharge performance test: Using LANHE blue battery test equipment, the button battery was discharged to 0.005V at a constant current of 0.1C at room temperature, and then charged to 1.5V at a constant current of 0.1C, and the first discharge capacity and first charge capacity of the battery were recorded. Coulomb efficiency (%) = first charge capacity / first discharge capacity × 100%.
[0088] Expansion test: Before assembling button cells, the original thickness of the electrode of each sample group was measured with a micrometer. After 50 cycles, the battery was discharged to 0% SOC, the battery was disassembled, the negative electrode was taken out, and cleaned with DMC solution, and the thickness was tested after drying, and the expansion rate was calculated. Expansion rate (%) = (thickness of the electrode after the cycle - original thickness of the electrode) / original thickness of the electrode × 100%.
[0089] Cycle performance test: Discharge the button battery at room temperature at a constant current of 0.1C to 0.005V, then charge it at a constant current of 0.1C to 1.5V. After 100 cycles, record the remaining capacity of the battery.
[0090] Example 1
[0091] This example is used to illustrate the preparation of a silicon-carbon composite material.
[0092] (1) Average particle size (D 50 ) is a porous carbon with a diameter of 4.8μm as the carbon matrix, and monosilane and ethylene are continuously introduced into a vacuum rotary furnace, wherein the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene gradually and evenly changes from 12:1 to 1:12. At the beginning of the introduction, the gas flow rate of monosilane is 60sccm, and the gas flow rate of ethylene is 5sccm; at the end, the gas flow rate of monosilane is 5sccm, the gas flow rate of ethylene is 60sccm, and the ventilation time is 360min; the gas flow rate of monosilane decreases uniformly over time at a rate of 0.153sccm / min, and the gas flow rate of ethylene increases uniformly over time at a rate of 0.153sccm / min. During the introduction of monosilane and ethylene, nitrogen gas is continuously introduced as a carrier gas, wherein the flow rate of nitrogen gas is 5 times the gas flow rate of monosilane or ethylene;
[0093] (2) Monosilane and ethylene are thermally decomposed in a vacuum rotary kiln, wherein monosilane decomposes into silicon atoms and ethylene decomposes into carbon atoms, and the silicon atoms and carbon atoms are deposited on the porous carbon to form a silicon-carbon composite layer in which the content of silicon element decreases from the inside to the outside; wherein the speed of the vacuum rotary kiln is 8° / min, the temperature in the kiln is 500°C, and the inclination angle of the rotary kiln is 15°;
[0094] (3) Outside the silicon-carbon composite layer, methane and acetylene (mass ratio of 1:1) are used as carbon sources for gas phase carbon coating to form a carbon coating layer, wherein the coating temperature is 900°C, the time is 300 min, and the gas flow rate of the carbon source is 20 sccm, thereby obtaining a silicon-carbon composite material.
[0095] Example 2
[0096] A silicon-carbon composite material was prepared according to the method of Example 1, except that the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene gradually and evenly changed from 16:1 to 1:16. At the beginning of the introduction, the gas flow rate of monosilane was 80 sccm, and the gas flow rate of ethylene was 5 sccm; at the end, the gas flow rate of monosilane was 5 sccm, and the gas flow rate of ethylene was 80 sccm; the gas flow rate of monosilane decreased uniformly over time at a rate of change of 0.208 sccm / min, and the gas flow rate of ethylene increased uniformly over time at a rate of change of 0.208 sccm / min. A silicon-carbon composite material was obtained.
[0097] Example 3
[0098] A silicon-carbon composite material was prepared according to the method of Example 1, except that the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene gradually and evenly changed from 8:1 to 1:8. At the beginning of the introduction, the gas flow rate of monosilane was 40 sccm, and the gas flow rate of ethylene was 5 sccm; at the end, the gas flow rate of monosilane was 5 sccm, and the gas flow rate of ethylene was 40 sccm; the gas flow rate of monosilane decreased uniformly over time at a rate of change of 0.097 sccm / min, and the gas flow rate of ethylene increased uniformly over time at a rate of change of 0.097 sccm / min. A silicon-carbon composite material was obtained.
[0099] Example 4
[0100] The silicon-carbon composite material was prepared according to the method of Example 1, except that the temperature of the vapor deposition was different. Specifically, in step (2), the temperature in the furnace was 620° C. to obtain the silicon-carbon composite material.
[0101] Example 5
[0102] The silicon-carbon composite material was prepared according to the method of Example 1, except that the temperature of the vapor deposition was different. Specifically, in step (2), the temperature in the furnace was 380° C. to obtain the silicon-carbon composite material.
[0103] Example 6
[0104] The silicon-carbon composite material was prepared according to the method of Example 1, except that in step (3), the coating temperature was 1100° C. to obtain a silicon-carbon composite material.
[0105] Example 7
[0106] The silicon-carbon composite material was prepared according to the method of Example 1, except that in step (3), the coating temperature was 700° C. to obtain a silicon-carbon composite material.
[0107] Example 8
[0108] A silicon-carbon composite material was prepared according to the method of Example 1, except that the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene gradually and evenly changed from 25:1 to 1:25. At the beginning of the introduction, the gas flow rate of monosilane was 125 sccm, and the gas flow rate of ethylene was 5 sccm; at the end, the gas flow rate of monosilane was 5 sccm, and the gas flow rate of ethylene was 125 sccm; the gas flow rate of monosilane decreased uniformly over time at a rate of change of 0.333 sccm / min, and the gas flow rate of ethylene increased uniformly over time at a rate of change of 0.333 sccm / min. A silicon-carbon composite material was obtained.
[0109] Example 9
[0110] A silicon-carbon composite material was prepared according to the method of Example 1, except that the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene gradually and evenly changed from 5:1 to 1:5. At the beginning of the introduction, the gas flow rate of monosilane was 25 sccm, and the gas flow rate of ethylene was 5 sccm; at the end, the gas flow rate of monosilane was 5 sccm, and the gas flow rate of ethylene was 25 sccm; the gas flow rate of monosilane decreased uniformly over time at a rate of change of 0.056 sccm / min, and the gas flow rate of ethylene increased uniformly over time at a rate of change of 0.056 sccm / min. A silicon-carbon composite material was obtained.
[0111] Example 10
[0112] The silicon-carbon composite material was prepared according to the method of Example 1, except that the temperature of the vapor deposition was different. Specifically, in step (2), the temperature in the furnace was 750° C. to obtain the silicon-carbon composite material.
[0113] Embodiment 11
[0114] The silicon-carbon composite material was prepared according to the method of Example 1, except that the temperature of the vapor deposition was different. Specifically, in step (2), the temperature in the furnace was 250° C. to obtain the silicon-carbon composite material.
[0115] Example 12
[0116] The silicon-carbon composite material was prepared according to the method of Example 1, except that in step (3), the coating temperature was 1300° C. to obtain a silicon-carbon composite material.
[0117] Embodiment 13
[0118] The silicon-carbon composite material was prepared according to the method of Example 1, except that in step (3), the coating temperature was 500° C. to obtain a silicon-carbon composite material.
[0119] Embodiment 14
[0120] The silicon-carbon composite material was prepared according to the method of Example 1, except that step (3) was not performed, that is, the silicon-carbon composite material was not carbon-coated, to obtain a silicon-carbon composite material.
[0121] Comparative Example 1
[0122] A silicon-carbon composite material was prepared according to the method of Example 14, except that in step (1), the gas flow rate of monosilane was 60 sccm, the gas flow rate of ethylene was 0 sccm, the ventilation time was 180 min, and the gas flow rate remained unchanged during the process; then the gas flow rate was adjusted to make the gas flow rate of monosilane 0 sccm, the gas flow rate of ethylene 60 sccm, the ventilation time was 180 min, and the gas flow rate remained unchanged during the process. A silicon-carbon composite material was obtained.
[0123] Comparative Example 2
[0124] A silicon-carbon composite material was prepared according to the method of Example 14, except that in step (1), the gas flow rate of monosilane was 0 sccm, the gas flow rate of ethylene was 60 sccm, the ventilation time was 180 min, and the gas flow rate remained unchanged during this process; then the gas flow rate was adjusted to make the gas flow rate of monosilane 60 sccm, the gas flow rate of ethylene 0 sccm, the ventilation time was 180 min, and the gas flow rate remained unchanged during this process. A silicon-carbon composite material was obtained.
[0125] Comparative Example 3
[0126] The silicon-carbon composite material was prepared according to the method of Example 14, except that the gas flow rates of monosilane and ethylene remained unchanged during the entire vapor deposition process, wherein the gas flow rates of monosilane and ethylene were both 30 sccm, and the ventilation time was 360 min. A silicon-carbon composite material was obtained.
[0127] The silicon element and the carbon element are evenly distributed in the silicon-carbon composite layer of the silicon-carbon composite material.
[0128] Comparative Example 4
[0129] A silicon-carbon composite material was prepared according to the method of Example 14, except that monosilane and ethylene were introduced periodically. Specifically, in step (1), monosilane was introduced first, with a gas flow rate of 60 sccm and a ventilation time of 10 min, and the gas flow rate remained unchanged during the ventilation process; then ethylene was introduced, with a gas flow rate of 60 sccm and a ventilation time of 10 min, and the gas flow rate remained unchanged during the ventilation process; the above process was repeated 20 times. A silicon-carbon composite material was obtained.
[0130] After silicon atoms and carbon atoms are deposited on the porous carbon, a silicon-carbon composite layer is formed in which silicon element layers and carbon element layers are periodically distributed.
[0131] Comparative Example 5
[0132] A silicon-carbon composite material was prepared according to the method of Example 14, except that in step (1), the gas flow rate of monosilane increased uniformly over time, and the gas flow rate of ethylene decreased uniformly over time, wherein the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene gradually and uniformly changed from 1:12 to 12:1. At the beginning of the introduction, the gas flow rate of monosilane was 5 sccm, and the gas flow rate of ethylene was 60 sccm; at the end, the gas flow rate of monosilane was 60 sccm, the gas flow rate of ethylene was 5 sccm, and the ventilation time was 360 min; the gas flow rate of monosilane increased uniformly over time at a rate of change of 0.153 sccm / min, and the gas flow rate of ethylene decreased uniformly over time at a rate of change of 0.153 sccm / min. A silicon-carbon composite material was obtained.
[0133] After silicon atoms and carbon atoms are deposited on the porous carbon, a silicon-carbon composite layer is formed in which the content of silicon elements increases from the inside to the outside, and the content of carbon elements decreases from the inside to the outside.
[0134] The parameters of the silicon-carbon composite materials obtained in each embodiment and comparative example are shown in Table 1.
[0135] Table 1
[0136]
[0137] Note: “-” means the parameter does not exist;
[0138] The silicon content is the total content of amorphous silicon and silicon grains;
[0139] The carbon content and silicon content in the silicon-carbon composite layer are both based on the total weight of the silicon-carbon composite material.
[0140] Test Example 1
[0141] The distribution of silicon in the silicon-carbon composite layer of each embodiment and comparative example was characterized by performing an X-ray energy spectrum (EDS) test on the cross section of the silicon-carbon composite material particles of each embodiment and comparative example. The test position is: taking the silicon-carbon composite layer as the reference, dividing it into five equal parts from the side close to the carbon matrix outward, and taking five points (A, B, C, D and E) at the division in sequence, and testing the silicon content respectively. The test results are shown in Table 2.
[0142] Table 2
[0143]
[0144] Test Example 2
[0145] The silicon-carbon composite material obtained in each embodiment and comparative example was used as the negative electrode active material, and acetylene black and sodium carboxymethyl cellulose were mixed uniformly at a mass ratio of 8:1:1, and then coated on a copper foil to obtain a negative electrode sheet; a metal lithium sheet was used as a counter electrode, and a PE / PP composite film was used as a separator, and a button battery was made by a conventional method in the art. The charge and discharge performance, expansion rate and cycle performance of the button battery were tested respectively, and the test results are shown in Table 3.
[0146] Table 3
[0147]
[0148] It can be seen from the results in Table 3 that the content of silicon in the silicon-carbon composite layer in the silicon-carbon composite materials prepared in Examples 1-14 of the present invention is distributed decreasingly from the inside to the outside, and the button batteries prepared using the silicon-carbon composite materials prepared in Examples 1-14 as the negative electrode active material have higher coulombic efficiency, lower expansion rate, and better cycle performance. The distribution of silicon and carbon elements in the silicon-carbon composite layer in the silicon-carbon composite material obtained in comparative example 1 is as follows: the inner layer is a silicon element layer and the outer layer is a carbon element layer; the distribution of silicon and carbon elements in the silicon-carbon composite layer in the silicon-carbon composite material obtained in comparative example 2 is as follows: the inner layer is a carbon element layer and the outer layer is a silicon element layer; the silicon and carbon elements in the silicon-carbon composite layer in the silicon-carbon composite material obtained in comparative example 3 are uniformly distributed; the silicon element layer and the carbon element layer in the silicon-carbon composite layer in the silicon-carbon composite material obtained in comparative example 4 are periodically distributed; the content of silicon in the silicon-carbon composite layer in the silicon-carbon composite material obtained in comparative example 5 is distributed increasing from the inside to the outside, and the button battery prepared with the silicon-carbon composite material obtained in comparative examples 1-5 as the negative electrode active material has significantly reduced coulomb efficiency and capacity retention rate after 100 cycles, and significantly increased expansion rate. This shows that when the content of silicon in the silicon-carbon composite layer in the silicon-carbon composite material is distributed decreasingly from the inside to the outside, the button battery prepared has excellent charge and discharge performance and cycle performance, and has a lower expansion rate. Among them, the button-type battery prepared by using the silicon-carbon composite material obtained in Examples 1-3 of the present invention as the negative electrode active material has the best performance, with a coulombic efficiency of more than 88%, an expansion rate of less than 38%, and a capacity retention rate of more than 55% after 100 cycles.
[0149] In addition, Examples 4, 5, 10 and 11 changed the temperature of vapor deposition, and Examples 6, 7, 12 and 13 changed the temperature of carbon coating. Compared with Example 1, the coulombic efficiency and capacity retention rate of the button battery obtained after 100 cycles were reduced; the silicon-carbon composite material of Example 14 was not carbon coated, and compared with Example 1, the coulombic efficiency and capacity retention rate of the button battery obtained after 100 cycles were reduced, and the expansion rate increased; Examples 8 and 9 changed the ratio of the gas flow rate of monosilane to the gas flow rate of ethylene, and compared with Example 1, the coulombic efficiency and capacity retention rate of the button battery obtained after 100 cycles were reduced. This shows that carbon coating of silicon-carbon composite materials and selecting appropriate vapor deposition temperature, carbon coating temperature, and the ratio of gas flow rates of silicon source and carbon source can make the button battery obtained from the silicon-carbon composite material have better charge and discharge performance and cycle performance, as well as lower expansion rate.
[0150] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A silicon-carbon composite material, It is characterized in that The silicon-carbon composite material comprises a carbon matrix and a silicon-carbon composite layer coated on the carbon matrix; Wherein, the content of silicon element in the silicon-carbon composite layer decreases from the inside to the outside.
2. The silicon-carbon composite material according to claim 1, in, The carbon matrix is selected from at least one of carbon nanotubes, graphene, carbon black and porous carbon, preferably porous carbon; Preferably, the average particle size of the porous carbon is 2-8 μm, preferably 4-6 μm.
3. The silicon-carbon composite material according to claim 1 or 2, in, The silicon in the silicon-carbon composite layer includes amorphous silicon and optional silicon grains; Preferably, the average particle size of the silicon grains is less than 8 nm, preferably less than 3 nm; Preferably, based on the total amount of the silicon-carbon composite material, the total content of amorphous silicon and optional silicon grains in the silicon-carbon composite layer is 20-40 wt %, preferably 25-35 wt %.
4. The silicon-carbon composite material according to any one of claims 1 to 3, in, The carbon in the silicon-carbon composite layer is amorphous carbon; Preferably, based on the total amount of the silicon-carbon composite material, the content of amorphous carbon in the silicon-carbon composite layer is 20-40 wt %, preferably 25-35 wt %.
5. The silicon-carbon composite material according to any one of claims 1 to 4, in, The silicon-carbon composite material further includes a carbon coating layer coated outside the silicon-carbon composite layer; Preferably, the thickness of the carbon coating layer is 5-100 nm, preferably 10-30 nm; Preferably, the average particle size of the silicon-carbon composite material is 3-15 μm, preferably 5-10 μm.
6. A method for preparing a silicon-carbon composite material, It is characterized in that The method comprises: vapor-depositing a silicon source and a carbon source on a carbon substrate, wherein the gas flow rate of the silicon source decreases over time, and the gas flow rate of the carbon source increases over time, so as to form a silicon-carbon composite layer in which the content of silicon element decreases from the inside to the outside, thereby obtaining a silicon-carbon composite material; Preferably, the gas flow rate of the silicon source decreases uniformly over time, and the gas flow rate of the carbon source increases uniformly over time.
7. The preparation method according to claim 6, in, During the vapor deposition process, the gas flow rate ratio of the silicon source and the carbon source changes uniformly from 8-17:1 to 1:8-17 over time.
8. The preparation method according to claim 6 or 7, in, The silicon source is selected from at least one of monosilane, disilane, trisilane, silicon chloride, silicon trichloride, hexachlorodisilane and dichlorosilane; Preferably, the carbon source is selected from at least one of acetylene, methane, ethane, ethylene, carbon monoxide and carbon dioxide; Preferably, the temperature of the vapor deposition is 300-700°C, preferably 400-600°C; Preferably, the gas flow rates of the silicon source and the carbon source are each independently 1-90 sccm, preferably 5-85 sccm; Preferably, the ventilation time of the silicon source and the carbon source is 250-500 min, preferably 300-400 min; Preferably, the silicon source and the carbon source are introduced together with the carrier gas respectively; Preferably, the ratio of the flow rate of the carrier gas to the flow rate of the silicon source or carbon source gas is 4-5.5:
1.
9. The preparation method according to any one of claims 6 to 8, in, After vapor deposition of a silicon source and a carbon source on a carbon substrate, vapor phase carbon coating is performed to form a carbon coating layer; Preferably, the carbon source for gas-phase carbon coating is selected from at least one of methane, ethylene, acetylene, propane and propylene; Preferably, the temperature of the gas phase carbon coating is 600-1200°C, preferably 800-1000°C; the time is 50-500min, preferably 100-400min; Preferably, the gas flow rate of the gas-phase carbon-coated carbon source is 5-60 sccm, preferably 10-50 sccm.
10. The preparation method according to claim 9, in, The carbon matrix is selected from at least one of carbon nanotubes, graphene, carbon black and porous carbon, preferably porous carbon; Preferably, the silicon in the silicon-carbon composite layer comprises amorphous silicon and optional silicon grains; Preferably, the average particle size of the silicon grains is less than 8 nm, preferably less than 3 nm; Preferably, the carbon in the silicon-carbon composite layer is amorphous carbon; Preferably, the thickness of the carbon coating layer is 5-100 nm, preferably 10-30 nm; Preferably, the average particle size of the silicon-carbon composite material is 3-15 μm, preferably 5-10 μm.
11. The preparation method according to claim 10, in, The average particle size of the porous carbon is 2-8 μm, preferably 4-6 μm; Preferably, the content of amorphous silicon and optional silicon grains in the silicon-carbon composite layer is 20-40wt%, preferably 25-35wt%, based on the total amount of the silicon-carbon composite material; Preferably, based on the total amount of the silicon-carbon composite material, the content of amorphous carbon in the silicon-carbon composite layer is 20-40 wt %, preferably 25-35 wt %.
12. A silicon-carbon composite material obtained by the preparation method according to any one of claims 6 to 11.
13. A negative electrode sheet, in, The negative electrode sheet comprises the silicon-carbon composite material according to any one of claims 1-5 and 12.
14. A lithium ion battery, in, The lithium-ion battery comprises the negative electrode sheet according to claim 13.
Citation Information
Patent Citations
Preparation method of silicon-carbon composite material
CN112133915A
Oxygen-pore double-gradient silicon monoxide@carbon composite material, and preparation method and application thereof
CN113851621A
Silicon-carbon composite material, preparation method thereof, negative plate and lithium secondary battery
CN115513432A
Silicon-carbon negative electrode material, preparation method and application thereof
CN116364935A
Silicon-carbon negative electrode material for lithium ion battery and preparation method therefor
WO2022007401A1
Cited By
Battery monomer and preparation method thereof, battery device, power utilization device and energy storage device
CN122267266A
Lithium secondary battery, negative electrode active material and preparation method therefor, and electric device