Composite material as well as preparation method and application thereof

By using graphite frameworks, nanosilicon and heteroatom doping materials in silicon-carbon composites, combined with a fluorine-containing lithium phosphate compound coating, forming a porous structure and amorphous carbon coating, the existing materials are solved in circulation and magnification. The performance deficiency has achieved efficient lithium-ion embedding and reduced side reactions, improving the overall performance of the battery.

CN119069681APending Publication Date: 2024-12-03SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411353517.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing silicon-carbon composite materials cannot have high cycle performance and high rate performance, and the fast charging performance improvement is limited.

Method used

Using a composite material, including a graphite skeleton, doped material and cladding material, each containing nanosilicon and heteroatoms, including nitrogen, lithium and carbon, the surface is coated with a fluorine-containing lithium phosphate compound , the porous structure and amorphous carbon cladding are formed through specific heat treatment and drying steps to enhance the electron and ion conductivity.

Benefits of technology

It significantly improves the rate performance and cycling performance of composite materials, enhances the lithium ion embedding rate, reduces side reactions, and improves the storage and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069681A_ABST
    Figure CN119069681A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a composite material and a preparation method and application thereof. The composite material comprises an inner core matrix and a coating layer coating the inner core matrix, the inner core matrix comprises a graphite skeleton, a doping material and a coating material, the doping material is located in pores of the graphite skeleton, and the coating material is located on the surface of the graphite skeleton; the doping material and the coating material respectively and independently comprise nano silicon and heteroatoms, and the heteroatoms comprise nitrogen, lithium and carbon; the coating layer includes a fluorine-containing lithium phosphate compound. In the composite material, the graphite skeleton is doped with the doping material, and the surface of the graphite skeleton is coated with the coating material, so that the electronic and ionic conductivity of the composite material is improved, and the rate capability is improved; the fluorine-containing lithium phosphate compound layer can reduce the leakage of silicon, reduce side reaction, improve the lithium ion intercalation and deintercalation rate of the material, improve the rate capability, and improve the cycle performance and the storage performance thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a composite material and a preparation method and application thereof. Background Art

[0002] As the market's requirements for lithium-ion battery range and fast charging performance increase, the negative electrode materials used in lithium-ion batteries are required to have high energy density while also improving fast charging. The maximum specific capacity (360mAh / g) of currently commercialized artificial graphite is close to its limit and is difficult to increase significantly. At the same time, in order to improve fast charging performance, it is necessary to reduce the particle size and increase the carbon coating amount of the material, but this will reduce the specific capacity, compaction density and its first efficiency. Although silicon-carbon materials have high specific capacity, they have high expansion and low first efficiency.

[0003] Patent application number CN201710195739.6 discloses a graphite / silicon / graphene composite material and a preparation method thereof. The composite material is a three-layer sandwich structure, which consists of graphite, nano-silicon and graphene from the inside to the outside. Nano-silicon is fixed between graphite and graphene, and is made of an inner layer of graphite as a skeleton. The outer layer of graphene serves as a buffer layer to reduce expansion and improve cycle performance. However, the initial efficiency of the material and its lithium ion diffusion rate are not improved, so that the rate performance improvement of the material is limited.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a composite material to solve the technical problem that the silicon-carbon composite material in the prior art cannot have both high cycle performance and high rate performance.

[0006] Another object of the present invention is to provide a method for preparing the composite, which is simple, easy to operate and environmentally friendly.

[0007] Another object of the present invention is to provide a negative electrode sheet as described above.

[0008] Another object of the present invention is to provide a battery as described above.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A composite material comprises a core matrix and a coating layer coating the core matrix; the core matrix comprises a graphite skeleton, a doping material and a coating material, the doping material is located in the pores of the graphite skeleton, and the coating material is located on the surface of the graphite skeleton; the doping material and the coating material each independently contain nano-silicon and heteroatoms, the heteroatoms include nitrogen, lithium and carbon; the coating layer comprises a fluorine-containing lithium phosphate compound.

[0011] In some embodiments, the fluorine-containing lithium phosphate compound includes at least one of lithium tetrafluorooxalate phosphate, lithium difluorooxalate phosphate, lithium hexafluorophosphate, lithium difluorobisoxalate phosphate, and lithium difluorophosphate.

[0012] In some embodiments, in the core matrix, the mass content of the graphite skeleton is 85% to 94%, the mass content of the nano-silicon is 1% to 5%, and the mass content of the heteroatoms is 5% to 10%.

[0013] In some embodiments, the mass of the coating layer accounts for 5% to 15% of the mass of the composite material.

[0014] In some embodiments, the tap density of the composite material is 1.04 to 1.2 g / cm 3 .

[0015] In some embodiments, the specific surface area of ​​the composite material is 1.65 to 1.8 m 2 / g.

[0016] In some embodiments, the OI value of the composite material is 2.3-2.9.

[0017] In some embodiments, the composite material has a particle size D50 of 8 to 16 μm.

[0018] In some embodiments, the diffusion coefficient of the battery prepared from the composite material is (3 to 8)×10 -8 m 2 / s.

[0019] In some embodiments, the first discharge capacity of a battery prepared from the composite material is 403-430 mAh / g.

[0020] In some embodiments, the first efficiency of the battery prepared from the composite material is 95% to 97%.

[0021] In some embodiments, the charging DCR of the battery prepared from the composite material is 18 to 23.5Ω.

[0022] A method for preparing a composite material comprises the following steps:

[0023] A graphite material, a pore-forming agent and a mixed acid solution are mixed and subjected to a first heat treatment to obtain a first material; the first material is mixed with an amino compound solution and an oxidant and subjected to a second heat treatment to obtain a second material; the second material is activated with water vapor to obtain a third material; a mixture of the third material, liquid silane, an amino lithium salt and a first organic solvent is subjected to a third heat treatment to obtain a fourth material; the fourth material is carbonized to obtain a core matrix; the core matrix, a fluorine-containing lithium phosphate compound and a second organic solvent are mixed and dried to obtain a composite material.

[0024] In some embodiments, the mass ratio of the graphite material, the pore former, the amino compound and the oxidant is 100:(1-5):(1-5):(1-5).

[0025] In some embodiments, the amino compound includes at least one of methylamine, ethylenediamine, propylenediamine and isopropylamine.

[0026] In some embodiments, the mass content of the amino compound in the amino compound solution is 0.1% to 1%.

[0027] In some embodiments, the pore former includes at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, and potassium carbonate.

[0028] In some embodiments, the oxidizing agent comprises ammonium persulfate.

[0029] In some embodiments, the mixed acid solution includes a sulfuric acid solution and a nitric acid solution, the volume ratio of the sulfuric acid solution to the nitric acid solution is 1:1, the concentration of the sulfuric acid solution is 55% to 60%, and the concentration of the nitric acid solution is 27% to 32%.

[0030] In some embodiments, the temperature of the first heat treatment is 50-100° C., and the time of the first heat treatment is 2-12 hours.

[0031] In some embodiments, the temperature of the second heat treatment is 0 to 15° C., and the time of the second heat treatment is 6 to 24 hours.

[0032] In some embodiments, the temperature of the activation treatment is 900-1200° C., and the time of the activation treatment is 1-6 hours.

[0033] In some embodiments, the liquid silane includes at least one of dimethylchlorosilane, dimethylsilane, trichloroethylsilane, methyltrimethoxysilane, and propyltrichlorosilane.

[0034] In some embodiments, the lithium amide salt includes at least one of lithium amide, lithium acetate, lithium amide borane, and lithium l-carnitine glutamate.

[0035] In some embodiments, the mass ratio of the third material, the liquid silane and the amino lithium salt is 100:(1-5):(1-5).

[0036] In some embodiments, the mass of the third material accounts for 1% to 10% of the total mass of the third material and the first organic solvent.

[0037] In some embodiments, the third heat treatment is performed under a vacuum degree of 0.01 to 0.05 MPa, the temperature of the third heat treatment is 50 to 100° C., and the time of the third heat treatment is 6 to 24 hours.

[0038] In some embodiments, the temperature of the carbonization treatment is 1000-2000° C., and the time of the carbonization treatment is 1-6 hours.

[0039] In some embodiments, the mass ratio of the core matrix, the fluorine-containing lithium phosphate compound, and the second organic solvent is 100:(1-5):(450-550).

[0040] In some embodiments, the fluorine-containing lithium phosphate compound includes at least one of lithium tetrafluorooxalate phosphate, lithium difluorooxalate phosphate, lithium hexafluorophosphate, lithium difluorobisoxalate phosphate, and lithium difluorophosphate.

[0041] In some embodiments, the drying is performed by spray drying, with an inlet temperature of 180-220° C., an outlet temperature of 70-90° C., a flow rate of 0.08-0.2 kg / h, and a drying time of 1-3 h.

[0042] A negative electrode sheet comprises the composite material, or a composite material prepared by the composite material preparation method.

[0043] A battery comprises the negative electrode sheet.

[0044] An electrical device comprises the battery.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] (1) In the composite material of the present invention, the graphite skeleton in the core matrix is ​​doped with a doping material and the surface is coated with a coating material, which is beneficial to improving the electronic and ionic conductivity of the composite material and improving the rate performance; the fluorine-containing lithium phosphate compound coated on the surface can reduce the leakage of its silicon and reduce its side reactions, and the fluorine-containing lithium phosphate compound has a good solvation ability with the electrolyte, which can increase the lithium ion insertion and extraction rate of the material, improve the rate performance, and improve the cycle performance and storage performance.

[0047] (2) The present invention obtains a third material (porous nitrogen-doped graphite) by combining graphite material, pore-forming agent, mixed acid solution, amino compound solution and oxidant. Liquid silane decomposes to generate nano-silicon which is embedded in the pores of the third material, thereby improving the specific capacity and having the advantage of good uniformity. At the same time, after being doped with amino lithium salt, carbonization is performed to form an amorphous carbon coating material layer co-doped with nitrogen and lithium to improve the electronic and ionic conductivity of the material and improve the rate performance. The core matrix, fluorine-containing lithium phosphate compound and the second organic solvent are mixed and dried to form a fluorine-containing lithium phosphate compound layer on the surface of the core matrix, thereby reducing the leakage of silicon in the core matrix and reducing its side reactions, thereby improving the storage performance of the battery, increasing the lithium ion insertion and extraction rate of the composite material, improving the rate performance, cycle performance and safety performance.

[0048] (3) The battery of the present invention has excellent cycle performance, rate performance and safety performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0050] Figure 1 This is a scanning electron microscope image of the composite material in Example 1 of the present invention. DETAILED DESCRIPTION

[0051] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0052] According to one aspect of the present invention, the present invention relates to a composite material, comprising a core matrix and a coating layer coating the core matrix; the core matrix comprises a graphite skeleton, a doping material and a coating material, the doping material is located in the pores of the graphite skeleton, and the coating material is located on the surface of the graphite skeleton; the doping material and the coating material each independently contain nano-silicon and heteroatoms, the heteroatoms include nitrogen, lithium and carbon; the coating layer includes a fluorine-containing lithium phosphate compound.

[0053] In the composite material of the present invention, the core matrix is ​​doped with a doping material, and the surface is coated with a coating material, which is beneficial to improving the electronic and ionic conductivity of the composite material and improving the rate performance; the fluorine-containing lithium phosphate compound coated on the surface can, on the one hand, reduce the leakage of its silicon and reduce its side reactions, and the fluorine-containing lithium phosphate compound has good solvation ability with the electrolyte, which can improve the lithium ion insertion and extraction rate of the material and improve the rate performance; on the other hand, lithium phosphate has good compatibility with the organic electrolyte, which can improve the cycle performance and its storage performance.

[0054] In some embodiments, the fluorine-containing lithium phosphate compound includes at least one of lithium tetrafluorooxalate phosphate, lithium difluorooxalate phosphate, lithium hexafluorophosphate, lithium difluorobisoxalate phosphate and lithium difluorophosphate. The fluorine-containing lithium phosphate compound can be any one of the above, or a combination of several thereof, such as a combination of lithium tetrafluorooxalate phosphate and lithium difluorooxalate phosphate, a combination of lithium hexafluorophosphate and lithium difluorobisoxalate phosphate, a combination of lithium difluorobisoxalate phosphate, lithium tetrafluorooxalate phosphate and lithium difluorophosphate, etc.

[0055] In some embodiments, in the core matrix, the mass content of the graphite skeleton is 85% to 94%, such as 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93% or 94%, etc., the mass content of nano silicon is 1% to 5%, such as 1%, 2%, 3%, 3.5%, 4%, 4.5%, 5%, etc., and the mass content of heteroatoms is 5% to 10%, such as 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 9%, 10%, etc. The core matrix of the present invention adopts a suitable proportion of graphite skeleton, nano silicon and heteroatoms to improve the electronic and ionic conductivity of the final composite material and improve the rate performance.

[0056] In some embodiments, the mass of the coating layer accounts for 5% to 15% of the mass of the composite material, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc.

[0057] In some embodiments, the tap density of the composite material is 1.04 to 1.2 g / cm 3 , for example 1.04 g / cm 3 , 1.05g / cm 3 , 1.08g / cm 3 , 1.1g / cm 3 , 1.15g / cm 3 In some embodiments, the specific surface area of ​​the composite material is 1.65 to 1.8 m 2 / g. For example, 1.65m 2 / g, 1.68m 2 / g, 1.7m2 / g, 1.75m 2 / g or 1.8m 2 / g, etc. In some embodiments, the OI value of the composite material is 2.3-2.9, such as 2.3, 2.4, 2.5, 2.6, 2.7, 2.8 or 2.9, etc. In some embodiments, the particle size D50 of the composite material is 8-16 μm, such as 8 μm, 10 μm, 12 μm, 13 μm, 14 μm, 16 μm, etc.

[0058] In some embodiments, the diffusion coefficient of the battery prepared by the composite material is (3 to 8)×10 -8 m 2 / s, for example 3×10 -8 m 2 / s, 4×10 -8 m 2 / s, 5×10 -8 m 2 / s, 6×10 -8 m 2 / s, 7×10 -8 m 2 / s or 8×10 -8 m 2 / s, etc.

[0059] In some embodiments, the first discharge capacity of the battery prepared from the composite material is 403-430 mAh / g, for example, 403 mAh / g, 410 mAh / g, 415 mAh / g, 420 mAh / g, 430 mAh / g, etc.

[0060] In some embodiments, the first efficiency of the battery prepared from the composite material is 95% to 97%, for example, 95%, 95.5%, 96%, 97%, etc.

[0061] In some embodiments, the charging DCR of the battery prepared from the composite material is 18 to 23.5Ω, and the charging DCR is 18Ω, 19Ω, 20Ω, 21Ω, 22Ω, 23.5Ω, etc.

[0062] According to another aspect of the present invention, the present invention also relates to a method for preparing a composite material, comprising the following steps:

[0063] A graphite material, a pore-forming agent and a mixed acid solution are mixed and subjected to a first heat treatment to obtain a first material; the first material is mixed with an amino compound solution and an oxidant and subjected to a second heat treatment to obtain a second material; the second material is activated with water vapor to obtain a third material; a mixture of the third material, liquid silane, an amino lithium salt and a first organic solvent is subjected to a third heat treatment to obtain a fourth material; the fourth material is carbonized to obtain a core matrix; the core matrix, a fluorine-containing lithium phosphate compound and a second organic solvent are mixed and dried to obtain a composite material.

[0064] The present invention obtains a third material (porous nitrogen-doped graphite) by combining graphite material, pore-forming agent, mixed acid solution, amino compound solution and oxidant. Liquid silane is decomposed to generate nano-silicon embedded in the pores of the third material, thereby improving the specific capacity and having the advantage of good uniformity. At the same time, after being doped with amino lithium salt, carbonization is performed to form an amorphous carbon coating material layer co-doped with nitrogen and lithium, thereby improving the electronic and ionic conductivity of the material and improving the rate performance. The core matrix, the fluorine-containing lithium phosphate compound and the second organic solvent are mixed and dried to form a fluorine-containing lithium phosphate compound layer on the surface of the core matrix, thereby reducing the leakage of silicon in the core matrix, reducing its side reactions, improving the storage performance of the battery, improving the lithium ion insertion and extraction rate of the composite material, improving the rate performance, the cycle performance and the safety performance.

[0065] In some embodiments, the mass ratio of the graphite material, the pore former, the amino compound and the oxidant is 100:(1-5):(1-5):(1-5), for example, 100:1:1:1, 100:1:2:1, 100:2:1:2, 100:2:3:4, 100:5:5:5, etc. The present invention adopts a suitable mass ratio of graphite material, pore former, amino compound and oxidant to make the graphite material have a suitable porosity and nitrogen content.

[0066] In some embodiments, the amino compound includes at least one of methylamine, ethylenediamine, propylenediamine and isopropylamine, such as a combination of methylamine and ethylenediamine, a combination of ethylenediamine and propylenediamine, and the like.

[0067] In some embodiments, the mass content of the amino compound in the amino compound solution is 0.1% to 1%, for example, 0.1%, 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, or any range between two values.

[0068] In some embodiments, the pore former includes at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate and potassium carbonate, such as a combination of ammonium bicarbonate and ammonium carbonate, a combination of sodium bicarbonate and sodium carbonate, a combination of sodium carbonate and potassium carbonate, and the like.

[0069] In some embodiments, the oxidizing agent comprises ammonium persulfate.

[0070] In some embodiments, the mixed acid solution includes sulfuric acid solution and nitric acid solution, the volume ratio of sulfuric acid solution to nitric acid solution is 1:1, the concentration of sulfuric acid solution is 55% to 60% (for example, 55%, 58%, 60%, etc.), and the concentration of nitric acid solution is 27% to 32% (27%, 28%, 29%, 30%, 32%, etc.).

[0071] In some embodiments, the temperature of the first heat treatment is 50-100°C, such as 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc., or any range between the two. The time of the first heat treatment is 2-12h, such as 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 12h, etc., or any range between the two. After the first heat treatment, filtering and washing are performed to obtain the first material.

[0072] In some embodiments, the temperature of the second heat treatment is 0 to 15°C, such as 0°C, 1°C, 2°C, 5°C, 8°C, 10°C, 12°C, 15°C, etc., or any range between the two. The time of the second heat treatment is 6 to 24h, such as 6h, 7h, 10h, 15h, 20h, 24h, etc., or any range between the two. After the second heat treatment, the mixture is filtered and the filter residue is washed to obtain the second material.

[0073] The suitable first heat treatment and second heat treatment of the present invention are beneficial to ensuring the porous structure of the graphite material and the uniform doping of nitrogen element.

[0074] In some embodiments, the temperature of the activation treatment is 900-1200°C, such as 900°C, 920°C, 950°C, 980°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, or any range between the two. The time of the activation treatment is 1-6h, such as 1h, 2h, 3h, 4h, 5h, 6h, or any range between the two. Appropriate activation treatment conditions are adopted to ensure that the third material has a suitable pore structure, so as to facilitate the subsequent loading effect of silicon materials, etc.

[0075] In some embodiments, the liquid silane includes at least one of dimethylchlorosilane, dimethylsilane, trichloroethylsilane, methyltrimethoxysilane and propyltrichlorosilane, such as a combination of dimethylchlorosilane and dimethylsilane, a combination of methyltrimethoxysilane and propyltrichlorosilane, and the like.

[0076] In some embodiments, the lithium amide salt includes at least one of lithium amide, lithium acetate, lithium borane and lithium l-carnitine glutamate, such as a combination of lithium amide and lithium acetate, a combination of lithium acetate and lithium borane, a combination of lithium borane and lithium l-carnitine glutamate, etc.

[0077] In some embodiments, the mass ratio of the third material, liquid silane and amino lithium salt is 100:(1-5):(1-5), for example, 100:1:1, 100:2:2, 100:3:3, 100:4:3, 100:5:5, etc. The third material, liquid silane and amino lithium salt adopt a suitable mass ratio to ensure the electrochemical performance of the final composite material.

[0078] In some embodiments, the mass of the third material accounts for 1% to 10% of the total mass of the third material and the first organic solvent, for example 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., or any range between the two.

[0079] In some embodiments, the third heat treatment is carried out under a vacuum degree of 0.01 to 0.05 MPa (e.g., 0.01 MPa, 0.02 MPa, 0.03 MPa, 0.04 MPa, 0.05 MPa, etc.), and the temperature of the third heat treatment is 50 to 100 ° C, such as 50 ° C, 55 ° C, 60 ° C, 70 ° C, 80 ° C, 90 ° C or 100 ° C, etc., or any range between the two. The time of the third heat treatment is 6 to 24 hours, such as 6 hours, 8 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours or 24 hours, etc., or any range between the two. The third heat treatment conditions suitable for the present invention are to ensure the doping and coating of nano-silicon and lithium elements, so as to improve the cycle performance and rate performance of the final composite material.

[0080] In some embodiments, the temperature of the carbonization treatment is 1000-2000°C, such as 1000°C, 1100°C, 1200°C, 1300°C, 1500°C, 1800°C, 1850°C, 1900°C, 2000°C, etc., or any range between the two. The time of the carbonization treatment is 1-6h, such as 1h, 2h, 3h, 4h, 5h, 6h, etc., or any range between the two. Suitable carbonization treatment conditions are used to ensure the electrochemical properties of the core matrix material.

[0081] In some embodiments, the mass ratio of the core matrix, the fluorine-containing lithium phosphate compound and the second organic solvent is 100:(1-5):(450-550), for example, 100:1:450, 100:2:490, 100:3:500, 100:4:510, 100:5:550, etc. The core matrix, the fluorine-containing lithium phosphate compound and the second organic solvent adopt a suitable mass ratio, which is more conducive to forming a fluorine-containing lithium phosphate compound coating layer of suitable thickness, so as to ensure that the final composite material has excellent comprehensive electrochemical properties.

[0082] In some embodiments, the fluorine-containing lithium phosphate compound includes at least one of lithium tetrafluorooxalate phosphate, lithium difluorooxalate phosphate, lithium hexafluoro phosphate, lithium difluorobisoxalate phosphate and lithium difluoro phosphate, such as a combination of lithium tetrafluorooxalate phosphate and lithium difluoro oxalate phosphate, a combination of lithium difluorooxalate phosphate and lithium hexafluoro phosphate, a combination of lithium difluorobisoxalate phosphate and lithium difluoro phosphate, and the like.

[0083] In some embodiments, drying is carried out by spray drying, and the inlet temperature is 180-220°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, etc., or any range value between two thereof; the outlet temperature is 70-90°C, for example, 70°C, 75°C, 80°C, 85°C, 90°C, etc., or any range value between two thereof; the flow rate is 0.08-0.2kg / h, for example, 0.08kg / h, 0.1kg / h, 0.12kg / h, 0.15kg / h or 0.2kg / h, etc., and the drying time is 1-3h, for example, 1h, 1.5h, 2h, 2.5h or 3h, etc., or any range value between two thereof.

[0084] According to another aspect of the present invention, the present invention also relates to a negative electrode sheet, comprising the above-mentioned composite material, or a composite material prepared by the above-mentioned method for preparing the composite material.

[0085] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode layer located on the surface of the negative electrode current collector, and the negative electrode layer includes the above composite material, a conductive agent and a binder.

[0086] According to another aspect of the present invention, the present invention also relates to a battery comprising the above-mentioned negative electrode sheet.

[0087] The battery of the present invention has excellent cycle performance, rate performance and safety performance.

[0088] According to another aspect of the present invention, the present invention also relates to an electric device, comprising the above-mentioned battery, and the electric device includes an electric car and the like.

[0089] The following is further described in conjunction with specific embodiments and comparative examples.

[0090] Example 1

[0091] A method for preparing a composite material comprises the following steps:

[0092] (1) 100 g of graphite and 3 g of ammonium bicarbonate were mixed evenly, and added to 500 g of a mixed acid solution, wherein the mixed acid solution included a sulfuric acid solution and a nitric acid solution in a volume ratio of 1:1, the concentration of the sulfuric acid solution was 58%, and the concentration of the nitric acid solution was 30%. The mixture was reacted at 80° C. for 6 h, filtered, and washed with deionized water three times to obtain a first material. The first material was then added to 500 g of a 0.5% methylamine aqueous solution, and 3 g of ammonium persulfate was added to react at 4° C. for 12 h, filtered, and obtained a second material. The second material was activated by passing water vapor at 1100° C. for 3 h to obtain a third material (porous nitrogen-doped graphite).

[0093] (2) Soak 100 g of the third material in 2000 g of N-methylpyrrolidone organic solvent to prepare a solution with a mass concentration of 5%, add 3 g of dimethylchlorosilane and 3 g of lithium amide, disperse evenly, and transfer to a vacuum reactor, evacuate to 0.03 MPa, and perform a chemical reaction at a temperature of 80°C for 12 h. Filter, vacuum dry at 80°C for 24 h, and then heat to 1100°C for carbonization treatment for 3 h to obtain a core matrix material.

[0094] (3) Add 3 g of fluorine-containing lithium phosphate compound (lithium tetrafluorooxalate phosphate) to 500 g of dimethyl carbonate organic solvent and disperse evenly, then add 100 g of core matrix material, disperse evenly and spray dry (inlet temperature is 200°C, outlet temperature is 80°C, flow rate is 0.1 kg / h, time is 2 h) to obtain a composite material.

[0095] Example 2

[0096] A method for preparing a composite material comprises the following steps:

[0097] (1) 100 g of artificial graphite and 1 g of ammonium carbonate were mixed evenly, and added to 500 g of a mixed acid solution, wherein the mixed acid solution included a sulfuric acid solution and a nitric acid solution in a volume ratio of 1:1, the concentration of the sulfuric acid solution was 58%, and the concentration of the nitric acid solution was 30%. The mixture was reacted at 50° C. for 12 h, filtered, and washed with deionized water to obtain a first material. The first material was then added to 1000 g of an aqueous solution of ethylenediamine with a mass concentration of 0.1%, and 1 g of ammonium persulfate was added. The mixture was reacted at 0° C. for 24 h, filtered, and a second material was obtained. The second material was activated by passing water vapor at 900° C. for 6 h to obtain a third material (porous nitrogen-doped graphite).

[0098] (2) Soak 100 g of the third material in 1000 g of N-methylpyrrolidone organic solvent to prepare a solution with a mass concentration of 1%, and add 1 g of dimethylsilane and 1 g of lithium acetate. After uniform dispersion, transfer to a vacuum reactor, evacuate to 0.01 MPa, and perform a chemical reaction at a temperature of 50°C for 24 hours. Filter, vacuum dry at 80°C for 24 hours, and then heat to 1000°C for carbonization treatment for 6 hours to obtain a core matrix material.

[0099] (3) Add 1 g of fluorine-containing lithium phosphate compound (lithium difluorooxalate phosphate) to 500 g of dimethyl carbonate organic solvent and disperse it evenly, then add 100 g of core matrix material, disperse it evenly, and then spray dry it (inlet temperature is 200°C, outlet temperature is 80°C, flow rate is 0.1 kg / h, time is 2 h) to obtain a composite material.

[0100] Example 3

[0101] A method for preparing a composite material comprises the following steps:

[0102] (1) 100 g of artificial graphite and 5 g of sodium bicarbonate were mixed evenly, and added to 500 g of a mixed acid solution, wherein the mixed acid solution included a sulfuric acid solution and a nitric acid solution in a volume ratio of 1:1, the concentration of the sulfuric acid solution was 58%, and the concentration of the nitric acid solution was 30%. The mixture was reacted at a temperature of 100 ° C for 2 h, filtered, and washed with deionized water for 3 times to obtain a first material. The first material was then added to 500 g of a 1% aqueous solution of propylenediamine by mass, and 5 g of an ammonium persulfate oxidant was added to react at a temperature of 15 ° C for 6 h, filtered, and obtained a second material. The second material was activated by passing water vapor at 1200 ° C for 1 h to obtain a third material (porous nitrogen-doped graphite).

[0103] (2) 100 g of the third material was soaked in 1000 g of N-methylpyrrolidone organic solvent to prepare a solution with a mass concentration of 10%, and 5 g of trichloroethylsilane and 5 g of lithium ammonia borane were added. After being evenly dispersed, the solution was transferred to a vacuum reactor and evacuated to 0.05 MPa. The solution was subjected to a chemical reaction at 100° C. for 6 h, filtered, vacuum dried at 80° C. for 24 h, and then heated to 1200° C. for carbonization treatment for 1 h to obtain a core matrix material.

[0104] (3) Add 5 g of fluorine-containing lithium phosphate compound (lithium tetrafluorooxalate phosphate) to 500 g of diethyl carbonate organic solvent and disperse evenly, then add 100 g of core matrix material, disperse evenly and spray dry (inlet temperature is 200°C, outlet temperature is 80°C, flow rate is 0.1 kg / h, time is 2 h) to obtain a composite material.

[0105] Example 4

[0106] A method for preparing a composite material, which differs from Example 3 in that:

[0107] The fluorine-containing lithium phosphate compound in step (3) is 2 g of lithium tetrafluorooxalate phosphate and 2 g of lithium difluorobisoxalate phosphate.

[0108] Example 5

[0109] A method for preparing a composite material, which differs from Example 3 in that:

[0110] The fluorine-containing lithium phosphate compound in step (3) is 1 g of lithium tetrafluorooxalate phosphate, 1 g of lithium difluorobisoxalate phosphate and 2.5 g of lithium hexafluorophosphate.

[0111] Example 6

[0112] A method for preparing a composite material comprises the following steps:

[0113] (1) 100 g of artificial graphite and 5 g of sodium bicarbonate were mixed evenly, and added to 500 g of a mixed acid solution, wherein the mixed acid solution included a sulfuric acid solution and a nitric acid solution in a volume ratio of 1:1, the concentration of the sulfuric acid solution was 58%, and the concentration of the nitric acid solution was 30%. The mixture was reacted at a temperature of 100 ° C for 2 h, filtered, and washed with deionized water for 3 times to obtain a first material. The first material was then added to 500 g of a 1% aqueous solution of propylenediamine by mass, and 5 g of an ammonium persulfate oxidant was added to react at a temperature of 15 ° C for 6 h, filtered, and obtained a second material. The second material was activated by passing water vapor at 1200 ° C for 1 h to obtain a third material (porous nitrogen-doped graphite).

[0114] (2) 100 g of the third material was immersed in 1000 g of N-methylpyrrolidone organic solvent to prepare a solution with a mass concentration of 10%, and 3 g of trichloroethylsilane, 2 g of propyltrichlorosilane, 2 g of lithium ammonia borane and 3 g of lithium l-carnitine glutamate were added. After being evenly dispersed, the solution was transferred to a vacuum reactor and evacuated to 0.05 MPa. The solution was subjected to a chemical reaction at a temperature of 100° C. for 6 h, filtered, vacuum dried at 80° C. for 24 h, and then heated to 1200° C. for carbonization treatment for 1 h to obtain a core matrix material.

[0115] (3) Add 5 g of fluorine-containing lithium phosphate compound (1 g of lithium tetrafluorooxalate phosphate, 1.5 g of lithium difluorobisoxalate phosphate and 2 g of lithium hexafluorophosphate) to 500 g of diethyl carbonate organic solvent and disperse evenly, then add 100 g of core matrix material, disperse evenly and spray dry (inlet temperature is 200°C, outlet temperature is 80°C, flow rate is 0.1 kg / h, time is 2 h) to obtain a composite material.

[0116] Comparative Example 1

[0117] A method for preparing a composite material, which differs from Example 1 in that:

[0118] In step (2), no lithium amide is added.

[0119] Comparative Example 2

[0120] A method for preparing a composite material, which differs from Example 1 in that:

[0121] The operation of step (3) is not performed, and the core matrix material is obtained according to steps (1) and (2).

[0122] Experimental example

[0123] 1. Scanning electron microscope (SEM) test results

[0124] The composite material obtained in Example 1 was subjected to SEM testing, and the results are as follows: Figure 1 As shown, from Figure 1 It can be seen that the composite material presents a single particle structure with uniform size distribution and a particle size of 10 to 15 μm.

[0125] 2. Composite material performance test and battery performance test

[0126] The composite materials in each embodiment and comparative example were tested for tap density, specific surface area, and powder OI value. The tap density and specific surface area were tested according to GBT-24533-2019 "Graphite Negative Electrode Materials for Lithium Ion Batteries"; the OI value was tested by XRD, and the OI value of the material was calculated.

[0127] The composite materials of each embodiment and comparative example are respectively prepared into button batteries. The preparation method of the button battery includes: adding a binder, a conductive agent and a solvent to the negative electrode material, stirring to obtain a negative electrode slurry, coating the negative electrode slurry on a copper foil, drying and rolling, the binder is LA132 binder, the conductive agent is SP, the negative electrode material is respectively the composite materials prepared in each embodiment and comparative example, the solvent is double distilled water, and the negative electrode sheet is prepared in the dosage ratio of: negative electrode material: SP: LA132: double distilled water = 94g: 2g: 4g: 220mL. The electrolyte is a 1.1mol / L LiPF6 solution, the solvent is EC and DEC (volume ratio 1:1); the metal lithium sheet is the counter electrode; the diaphragm is a polyethylene PE film; the simulated battery assembly is carried out in an argon-filled glove box.

[0128] The electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester, with a charge and discharge voltage range of 0.005V-2.0V and a charge and discharge rate of 0.1C. The charging DCR (50% SOC) of the button cell was also tested, and the diffusion coefficient of the composite materials in each embodiment and comparative example was tested by GITT.

[0129] The performance test results of the composite materials are shown in Table 1.

[0130] Table 1 Performance test results of composite materials

[0131]

[0132] The performance test results of the button battery are shown in Table 2.

[0133] Table 2 Performance test results of button batteries

[0134]

[0135]

[0136] As can be seen from Table 1, the composite material obtained by the method of the present invention has a suitable tap density, specific surface area and OI value, and the first discharge capacity, first efficiency, rate performance and cycle performance of the corresponding battery are significantly improved, which can improve the diffusion coefficient of lithium ions in the charge and discharge process and reduce DCR.

[0137] The OI value of the composite material obtained by the methods of Comparative Examples 1 to 2 is relatively high, the initial efficiency of the obtained battery is relatively low, the diffusion coefficient of lithium ions is low, and the DCR is relatively high.

[0138] 3. Soft pack battery test

[0139] The composite material is used as the negative electrode material, and the negative electrode sheet is obtained according to the above method; the ternary material (LiNi 1 / 3 Co 1 / 3Mn 1 / 3 O2) was used as the positive electrode material to prepare the positive electrode sheet; LiPF6 with a concentration of 1.1 mol / L was used as the electrolyte, and the solvents were EC and DEC with a volume ratio of 1:1; celegard2400 was used as the separator; and a 2Ah soft-pack battery was prepared.

[0140] Rate performance test: the charge and discharge voltage range is 2.8-4.2V, the test temperature is 25±3.0℃, and the constant current ratio is tested by charging at 1.0C, 2.0C, 3.0C, and 5.0C, and the discharge is tested at 1.0C. The results are shown in Table 3.

[0141] Table 3 Soft pack battery test results

[0142]

[0143] It can be seen from Table 3 that the rate charging performance of the soft-pack batteries prepared from the composite materials of each embodiment of the present invention is significantly better than that of Comparative Examples 1 to 2, that is, the charging time is shorter, indicating that the composite materials of the present invention have good fast charging performance. The reasons include: the composite materials of each embodiment of the present invention have a lower OI value, which can improve the kinetic properties of the material, and have a high specific surface area, which can improve the rate performance of the material.

[0144] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite material, characterized in that: It comprises a core matrix and a coating layer covering the core matrix; the core matrix comprises a graphite skeleton, a doping material and a coating material, the doping material is located in the pores of the graphite skeleton, and the coating material is located on the surface of the graphite skeleton; The doping material and the coating material each independently contain nano-silicon and heteroatoms, and the heteroatoms include nitrogen, lithium and carbon; The coating layer includes a fluorine-containing lithium phosphate compound.

2. The composite material according to claim 1, characterized in that Contains at least one of the following features (1) to (3): (1) The fluorine-containing lithium phosphate compound includes at least one of lithium tetrafluorooxalate phosphate, lithium difluorooxalate phosphate, lithium hexafluorophosphate, lithium difluorobisoxalate phosphate and lithium difluorophosphate; (2) In the core matrix, the mass content of the graphite skeleton is 85% to 94%, the mass content of the nano-silicon is 1% to 5%, and the mass content of the heteroatoms is 5% to 10%; (3) The mass of the coating layer accounts for 5% to 15% of the mass of the composite material.

3. The composite material according to claim 1, characterized in that Contains at least one of the following features (1) to (8): (1) The tap density of the composite material is 1.04 to 1.2 g / cm 3 ; (2) The specific surface area of ​​the composite material is 1.65 to 1.8 m 2 / g; (3) The OI value of the composite material is 2.3 to 2.9; (4) The particle size D50 of the composite material is 8 to 16 μm; (5) The diffusion coefficient of the battery prepared by the composite material is (3-8)×10 -8 m 2 / s; (6) The first discharge capacity of the battery prepared from the composite material is 403-430 mAh / g; (7) The initial efficiency of the battery prepared from the composite material is 95% to 97%; (8) The charging DCR of the battery prepared from the composite material is 18 to 23.5Ω.

4. A method for preparing a composite material, characterized in that: The following steps are involved: Mixing a graphite material, a pore-forming agent and a mixed acid solution and performing a first heat treatment to obtain a first material, mixing the first material with an amino compound solution and an oxidant and performing a second heat treatment to obtain a second material, and activating the second material with water vapor to obtain a third material; Performing a third heat treatment on a mixture of the third material, liquid silane, amino lithium salt and the first organic solvent to obtain a fourth material, and performing a carbonization treatment on the fourth material to obtain a core matrix; The core matrix, the fluorine-containing lithium phosphate compound and the second organic solvent are mixed and then dried to obtain a composite material.

5. The method for preparing a composite material according to claim 4, characterized in that: The invention comprises at least one of the following features (1) to (9): (1) The mass ratio of the graphite material, the pore former, the amino compound and the oxidant is 100:(1-5):(1-5):(1-5); (2) the amino compound comprises at least one of methylamine, ethylenediamine, propylenediamine and isopropylamine; (3) The amino compound solution has a mass content of 0.1% to 1% of the amino compound; (4) the pore-forming agent comprises at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate and potassium carbonate; (5) The oxidant comprises ammonium persulfate; (6) The mixed acid solution comprises a sulfuric acid solution and a nitric acid solution, wherein the volume ratio of the sulfuric acid solution to the nitric acid solution is 1:1, the concentration of the sulfuric acid solution is 55% to 60%, and the concentration of the nitric acid solution is 27% to 32%; (7) The temperature of the first heat treatment is 50 to 100° C., and the time of the first heat treatment is 2 to 12 hours; (8) The temperature of the second heat treatment is 0 to 15° C., and the time of the second heat treatment is 6 to 24 hours; (9) The temperature of the activation treatment is 900 to 1200° C., and the time of the activation treatment is 1 to 6 hours.

6. The method for preparing a composite material according to claim 4, characterized in that: Contains at least one of the following features (1) to (6): (1) The liquid silane comprises at least one of dimethylchlorosilane, dimethylsilane, trichloroethylsilane, methyltrimethoxysilane and propyltrichlorosilane; (2) The lithium amide salt comprises at least one of lithium amide, lithium acetate, lithium amine borane and lithium l-carnitine glutamate; (3) The mass ratio of the third material, the liquid silane and the amino lithium salt is 100:(1-5):(1-5); (4) The mass of the third material accounts for 1% to 10% of the total mass of the third material and the first organic solvent; (5) the third heat treatment is performed under a vacuum degree of 0.01 to 0.05 MPa, the temperature of the third heat treatment is 50 to 100° C., and the time of the third heat treatment is 6 to 24 hours; (6) The temperature of the carbonization treatment is 1000-2000° C., and the time of the carbonization treatment is 1-6 hours.

7. The method for preparing a composite material according to claim 4, characterized in that: Contains at least one of the following features (1) to (3): (1) The mass ratio of the core matrix, the fluorine-containing lithium phosphate compound and the second organic solvent is 100:(1-5):(450-550); (2) the fluorine-containing lithium phosphate compound comprises at least one of lithium tetrafluorooxalate phosphate, lithium difluorooxalate phosphate, lithium hexafluorophosphate, lithium difluorobisoxalate phosphate and lithium difluorophosphate; (3) The drying is carried out by spray drying, with an inlet temperature of 180-220° C., an outlet temperature of 70-90° C., a flow rate of 0.08-0.2 kg / h, and a drying time of 1-3 h.

8. A negative electrode sheet, characterized in that: A composite material comprising the composite material according to any one of claims 1 to 3, or a composite material prepared by the method for preparing a composite material according to any one of claims 4 to 7.

9. A battery, characterized in that: A negative electrode sheet comprising the negative electrode sheet according to claim 8.

10. An electrical device, characterized in that: A battery comprising the battery of claim 9.

Citation Information

Cited By

  • Negative active material and preparation method thereof, negative plate and lithium ion battery

    CN121726374A

  • A negative electrode active material, a preparation method thereof, a negative electrode sheet, and a lithium ion battery

    CN121726374B