Vanadium-based Prussian blue analogue positive electrode material as well as preparation method and application thereof

By using vanadium-yl Prussian blue analog positive electrode material and adding EDTA-2K during the preparation process and removing crystallization water, the problems of stability and electrochemical performance of the positive electrode material of potassium ion battery were solved, and high specific capacity and long cycle stability were achieved , suitable for potassium ion secondary batteries.

CN119069690APending Publication Date: 2024-12-03FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310652828.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing potassium ion battery positive electrode materials are prone to manganese dissolution during the cycle, resulting in capacity attenuation and short cycle life. The specific capacity and working voltage of iron-based Prussian blue analogs are generally low, making it difficult to take into account high specific capacity and circulation. Stability and high operating voltage.

Method used

The positive electrode material of vanadium-based Prussian blue analog is KxVOy[Fe(CN)6]1-y/6·nH2O. By adding EDTA-2K during the preparation process, it inhibits the nucleation and growth rate of the material and reduces structural defects. Improve potassium storage capacity and structural stability, and remove crystallized water by drying to improve the overall electrochemical performance of the battery.

Benefits of technology

The potassium ion battery has both high specific capacity, high operating voltage and long cycle stability, which significantly improves the electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069690A_ABST
    Figure CN119069690A_ABST
Patent Text Reader

Abstract

The invention discloses a vanadium-based Prussian blue analogue positive electrode material. The chemical formula of the vanadium-based Prussian blue analogue positive electrode material is KxVOy [Fe (CN) 6] (1-y / 6. NH2O, wherein 0 lt; xlt; 8, 0lt; yt; Yt; 6, 0 < = nlt; 9. The potassium-rich vanadium-based Prussian blue analogue positive electrode material is used for a potassium ion secondary battery, so that the battery has high specific capacity, high working voltage and long cycle stability at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a vanadium-based Prussian blue analogue positive electrode material and a preparation method and application thereof, belonging to the technical field of potassium ion batteries. Background Art

[0002] With the massive consumption of traditional fossil resources such as coal, oil and natural gas and increasingly serious environmental problems, the development of sustainable clean new energy is urgent. The rapid rise of new energy industries such as tidal energy, geothermal energy, solar energy and wind energy urgently requires the development of large-scale electrochemical energy storage technology. Existing lithium-ion batteries are difficult to meet the needs of large-scale energy storage due to the scarcity and uneven distribution of lithium resources. Compared with lithium, potassium is abundant and evenly distributed in the earth's crust. Therefore, potassium-ion batteries have the advantage of low cost and have application potential in the field of large-scale energy storage.

[0003] The selection of positive electrode materials for potassium ion batteries is crucial. The positive electrode materials for potassium ion batteries currently developed mainly include Prussian blue analogues, layered metal oxides, polyanionic compounds, organic matter, etc. Among them, Prussian blue analogues are conducive to the rapid deintercalation of potassium ions due to their unique open framework and three-dimensional macroporous structure. As positive electrode materials for potassium ion batteries, they have great potential and have received widespread attention. The reported Prussian blue-based positive electrode materials for potassium ion batteries are mainly divided into two categories: manganese-based Prussian blue analogues and iron-based Prussian blue analogues. Among them, manganese-based Prussian blue analogue positive electrode materials can usually provide high working voltage and specific capacity, but they are prone to manganese dissolution during the cycle process, which leads to capacity decay and short cycle life; while the specific capacity and working voltage of iron-based Prussian blue analogue positive electrode materials are generally low. Therefore, the development of Prussian blue analogue positive electrode materials that take into account specific capacity, cycle stability and high working voltage is of great significance to the development of potassium ion batteries. Summary of the invention

[0004] According to one aspect of the present application, a vanadium-based Prussian blue analogue positive electrode material is provided, which overcomes the problem of positive electrode material structural stability that has always existed in the prior art and can be used in potassium ion secondary batteries, so that the battery has high specific capacity, high operating voltage and long cycle stability.

[0005] This application adopts the following technical solutions:

[0006] A vanadium-based Prussian blue analogue positive electrode material, wherein the chemical formula of the vanadium-based Prussian blue analogue positive electrode material is K x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 O;

[0007] Among them, 0 <x<8,0<y<6,0≤n<9。

[0008] Optionally, the chemical formula of the vanadium-based Prussian blue analogue positive electrode material is K x VO y [Fe(CN) 6 ] 1-y / 6 ;

[0009] Among them, 0 <x<8,0<y<6。

[0010] Optionally, the vanadium-based Prussian blue analogue positive electrode material is nanoparticles with a particle size of 40 to 60 nm.

[0011] According to another aspect of the present application, a method for preparing the above-mentioned vanadium-based Prussian blue analogue positive electrode material is provided, comprising the following steps:

[0012] S1, will contain V 2 O 5 , H 2 C 2 O 4 , a suspension I in water, heating it, and then adding dipotassium ethylenediaminetetraacetate to obtain a solution I;

[0013] S2, K 4 Fe(CN) 6 Dissolve in water to obtain solution II;

[0014] S3. In an inactive atmosphere, adding solution II to solution I to obtain suspension II, aging, centrifugal washing, and drying to obtain the vanadium-based Prussian blue analogue positive electrode material.

[0015] Optionally, in step S1, the V 2 O 5 , H 2 C 2 O 4 , the molar ratio of dipotassium ethylenediaminetetraacetate is 1:(2~4):(1~3).

[0016] Optionally, in step S1, the V 2 O 5 The dosage ratio with water is 1mmol:25~25mL.

[0017] Optionally, in step S1, the heating conditions are: heating to 60-100° C. and keeping warm for 1-3 hours;

[0018] Optionally, in step S2, the V 2 O 5 With K 4 Fe[CN) 6The molar ratio is 1:1.5-2.5;

[0019] Optionally, in step S2, the K 4 Fe(CN) 6 The dosage ratio with water is 1mmol:5~15mL.

[0020] Optionally, in step S3, the conditions for adding solution II into solution I are: continuous stirring, and the adding speed is 3-5 mL / min.

[0021] Optionally, the addition rate is selected from any value of 3 mL / min, 3.5 mL / min, 4 mL / min, 4.5 mL / min, 5 mL / min, or any range therebetween.

[0022] Optionally, in step S3, the aging time is 30 to 42 hours.

[0023] In the prior art, Prussian blue analogue positive electrode materials have always had stability problems. In the technical solution of the present application, EDTA-2K is added during the preparation process to inhibit the nucleation and growth rate of the material, thereby reducing the structural defects of the material and increasing the redox active centers, thereby improving the potassium storage capacity and structural stability of the material, so that the battery has both high specific capacity and long cycle stability.

[0024] According to another aspect of the present application, a positive electrode plate is also provided, which comprises at least one of the above-mentioned vanadium-based Prussian blue analogue positive electrode material and the vanadium-based Prussian blue analogue positive electrode material prepared according to the above-mentioned preparation method.

[0025] Optionally, the following steps are included:

[0026] Applying a mixed slurry containing a vanadium-based Prussian blue analogue positive electrode material, a conductive agent, a binder, and an organic solvent to the surface of a current collector, and drying to form a positive electrode film to obtain the positive electrode sheet;

[0027] The vanadium-based Prussian blue analogue positive electrode material is selected from at least one of the above-mentioned vanadium-based Prussian blue analogue positive electrode material and the vanadium-based Prussian blue analogue positive electrode material prepared according to the above-mentioned preparation method.

[0028] Optionally, the content of the positive electrode material in the positive electrode film is ≥ 60wt%.

[0029] Optionally, the weight ratio of the vanadium-based Prussian blue analogue positive electrode material, the conductive agent, and the binder is (6-8):(1-3):1;

[0030] Optionally, the usage ratio of the binder to the organic solvent is 1 mg: 0.1-0.3 mL.

[0031] Optionally, the conductive agent is selected from at least one of conductive graphite, carbon nanotubes, graphene, amorphous carbon, Ketjen black, acetylene black, and Super-P carbon black.

[0032] Optionally, the binder is selected from at least one of sodium hydroxymethyl cellulose, styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, polybutyl acrylate, and polyacrylonitrile.

[0033] Optionally, the current collector is selected from at least one of aluminum foil, copper foil, stainless steel mesh, nickel foil and titanium foil.

[0034] Optionally, the organic solvent is selected from at least one of NMP, DMAs, DMF, TEP and DMSO.

[0035] The drying conditions are: drying in a vacuum drying oven at a temperature of 160-200° C. to a constant weight.

[0036] The drying temperature is selected from any value of 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, or any range therebetween.

[0037] The crystal water in the Prussian blue analog positive electrode material not only occupies potassium storage sites, but also causes side reactions, thereby reducing the comprehensive electrochemical performance of the battery. In the technical solution of the present application, the crystal water and solvent in the positive electrode material are completely removed after drying to constant weight, thereby avoiding the negative impact of the crystal water on the comprehensive electrochemical performance of the battery.

[0038] According to another aspect of the present application, another positive electrode sheet as described above and the use of the positive electrode sheet prepared according to the above preparation method in the preparation of a potassium ion secondary battery are also provided.

[0039] Optionally, the application includes:

[0040] The battery assembly including the positive electrode plate, electrolyte and potassium plate is assembled into a potassium ion battery.

[0041] Other components in the battery assembly can be selected according to actual needs.

[0042] In the present application, EDTA-2K is dipotassium ethylenediaminetetraacetate.

[0043] The beneficial effects of this application include:

[0044] The vanadium-based Prussian blue analog positive electrode material provided in the present application is the potassium-rich vanadium-based Prussian blue analog positive electrode material, which is used in potassium ion secondary batteries, so that the battery has high specific capacity, high operating voltage and long cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 K in Example 1 of this application x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 XRD test pattern of O;

[0046] Figure 2 K in Example 1 of this application x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 SEM image of O;

[0047] Figure 3 K in Example 1 of this application x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 Transmission electron microscopy image of O;

[0048] Figure 4 This is a cyclic voltammetry curve of the potassium ion battery obtained in Example 2 of the present application;

[0049] Figure 5 This is a charge and discharge curve of the potassium ion battery obtained in Example 2 of the present application (current density: 20 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate);

[0050] Figure 6 This is a cycle performance diagram of the potassium ion battery obtained in Example 2 of the present application (current density: 50 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate);

[0051] Figure 7 This is a charge and discharge curve of the potassium ion battery obtained in Example 2 of the present application (current density: 50 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate);

[0052] Figure 8 This is a cycle performance diagram of the potassium ion battery obtained in Example 2 of the present application (current density: 300 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate);

[0053] Fig. 9 This is a charge and discharge curve of the potassium ion battery obtained in Example 2 of the present application (current density: 300 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate);

[0054] Fig.10 This is a cycle performance diagram of the potassium ion battery obtained in Example 2 of the present application (current density: 500 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate);

[0055] Fig.11 This is a charge and discharge curve of the potassium ion battery obtained in Example 2 of the present application (current density: 500 mA / g; electrolyte: 3 mol / L potassium bis(fluorosulfonyl)imide dissolved in triethyl phosphate). DETAILED DESCRIPTION

[0056] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0057] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0058] X-ray powder diffraction phase analysis (XRD) was performed using a Rigaku Ultima lV instrument under the following analysis conditions: scanning rate of 1° / min; scanning range of 10-50°; target material was a copper target.

[0059] The electrochemical performance test of potassium ion battery was carried out using LANHE CT2001 instrument, and the analysis conditions were as follows: current density was 20, 50, 300 and 500 mA / g; voltage window was 2-4.5V.

[0060] Example 1 Preparation of K x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 O cathode material

[0061] (1) 1mmo1 V 2 O 5 and 3 mmol H 2 C 2 O 4 Add to 20 mL of deionized water to prepare suspension A;

[0062] (2) 2mmol K 4 Fe(CN) 6 Dissolve in 20 mL of deionized water to prepare solution B;

[0063] (3) The suspension A was heated to 80°C for 2 hours, and then 2 mmol of EDTA-2K was added to prepare solution C;

[0064] (4) adding solution C to solution B at a rate of 4 mL / min under argon atmosphere and stirring to obtain suspension D;

[0065] (5) The suspension D is aged for 36 hours, centrifuged, washed, and dried to obtain K. x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 O (x=1.96, y=1, n=1.6) positive electrode material powder.

[0066] The prepared positive electrode material was subjected to XRD analysis, and its XRD spectrum was as follows: Figure 1 As shown; Figure 2 This is the SEM image of the material, showing that its particles are evenly distributed; Figure 3 This is the TEM image of the material, and its particle size is about 50nm.

[0067] Example 2 Preparation of potassium ion battery

[0068] The raw material composition of the positive electrode membrane of the potassium ion battery (based on the mass fraction of the positive electrode membrane as 100%): 70% of the positive electrode material powder in Example 1, 20% of Ketjen black, and 10% of polyvinylidene fluoride.

[0069] The counter electrode of potassium ion battery is: metallic potassium.

[0070] The solvent of the electrolyte is triethyl phosphate.

[0071] The electrolyte salt is potassium bis(fluorosulfonyl)imide, and its molar concentration in the electrolyte is 3 mol / L.

[0072] The preparation method of potassium ion battery is as follows:

[0073] Preparation of positive electrode: Weigh each raw material (a total of 100 mg) according to the weight fraction of the raw materials of the above-mentioned positive electrode film, dissolve polyvinylidene fluoride in N-methyl-2-pyrrolidone (NMP) (wherein the concentration of polyvinylidene fluoride is 5 mg / mL), and then add the positive electrode material powder and Ketjen black in Example 1 and stir to prepare a mixed slurry for the positive electrode, and apply the slurry on the positive electrode current collector aluminum foil, dry it in a vacuum drying oven at 180°C for 12 hours (to remove all water in the positive electrode material), and slice it to obtain a positive electrode sheet.

[0074] The positive electrode sheet, electrolyte and potassium sheet of the potassium ion battery prepared above and other necessary battery components, such as a diaphragm (Glass fiber) and a shell, are assembled into a 2032-type button battery.

[0075] Example 3 Testing the performance of potassium ion batteries

[0076] The potassium ion battery prepared in Example 2 was tested for charge and discharge capacity: constant current charge and discharge test was performed at 28°C using a LANHE CT2001 battery test system, with the test voltage range being 2 to 4.5V. The test is as follows:

[0077] Figure 4 The cyclic voltammetry curve of the battery at a scan rate of 0.1 mV / s. It can be seen from the figure that K x VO y [Fe(CN) 6 ] 1-y / 6 ·nH 2 O exhibits a pair of strong redox peaks (3.78 / 4.12 V) that remain stable during the cycling process, indicating that the extraction and insertion of potassium ions are reversible.

[0078] Figure 5 The charge and discharge curves for the 1st, 2nd, 3rd, 4th and 5th cycles are shown in Figure 1. The charge and discharge current density is 20mA / g, the first cycle charge capacity is 130.9mAh / g, the discharge capacity is 119.3mAh / g, the first cycle coulomb efficiency is as high as 90%, and the discharge voltage is 3.81V. After five cycles, the battery is in a stable state. When the current density is greater than 20mA / g, all batteries are activated at 20mA / g for five cycles before the charge and discharge test.

[0079] Figure 6 This is a cycle performance diagram at a current density of 50 mA / g. After 300 cycles, the capacity retention rate can reach 82%, showing excellent cycle performance and stable electrochemical performance.

[0080] Figure 7 These are the charge and discharge curves for the 6th, 50th, 100th, 200th and 300th cycles. The charge and discharge current density is 50mA / g, the discharge specific capacity is 108.6mAh / g, and the specific capacity is 89mAh / g after 300 cycles.

[0081] Figure 8 This is a cycle performance diagram at a current density of 300 mA / g. After 2000 cycles, the capacity retention rate can reach 73% and the coulombic efficiency reaches more than 99%, showing excellent cycle performance and stable electrochemical performance.

[0082] Fig. 9 These are the charge and discharge curves for the 6th, 100th, 500th, 1000th and 2000th cycles. The charge and discharge current density is 300mA / g, the discharge specific capacity is 88.4mAh / g, and the specific capacity is 64.5mAh / g after 2000 cycles.

[0083] Fig.10This is a cycle performance diagram at a current density of 500 mA / g. After 4000 cycles, the capacity retention rate can reach 70% and the coulombic efficiency reaches more than 99%, showing excellent cycle performance and stable electrochemical performance.

[0084] Fig.11 These are the charge and discharge curves for the 6th, 1000th, 2000th, 3000th and 4000th cycles. The charge and discharge current density is 500mA / g, the discharge specific capacity is 78.4mAh / g, and the specific capacity is 54.9mAh / g after 4000 cycles.

[0085] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A vanadium-based Prussian blue analogue positive electrode material, characterized in that: The chemical formula of the vanadium-based Prussian blue analog positive electrode material is K x VO y [Fe(CN)6] 1-y / 6 nH2O; Among them, 0 <x<8,0<y<6,0≤n<9。 2. The vanadium-based Prussian blue analogue positive electrode material according to claim 1, characterized in that: The chemical formula of the vanadium-based Prussian blue analog positive electrode material is K x VO y [Fe(CN)6] 1-y / 6 ; Among them, 0 <x<8,0<y<6; Preferably, the vanadium-based Prussian blue analogue positive electrode material is nanoparticles with a particle size of 40 to 60 nm.

3. The method for preparing the vanadium-based Prussian blue analogue positive electrode material according to claim 1 or 2, characterized in that: The steps include: S1, heating a suspension I containing V2O5, H2C2O4 and water, and then adding dipotassium ethylenediaminetetraacetate to obtain a solution I; S2, dissolving K4Fe(CN)6 in water to obtain solution II; S3. In an inactive atmosphere, adding solution II to solution I to obtain suspension II, aging, centrifugal washing, and drying to obtain the vanadium-based Prussian blue analogue positive electrode material.

4. The preparation method according to claim 3, characterized in that: In the step S1, the molar ratio of V2O5, H2C2O4 and dipotassium ethylenediaminetetraacetate is 1:(2-4):(1-3); Preferably, in step S1, the heating conditions are: heating to 60-100° C. and keeping warm for 1-3 hours; Preferably, in step S2, the molar ratio of V2O5 to K4Fe(CN)6 is 1:1.5-2.5; Preferably, in step S3, the conditions for adding solution II to solution I are: continuous stirring, and the adding speed is 3-5 mL / min; Preferably, in step S3, the aging time is 30 to 42 hours.

5. A positive electrode sheet, characterized in that: The positive electrode plate comprises at least one of the vanadium-based Prussian blue analogue positive electrode material according to claim 1 or 2 and the vanadium-based Prussian blue analogue positive electrode material prepared according to the preparation method according to claim 3 or 4.

6. The method for preparing the positive electrode sheet according to claim 5, characterized in that: The steps include: Applying a mixed slurry containing a vanadium-based Prussian blue analogue positive electrode material, a conductive agent, a binder, and an organic solvent to the surface of a current collector, and drying to form a positive electrode film to obtain the positive electrode sheet; The vanadium-based Prussian blue analogue positive electrode material is selected from at least one of the vanadium-based Prussian blue analogue positive electrode material according to claim 1 or 2, and the vanadium-based Prussian blue analogue positive electrode material prepared according to the preparation method according to claim 3 or 4.

7. The preparation method according to claim 6, characterized in that: The drying conditions are: drying in a vacuum drying oven at a temperature of 160-200° C. to a constant weight.

8. The preparation method according to claim 6, characterized in that: The content of the positive electrode material in the positive electrode film is ≥60wt%.

9. The preparation method according to claim 6, characterized in that: The weight ratio of the vanadium-based Prussian blue analogue positive electrode material, the conductive agent, and the binder is (6-8):(1-3):1; Preferably, the usage ratio of the binder to the organic solvent is 1 mg: 0.1-0.3 mL.

10. Use of the positive electrode sheet according to claim 5 or the positive electrode sheet prepared by the preparation method according to any one of claims 6 to 9 in preparing a potassium ion secondary battery.