Silicon-carbon negative electrode active material and preparation method thereof
By using a combination of nanosilicon powder, graphite and conductive agent in the silicon carbon negative electrode active material, copper and carbon black are added to form a uniform carbon nanotube cladding layer, the problem of volume expansion of silicon carbon negative electrode material during charging and discharging is solved. , improves the stability and cycle life of the electrode structure, reduces internal resistance and side reactions, and improves the charging and discharging performance and safety of the battery.
Patent Information
- Application Number
- CN202410537620.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-12-03
AI Technical Summary
The volume expansion of silicon carbon negative electrode active material during charging and discharging leads to reduced electrode structure integrity, short cycle life, and the prior art preparation process is complex and costly.
Using a combination of nano-silicon powder, graphite, conductive agent, binder and dispersant, silicon carbon negative electrode active material is prepared by stirring and drying. 12% copper and 88% carbon black are added to the conductive agent to form a uniform carbon nanometer The tube cladding adjusts the viscosity and dispersion of the slurry to ensure uniform mixing and bonding of the components.
It improves electron transmission efficiency, buffers volume expansion, maintains electrode structure integrity, extends cycle life, reduces internal resistance and side reactions, significantly reduces the irreversible expansion rate of charging, and improves battery safety and energy density.
Smart Images

Figure CN119069701A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a silicon-carbon negative electrode active material and a preparation method thereof. Background Art
[0002] With the rapid development of the lithium battery industry, the stability of the pole piece inside the battery is also relatively high. The negative electrode material is an important component of lithium-ion batteries, which directly affects the key indicators of the battery's energy density and safety performance. Traditional negative electrode materials (artificial graphite, natural graphite) can no longer meet the design improvement of high-energy-density batteries. Silicon-based materials as high-energy-density negative electrode materials have become a new focus for enterprises and various scientific research institutes. And among the currently known materials, the specific capacity is the highest (4200mAh / g), which is much larger than the theoretical capacity of carbon materials (372mAh / g); at the same time, silicon is more reliable as a negative electrode than graphite in terms of safety, but silicon is directly used as a negative electrode material. The lithium insertion potential of silicon is low, the cost is very high, and the requirements for the production environment are also very high. At the same time, the SEI film on the surface of silicon particles breaks and regenerates, which will consume a lot of lithium, resulting in low initial efficiency and it is difficult to release production capacity in the short term. By mixing silicon-based materials with carbon materials, the lithium insertion capacity is effectively solved and the electronic conductivity is improved.
[0003] Patent Publication No. CN115312699A discloses carbon silicon negative electrode active materials and secondary batteries. The use of silicon-based carbon doping can further inhibit the expansion of silicon negative electrodes, effectively increase the lithium insertion capacity, thereby reducing the internal resistance of the battery and increasing the energy density of the battery. At the same time, it can increase the roller compaction, reduce the crushing of active material particles, improve the problem of too small porosity, form a carbon coating layer on the surface to reduce the specific surface area of the carbon layer, and better stabilize the irreversible loss caused by the SEI film. This further improves the first coulomb efficiency and energy density issues. Carbon materials can be used to elastically buffer the expansion and contraction of the volume during the charge and discharge process, thereby increasing the reversible capacity of the silicon negative electrode material of the lithium-ion battery and increasing the cycle stability.
[0004] Patent publication number CN110697685B discloses a silicon-carbon negative electrode active material and a preparation method thereof, a silicon-carbon negative electrode material, and a lithium-ion battery, including: mixing metal catalyst powder and silicon powder, and ball milling under an inert atmosphere to obtain silicon particles with metal catalyst particles evenly distributed on the surface; mixing a carbon source and the silicon particles with metal catalyst particles evenly distributed on the surface to obtain a mixed material; carbonizing the mixed material under an inert atmosphere to obtain a silicon-carbon negative electrode active material. The surface of the silicon particles is evenly coated with a point-line combined conductive network of one-dimensional linear carbon nanotubes and composite point-like metal particles, and the coating layer is complete and uniform. The embodiment of the present invention adopts a method of in-situ generating a carbon nanotube coating layer on the surface of silicon particles, which not only simplifies the preparation process, but also can obtain a more uniform carbon nanotube coating layer structure.
[0005] It can be seen from the above scheme that during the charge and discharge process of the silicon-carbon negative electrode active material, silicon will undergo significant volume changes, causing the volume expansion of the material, causing problems with the integrity of the electrode structure, and reducing the cycle life of the silicon-carbon negative electrode active material. Summary of the invention
[0006] The object of the present invention is to provide a silicon-carbon negative electrode active material and a preparation method thereof to solve the problems raised in the above background technology.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a silicon-carbon negative electrode active material and a preparation method thereof, comprising the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, the graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass; the conductive agent comprises the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, Graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass; the conductive agent includes the following components: 82-90% of carbon black and 8-15% of copper, the binder includes the following components: 40-43% of polyvinylidene fluoride, 24-30% of styrene-butadiene rubber and 25-32% of sodium carboxymethyl cellulose, and the dispersant includes the following components: 52-58% of methyl pyrrolidone, 18-24% of polyethylene glycol and 22-26% of sodium dodecyl sulfate.
[0008] As a preferred technical solution of the present invention, the particle size of the nano silicon powder ranges from 10 to 500 nanometers.
[0009] As a preferred technical solution of the present invention, the graphite particle size ranges from 0.5 to 50 microns.
[0010] As a preferred technical solution of the present invention, the carbon black particle size ranges from 20 to 500 nanometers.
[0011] As a preferred technical solution of the present invention, the particle size of the copper is in the range of 100 to 1000 nanometers.
[0012] As a preferred technical solution of the present invention, the mass ratio of the total mass of the polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose to the mass ratio of deionized water is 1:1.
[0013] As a preferred technical solution of the present invention, the preparation method is as follows:
[0014] (1) The prepared carbon black and copper were mixed according to the proportion, and stirred in a mixer at a speed of 1500 rpm for 30 minutes to ensure uniform mixing, thereby obtaining a conductive agent mixture.
[0015] (2) The prepared polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in proportion, and deionized water is added to form a viscous slurry. The slurry is heated in a mixer and maintained at 60° C. and stirred at 1000 rpm for 1 hour to ensure that all components are fully dissolved and mixed, thereby obtaining a binder mixture.
[0016] (3) The prepared methyl pyrrolidone, polyethylene glycol and sodium lauryl sulfate were mixed according to a certain proportion, and stirred in a blender at a speed of 1000 rpm until uniform, to obtain a dispersant mixture.
[0017] (4) Mix the prepared nano-silicon powder and graphite according to the proportion, and dry-mix them in a blender at a speed of 1500 rpm for 15 minutes.
[0018] (5) Add the prepared conductive agent mixture to the mixture of nano-silicon powder and graphite, and continue stirring at a speed of 1500 rpm for 15 minutes.
[0019] (6) Slowly add the binder mixture and the dispersant mixture to adjust the viscosity and dispersibility of the slurry. Continue stirring at a speed of 1500 rpm for 1 hour to ensure that all components are evenly mixed to obtain a silicon-carbon negative electrode active material slurry.
[0020] (6) The prepared silicon-carbon negative electrode active material slurry is evenly coated on the metal current collector.
[0021] (7) The coated electrode sheet is placed in an oven and dried at 80° C. for 12 hours to ensure that the moisture in the slurry is completely removed to obtain a silicon-carbon negative electrode active material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention adds 12% copper and 88% carbon black to the conductive agent, which not only reduces the internal resistance, improves the transmission efficiency of electrons in the negative electrode material, and enhances the charge and discharge performance of the battery, but also helps to buffer the volume expansion, thereby maintaining the integrity of the electrode structure, reducing the occurrence of side reactions, extending the cycle life and safety of the battery, and can significantly reduce the irreversible expansion rate during charging. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Flow chart of the method for preparing the silicon-carbon negative electrode active material of the present invention;
[0025] Figure 2 This is a scanning electron microscope image of the silicon-carbon negative electrode active material of the present invention;
[0026] Figure 3 It is a curve diagram of the charge and discharge voltage and expansion thickness change of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] See also Figure 1 , Figure 2 and Figure 3 The present invention provides a technical solution of a silicon-carbon negative electrode active material and a preparation method thereof: the materials include the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, the graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass; the conductive agent includes the following components: 82-90% of carbon black and 8-15% of copper, the binder includes the following components: 40-43% of polyvinylidene fluoride, 24-30% of styrene-butadiene rubber and 25-32% of sodium carboxymethyl cellulose, and the dispersant includes the following components: 52-58% of methyl pyrrolidone, 18-24% of polyethylene glycol and 22-26% of sodium dodecyl sulfate.
[0029] In some specific embodiments of the present invention, the nano silicon powder can be used as the main active material, and the nano silicon powder has a high specific capacity, which can significantly improve the energy density of the battery. At the same time, the nano size helps to alleviate the huge volume change of silicon during the charging and discharging process and improve the structural stability.
[0030] In some specific embodiments of the present invention: the graphite can be used as the main conductive and structural support material to provide good conductivity and structural stability, and the composite with silicon powder can buffer the volume expansion of silicon and maintain the integrity of the electrode.
[0031] In some specific embodiments of the present invention: the conductive agent constructs a conductive network between the active materials, improves the overall conductivity of the electrode, and ensures the rapid transmission of lithium ions and electrons during the charging and discharging process.
[0032] In some specific embodiments of the present invention: the addition of the carbon black into the mixture can significantly improve the overall electrical conductivity, and the carbon black particles with a smaller particle size can fill the tiny gaps in the material, thereby enhancing the density and mechanical strength of the material.
[0033] In some specific embodiments of the present invention, the copper added to the silicon-carbon negative electrode active material can effectively improve the conductivity of the material, help reduce internal resistance, improve the transmission efficiency of electrons in the negative electrode material, and enhance the charge and discharge performance of the battery.
[0034] In some specific embodiments of the present invention, the copper promotes the diffusion and reaction of lithium ions in the silicon-carbon negative electrode material. By reducing the energy barrier of lithium ion embedding and de-embedding, the addition of copper can improve the charge and discharge of the silicon-based negative electrode and improve the capacity and rate performance of the battery.
[0035] In some specific embodiments of the present invention, the copper can have a positive effect on the structural stability of the silicon-carbon negative electrode material. During the charge and discharge process, silicon undergoes significant volume changes, and the addition of copper helps to buffer the volume expansion, thereby maintaining the integrity of the electrode structure and extending the cycle life of the battery.
[0036] In some specific embodiments of the present invention, the copper can affect the interface properties between the silicon-carbon negative electrode and the electrolyte, which helps to form a more stable solid electrolyte interface, reduce the occurrence of side reactions, and improve the safety and cycle stability of the battery.
[0037] In some specific embodiments of the present invention: the binder can tightly bind the active material, the conductive agent, etc. together to form a stable electrode structure, and enhance the mechanical strength of the electrode to prevent powdering or falling off during the charge and discharge process.
[0038] In some specific embodiments of the present invention, the mass ratio of the total mass of the polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose to the mass ratio of deionized water is 1:1.
[0039] In some specific embodiments of the present invention: the dispersant can help the components to be evenly dispersed during the slurry preparation process to avoid agglomeration, and adjust the viscosity of the slurry to facilitate coating and subsequent processing.
[0040] In some specific embodiments of the present invention: the polyethylene glycol is a non-ionic surfactant, sodium dodecyl sulfate is an anionic surfactant, the anionic surfactant and the non-ionic surfactant can form mixed micelles in the solution, the formation of mixed micelles can reduce the electrostatic repulsion between the charged surfactant head groups, facilitate the formation of mixed micelles, improve the surface activity of the solution, and increase the dispersion effect.
[0041] Embodiment 1:
[0042] A silicon-carbon negative electrode active material, comprising the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, the graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass;
[0043] The conductive agent comprises the following components:
[0044] Carbon black 88%
[0045] Copper 12%
[0046] The binder comprises the following components:
[0047] Polyvinylidene fluoride 42%
[0048] Styrene butadiene rubber 27%
[0049] Sodium carboxymethyl cellulose 31%
[0050] The dispersant comprises the following components:
[0051] Methylpyrrolidone 56%
[0052] Polyethylene glycol 20%
[0053] Sodium Lauryl Sulfate 24%
[0054] (1) The prepared carbon black and copper were mixed according to the proportion, and stirred in a mixer at a speed of 1500 rpm for 30 minutes to ensure uniform mixing, thereby obtaining a conductive agent mixture.
[0055] (2) The prepared polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in proportion, and deionized water is added to form a viscous slurry. The slurry is heated in a mixer and maintained at 60° C. and stirred at 1000 rpm for 1 hour to ensure that all components are fully dissolved and mixed, thereby obtaining a binder mixture.
[0056] (3) The prepared methyl pyrrolidone, polyethylene glycol and sodium lauryl sulfate were mixed according to a certain proportion, and stirred in a blender at a speed of 1000 rpm until uniform, to obtain a dispersant mixture.
[0057] (4) Mix the prepared nano-silicon powder and graphite according to the proportion, and dry-mix them in a blender at a speed of 1500 rpm for 15 minutes.
[0058] (5) Add the prepared conductive agent mixture to the mixture of nano-silicon powder and graphite, and continue stirring at a speed of 1500 rpm for 15 minutes.
[0059] (6) Slowly add the binder mixture and the dispersant mixture to adjust the viscosity and dispersibility of the slurry. Continue stirring at a speed of 1500 rpm for 1 hour to ensure that all components are evenly mixed to obtain a silicon-carbon negative electrode active material slurry.
[0060] (6) The prepared silicon-carbon negative electrode active material slurry is evenly coated on the metal current collector.
[0061] (7) The coated electrode sheet is placed in an oven and dried at 80° C. for 12 hours to ensure that the moisture in the slurry is completely removed to obtain a silicon-carbon negative electrode active material.
[0062] Embodiment 2:
[0063] On the basis of Example 1, a silicon-carbon negative electrode active material comprises the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, the graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass;
[0064] The conductive agent comprises the following components:
[0065] Carbon black 85%
[0066] Copper 15%
[0067] The binder comprises the following components:
[0068] Polyvinylidene fluoride 42%
[0069] Styrene butadiene rubber 27%
[0070] Sodium carboxymethyl cellulose 31%
[0071] The dispersant comprises the following components:
[0072] Methylpyrrolidone 56%
[0073] Polyethylene glycol 20%
[0074] Sodium Lauryl Sulfate 24%
[0075] (1) The prepared carbon black and copper were mixed according to the proportion, and stirred in a mixer at a speed of 1500 rpm for 30 minutes to ensure uniform mixing, thereby obtaining a conductive agent mixture.
[0076] (2) The prepared polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in proportion, and deionized water is added to form a viscous slurry. The slurry is heated in a mixer and maintained at 60° C. and stirred at 1000 rpm for 1 hour to ensure that all components are fully dissolved and mixed, thereby obtaining a binder mixture.
[0077] (3) The prepared methyl pyrrolidone, polyethylene glycol and sodium lauryl sulfate were mixed according to a certain proportion, and stirred in a blender at a speed of 1000 rpm until uniform, to obtain a dispersant mixture.
[0078] (4) Mix the prepared nano-silicon powder and graphite according to the proportion, and dry-mix them in a blender at a speed of 1500 rpm for 15 minutes.
[0079] (5) Add the prepared conductive agent mixture to the mixture of nano-silicon powder and graphite, and continue stirring at a speed of 1500 rpm for 15 minutes.
[0080] (6) Slowly add the binder mixture and the dispersant mixture to adjust the viscosity and dispersibility of the slurry. Continue stirring at a speed of 1500 rpm for 1 hour to ensure that all components are evenly mixed to obtain a silicon-carbon negative electrode active material slurry.
[0081] (6) The prepared silicon-carbon negative electrode active material slurry is evenly coated on the metal current collector.
[0082] (7) The coated electrode sheet is placed in an oven and dried at 80° C. for 12 hours to ensure that the moisture in the slurry is completely removed to obtain a silicon-carbon negative electrode active material.
[0083] Embodiment three:
[0084] On the basis of Example 1, a silicon-carbon negative electrode active material comprises the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, the graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass;
[0085] The conductive agent comprises the following components:
[0086] Carbon black 91%
[0087] Copper 9%
[0088] The binder comprises the following components:
[0089] Polyvinylidene fluoride 42%
[0090] Styrene butadiene rubber 27%
[0091] Sodium carboxymethyl cellulose 31%
[0092] The dispersant comprises the following components:
[0093] Methylpyrrolidone 56%
[0094] Polyethylene glycol 20%
[0095] Sodium Lauryl Sulfate 24%
[0096] (1) The prepared carbon black and copper were mixed according to the proportion, and stirred in a mixer at a speed of 1500 rpm for 30 minutes to ensure uniform mixing, thereby obtaining a conductive agent mixture.
[0097] (2) The prepared polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in proportion, and deionized water is added to form a viscous slurry. The slurry is heated in a mixer and maintained at 60° C. and stirred at 1000 rpm for 1 hour to ensure that all components are fully dissolved and mixed, thereby obtaining a binder mixture.
[0098] (3) The prepared methyl pyrrolidone, polyethylene glycol and sodium lauryl sulfate were mixed according to a certain proportion, and stirred in a blender at a speed of 1000 rpm until uniform, to obtain a dispersant mixture.
[0099] (4) Mix the prepared nano-silicon powder and graphite according to the proportion, and dry-mix them in a blender at a speed of 1500 rpm for 15 minutes.
[0100] (5) Add the prepared conductive agent mixture to the mixture of nano-silicon powder and graphite, and continue stirring at a speed of 1500 rpm for 15 minutes.
[0101] (6) Slowly add the binder mixture and the dispersant mixture to adjust the viscosity and dispersibility of the slurry. Continue stirring at a speed of 1500 rpm for 1 hour to ensure that all components are evenly mixed to obtain a silicon-carbon negative electrode active material slurry.
[0102] (6) The prepared silicon-carbon negative electrode active material slurry is evenly coated on the metal current collector.
[0103] (7) The coated electrode sheet is placed in an oven and dried at 80° C. for 12 hours to ensure that the moisture in the slurry is completely removed to obtain a silicon-carbon negative electrode active material.
[0104] Comparative Example 1: Carbon-silicon negative electrode active material and secondary battery and Comparative Example 2: A silicon-carbon negative electrode active material and a preparation method thereof, a silicon-carbon negative electrode material, and a lithium-ion battery, all of which do not add copper to the conductive agent.
[0105] The present invention provides a silicon-carbon negative electrode active material and a preparation method thereof. The silicon-carbon negative electrode active materials obtained in Examples 1 to 3 and Comparative Examples 1 to 2 are subjected to performance tests. According to the corresponding national testing standards, the performance test results of the silicon-carbon negative electrode active materials are as follows:
[0106]
[0107] From the above data, it can be concluded that by adding 12% copper and 88% carbon black to the conductive agent, it can not only reduce the internal resistance, improve the transmission efficiency of electrons in the negative electrode material, and enhance the charge and discharge performance of the battery, but also help buffer the volume expansion, thereby maintaining the integrity of the electrode structure, reducing the occurrence of side reactions, and extending the cycle life and safety of the battery.
[0108] Initial charge irreversible expansion rate (%) Mid-term charging irreversible expansion rate (%) Irreversible expansion rate after late charging (%) Embodiment 1 3.4 8.6 18.4 Embodiment 2 3.6 8.7 18.9 Embodiment 3 4.1 9.1 18.8 Comparative Example 1 4.7 9.5 20.1 Comparative Example 2 4.4 10.1 22.3
[0109] The above data show that by adding 12% copper and 88% carbon black to the conductive agent, the irreversible expansion rate during charging can be significantly reduced.
[0110] Carbon black complies with the standards of GB / T 3782;
[0111] Copper complies with the standards of GB / T 5231-2012;
[0112] The polyvinylidene fluoride model is PVDFR909W;
[0113] The model of sodium carboxymethyl cellulose is MAC350HC;
[0114] The model of styrene butadiene rubber is 307R;
[0115] The model of polyethylene glycol is PEG-800.
[0116] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A silicon-carbon negative electrode active material, comprising the following components: nano silicon powder, graphite, a conductive agent, a binder and a dispersant, wherein the nano silicon powder accounts for 35% of the total mass, the graphite accounts for 40% of the total mass, the conductive agent accounts for 14% of the total mass, the binder accounts for 6% of the total mass, and the dispersant accounts for 5% of the total mass; The conductive agent comprises the following components: Carbon black 82~90% Copper 8~15% The binder comprises the following components: Polyvinylidene fluoride 40~43% Styrene butadiene rubber 24~30% Sodium carboxymethyl cellulose 25-32% The dispersant comprises the following components: Methylpyrrolidone 52~58% Polyethylene glycol 18-24% Sodium dodecyl sulfate 22-26% The above percentages are mass percentages.
2. A silicon-carbon negative electrode active material according to claim 1, characterized in that: The particle size of the nano silicon powder ranges from 10 to 500 nanometers.
3. The silicon-carbon negative electrode active material according to claim 1, characterized in that: The graphite particle size ranges from 0.5 to 50 microns.
4. The silicon-carbon negative electrode active material according to claim 1, characterized in that: The carbon black particle size ranges from 20 to 500 nanometers.
5. The silicon-carbon negative electrode active material according to claim 1, characterized in that: The copper particle size ranges from 100 to 1000 nanometers.
6. The silicon-carbon negative electrode active material according to claim 1, characterized in that: The mass ratio of the total mass of the polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose to the mass of deionized water is 1:
1.
7. A method for preparing a silicon-carbon negative electrode active material, the preparation method is as follows: (1) The prepared carbon black and copper were mixed according to the proportion, and stirred in a mixer at a speed of 1500 rpm for 30 minutes to ensure uniform mixing, thereby obtaining a conductive agent mixture. (2) The prepared polyvinylidene fluoride, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in proportion, and deionized water is added to form a viscous slurry. The slurry is heated in a mixer and maintained at 60° C. and stirred at 1000 rpm for 1 hour to ensure that all components are fully dissolved and mixed, thereby obtaining a binder mixture. (3) The prepared methyl pyrrolidone, polyethylene glycol and sodium lauryl sulfate were mixed according to a certain proportion, and stirred in a blender at a speed of 1000 rpm until uniform, to obtain a dispersant mixture. (4) Mix the prepared nano-silicon powder and graphite according to the proportion, and dry-mix them in a blender at a speed of 1500 rpm for 15 minutes. (5) Add the prepared conductive agent mixture to the mixture of nano-silicon powder and graphite, and continue stirring at a speed of 1500 rpm for 15 minutes. (6) Slowly add the binder mixture and the dispersant mixture to adjust the viscosity and dispersibility of the slurry. Continue stirring at a speed of 1500 rpm for 1 hour to ensure that all components are evenly mixed to obtain a silicon-carbon negative electrode active material slurry. (6) The prepared silicon-carbon negative electrode active material slurry is evenly coated on the metal current collector. (7) The coated electrode sheet is placed in an oven and dried at 80° C. for 12 hours to ensure that the moisture in the slurry is completely removed to obtain a silicon-carbon negative electrode active material.
Citation Information
Patent Citations
Electrode composition, method of making the same, and lithium ion battery including the same
CN101454927A
Metal conductive agent and lithium ion battery using conductive agent
CN105244509A
Silicon-carbon composite negative electrode material and manufacturing method thereof
CN112510185A
Lithium ion battery negative electrode and preparation method thereof
CN115548343A
Silicon-carbon negative electrode slurry, preparation method thereof and lithium ion battery
CN115810739A