Lithium supplement material and preparation method thereof, positive electrode material and secondary battery

By introducing electron-delivery groups and transition metal ions into the organic lithium salt, the problem of high delitting potential of the positive electrode lithium supplement material is solved, and the performance of lithium-ion batteries is improved, reducing the difficulty of lithium-ion removal and the working voltage of the battery is carried out. Range limit.

CN119069708APending Publication Date: 2024-12-03SHENZHEN DYNANONIC INNOVAZONE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411343659.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The delitting potential of existing positive electrode lithium supplement materials is high, which makes it more difficult to apply organic lithium salts outside the commonly used operating voltage range.

Method used

Introducing electron donor groups and transition metal ions into the organolithium salt, providing electron density through conjugation or electronegativity, weakening the binding strength of O-Li bonds and reducing the difficulty of extrusion of lithium ions.

Benefits of technology

It effectively reduces the deliquency potential of organic lithium salts, improves the first charge and discharge efficiency and capacity of lithium-ion batteries, promotes the decomposition kinetics of materials, and enhances the conductivity and practical value of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069708A_ABST
    Figure CN119069708A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery, the lithium material comprises an organic lithium salt, and the organic lithium salt comprises an electron donating group. The organic lithium salt has relatively low lithium removal potential under the action of an electron-donating group, and can fully release capacity under relatively low potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery. Background Art

[0002] Positive electrode lithium supplement materials can make up for the irreversible capacity loss caused by the formation of solid electrolyte interface film during the first charging process of lithium-ion batteries. It is one of the key technologies to improve the performance of lithium-ion batteries and has a broad application market and development prospects. However, there are also some problems with positive electrode lithium supplement materials. For example, the existing positive electrode lithium supplement materials mainly use inorganic transition metal lithium-rich compounds (transition metal oxide lithium salts), such as Li6CoO4, Li2NiO2 and Li5FeO4. However, these lithium-rich compounds have the disadvantages of low air stability and complex operation process, which is not conducive to large-scale production.

[0003] In contrast, lithium-replenishing materials based on organic lithium salts have greater advantages. Organic lithium salts have advantages such as high capacity, good air stability, excellent solvent compatibility, low cost, etc., and have higher practical value, so they are expected to become the most promising positive electrode lithium-replenishing materials. However, the low electrochemical activity of organic lithium salts leads to a high delithiation potential. Such a high voltage exceeds the commonly used operating voltage range of existing battery systems, increasing the difficulty of applying organic lithium salts, so how to reduce the delithiation potential of organic lithium salts has become the key. Summary of the invention

[0004] The purpose of the present application is to provide a lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery to solve the problem of high decomposition potential of organic lithium salts.

[0005] To achieve the purpose of this application, this application provides the following technical solutions:

[0006] In a first aspect, the present invention provides a lithium supplement material, wherein the lithium supplement material comprises an organic lithium salt, and the organic lithium salt comprises an electron donating group.

[0007] The present invention introduces an electron-donating group 12 into the organic lithium salt 10, and the electron-donating group 12 is actually a functional group grafted onto the organic lithium salt 10. The electron-donating group 12 has the ability to provide electrons, and can provide electron density to the lithium ions on the organic lithium salt 10 through conjugation or electronegativity of atoms. The electrons provided by the electron-donating group 12 can greatly weaken the binding strength of the O-Li bond, thereby reducing the difficulty of lithium ion escape, so that the delithiation potential of the organic lithium salt 10 is reduced.

[0008] In one embodiment, the lithium supplement material further includes transition metal ions, and the transition metal ions are doped in the organic lithium salt and replace part of the lithium ions in the organic lithium salt.

[0009] In one embodiment, the molecular formula of the organic lithium salt doped with the transition metal comprises: a H b O c (Li d1 M d2 ) k , wherein M includes at least one of Co, Ni, Mn, Fe, Cu, Mg, Cr, Zn, Ti, and Zr, 1≤a≤5, 1≤b≤7, 2≤c≤8, 0.8≤d1<1, 0<d2≤0.1, 1≤k≤4, and a, b, c, and k are all integers.

[0010] In one embodiment, the organic lithium salt comprises a carboxylic acid organic lithium salt, and the general structural formula of the carboxylic acid organic lithium salt comprises: (COOLi d1 M d2 ) n R1, wherein n≥1, R1 is the electron-donating group, and R1 includes at least one of a methyl group, a methylene group, a methine group, a carbonyl group, and a hydroxyl group.

[0011] In one embodiment, the organic lithium salt comprises CH3-COOLi d1 M d2 、CH2OH-COOLi d1 M d2 、(COOLi d1 M d2 )2(CH2) m , (COOLi d1 M d2 )2C=O,(COOLi d1 M d2 )2CHOH, wherein 1≤m≤3.

[0012] In one embodiment, the organic lithium salt comprises a non-carboxylic acid organic lithium salt, and the general structural formula of the non-carboxylic acid organic lithium salt comprises: (R2R3R4COLi d1 M d2 ) n , wherein C is directly single-bonded to R2, R3, R4 and the oxygen atom, 1≤n≤3, at least one of R2, R3 and R4 is the electron-donating group, and R2, R3 and R4 independently include at least one of a methyl group, an aldehyde group, a hydroxyl group and a hydrogen atom.

[0013] In one embodiment, the particle size D50 of the primary particles of the lithium supplementing material is 50 nm to 500 nm.

[0014] In one embodiment, the particle size D50 of the secondary particles of the lithium supplementing material is 500 nm to 4 μm.

[0015] In a second aspect, the present invention provides a method for preparing a lithium-supplementing material, comprising: mixing a lithium-containing compound and an electron-donating group precursor in proportion to obtain a lithium-supplementing mixture; after the lithium-supplementing mixture is fully reacted, the lithium-supplementing mixture is converted into an organic lithium salt, and the lithium-supplementing material is obtained, wherein the organic lithium salt includes an electron-donating group.

[0016] In one embodiment, the lithium-containing compound and the electron-donating group precursor are mixed in proportion to obtain a lithium-replenishing mixture, including: the organic compound, the lithium source, and the transition metal source are mixed in proportion to obtain a lithium-replenishing mixture, the organic compound includes the electron-donating group, and the transition metal ions are doped in the lithium-replenishing mixture.

[0017] In a third aspect, the present invention further provides a positive electrode material, which includes a positive electrode active material and a lithium supplement material, wherein the lithium supplement material includes the lithium supplement material described in the first aspect, or the positive electrode material includes the lithium supplement material obtained by the preparation method of the lithium supplement material described in the second aspect.

[0018] In a fourth aspect, the present invention further provides a secondary battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the positive electrode material described in the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0020] Figure 1 is a schematic diagram of the cross-sectional structure of a lithium supplement material according to an embodiment;

[0021] Figure 2 is a flow chart of a method for preparing a lithium supplement material according to an embodiment;

[0022] Figure 3 It is a flow chart of a method for preparing lithium supplement materials according to another embodiment. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0024] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.

[0025] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.

[0026] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0027] The present invention provides a lithium supplement material, please refer to Figure 1 The lithium supplement material includes an organic lithium salt 10 , and the organic lithium salt 10 includes an electron donating group 12 .

[0028] Specifically, the organic lithium salt 10 is the main body for lithium supplementation, which can contribute a large amount of lithium ions. During the first charging process, the lithium in the organic lithium salt 10 can be released and migrated to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby increasing the total capacity and energy density of the battery. However, most of the existing high-capacity organic lithium salts 10 have problems of low electrochemical activity and high desorption potential. For example, lithium oxalate (Li2C2O4) has a high theoretical specific capacity and is considered to be a positive electrode lithium supplement material with great application prospects. However, lithium oxalate has poor electrochemical activity, the actual capacity is far lower than the theoretical value, and the delithiation potential is high (>4.7V), which cannot match most commercial positive electrode materials, greatly hindering its commercial application. Therefore, promoting the capacity of such organic lithium salts 10 and reducing their delithiation potential are of great significance to the commercialization of lithium supplementation technology.

[0029] In order to solve the problem of high delithiation potential in the organic lithium salt 10, the present invention introduces an electron donating group 12 into the organic lithium salt 10, and the electron donating group 12 is actually a functional group grafted onto the organic lithium salt 10. The electron donating group 12 has the ability to provide electrons, and can provide electron density to the lithium ions on the organic lithium salt 10 through conjugation or atomic electronegativity. The electrons provided by the electron donating group 12 can greatly weaken the binding strength of the O-Li bond, thereby reducing the difficulty of lithium ion extraction, so that the delithiation potential of the organic lithium salt 10 is reduced.

[0030] Optionally, the electron-donating group 12 includes an amino group (-NH2), a hydroxyl group (-OH), an alkoxy group (-OR), an alkyl group (-R), etc. These groups can increase the electron density of the organic lithium salt 10, so that the organic lithium salt 10 exhibits a stronger nucleophilicity. For example, a hydroxyl group (-OH) is a group composed of an oxygen atom and a hydrogen atom, has a higher electron density, can increase the nucleophilicity of the organic lithium salt 10, and participate in the formation of hydrogen bonds.

[0031] In one embodiment, the lithium supplement material further includes transition metal ions 11 , which are doped in the organic lithium salt 10 and replace part of the lithium ions in the organic lithium salt 10 .

[0032] On the basis of introducing the electron-donating group 12, the present invention further dopes the organic lithium salt 10 with transition metal ions 11, and uses the transition metal ions 11 to replace part of the lithium ions, so that the delithiation potential of the organic lithium salt 10 is reduced. The transition metal ions 11 are doped into the organic lithium salt 10 to replace the position of the lithium ions, thereby stimulating the catalytic effect of the transition metal ions 11 and inducing the organic lithium salt 10 to form defects, thereby changing the chemical bond strength of the organic lithium salt 10, making the O-Li bond strength weaker, and then transforming the organic lithium salt 10 from an inherent insulator into a lithium-supplementing material with stronger conductivity and easier decomposition, thereby significantly promoting the decomposition kinetics of the organic lithium salt 10. In a specific embodiment, the transition metal ions 11 include at least one of Co, Ni, Mn, Fe, Cu, Mg, Cr, Zn, Ti, and Zr.

[0033] The lithium supplement material provided by the present invention includes an organic lithium salt 10 and a transition metal ion 11, and the transition metal ion 11 is doped in the organic lithium salt 10, and the organic lithium salt 10 also includes an electron-donating group 12. The lithium supplement material has the following advantages: 1) the transition metal ion 11 in the organic lithium salt 10 has a catalytic effect, and can catalyze the decomposition of the organic lithium salt 10, thereby reducing the delithiation potential of the organic lithium salt 10; 2) the electron-donating effect of the electron-donating group 12 and the transition metal ion 11 jointly weaken the O-Li bond, and both of them form a certain degree of competition for the electron cloud of oxygen, resulting in the weakening of the O-Li bond; and the transition metal ion 11 has a large positive charge, which forms a certain degree of repulsion for lithium ions, which also weakens the bond energy of the O-Li bond; 3) the organic lithium salt 10 can have good synergy with the positive electrode active material, which helps to reduce the initial charge and discharge capacity loss and improve the initial charge and discharge efficiency of the lithium-ion battery.

[0034] In the prior art, organic lithium salts include LiOOC-CH2-COOLi, LiOOC-CO-COOLi, and OH-CO-O-Li. Based on these organic lithium salts, they can be used as positive electrode lithium supplements by substitution with electrophilic groups and / or doping at the Li position.

[0035] In one embodiment, the molecular formula of the transition metal-doped organic lithium salt 10 includes: a H b O c (Li d1 M d2 ) k , wherein M includes at least one of Co, Ni, Mn, Fe, Cu, Mg, Cr, Zn, Ti, and Zr, 1≤a≤5, 1≤b≤7, 2≤c≤8, 0.8≤d1<1, 0<d2≤0.1, 1≤k≤4, and a, b, c, and k are all integers.

[0036] Specifically, the organic lithium salt 10 provided by the present invention can be modified based on lithium oxalate (Li2C2O4) in the prior art, and an electron-donating group 12 and a transition metal ion 11 are further introduced on the basis of lithium oxalate, so that the molecular formula of the organic lithium salt 10 can be obtained as C a H b O c (Li d1 M d2 ) k . Wherein, M in the molecular formula is the transition metal ion 11 mentioned above, so the type of M is not described here. Due to the introduction of the electron-donating group 12, the organic lithium salt 10 provided by the present invention needs to be distinguished from the lithium oxalate (Li2C2O4) and transition metal-doped lithium oxalate in the prior art; the present invention can effectively reduce the delithiation potential of the lithium supplement material through the synergistic effect of the electron-donating group 12 and the transition metal.

[0037] Furthermore, the present invention controls the content of transition metal ions 11 doped in the organic lithium salt 10 within the above range, and can obtain a lithium supplement material with high lithium supplement capacity and low separation potential. When the content of transition metal ions 11 is greater than the above range (d2>0.1), the content of transition metal ions 11 increases, resulting in a decrease in lithium ion content and a decrease in lithium supplement capacity; when the content of transition metal is less than the above range (d2<0.01), the catalytic effect of transition metal ions 11 deteriorates, and it is difficult to control the reaction process if the doping is too low.

[0038] In one embodiment, the organic lithium salt 10 includes a carboxylic acid organic lithium salt, and the general structural formula of the carboxylic acid organic lithium salt includes: (COOLi d1 M d2 ) n R1, wherein n≥1, R1 is an electron-donating group 12, and R1 includes at least one of a methyl group (-CH3), a methylene group (-CH2-), a methine group (-CH-), a carbonyl group (-C=O), and a hydroxyl group (-OH).

[0039] The carboxylic acid organic lithium salt should contain a molecular structure as shown in Formula I:

[0040]

[0041] Formula I:

[0042] Specifically, in the carboxylic acid organic salt, the lithium ion and the transition metal ion 11 are connected to the carboxyl group (-COOH) and replace the hydrogen atom in the carboxyl group, and the substituted carboxylate is connected to the electron-donating group 12, and R1 is the electron-donating group 12 introduced into the organic lithium salt 10. For example, hydroxyl is a common and important polar functional group, which itself has nucleophilicity and can provide electrons to O-Li, thereby weakening the binding strength and allowing the lithium ion to be quickly released. In a specific embodiment, n=1 or n=2 or n=3 or n=4.

[0043] In a specific embodiment, the organic lithium salt 10 may include CH3-COOLi d1 M d2 、CH2OH-COOLi d1 M d2 、(COOLi d1 M d2 )2(CH2) m , (COOLi d1 M d2 )2C=O,(COOLi d1 M d2 )2CHOH, wherein (COOLi d1 M d2)2(CH2) m In the expression, m≥1, specifically, m=1, m=2, or m=3.

[0044] In one embodiment, the organic lithium salt 10 includes a non-carboxylic acid organic lithium salt, and the general structural formula of the non-carboxylic acid organic lithium salt includes: (R2R3R4COLi d1 M d2 ) n , wherein C and R2, R3, R4 and the oxygen atom are directly connected by single bonds, 1≤n≤3, at least one of R2, R3, and R4 is an electron-donating group 12, and R2, R3, and R4 independently include at least one of a methyl group (-CH3), an aldehyde group (-CHO), a hydroxyl group (-OH), and a hydrogen atom (-H). R2, R3, and R4 may be the same, and at least one of the three exists.

[0045] The non-carboxylic acid organic lithium salt should contain a molecular structure as shown in Formula II:

[0046]

[0047] Formula II:

[0048] Specifically, in non-carboxylic acid organic salts, lithium ions and transition metal ions 11 are connected to the carbonyl group (C=O). Since the electronegativity of the oxygen atom on the carbonyl group is relatively large, the lithium ions are firmly adsorbed on the oxygen atom and are difficult to release. After the electron donating group 12 is introduced to the carbonyl group, the electron donating group 12 provides electron density to the O-Li bond, so that the adsorption of lithium ions by the oxygen atom is weakened after obtaining extra electrons, thereby allowing the lithium ions to be released at a lower delithiation potential.

[0049] In a specific embodiment, the organic lithium salt 10 may include lithium methoxide (CH3OLi), lithium ethoxide (CH3CH2OLi), and lithium ethylene glycol (LiOCH2-CH2OLi).

[0050] In one embodiment, the lithium supplement material further includes a conductive carrier, which is mixed with the organic lithium salt 10. Optionally, the conductive carrier is coated on the outer layer of the organic lithium salt 10. The conductive carrier includes one or more of conductive carbon black, graphite, hard carbon, soft carbon, graphene, carbon nanotubes, and carbon fibers. Adding a conductive carrier to the lithium supplement material can increase the overall conductivity of the lithium supplement material, thereby improving the electrical properties of the lithium supplement material.

[0051] In one embodiment, the mass ratio of the organic lithium salt 10 to the conductive carrier is (80-95): (5:20). Optionally, the mass ratio of the organic lithium salt 10 to the conductive carrier may be 80:20, 85:15, 90:10, or 95:5. When the mass ratio of the organic lithium salt 10 to the conductive carrier is within the above range, the lithium replenishment capacity and conductivity of the lithium replenishment material can be ensured.

[0052] In one embodiment, the particle size D50 of the primary particles of the lithium supplement material is 50nm to 500nm. Optionally, the particle size D50 of the primary particles of the lithium supplement material can be 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, or 500nm.

[0053] In one embodiment, the particle size D50 of the secondary particles of the lithium supplementing material is 500nm-4μm. Optionally, the particle size D50 of the secondary particles of the lithium supplementing material can be 500nm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, or 4μm.

[0054] When the particle size of the lithium supplement material is within the above range, the specific surface area of ​​the material can be controlled, so that the organic lithium salt 10 and the conductive carrier are in full contact, thereby improving the conductivity and the lithium ion extraction efficiency; in addition, the difficulty of preparing the lithium supplement material can be reduced.

[0055] In one embodiment, the O-Li ion bond energy in the lithium supplement material is 3.1eV-6.8eV. Among them, the O-Li ion bond energy of the lithium supplement material without electron donating groups and without transition metal ion doping is 5.7eV-6.8eV; the O-Li ion bond energy of the lithium supplement material containing only electron donating groups and not doped with transition metal ions is 4.2eV-5.9eV, the O-Li ion bond energy of the lithium supplement material doped only with transition metal ions and without electron donating groups is 4.5eV-5.7eV, and the O-Li ion bond energy of the lithium supplement material containing electron donating groups and doped with transition metal ions is 3.1eV-4.2eV.

[0056] In one embodiment, the present invention also provides a method for preparing a lithium supplement material, please refer to Figure 2 , specifically including the following steps:

[0057] Step S10, mixing the lithium-containing compound and the electron-donating group precursor in proportion to obtain a lithium-supplementing mixture.

[0058] Step S20, after the lithium replenishing mixture is fully reacted, the lithium replenishing mixture is converted into an organic lithium salt, and a lithium replenishing material is obtained, wherein the organic lithium salt includes an electron donating group.

[0059] In one embodiment, a lithium-containing compound and a transition metal source are mixed in proportion to obtain a lithium-supplementing mixture, comprising:

[0060] The lithium-containing compound includes a lithium source and an organic compound, the organic compound includes an electron-donating group, and the organic compound, the lithium source, and the transition metal source are mixed in proportion to obtain a lithium-supplementing mixture.

[0061] Optionally, the type of lithium source is not specifically limited, and can be an inorganic lithium source or an organic lithium source. After the lithium source, the organic compound and the transition metal source are mixed and reacted, the transition metal ions and the electron-donating groups can be introduced into the organic lithium salt at the same time.

[0062] In one embodiment, the present invention also provides a method for preparing a lithium supplement material, please refer to Figure 3 , specifically including the following steps:

[0063] Step SS10, reducing the organic compound precursor to obtain an organic compound, wherein the organic compound includes an electron-donating group.

[0064] Step SS20, mixing the organic compound, the lithium source and the transition metal source in proportion to obtain a lithium supplement mixture.

[0065] Step SS30, after the lithium replenishing mixture is fully reacted, the lithium replenishing mixture is converted into an organic lithium salt, and a lithium replenishing material is obtained.

[0066] The preparation method of the lithium supplement material provided by the present invention can introduce transition metal ions into the obtained organic lithium salt by mixing a lithium-containing compound and a transition metal source and then causing the two to react, and the lithium-containing compound includes an electron-donating group. During the reaction of the two, the electron-donating group also participates in the reaction at the same time, thereby obtaining an organic lithium salt including transition metal ions and electron-donating groups. The organic lithium salt has a lower delithiation potential under the synergistic effect of the transition metal ions and the electron-donating groups, and can fully release capacity at a lower potential.

[0067] In one embodiment, the present invention further provides a positive electrode material, the positive electrode material includes a positive electrode active material and a lithium supplement material. The lithium supplement material includes the composite lithium supplement material provided in the above embodiment. Optionally, the positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material, and in a specific embodiment, includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0068] In one embodiment, the content of the composite lithium-supplementing material in the positive electrode material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just make up for the loss of active lithium in the battery during the first charging process. If the amount of composite lithium-supplementing material added to the positive electrode material is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of composite lithium-supplementing material added to the positive electrode active material is too high, the original reversible capacity will be occupied and the cost will be increased. In some specific embodiments, in the positive electrode material, the mass percentage of the composite lithium-supplementing material can be 1%, 2%, 4%, 6%, etc.

[0069] In one embodiment, the present invention further provides a positive electrode plate, the positive electrode plate includes a current collector and an active material layer disposed on the current collector, the active material layer includes the composite lithium supplement material of any one of the above embodiments. Or the active material layer includes the composite lithium supplement material obtained by the preparation method of the composite lithium supplement material in the above embodiments.

[0070] In one embodiment, the positive electrode sheet includes a positive current collector, and the positive current collector has a positive active layer, and the positive active layer includes components such as positive active materials, composite lithium supplement materials, conductive agents, and binders. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive current collector includes but is not limited to any one of copper foil and aluminum foil. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes, and the content of the conductive agent in the positive active layer is 3wt% to 5wt%. The types of binders include polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive active layer is 2wt% to 4wt%.

[0071] In one embodiment, the present invention also provides a secondary battery, including a positive electrode and a negative electrode electrolyte, wherein the positive electrode and the negative electrode are arranged in the electrolyte, and the negative electrode includes the negative electrode plate provided in the above embodiment. Optionally, the electrolyte includes a liquid electrolyte or a solid electrolyte. If a liquid electrolyte is selected, a diaphragm is also required. During the battery charge and discharge process, the active positive electrode ions are embedded and removed back and forth between the positive electrode and the negative electrode. The electrolyte plays the role of conducting positive electrode ions between the positive electrode and the negative electrode. The diaphragm is arranged between the positive electrode and the negative electrode, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing the positive electrode ions to pass through.

[0072] The technical solution of the present invention is described in detail below through specific embodiments.

[0073] Example 1

[0074] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi 0.9 Co 0.05 and carbon nanotubes (CNT). The particle size D50 of the primary particles of the lithium supplement material is 100 nm, the particle size D50 of the secondary particles of the lithium supplement material is 1 μm, and CH3COOLi 0.9 Co 0.05 The mass ratio of carbon nanotubes is 9: 1. The electron-donating group is methyl (-CH3), connected to carboxyl lithium salt, and the corresponding organic lithium salt without electron-donating group is lithium formate (HCOOLi).

[0075] The preparation method of the composite lithium supplement material comprises the following steps:

[0076] (1) Cobalt acetate ((CH3COO)2Co) and lithium acetate (CH3COOLi) are mixed in a molar ratio of 0.5:9 to obtain a lithium supplement mixture.

[0077] (2) Then, 10% carbon nanotubes are added to the lithium supplement mixture and freeze-dried.

[0078] (3) The freeze-dried product is then placed in a tube furnace, heated to 200°C for drying, and taken out after cooling to room temperature.

[0079] (4) The dried product was placed in a ball mill and ball milled at 60 r / min for 2 h to obtain CH3COOLi 0.9 Co 0.05 .

[0080] Example 2

[0081] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi 0.98 Co 0.01 and carbon nanotubes.

[0082] The difference between the preparation method of the composite lithium supplement material and that of Example 1 is that cobalt acetate ((CH3COO)2Co) and lithium acetate (CH3COOLi) are mixed in a molar ratio of 0.1:9.8.

[0083] Example 3

[0084] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi 0.8 Co 0.1 and carbon nanotubes.

[0085] The difference between the preparation method of the composite lithium supplement material and that of Example 1 is that cobalt acetate ((CH3COO)2Co) and lithium acetate (CH3COOLi) are mixed in a molar ratio of 1:8.

[0086] Example 4

[0087] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi 0.6 Co 0.2 Carbon nanotubes.

[0088] The difference between the preparation method of the composite lithium supplement material and that of Example 1 is that cobalt acetate ((CH3COO)2Co) and lithium acetate (CH3COOLi) are mixed in a molar ratio of 2:6.

[0089] Example 5

[0090] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi 0.9 Ni 0.05 and carbon nanotubes.

[0091] The difference between the preparation method of the composite lithium supplement material and that of Example 1 is that cobalt acetate is replaced with nickel acetate ((CH3COO)2Ni).

[0092] Example 6

[0093] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi 0.9 Co 0.05 .

[0094] The difference between the preparation method of the composite lithium supplement material and that of Example 1 is that step (2) is not performed.

[0095] Example 7

[0096] This embodiment provides a lithium supplement material. The lithium supplement material includes Li 0.9 Co 0.05 OOC-CO-COOLi 0.9 Co 0.05 The particle size D50 of the primary particles of the lithium supplement material is 120 nm, and the particle size D50 of the secondary particles of the lithium supplement material is 1.5 μm.

[0097] The preparation method of the composite lithium supplement material comprises the following steps:

[0098] (1) Disperse sodium methoxysalicylate in 50% ethanol, add an appropriate amount of sulfuric acid, evaporate to dryness under reduced pressure, and extract with 100% ethanol to obtain (HO)2C(COOH)2.

[0099] (2) Then (HO)2C(COOH)2 was reacted with excess LiOH and Co(OH)2, wherein the molar ratio of Co(OH)2 to LiOH was 0.5:9, and washed by centrifugation with ethanol three times to obtain Li 0.9 Co 0.05OOC-CO-COOLi 0.9 Co 0.05 .

[0100] Example 8

[0101] This embodiment provides a lithium supplement material. The lithium supplement material includes Li 0.98 Co 0.01 OOC-CO-COOLi 0.98 Co 0.01 .

[0102] The difference between the preparation method of the composite lithium supplement material and that of Example 6 is that the molar ratio of Co(OH)2 to LiOH is 0.1:9.8.

[0103] Example 9

[0104] This embodiment provides a lithium supplement material. The lithium supplement material includes Li 0.8 Co 0.1 OOC-CO-COOLi 0.8 Co 0.1 .

[0105] The difference between the preparation method of the composite lithium supplement material and that of Example 6 is that the molar ratio of Co(OH)2 to LiOH is 1:8.

[0106] Example 10

[0107] This embodiment provides a lithium supplement material. The lithium supplement material includes Li 0.6 Co 0.2 OOC-CO-COOLi 0.6 Co 0.2 .

[0108] The difference between the preparation method of the composite lithium supplement material and that of Example 6 is that the molar ratio of Co(OH)2 and LiOH is 2:6.

[0109] Embodiment 11

[0110] This embodiment provides a lithium supplement material. The lithium supplement material includes Li 0.9 Cu 0.05 OOC-CO-COOLi 0.9 Cu 0.05 .

[0111] The difference between the preparation method of the composite lithium supplement material and that of Example 6 is that Co(OH)2 is replaced by Cu(OH)2.

[0112] Example 12

[0113] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3CH2OLi0.9 Co 0.05 The particle size D50 of the primary particles of the lithium supplement material is 150 nm, and the particle size D50 of the secondary particles of the lithium supplement material is 1.7 μm.

[0114] The preparation method of the composite lithium supplement material comprises the following steps:

[0115] 1) In a glove box, lithium and cobalt are mixed evenly in a molar ratio of 9:0.5, and then heated to 250°C. The lithium metal melts and the two materials become a whole.

[0116] 2) The Li-Co mixture and excess ethanol (CH3CH2OH) are transferred to a sealed, dry, high-temperature and high-pressure device filled with argon, heated to 500°C, kept warm for 10 hours, cooled, and then the resulting reactant is separated from the excess ethanol.

[0117] The resulting reactant is CH3CH2-OLi 0.9 Co 0.05 .

[0118] Embodiment 13

[0119] This embodiment provides a lithium supplement material. The lithium supplement material includes (CH3)2CHOLi 0.9 Co 0.05 The particle size D50 of the primary particles of the lithium supplement material is 130 nm, and the particle size D50 of the secondary particles of the lithium supplement material is 1.6 μm.

[0120] The difference between the preparation method of the composite lithium supplement material and that of Example 12 is that CH3CH2OH is replaced by (CH3)2CHOH.

[0121] Embodiment 14

[0122] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3COOLi. The particle size D50 of the primary particles of the lithium supplement material is 100 nm, and the particle size D50 of the secondary particles of the lithium supplement material is 1 μm.

[0123] The difference between the preparation method of the composite lithium supplement material and that of Example 1 is that no cobalt acetate is added.

[0124] Embodiment 15

[0125] This embodiment provides a lithium supplement material. The lithium supplement material includes CH3CH2OLi. The particle size D50 of the primary particles of the lithium supplement material is 150nm, and the particle size D50 of the secondary particles of the lithium supplement material is 1.7μm.

[0126] The difference between the preparation method of the composite lithium supplement material and that of Example 12 is that no single substance Co is added.

[0127] Comparative Example 1

[0128] This comparative example provides a lithium supplement material, which includes an organic lithium salt Li2C2O4 and carbon nanotubes.

[0129] Comparative Example 2

[0130] This comparative example provides a lithium supplement material, which includes an organic lithium salt CH3COOLi, CoO and carbon nanotubes.

[0131] The negative electrode material parameters provided by Examples 1 to 15 and Comparative Examples 1 to 2 are shown in Table 1:

[0132] Table 1 Negative electrode material parameters provided in Examples and Comparative Examples

[0133]

[0134] The composite lithium supplement materials provided in the above-mentioned Examples 1 to 15 and the lithium supplement materials provided in Comparative Examples 1 and 2 are respectively assembled into positive electrode sheets and lithium-ion batteries according to the following methods:

[0135] Positive electrode sheet: The lithium supplement material, SP and PVDF are mixed in a mass ratio of 90:4:6 to prepare a positive electrode slurry, the positive electrode slurry is coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;

[0136] Negative electrode: lithium sheet;

[0137] Electrolyte: Ethylene carbonate and ethyl methyl carbonate are mixed in a volume ratio of 3:7, and electrolyte LiPF6 is added, and the concentration of LiPF6 is 1 mol / L; forming an electrolyte;

[0138] Diaphragm: Polypropylene microporous separator;

[0139] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of negative electrode sheet - separator - electrolyte - positive electrode sheet.

[0140] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:

[0141] The battery was charged at a rate of 0.1C with a cut-off voltage of 4.7V. The battery was charged at a constant voltage of 4.7V. After the charging process was completed, the battery was allowed to stand for 10 minutes and then discharged at a rate of 0.1C with a cut-off voltage of 2.5V. The charging platform was observed during the charging process to obtain the delithiation potential of the lithium supplement material.

[0142] The test results of the above lithium supplement materials and lithium batteries are shown in Table 2 below:

[0143] Table 2. Formation test results of the assembled batteries of the examples and comparative examples

[0144]

[0145] It can be seen from the test results of Examples 1 to 15 and Comparative Examples 1 to 2 in Tables 1 and 2 that the conductivity and delithiation percentage of the organic lithium salt containing an electron-donating group or an electron-donating group and a transition metal ion provided by the present invention are higher than those of the comparative example, and the delithiation platform potential of the lithium supplementing material provided by Examples 1 to 15 is lower than that of ordinary lithium oxalate (Comparative Example 1). Therefore, it is shown that the solution provided by the present invention has a significant improvement in the performance of the lithium supplementing material compared with the prior art.

[0146] It can be seen from the test results of Examples 1-5 and Example 14 in Table 1 and Table 2 that after the addition of different proportions of catalytic elements (Co or Ni), the lithium-replenishing material's de-lithium platform potential is further reduced, from 4.2V to between 4.00V-4.15V. With the increase of doping amount, the de-lithium platform potential is continuously reduced. However, when the doping amount is too large (Example 4), the de-lithium platform potential decreases significantly, but the lithium-replenishing capacity decreases significantly, with less than 193mAh / g. Therefore, considering the de-lithium capacity and the de-lithium voltage platform, the doping amount has a relatively suitable range, especially in the case where it is necessary to introduce an electron-donating group, which is different from the doping of ordinary organic lithium salts, and it is necessary to consider the balance of the positive and negative effects and doping brought by the electron-donating group at the same time.

[0147] It can also be seen from the test results of Examples 7-11 in Tables 1 and 2 that the solution provided by the present invention is applicable to most organic lithium salts, and the doping amount has a significant effect on the comprehensive delithiation capacity and the delithiation voltage platform, so the doping amount of the electron donating group and the transition metal ion needs to be controlled within a relatively appropriate range.

[0148] It can also be seen from the test results of Example 1 and Example 6 in Table 1 and Table 2 that the lithium desorption platform potential of the lithium supplement material in Example 1 is lower than that in Example 6. This is because the lithium supplement in Example 6 does not contain carbon nanotubes (CNTs), and the conductive carrier is very important for reducing the ohmic polarization of the organic lithium salt in the battery cell and the electrode, which is beneficial to reducing the lithium desorption platform potential.

[0149] It can also be seen from the test results of Examples 12 and 13 in Tables 1 and 2 that the delithiation platform potential in Example 13 is lower. This is because it contains two -CH3, the electron donation effect is more obvious, and the O-Li bond can be better weakened, thereby reducing the delithiation platform potential.

[0150] It can also be seen from the test results of Example 14, Example 15 and Comparative Example 1 in Table 1 and Table 2 that the delithiation percentages of Example 14 and Example 15 are higher than that of Comparative Example 1, and the delithiation platform potentials (4.20V, 4.31V) of Example 14 and Example 15 are significantly lower than those of Comparative Example 1 (4.70V). In the absence of catalytic elements, the lithium-supplementing materials in Examples 14 and 15 contain the electron-donating group -CH3, which weakens the O-Li bond, thereby reducing the delithiation potential and is also beneficial to improving the delithiation efficiency.

[0151] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0152] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.

Claims

1. A lithium supplement material, characterized in that: The lithium supplement material includes an organic lithium salt, and the organic lithium salt includes an electron-donating group.

2. The lithium supplement material according to claim 1, characterized in that: The lithium supplement material further comprises transition metal ions, which are doped in the organic lithium salt and replace part of the lithium ions in the organic lithium salt. The molecular formula of the organic lithium salt doped with the transition metal comprises: a H b O c (Li d1 M d2 ) k , wherein M includes at least one of Co, Ni, Mn, Fe, Cu, Mg, Cr, Zn, Ti, and Zr, 1≤a≤5, 1≤b≤7, 2≤c≤8, 0.8≤d1<1, 0<d2≤0.1, 1≤k≤4, and a, b, c, and k are all integers.

3. The lithium supplement material according to claim 2, characterized in that: The organic lithium salt includes a carboxylic acid organic lithium salt, and the general structural formula of the carboxylic acid organic lithium salt includes: (COOLi d1 M d2 ) n R1, wherein n≥1, R1 is the electron-donating group, and R1 includes at least one of a methyl group, a methylene group, a methine group, a carbonyl group, and a hydroxyl group.

4. The lithium supplement material according to claim 3, characterized in that: The organic lithium salt includes CH3-COOLi d1 M d2 、CH2OH-COO Li d1 M d2 、(COOLi d1 M d2 )2(CH2) m , (COOLi d1 M d2 )2C=O,(COOLi d1 M d2 )2CHOH, wherein 1≤m≤3.

5. The lithium supplement material according to claim 2, characterized in that: The organic lithium salt includes a non-carboxylic acid organic lithium salt, and the general structural formula of the non-carboxylic acid organic lithium salt includes: (R2R3R4COLi d1 M d2 ) n , 1≤n≤3, at least one of R2, R3, and R4 is the electron donating group, and R2, R3, and R4 independently include at least one of a methyl group, an aldehyde group, a hydroxyl group, and a hydrogen atom.

6. The lithium supplement material according to any one of claims 1 to 5, characterized in that: The particle size D50 of the primary particles of the lithium supplement material is 50nm to 500nm; and / or The particle size D50 of the secondary particles of the lithium supplement material is 500nm-4μm.

7. A method for preparing a lithium supplement material, characterized in that: include: The lithium-containing compound and the electron-donating group precursor are mixed in proportion to obtain a lithium-supplementing mixture; After the lithium replenishing mixture is fully reacted, the lithium replenishing mixture is converted into an organic lithium salt to obtain the lithium replenishing material, wherein the organic lithium salt includes an electron-donating group.

8. The preparation method according to claim 7, characterized in that: The lithium-containing compound and the electron-donating group precursor are mixed in proportion to obtain a lithium-supplementing mixture, comprising: The organic compound, the lithium source, and the transition metal source are mixed in proportion to obtain a lithium supplement mixture, wherein the organic compound includes the electron-donating group, and the transition metal ions are doped in the lithium supplement mixture.

9. A positive electrode material, characterized in that: The positive electrode material includes an active material and a lithium supplement material, and the lithium supplement material includes the lithium supplement material according to any one of claims 1 to 6, or includes a lithium supplement material obtained by the preparation method of the lithium supplement material according to claim 7 or 8.

10. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the positive electrode material as claimed in claim 9.