All-dielectric wave absorber and preparation method and application thereof

Through the combination of composite material preparation of dielectric loss materials and magnetic loss materials and adaptive camouflage jackets, the broadband microwave absorption and multi-spectral compatible stealth of the full dielectric absorber are achieved, and the solution is that the absorber cannot meet the same time in the prior art. The problem of broadband microwave absorption is compatible with multi-spectrum stealth, improving stealth performance and adaptability.

CN119072098APending Publication Date: 2024-12-03NINGBO INST OF NORTHWESTERN POLYTECHNICAL UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411127257.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing full-difference three-dimensional structure absorbers cannot meet the compatible stealth of broadband microwave absorption and multi-spectral stealth at the same time, and their design is not tunable, which limits its application in multi-spectral detection technology.

Method used

By mixing the dielectric loss material with magnetic loss material and mixing and stirring with the adhesive in a specific proportion, vacuum drying is performed to prepare a full dielectric absorber with ultra-wideband absorption performance, and combined with an adaptive camouflage jacket and Heating layer to achieve radar and visible light stealth.

Benefits of technology

Achieves broadband microwave absorption in the range of 3.28-40GHz, and dynamically discolors in different environments through adaptive camouflage jackets, enhancing the visible light stealth performance, expanding the absorbing bandwidth to 2.87-40GHz, solving the bottleneck of multi-spectrum compatible stealth question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072098A_ABST
    Figure CN119072098A_ABST
Patent Text Reader

Abstract

The invention discloses an all-dielectric wave absorber and a preparation method and application thereof, and the preparation method comprises the following steps: S1, mixing a dielectric loss material and a magnetic loss material, and carrying out stirring and vibration treatment to obtain a composite material; s2, the composite material and an adhesive are mixed and stirred, then the composite material is placed in a vacuum drying machine, and the vacuum degree is pumped to be 1t; the pressure is 3.0 * 10 <-3 > Pa, and bubbles are removed after standing; s3, the composite material is taken out and poured into a mold; s4, the mold is placed in a vacuum drying machine, and the vacuum degree is reduced to 1t; and heating to the temperature of more than 80 DEG C under the pressure of 3.0 * 10 <-3 > Pa, standing for 1 hour, and demolding to obtain the all-dielectric wave absorber. According to the application, the all-medium wave absorber is applied to the all-medium wave absorbing device with the self-adaptive camouflage outer sleeve, and the stealth effect of the device is further improved. Through the all-dielectric wave absorber and the all-dielectric wave absorbing device provided by the invention, the problem that similar devices in the prior art cannot meet broadband microwave absorption and multispectral compatible stealth at the same time is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adaptive stealth absorbers, and in particular to an all-dielectric absorber and a preparation method and application thereof. Background Art

[0002] With the advancement of science and technology and the rapid development of strategic weapons, precision strikes based on multi-band combination and multi-gradient depth detection technology have become the mainstream of modern battlefields. Among them, the multi-gradient detection system composed of long-range radar detection, medium-range infrared detection and close-range visible light remote sensing has been widely used. Therefore, for various strategic equipment that need to be protected, having radar stealth, infrared stealth and visible light stealth at the same time can greatly improve the survival rate on the battlefield. For mobile military equipment such as tanks and chariots, visible light stealth needs to be adaptive to the surrounding environment.

[0003] Microwave absorber is a special material that can convert electromagnetic waves into heat energy, thereby reducing the reflection of electromagnetic waves. It is widely used in military and civilian fields such as radar cross-section control, shielding of complex electromagnetic environments, and radar stealth. Common microwave absorbers include all-dielectric three-dimensional structures, multi-layer lossy frequency selective surface structures, and multi-layer dielectric structures. Compared with other types of absorbers, all-dielectric three-dimensional structures are thinner, easier to manufacture, and can achieve ultra-wideband microwave absorption. However, the singleness of its stealth type and the non-tunability of its performance after the design is completed limit its further development. With the rapid development of multi-spectral detection technology, single-band stealth materials face huge challenges, and multi-spectrum compatible stealth materials have become a current research hotspot.

[0004] For all-dielectric three-dimensional structure absorbers, since impedance matching is difficult after being combined with other superstructures, achieving multi-spectrum compatible stealth while ensuring broadband microwave absorption is a bottleneck problem in current research. The all-dielectric absorbers prepared by conventional methods cannot meet the requirements of broadband microwave absorption and multi-spectrum compatible stealth at the same time. Summary of the invention

[0005] One of the technical problems to be solved by the present invention is to provide a method for preparing an all-dielectric absorber, so as to solve the problem that the all-dielectric absorber prepared by conventional methods cannot simultaneously meet the requirements of broadband microwave absorption and multi-spectrum compatible stealth.

[0006] In order to solve the above technical problems, the present invention provides a method for preparing an all-dielectric absorber, comprising the following steps:

[0007] S1: mixing the dielectric loss material and the magnetic loss material, stirring and shaking to obtain a composite material;

[0008] S2: Mix and stir the composite material obtained in step S1 with the adhesive, and control the mass ratio of the dielectric loss material, the magnetic loss material and the adhesive to be (0.01-3):(6-15):4, then place the composite material in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, remove air bubbles after placement;

[0009] S3: taking out the composite material obtained in step S2 and pouring it into a mold;

[0010] S4: Place the composite material in step S3 together with the mold in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, the temperature is raised to above 80 °C, and after standing for one hour, the mold is removed to obtain a full dielectric absorber.

[0011] Compared with the prior art, the preparation method of the all-dielectric absorber in the present invention has the following advantages: the all-dielectric absorber of the present invention adopts a composite material of dielectric loss material and magnetic loss material, and achieves sufficient loss absorption of the electric field and magnetic field components of electromagnetic waves by adjusting a reasonable ratio, thereby achieving ultra-wideband radar stealth. In the preparation method of the all-dielectric absorber of the present invention, a mature mold injection molding process is adopted, which can realize rapid batch large-area preparation, reduce the preparation cost, and realize large-area application.

[0012] In a possible implementation, in step S1, the dielectric loss material is selected from one or more of dielectric loss materials carbon nanotubes, ceramic powders, conductive polymers and SiC; the magnetic loss material is selected from one or more of ferrite, spherical hydroxyl iron powder, flaky hydroxyl iron powder and sendust powder.

[0013] In a possible implementation, in step S2, the adhesive is silicone rubber or epoxy resin adhesive, and the mass ratio of the dielectric loss material, magnetic loss material and adhesive is (0.1-3):(6-15):4.

[0014] The present invention achieves good matching of dielectric loss and magnetic loss and maximization of dielectric constant and magnetic permeability by further selecting the components of the above-mentioned dielectric loss material, magnetic loss material and adhesive and the mass ratio of the dielectric loss material, magnetic loss material and adhesive, thereby realizing ultra-wideband absorption under ultra-thin structure; the selection of mature industrial materials enables the absorber to be prepared on a large area at low cost.

[0015] In a possible implementation, in step S2, the standing time is more than 20 minutes, and in step S4, the standing time is more than 1 hour.

[0016] The present invention removes bubbles in the reaction by controlling the placement time of the step S2, and makes the shape of the composite material more solid by controlling the placement time of S4.

[0017] The second technical problem to be solved by the present invention is to provide an all-dielectric absorber, characterized in that the all-dielectric absorber is prepared by the above-mentioned preparation method, and the all-dielectric absorber can simultaneously meet the requirements of broadband microwave absorption and multi-spectrum compatible stealth.

[0018] Another technical problem to be solved by the present invention is to provide an application of an all-dielectric absorber to solve the problem that the all-dielectric absorber in the prior art cannot simultaneously meet the requirements of broadband microwave absorption and multi-spectrum compatible stealth.

[0019] In order to solve the above technical problems, the present invention provides an application of an all-dielectric absorber, wherein the application includes applying the all-dielectric absorber to an all-dielectric absorbing device, and the all-dielectric absorbing device includes an adaptive camouflage jacket, the all-dielectric absorber and a bottom heating layer connected in sequence from top to bottom, and the adaptive camouflage jacket is made of thermochromic capsules and polydimethylsiloxane by injection molding process.

[0020] In the above application of the present invention, the principles implemented include:

[0021] Visible light invisibility: The adaptive camouflage jacket can mimic the background environment and adjust the temperature of the heating plate to change the color of the adaptive camouflage jacket to adapt to the background changes, thereby achieving visible light invisibility; the adaptive camouflage jacket can choose different color changes from colorless to colored, colored to colorless, two-stage or multi-stage color changes according to different environments.

[0022] Radar stealth: The all-dielectric absorber converts microwaves into heat through resonance absorption and dielectric loss, thereby suppressing the reflection of microwaves and making it impossible for radar to detect, thereby achieving radar stealth.

[0023] In a possible implementation, the adaptive camouflage jacket and the all-dielectric absorber are bonded with a low-viscosity glue of 20-500 centipoise, and the all-dielectric absorber and the bottom heating layer are bonded with a high-viscosity glue of 2000-5000 centipoise.

[0024] In a possible implementation, the bottom heating layer is one of a graphene heating plate, a silicone heating plate, a ceramic heating plate, or a composite heating plate of graphene, silicone and ceramic; the all-dielectric absorber and the adaptive camouflage jacket are both quadrangular pyramid structures, and the bottom of the adaptive camouflage jacket has a groove that is adapted to the shape and size of the all-dielectric absorber, so that the all-dielectric absorber and the adaptive camouflage jacket form an integral quadrangular pyramid structure after being fitted together; the shape and size of the bottom heating layer are the same as those of the bottom of the all-dielectric absorber.

[0025] In the above possible implementation manner of the present invention, the adaptive camouflage jacket and the all-dielectric absorber are bonded with low-viscosity glue to facilitate the disassembly of the camouflage jacket; the all-dielectric absorber and the bottom heating layer are bonded with high-viscosity glue to ensure close contact and efficient heat conduction; and the all-dielectric absorber and the adaptive camouflage jacket are designed with a tetrahedral structure, and the all-dielectric absorber is embedded in the adaptive camouflage jacket. The embedded structure facilitates the disassembly and assembly of the adaptive camouflage jacket, and the tetrahedral structure refers to the classic pyramid structure in the microwave absorber, which can ensure ultra-wideband microwave absorption and further improve the absorption performance of the all-dielectric absorber after application.

[0026] In a possible implementation, the method for preparing the adaptive camouflage coat includes:

[0027] A1: Glue is prepared by mixing polydimethylsiloxane and curing agent;

[0028] A2: adding thermochromic capsules to the glue in step A1 and stirring to obtain a composite material, then placing the composite material in a vacuum dryer and drawing the vacuum degree to <3.0×10-3Pa, and removing bubbles after standing;

[0029] A3: taking out the composite material obtained in step A2 and pouring it into a mold;

[0030] A4: Place the camouflage jacket mold in step A3 in a vacuum dryer and draw the vacuum degree to <3.0×10-3Pa, raise the temperature to 100°C, and demould after standing for a certain period of time to obtain an adaptive camouflage jacket.

[0031] In a possible implementation, in step A1, the curing agent is curing agent SE1700; the mass ratio of the polydimethylsiloxane, SE1700 curing agent and the temperature-dependent capsule composite material is 10:1:(0.1-5); in step A2, the placement time is more than 40 minutes; in step A4, the placement time is more than 2 hours.

[0032] Through the selection and proportion control of the color-changing capsules in the above-mentioned adaptive camouflage jacket preparation method, dynamic environmental mimicry in different background environments can be achieved, such as the dynamic switching between grass green and khaki in grassland and desert environments; the dielectric constant and magnetic permeability of the adaptive camouflage jacket close to those of air enhance the impedance matching of the all-dielectric absorber, thereby improving the absorption of low-frequency electromagnetic waves by the all-dielectric absorber, further improving the radar stealth performance, and providing a new solution for the multi-spectral compatible stealth of the all-dielectric absorber. The adaptive camouflage jacket also uses a mature injection molding process, which can be prepared on a large scale at low cost. . BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a structural schematic diagram of the all-dielectric absorbing device;

[0034] Figure 2 It is a schematic diagram of the cross-sectional structure of the all-dielectric absorbing device;

[0035] Figure 3 This is a physical structure diagram of the adaptive camouflage jacket in Example 1;

[0036] Figure 4 This is a test diagram of electromagnetic parameters of the adaptive camouflage jacket in Example 1;

[0037] Figure 5 This is a structural diagram of the all-dielectric absorbing device;

[0038] Figure 6 This is a test diagram of electromagnetic parameters of the all-dielectric absorber in Example 1;

[0039] Figure 7 This is a diagram showing the mimicry test results of the all-dielectric absorbing device in Example 1 in a grass environment;

[0040] Figure 8 This is a diagram showing the results of a simulated test of the all-dielectric absorbing device in Example 1 in a desert environment;

[0041] Fig. 9 is a comparison chart of simulation results and experimental results of the all-dielectric absorber in Example 1;

[0042] Fig.10 This is a comparison chart between the simulation results and the experimental results of the all-dielectric absorbing device equipped with an adaptive camouflage jacket in Example 1. DETAILED DESCRIPTION

[0043] First, those skilled in the art should understand that these implementations are only used to explain the technical principles of the embodiments of the present application, and are not intended to limit the protection scope of the embodiments of the present application. Those skilled in the art can make adjustments to them as needed to adapt to specific application scenarios.

[0044] In the description of the embodiments of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to specific circumstances.

[0045] In the embodiments of the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0046] The present invention provides a method for preparing an all-dielectric absorber, comprising the following steps:

[0047] S1: mixing the dielectric loss material and the magnetic loss material, stirring and shaking to obtain a composite material;

[0048] S2: Mix and stir the composite material obtained in step S1 with the adhesive, and control the mass ratio of the dielectric loss material, the magnetic loss material and the adhesive to be (0.01-3):10:4, then place the composite material in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, remove air bubbles after standing;

[0049] S3: taking out the composite material obtained in step S2 and pouring it into a mold;

[0050] S4: Place the composite material in step S3 together with the mold in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, the temperature is raised to above 80°C, and after being placed for a certain period of time, the mold is released to obtain a full dielectric absorber.

[0051] As a preferred solution, in step S1, the dielectric loss material is selected from one or more of dielectric loss materials carbon nanotubes, ceramic powders, conductive polymers and SiC; the magnetic loss material is selected from one or more of ferrite, spherical hydroxyl iron powder, flaky hydroxyl iron powder and sendust powder.

[0052] As a preferred solution, in step S2, the adhesive is silicone rubber or epoxy resin glue, and the mass ratio of the dielectric loss material, magnetic loss material and adhesive is (0.1-3):(6-15):4.

[0053] As a preferred solution, in step S2, the standing time is more than 20 minutes, and in step S4, the standing time is more than 1 hour.

[0054] The present invention also provides an all-dielectric absorber, which is prepared by the above-mentioned preparation method.

[0055] The present invention also provides an application of an all-dielectric absorber, which includes applying the all-dielectric absorber to an all-dielectric absorber device, and the all-dielectric absorber device includes an adaptive camouflage jacket, the all-dielectric absorber and a bottom heating layer connected in sequence from top to bottom, and the adaptive camouflage jacket is made of thermochromic capsules and polydimethylsiloxane by injection molding process.

[0056] As a preferred solution, the adaptive camouflage jacket and the all-dielectric absorber are bonded with a low-viscosity glue of 20-500 centipoise, and the all-dielectric absorber and the bottom heating layer are bonded with a high-viscosity glue of 2000-5000 centipoise.

[0057] As a preferred solution, the bottom heating layer is one of a graphene heating plate, a silicone heating plate, a ceramic heating plate, or a composite heating plate of graphene, silicone and ceramic; the all-dielectric absorber and the adaptive camouflage jacket are both quadrangular pyramid structures, and the bottom of the adaptive camouflage jacket has a groove that is adapted to the shape and size of the all-dielectric absorber, so that the all-dielectric absorber and the adaptive camouflage jacket form an integral quadrangular pyramid structure after being fitted together; the shape and size of the bottom heating layer are the same as those of the bottom of the all-dielectric absorber.

[0058] As a preferred solution, the method for preparing the adaptive camouflage coat includes:

[0059] A1: Glue is prepared by mixing polydimethylsiloxane and curing agent;

[0060] A2: adding thermochromic capsules to the glue in step A1 and stirring to obtain a composite material, then placing the composite material in a vacuum dryer and drawing the vacuum degree to <3.0×10-3Pa, and removing bubbles after standing;

[0061] A3: taking out the composite material obtained in step A2 and pouring it into a mold;

[0062] A4: Place the camouflage jacket mold in step A3 in a vacuum dryer and draw the vacuum degree to <3.0×10-3Pa, raise the temperature to 100°C, and demould after standing for a certain period of time to obtain an adaptive camouflage jacket.

[0063] As a preferred solution, in the step A1, the curing agent is curing agent SE1700; the mass ratio of the polydimethylsiloxane, SE1700 curing agent and the temperature-dependent capsule composite material is 10:1:(0.1-5); in the step A2, the placement time is more than 40 minutes; in the step A4, the placement time is more than 2 hours.

[0064] The following provides embodiments combined with specific data and performance tests of corresponding embodiments to further describe the above technical solutions of the present invention:

[0065] Embodiment 1:

[0066] This embodiment provides an all-dielectric absorber and a preparation method and application thereof.

[0067] The preparation method of the all-dielectric absorber comprises the following steps:

[0068] S1. Mix the dielectric loss material carbon nanotubes and the magnetic loss material spherical hydroxyl iron powder, stir vigorously for 5 minutes and then ultrasonically vibrate for 20 minutes; the carbon nanotubes have an outer diameter of 8-15μm, an inner diameter of 3-5μm, a length of 8-14μm, and a purity of 99%; the spherical hydroxyl iron powder has a size of 1-3μm and a purity of 99.99%.

[0069] S2. The composite material obtained in step S1 is mixed with the addition type silicone rubber and stirred evenly. The mixing mass ratio of the dielectric loss material, the magnetic loss material and the addition type silicone rubber or the epoxy resin adhesive is 0.1:10:4. The composite material is then placed in a vacuum dryer and the vacuum degree is drawn to <3.0×10 -3 Pa, leave for 20 minutes to remove bubbles.

[0070] S3. The composite material obtained in step S2 is taken out and poured into the absorber mold and the coaxial mold;

[0071] S4. Place the camouflage coat mold in step S3 in a vacuum dryer and reduce the vacuum degree to <3.0×10-3Pa, increase the temperature to 80°C, and leave it for 1 hour.

[0072] S5. Demould and take out the all-dielectric absorber 2. Figure 5 As shown; take out the coaxial ring and perform electromagnetic parameter test, the results are as shown in the attached Figure 6 shown.

[0073] The material of the all-dielectric absorber is a composite material obtained by mixing dielectric loss materials such as carbon nanotubes, ceramic powders, conductive polymers and SiC or a composite material with magnetic loss materials such as ferrite, spherical hydroxyl iron powder, flaky hydroxyl iron powder and sendust powder or a composite material. The composite material is mixed with addition-type silicone rubber or epoxy resin glue to obtain the material of the all-dielectric absorber; and the mixing mass ratio of the dielectric loss material, the magnetic loss material and the addition-type silicone rubber or epoxy resin glue is 0.1:10:4.

[0074] The application includes applying the all-dielectric absorber to an all-dielectric absorber, as shown in the attached Figure 1 As shown, Figure 1 The all-dielectric absorber wearing an adaptive camouflage coat provided in this embodiment includes an adaptive camouflage coat 1, an all-dielectric absorber 2, and a bottom heating layer 3 from top to bottom.

[0075] The all-dielectric absorber 2 is the all-dielectric absorber prepared in the above-mentioned embodiment 1;

[0076] The self-adaptive camouflage jacket 1 and the all-dielectric absorber 2 are of an embedded quadrangular pyramid structure. Figure 2 As shown, the embedded structure facilitates the disassembly and assembly of the adaptive camouflage jacket 1, and the four-sided pyramid structure refers to the classic pyramid structure in the microwave absorber to ensure ultra-wideband microwave absorption.

[0077] The material of the adaptive camouflage jacket 1 is a composite material obtained by mixing one of the colorless to colored, colored to colorless, two-stage color-changing and multi-stage color-changing thermochromic capsules or a composite material with polydimethylsiloxane, and the mass ratio of the thermochromic capsule composite material to polydimethylsiloxane is 1:10.

[0078] The preparation method of the adaptive camouflage jacket 1 comprises:

[0079] A1: Mix polydimethylsiloxane PDMA and SE1700 curing agent in a mass ratio of 10:1 and make glue;

[0080] A2: Add thermochromic capsules to the mixture in step A1 and stir evenly. Select thermochromic capsules that can change from grass green to khaki at 31°C. The mass ratio of thermochromic capsules to polydimethylsiloxane is 1:10. Then place the composite material in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, leave for 40 min to remove bubbles;

[0081] A3: taking out the composite material obtained in step A2, and pouring it into the camouflage jacket mold and the coaxial method mold;

[0082] A4: Place the camouflage coat mold in step A3 in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, the temperature was raised to 100°C and left for 3h;

[0083] A5. Demould and take out the adaptive camouflage jacket 1, as shown in the attached Figure 3 As shown; take out the coaxial ring and perform electromagnetic parameter test, the results are as shown in the attached Figure 4 shown.

[0084] The heating layer 3 is a graphene heating plate.

[0085] The adaptive camouflage jacket 1 and the all-dielectric absorber 2 are bonded with low-viscosity glue to facilitate the disassembly of the camouflage jacket; the all-dielectric absorber 2 and the heating layer 3 are bonded with high-viscosity glue to ensure close contact and efficient heat conduction.

[0086] The working process of the all-dielectric absorber wearing an adaptive camouflage coat includes:

[0087] Visible light invisibility: The adaptive camouflage jacket 1 mimics the background environment, and adjusts the temperature of the heating plate 3 to change the color of the adaptive camouflage jacket 1 to adapt to the background changes, thereby achieving visible light invisibility. The adaptive camouflage jacket 1 can choose different color changes from colorless to colored, colored to colorless, two-stage or multi-stage color changes according to different environments.

[0088] Radar stealth: The all-dielectric absorber 2 converts microwaves into heat through resonance absorption and dielectric loss, thereby suppressing the reflection of microwaves and making it impossible for radar to detect, thereby achieving radar stealth.

[0089] Embodiment 2:

[0090] This embodiment provides an all-dielectric absorber and a preparation method and application thereof.

[0091] The preparation method of the all-dielectric absorber comprises the following steps:

[0092] S1. Mixing dielectric loss material ceramic powder and magnetic loss material ferrite, vigorously stirring for 5 minutes and then ultrasonically vibrating for 20 minutes to obtain a composite material;

[0093] S2. The composite material obtained in step S1 is mixed with epoxy resin glue and stirred evenly, and then the composite material is placed in a vacuum dryer and the vacuum degree is reduced to <3.0×10 -3 Pa, leave for 20 minutes to remove bubbles.

[0094] S3. The composite material obtained in step S2 is taken out and poured into the absorber mold and the coaxial mold;

[0095] S4. Place the camouflage coat mold in step S3 in a vacuum dryer and reduce the vacuum degree to <3.0×10-3Pa, increase the temperature to 80°C, and leave it for 1 hour.

[0096] S5. Demould and take out the all-dielectric absorber 2.

[0097] The material of the all-dielectric absorber is a composite material obtained by mixing dielectric loss materials such as carbon nanotubes, ceramic powders, conductive polymers and SiC or a composite material with magnetic loss materials such as ferrite, spherical hydroxyl iron powder, flaky hydroxyl iron powder and sendust powder or a composite material. The composite material is mixed with addition-type silicone rubber or epoxy resin glue to obtain the material of the all-dielectric absorber; and the mixing mass ratio of the dielectric loss material, the magnetic loss material and the addition-type silicone rubber or epoxy resin glue is 1:10:4.

[0098] The application includes applying the all-dielectric absorber to an all-dielectric absorber device, wherein the all-dielectric absorber device includes an adaptive camouflage jacket 1, an all-dielectric absorber 2, and a bottom heating layer 3 from top to bottom.

[0099] The all-dielectric absorber 2 is the all-dielectric absorber prepared in the above-mentioned embodiment 1;

[0100] The adaptive camouflage jacket 1 and the all-dielectric absorber 2 adopt an embedded tetrahedral structure. The embedded structure facilitates the disassembly and assembly of the adaptive camouflage jacket 1. The tetrahedral structure refers to the classic pyramid structure in the microwave absorber to ensure ultra-wideband microwave absorption.

[0101] The material of the adaptive camouflage jacket 1 is a composite material obtained by mixing one of the colorless to colored, colored to colorless, two-stage color-changing and multi-stage color-changing thermochromic capsules or a composite material with polydimethylsiloxane, and the mass ratio of the thermochromic capsule composite material to polydimethylsiloxane is 0.1:10.

[0102] The preparation method of the adaptive camouflage jacket 1 comprises:

[0103] A1: Mix polydimethylsiloxane PDMA and SE1700 curing agent in a mass ratio of 10:1 and make glue;

[0104] A2: Add thermochromic capsules to the mixture in step A1 and stir evenly. Select thermochromic capsules that can change from grass green to khaki at 31°C. The mass ratio of thermochromic capsules to polydimethylsiloxane is 1:10. Then place the composite material in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, leave for 40 min to remove bubbles;

[0105] A3: taking out the composite material obtained in step A2, and pouring it into the camouflage jacket mold and the coaxial method mold;

[0106] A4: Place the camouflage coat mold in step A3 in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, the temperature was raised to 100°C and left for 3h;

[0107] A5. De-mould and take out the adaptive camouflage jacket 1.

[0108] The heating layer 3 is a ceramic heating plate.

[0109] The adaptive camouflage jacket 1 and the all-dielectric absorber 2 are bonded with low-viscosity glue to facilitate the disassembly of the camouflage jacket; the all-dielectric absorber 2 and the heating layer 3 are bonded with high-viscosity glue to ensure close contact and efficient heat conduction.

[0110] Embodiment 3:

[0111] This embodiment provides an all-dielectric absorber and a preparation method and application thereof.

[0112] The preparation method of the all-dielectric absorber comprises the following steps:

[0113] S1. Mix the dielectric loss material SiC and the magnetic loss material Sendust powder, vigorously stir for 5 minutes and then ultrasonically vibrate for 20 minutes to obtain a composite material;

[0114] S2. The composite material obtained in step S1 is mixed with the addition type silicone rubber and stirred evenly, and then the composite material is placed in a vacuum dryer and the vacuum degree is reduced to <3.0×10 -3 Pa, leave for 20 minutes to remove bubbles.

[0115] S3. The composite material obtained in step S2 is taken out and poured into the absorber mold and the coaxial mold;

[0116] S4. Place the camouflage coat mold in step S3 in a vacuum dryer and reduce the vacuum degree to <3.0×10-3Pa, increase the temperature to 80°C, and leave it for 1 hour.

[0117] S5. Demould and take out the all-dielectric absorber 2.

[0118] The material of the all-dielectric absorber is a composite material obtained by mixing dielectric loss materials such as carbon nanotubes, ceramic powders, conductive polymers and SiC or a composite material with magnetic loss materials such as ferrite, spherical hydroxyl iron powder, flaky hydroxyl iron powder and sendust powder or a composite material. The composite material is mixed with addition-type silicone rubber or epoxy resin glue to obtain the material of the all-dielectric absorber; and the mixing mass ratio of the dielectric loss material, the magnetic loss material and the addition-type silicone rubber or epoxy resin glue is 3:10:4.

[0119] The application includes applying the all-dielectric absorber to an all-dielectric absorber device, wherein the all-dielectric absorber device includes an adaptive camouflage jacket 1, an all-dielectric absorber 2, and a bottom heating layer 3 from top to bottom.

[0120] The all-dielectric absorber 2 is the all-dielectric absorber prepared in the above-mentioned embodiment 1;

[0121] The adaptive camouflage jacket 1 and the all-dielectric absorber 2 adopt an embedded tetrahedral structure. The embedded structure facilitates the disassembly and assembly of the adaptive camouflage jacket 1. The tetrahedral structure refers to the classic pyramid structure in the microwave absorber to ensure ultra-wideband microwave absorption.

[0122] The material of the adaptive camouflage jacket 1 is a composite material obtained by mixing one of the colorless to colored, colored to colorless, two-stage color-changing and multi-stage color-changing thermochromic capsules or a composite material with polydimethylsiloxane, and the mass ratio of the thermochromic capsule composite material to polydimethylsiloxane is 5:10.

[0123] The preparation method of the adaptive camouflage jacket 1 comprises:

[0124] A1: Mix polydimethylsiloxane PDMA and SE1700 curing agent in a mass ratio of 10:1 and make glue;

[0125] A2: Add thermochromic capsules to the mixture in step A1 and stir evenly. Select thermochromic capsules that can change from grass green to khaki at 31°C. The mass ratio of thermochromic capsules to polydimethylsiloxane is 5:10. Then place the composite material in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, leave for 40 min to remove bubbles;

[0126] A3: taking out the composite material obtained in step A2, and pouring it into the camouflage jacket mold and the coaxial method mold;

[0127] A4: Place the camouflage coat mold in step A3 in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, the temperature was raised to 100°C and left for 3h;

[0128] A5. De-mould and take out the adaptive camouflage jacket 1.

[0129] The heating layer 3 is a composite heating plate of graphene, silica gel and ceramic.

[0130] The adaptive camouflage jacket 1 and the all-dielectric absorber 2 are bonded with low-viscosity glue to facilitate the disassembly of the camouflage jacket; the all-dielectric absorber 2 and the heating layer 3 are bonded with high-viscosity glue to ensure close contact and efficient heat conduction.

[0131] Performance test: The all-dielectric absorbing device wearing an adaptive camouflage jacket prepared in the above embodiment 1 was tested for visible light and radar stealth performance. The test process and results include:

[0132] Visible light stealth performance:

[0133] The all-medium absorbing device wearing the adaptive camouflage jacket was placed in the grassland and desert environments for mimicry. The test results are shown in the attached Figure 7 With attached Figure 8 shown.

[0134] Radar stealth performance:

[0135] The microwave absorption characteristics of the sample were measured in a microwave anechoic chamber using an AV3655 stealth target radar cross section tester, and two pairs of broadband horn antennas with operating frequencies of 2-18 GHz and 18-40 GHz were used for measurement. Fig. 9 As shown in the figure, in the radar band of 3.28-40GHz, the reflection coefficient is less than -10dB; the simulation results and experimental results of the all-dielectric absorbing device wearing an adaptive camouflage jacket are compared in the attached figure. Fig.10 As shown, in the radar band of 2.87-40GHz, the reflection coefficient is less than -10dB.

[0136] Through the above embodiments and the test of the all-dielectric absorbing device prepared in the embodiments, it is further proved that the all-dielectric absorber and the all-dielectric absorbing device using the all-dielectric absorber provided by the present invention have adaptive visible light stealth capability in various environments. The all-dielectric absorber itself can achieve broadband microwave absorption (>90%) at 3.28 to 40 GHz. The all-dielectric absorbing device obtained after wearing the adaptive camouflage jacket has an absorbing bandwidth extended to 2.87 to 40 GHz, which solves the technical problems existing in the background technology.

[0137] In the description of the embodiments of the present application, it should be noted that in the description of the present application, terms such as "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is only for the convenience of description, and does not indicate or imply that the device or component must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present application.

[0138] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "in the present embodiment", "specific example", or "some examples" etc. means that the specific features, mechanisms, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, mechanisms, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0139] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for preparing an all-dielectric absorber, characterized in that: The following steps are involved: S1: mixing the dielectric loss material and the magnetic loss material, stirring and shaking to obtain a composite material; S2: Mix and stir the composite material obtained in step S1 with the adhesive, and control the mass ratio of the dielectric loss material, the magnetic loss material and the adhesive to be (0.01-3):(6-15):4, then place the composite material in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, placed to remove air bubbles; S3: taking out the composite material obtained in step S2 and pouring it into a mold; S4: Place the composite material in step S3 together with the mold in a vacuum dryer and draw the vacuum degree to <3.0×10 -3 Pa, the temperature is raised to above 80 °C, and after standing for one hour, the mold is removed to obtain a full dielectric absorber.

2. The method for preparing the all-dielectric absorber according to claim 1, characterized in that: In step S1, the dielectric loss material is selected from one or more of dielectric loss materials carbon nanotubes, ceramic powders, conductive polymers and SiC; the magnetic loss material is selected from one or more of ferrite, spherical hydroxyl iron powder, flaky hydroxyl iron powder and sendust powder.

3. The method for preparing the all-dielectric absorber according to claim 1, characterized in that: In step S2, the adhesive is silicone rubber or epoxy resin adhesive, and the mass ratio of the dielectric loss material, magnetic loss material and adhesive is (0.1-3):(6-15):

4.

4. The method for preparing the all-dielectric absorber according to claim 1, characterized in that: In the step S2, the standing time is more than 20 minutes, and in the step S4, the standing time is more than 1 hour.

5. An all-dielectric absorber, characterized in that: The all-dielectric absorber is prepared by any one of the preparation methods of claims 1-4.

6. An application of an all-dielectric absorber, characterized in that: The application includes applying the all-dielectric absorber described in claim 5 to an all-dielectric absorber, and the all-dielectric absorber includes an adaptive camouflage jacket, the all-dielectric absorber and a bottom heating layer connected in sequence from top to bottom, and the adaptive camouflage jacket is made by mixing thermochromic capsules and polydimethylsiloxane using an injection molding process.

7. The use of the all-dielectric absorber according to claim 6, characterized in that: The adaptive camouflage jacket and the all-dielectric absorber are bonded with a low-viscosity glue of 20-500 centipoise, and the all-dielectric absorber and the bottom heating layer are bonded with a high-viscosity glue of 2000-5000 centipoise.

8. The use of the all-dielectric absorber according to claim 6, characterized in that: The bottom heating layer is one of a graphene heating plate, a silica gel heating plate, a ceramic heating plate, or a composite heating plate composed of graphene, silica gel and ceramic.

9. The use of the all-dielectric absorber according to claim 6, characterized in that: The preparation method of the adaptive camouflage coat comprises: A1: Glue is prepared by mixing polydimethylsiloxane and curing agent; A2: adding thermochromic capsules to the glue in step A1 and stirring to obtain a composite material, then placing the composite material in a vacuum dryer and drawing the vacuum degree to <3.0×10-3Pa, and removing bubbles after standing; A3: taking out the composite material obtained in step A2 and pouring it into a mold; A4: Place the camouflage jacket mold in step A3 in a vacuum dryer and draw the vacuum degree to <3.0×10-3Pa, raise the temperature to 100°C, and demould after standing to obtain an adaptive camouflage jacket.

10. The use of the all-dielectric absorber according to claim 9, characterized in that: In the step A1, the curing agent is curing agent SE1700; the mass ratio of the polydimethylsiloxane, SE1700 curing agent and the temperature-dependent capsule composite material is 10:1:(0.1-5); in the step A2, the placement time is more than 40 minutes; in the step A4, the placement time is more than 2 hours.