Winding device
A three-layered device with a nylon core, active sheath, and protective sheath, actuated by magnetic fields, addresses the limitations of soft devices by achieving high force and work capacity, suitable for medical and robotic applications.
Patent Information
- Application Number
- CN202380036040.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-24
- Filing Date
- 2023-02-20
- Publication Date
- 2024-12-03
AI Technical Summary
Existing soft medical devices face limitations in force output and work capacity, making them unsuitable for applications requiring large force and high work capacity, such as squeezing, clamping, and cutting, due to their softness and inability to store and release mechanical energy effectively.
A device composed of at least three layers: a core of nylon fiber, an active sheath with graphene oxide (GO) and magnetic particles embedded in a resin, and a protective sheath of an elastic material, which can be actuated wirelessly through magnetic fields, allowing for high force output and work capacity.
The device achieves untethered actuation with force outputs up to 3 N and work capacities up to 3.5 kJ/kg, enabling applications like suturing, drilling, and gripping with improved mechanical performance and compatibility with biological tissues.
Smart Images

Figure BDA0005099675810000211 
Figure BDA0005099675810000212 
Figure BDA0005099675810000221
Abstract
Description
Technical Field
[0001] The present invention relates to a device comprising one or more structures. The present invention also relates to a method of forming a device having one or more structures. Background Art
[0002] Wireless, small, soft medical devices as small as a few millimeters or even smaller have been able to safely and adaptably navigate confined spaces, such as within machines with small-diameter pipes and channels, or even within the human or animal body. This unique capability can also have potential advantages in a variety of medical applications, such as minimally invasive surgery and localized on-demand treatment procedures.
[0003] For such micro-devices, various optical, thermal, and acoustic soft actuation approaches have been explored. While the softness of these devices gives them the ability to have large programmed deformations and safely interact with the environment, it also limits their output force and weight-normalized work capacity.
[0004] Typically, soft devices exhibit small force output and large deformation. The softness of the material makes it difficult to store and release large amounts of mechanical energy. Therefore, they cannot be used in devices and robotic applications that require large force output and high work capacity.
[0005] According to one example, without considering increasing the external magnetic field amplitude, it is calculated that the output force of the existing magnetic soft device is saturated at around 60 μN.
[0006] However, some medical procedures (such as squeezing, clamping, and cutting) require devices with higher force output (i.e., force output greater than 1 N), which is about 10 times higher than the maximum capability of previously reported magnetic soft devices. 5 times.
[0007] At scales in the range of a few centimeters or more, coiled artificial muscles have proven to be promising devices that can be manufactured by continuously twisting polymer fibers into a coiled shape. Recent studies have shown that coiled muscles can have higher work capacity and greater output force than previously proposed methods. Specifically, the work capacity of coiled muscles is 50 times greater than that of biological skeletal muscles. In addition, when the muscles are composed of carbon nanotubes, shape memory polymers, and fishing line, coiled muscles may provide output more than 1,000 times higher than their own weight.
[0008] In addition, the force output and work capacity of the coiled muscle may be greatly increased by tailoring the composition or structure of its precursor fibers (e.g., by adding graphene oxide (GO) sheets to the precursor fibers or designing a tough sheath on their surface). Such coiled muscles are expected to advance the fields of humanoid robots, prosthetics, and microfluidic devices. Summary of the invention
[0009] In view of this background, it is an object of the present invention to provide a device with a large output force and a high work capacity.
[0010] This object is solved by the subject-matter of the independent claims.
[0011] In particular, the device according to the present invention is composed of one or more structures, each of which comprises at least three layers. That is, the device comprises at least a core, an active sheath and a protective sheath. The core is formed by at least one nylon fiber, the active sheath comprises a resin, and graphene oxide (GO) and the first type of magnetic particles are respectively embedded in the resin. In addition, the protective sheath is formed by an elastic material, which protects the inner layer from the external environment.
[0012] Therefore, in other words, the device of the present invention includes one or more structures (e.g., artificial coiled muscles) that are integrated into a device (such as a micro-soft device) so that the application of the device can be expanded to devices requiring large output force and high work capacity.
[0013] One or more structures are built up as at least three layers, including a core, an active sheath and a protective sheath. Each layer has a specific function.
[0014] For example, the function of the core is to provide an intrinsic function of the device, ie if a clamping or gripping function of the device is required, the core can be formed by a structure enabling such clamping or gripping function, for example in the form of a wound structure.
[0015] The active sheath allows for external actuation of the device in a tethered manner or, more preferably, in an untethered manner (eg, by application of magnetic and / or electromagnetic fields).
[0016] Finally, the function of the protective sheath is to protect the core and the active sheath from external influences such as the fluids present in the human body.
[0017] The core is formed from at least one nylon fiber. Such a fiber has proven to be advantageous because, for example, it can be twisted to use as a wound structure as described above.
[0018] The active sheath comprises a resin, in which graphene oxide (GO) and a first type of magnetic particles (particularly nanoparticles) are respectively embedded. The first type of magnetic particles can also include paramagnetic and / or superparamagnetic (nano) particles. The combination of GO particles and magnetic particles can increase the toughness of the active sheath and can respectively achieve, for example, wireless heating, such as radio frequency magnetic heating. The heating process is necessary for the actuation structure.
[0019] Furthermore, the introduction of (super)para)magnetic particles and GO particles into the active layer can facilitate the realization of untethered actuation with force outputs up to more than 3 N and high work capacities reaching values up to 3.5 kJ / kg.
[0020] The function of the protective sheath is to protect the inner layer from the influence of the external environment. For example, the fluid environment can reduce the heating efficiency of the device, thereby affecting the actuation strain and output force of the device. The protective layer can be configured to protect the inner layer from such influences. Another function of the protective layer is to protect the inner layer from possible structural damage when the device is in action, for example, due to mechanical collision with other structures. Another function of the protective layer can also be to protect the external environment from the heat generated by the active sheath. It can be shown that, for example, when measuring the temperature at a small distance from the surface of the device (such as 2 mm), the surface temperature of the device without the protective layer rises to more than 120°C, while the surface temperature of the device including the protective layer can be maintained at about 60°C or even lower, such as 30°C.
[0021] Therefore, it can be concluded that the protective layer of the structure includes several important functions.
[0022] It is also noted in this regard that by integrating one or more of these structures into different devices, a wide variety of microdevices can be realized, such as suturing devices, scissors, drills, and energy storage bistable structures, all of which require high force output and work capacity.
[0023] According to a first embodiment of the invention, the device further comprises a fourth layer, which is a magnetization sheath. For example, the fourth layer can be used to encode a magnetization curve on the device to achieve magnetic deformation and high output contraction force.
[0024] According to another embodiment, the magnetizing sheath comprises a combination of magnetic particles and an elastomer, such as a combination of NdFeB and PDMS. Other examples of the fourth layer of magnetic particles can be permanent magnetic particles, such as AlNiCo magnets and / or SmCo magnets. The elastomer matrix can also include silicone rubber, such as Ecoflex 00-30 TM 、Ecoflex 00-50 TM or Dragon skin 30 TM .
[0025] The resin of the active sheath may also include a polyurethane casting resin such as Crystal Clear TM Or nylon. The base material of the active sheath, that is, the resin of the active sheath, must include a very durable tough material.
[0026] According to another embodiment, the first type of magnetic particles is formed of Fe3O4. That is, the magnetic particles present in the active sheath are formed of Fe3O4 particles, which can be used to generate heat under conditions such as radio frequency magnetic heating. For example, such a heating process can cause the coiled structure to shrink and thus generate movement.
[0027] The first type of magnetic particles, ie the Fe3O4 particles, can comprise a size selected in the range of 10 nm to 500 nm, in particular in the range of 20 nm to 200 nm, in particular in the range of 50 nm to 100 nm.
[0028] According to another embodiment, the device comprises a second type of magnetic particles formed of NdFeB, the second type of magnetic particles comprising a size selected in the range of 0.1 μm to 10 μm, in particular in the range of 2 μm to 6 μm. The second type of magnetic particles can be embedded in the fourth layer (if present). For example, such particles can be used to propel different devices according to the invention under magnetic torque and magnetic gradient. The average diameter of such particles is typically around 5 μm.
[0029] The active sheath may also comprise a thickness ranging from 50 μm to 300 μm, in particular from 100 μm to 250 μm, especially 200 μm.
[0030] The active sheath can include a GO concentration selected in the range of 1 wt% to 6 wt%, particularly in the range of 2 wt% to 4 wt%. Increasing the GO concentration of the device can enhance the output performance of the device. However, as the GO concentration increases, the active sheath becomes more fragile and brittle. Therefore, the correct selection of GO concentration is not easy.
[0031] In another embodiment, the active sheath comprises a magnetic particle concentration of the first type of magnetic particles selected in the range of 10 wt% to 30 wt%. The heating efficiency of the active sheath increases with the increase of the concentration of the first type of magnetic particles, which is beneficial to the device of the present invention. However, if the concentration is too high, the device is more susceptible to damage. Therefore, the above range of 10 wt% to 30 wt% has proven to be desirable.
[0032] The device can also include a coiled shape. As mentioned in the introduction to this application, coiled structures have been shown to have higher work capacity and greater output force.
[0033] According to another embodiment, the nylon fiber comprises a diameter selected in the range of 0.1 mm to 0.5 mm, in particular 0.2 mm to 0.5 mm, in particular 0.45 mm.
[0034] It is also noted in this context that the nylon fibers can have a length selected in the range of 1 cm to 100 cm, in particular in the range of 1 cm to 50 cm, in particular in the range of 5 cm to 40 cm.
[0035] According to another embodiment, the device comprises a diameter selected in the range of 0.1 mm to 10 mm, in particular a diameter of 0.4 mm to 5 mm, especially 0.4 mm to 1.2 mm.
[0036] In this regard, it is noted that the nylon fiber as described above can be twisted a number of times to form a wound structure, for example the number of twists can be selected between 100 and 10,000 twists, i.e. the wound structure comprises 100 to 10,000 turns of a single nylon fiber in each core. The exact number of turns depends on the length of the fiber that should be twisted. For example, for a fiber length ranging from 1 cm to 50 cm, approximately 100 to 1,000 turns are required.
[0037] According to yet another embodiment, the device comprises at least one functional component, such as a frame, a blade, a rod, a screw, a chassis and / or a combination of the foregoing. These functional components enable the device to be used in various applications, such as non-tethered micro soft (medical) devices and robotic applications, thereby expanding the application field of currently known devices. That is, different device examples of staplers, drills, scissors, clamps and even multi-connected devices can be realized, each device having a corresponding potential function.
[0038] According to another aspect of the present invention, a method for forming a device having one or more three-layer structures is provided. The method comprises the following steps: providing a fiber; coating the fiber with an active sheath material, wherein the active sheath material comprises a resin, graphene oxide (GO) and a first type of magnetic particles embedded in the resin; further coating the fiber with a protective sheath material, wherein the protective sheath material comprises an elastic material; and continuously twisting and winding the coated fiber to form the device. Optionally, the coated fiber may also be cured before twisting and winding.
[0039] According to one embodiment of the present invention, the method further comprises the step of coating the fiber with an additional magnetic sheath before winding the coated fiber. The additional magnetic sheath is a combination of magnetic particles and an elastomer, such as a combination of NdFeB and PDMS. Other examples of magnetic particles for the fourth layer can be permanent magnetic particles, such as AlNiCo magnets and / or SmCo magnets. The elastomer matrix can also include silicone rubber, such as Ecoflex 00-30TM 、Ecoflex 00-50 TM or Dragonskin30 TM .
[0040] The step of winding the coated fiber may also include at least 250 turns, preferably 300 to 400 turns. The exact number of turns generally depends on the length of the fiber. For example, 100 to 800 turns are required to wind a fiber with a length of 5 cm to 40 cm. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Embodiments of the present invention are further described in the following description of the drawings. The present invention will be described in detail below by way of embodiments and with reference to the accompanying drawings shown:
[0042] Figure 1 :Design, fabrication process, actuation mode and actuation mechanism of magnetically heated coiled muscle structure;
[0043] Figure 2 : Characterization of coiled muscle structure and performance;
[0044] Figure 3 : Wireless suture equipment;
[0045] Figure 4 : Wireless medical scissors equipment;
[0046] Figure 5 : Wireless medical drilling equipment;
[0047] Figure 6 : Wireless bistable gripper;
[0048] Figure 7 : A multi-jointed coiled muscle structure;
[0049] Figure 8 : Comparison of different types of soft devices and muscle devices in terms of actuation strain, work capacity and energy density;
[0050] Fig. 9 : Modeling of magnetic soft actuator devices;
[0051] Fig.10 :Calculation of functional capacity of magnetic soft actuator devices;
[0052] Fig.11 : Thermal characterization of coiled muscle structures;
[0053] Fig.12 :SEM morphological characterization;
[0054] Fig.13 : Output force characterization;
[0055] Fig.14: tensile strain and torsional stroke of the coiled muscle structure;
[0056] Fig.15 : Reversible torsional actuation;
[0057] Fig.16 : Cross-sectional diagram of strain distribution of coiled muscle structure;
[0058] Fig.17 : Characterization of the structural properties of muscles coiled in deionized water;
[0059] Fig.18 :Performance evaluation and application prospects of coiled muscle structures;
[0060] Fig.19 : Force testing of suture equipment;
[0061] Fig. 20 : Design of reversible gripper device;
[0062] Fig.21 : Precursor fiber design of multi-connected coiled muscle structure;
[0063] Fig. 22 : Surface walking movement of multi-jointed coiled muscle structures;
[0064] Fig.23 : Characterization of active sheath thickness;
[0065] Fig.24 : Measurement schematic diagram;
[0066] Fig.25 : Different methods for measuring actuation strain;
[0067] Fig.26 :Calculation of output force of magnetic soft actuator device;
[0068] Fig. 27 : Calculation of actuation strain and work capacity of coiled muscle structure;
[0069] Fig.28 : Comparison of theoretical and experimental results for coiled muscle structures;
[0070] Fig.29 : Measurement schematic diagram of the gripper device;
[0071] Fig.30 :Optimization method for bistable design;
[0072] Fig.31 : static gripping force and potential energy of a bistable gripper device; and
[0073] Fig.32 : Characterization of pre-stretched elastomers. DETAILED DESCRIPTION
[0074] In the following, the same reference numerals will be used for components having the same or equivalent functions. Any statements regarding the orientation of components are made relative to the position shown in the figures and can naturally differ from the actual position of use.
[0075] Figure 1 The design, manufacturing process, actuation mode and actuation mechanism of the magnetically heated coiled muscle structure 10 according to the present invention are shown. Figure 1 a shows a schematic cross-sectional view of the rolled muscle structure 10 before rolling. Figure 1 b shows the manufacturing process of the coiled muscle structure 10, including the steps of coating, twisting and coiling, annealing and training. Figure 1 c shows a photograph of the fabricated coiled muscle structure 10 with a diameter of 1 mm. Figure 1 d shows the contraction actuation of the coiled muscle structure 10 under radio frequency magnetic heating, Figure 1 e shows the torsional actuation mode of the coiled muscle structure 10 under radio frequency (RF) magnetic heating. Figure 1 f shows a photograph of the structural changes of the coiled muscle structure 10 before and after radio frequency magnetic heating. Figure 1 g shows the changes in length and diameter of the three-layer precursor fiber 10 before winding under different temperature conditions.
[0076] In this regard, it is noted that Figure 1 a and Figure 1 In the cross section of FIG. 1 b , the three-layer structure 10 of the device according to the invention can be clearly seen, comprising the core 12 , the active sheath 14 and the protective sheath 16 .
[0077] Figure 1 b also shows that the core is made of nylon fiber 18, while the active sheath comprises a resin (in this case CrystalClear) 20, in which graphene oxide flakes GO and first type magnetic particles 22 are respectively embedded. Figure 1 The protective sheath 18 of b is made of an elastic material 24 (ie, for example, PDMS).
[0078] Figure 2 The results of characterization of the performance of the coiled muscle structure 10 are shown. Figure 2 a and Figure 2 In b, the effect of GO flake concentration can be seen, while Figure 2 c and Figure 2 d shows the effect of the thickness of the active sheath 14 on the muscle actuation strain and work capacity under different tensile forces. The torque output of the coiled muscle 10 with different GO flake concentrations and active sheath 14 thicknesses is Figure 2 c and Figure 2 f is shown.
[0079] Figure 3 A demonstration of the wireless stitching device 100 is shown. Figure 3 a shows a schematic diagram of a design comprising a suturing device 100 . Figure 3 b shows that the suturing device 100 consists of two printed barrier plates 102 , a coiled muscle structure 10 , and a cylindrical NdFeB magnet 104 . Figure 3 c shows the winding action of the suturing device 100 during the wound suturing process controlled by the tension based on the external magnetic field gradient and the radio frequency magnetic heating generated by the external permanent magnet 104 .
[0080] Figure 4 A demonstration of a wireless medical scissors device 200 is shown. Figure 4 a shows a schematic diagram of the cutting behavior of the scissors device 200 including the design. Figure 4 b shows an image of a scissor device 200 consisting of a 3D printed polymer frame 202 , a coiled muscle actuator 10 , a magnetic component (NdFeB microparticles embedded in an Ecoflex-30 silicone rubber matrix) 204 , and two cutting blades 206 . Figure 4 c shows the cutting behavior of the scissors device 200 under radio frequency magnetic heating. Figure 4 d shows the cutting force of the scissors device 200 measured during the cutting process. Figure 4 e is a video snapshot of the device 200 being rotated by an external magnetic field, rolling on a surface using a permanent magnet to reach a target agarose gel column, and cutting the column by radio frequency heating.
[0081] Figure 5 A demonstration of a wireless medical drill device 300 is shown. Figure 5 a shows a schematic diagram of the designed drilling rig 300. Figure 5 b is an image of a drilling rig 300 consisting of a 3D printed polymer frame 202 and a coiled muscle 10 . Figure 5 c shows a video snapshot of the device 300 drilling a hole a distance into the surface of an agarose gel (similar to soft biological tissue) while being magnetically heated. Figure 5 d shows the drilling torque measured for the apparatus 300 under RF heating.
[0082] Figure 6 A demonstration of a wireless bistable clamp 400 is shown. Figure 6 a shows a schematic diagram of a clamp 400 designed with a bistable structure 10. The clamp 400 further comprises a body 402, which may be formed of the aforementioned polymer frame and a pre-tensioned elastic body 404, for example. Figure 6 b is a simplified diagram showing the clamping process under radio frequency heating. Figure 6 c shows the energy distribution with different joint angles during the clamping process. Figure 6 d shows the experimental clamping force and simulated clamping force of the clamp 400 with different designed joint angles. Figure 6 e includes an image showing the clamping device 400 clamping an ex vivo chicken tissue wound.
[0083] Figure 7 A multi-linked coiled muscle device 500 is shown. Figure 7 a is a schematic diagram showing the bending of the multi-connected coiled muscle device 500 under magnetic moment and under radio frequency magnetic heating. The multi-connected coiled muscle device 500 is encoded with a magnetization curve. That is, the coiled muscle structure 10 of the multi-connected coiled muscle device 500 includes a fourth layer 26, which is a magnetized sheath 26. The magnetized sheath 26 includes a combination of a second type of magnetic particles 28 and an elastomer 30. The multi-connected coiled muscle device 500 includes two rods 502 and four coiled muscle structures 10, which are connected by a connector 504. Figure 7 b shows an image showing the "walking" behavior of the multi-linked coiled muscle device 500 under magnetic torque and magnetic gradient. Figure 7 c shows a video snapshot demonstrating the contraction performance of the same multi-linked coiled muscle device 500 under RF magnetic heating. Figure 7 d shows the actuation strain of the multi-linked coiled muscle device 500 under different tensile forces.
[0084] Figure 8 Table 1 is included, which shows a comparison of different types of soft actuators and muscle actuators in terms of actuation strain, work capacity and energy density, wherein the expression "LCE" stands for "liquid crystal elastomer", "HASEL" stands for "hydraulic amplified self-healing electrostatic actuator", and "IPMC" stands for "ionic polymer-metal composite". It can be clearly seen that the magnetic soft robot according to the device of the present invention comprises a higher actuation strain and work capacity than the other examples given in said table.
[0085] Fig. 9 FIG. 1 is a schematic diagram showing the actuation of the magnetic soft actuator 10 according to the present invention. The detailed explanation of the figure is as follows.
[0086] Fig.10 A graph is included that shows the calculation of the work capacity of the magnetic soft actuator 10, wherein the theoretical work capacity of the magnetic soft component actuator is a function of the applied magnetic field. A detailed explanation is given below.
[0087] Fig.11 Thermal characterization of a coiled muscle structure 10 according to the invention is shown. Fig.11 a shows the surface temperature variation of the rolled muscle structure 10 with different PDMS coating thicknesses under RF heating. Fig.11 b and Fig.11 c shows infrared thermal images of a coiled muscle structure 10 with a PDMS sheath 16 having a thickness of 200 μm before and after radio frequency heating, respectively. Note in this regard that the black dashed rectangle indicates the position of the coiled muscle structure 10 .
[0088] Fig.12 Including SEM morphological characterization, namely Fig.12 a shows the cross-sectional structure of the precursor fiber 10, Fig.12 b shows the final coiled muscle structure 10 .
[0089] Fig.13 Output force characterization is shown, where the tensile force of the coiled muscle 10 has a constant strain of 0.1% under heating.
[0090] Fig.14 The tensile strain and torsional stroke of the coiled muscle 10 are shown. Fig.14 a and Fig.14 b shows the changes of tensile actuation strain with time and temperature in contraction actuation, respectively. Fig.14 c shows the torsion stroke in torsion actuation. In this regard, it is noted that Fig.14 In b, the red and black lines represent the temperature increase and decrease processes, respectively.
[0091] Fig.15 Reversible torsional actuation is shown. The lower clockwise portion of the coiled muscle 10 is shown Fig.15 As shown in a, Fig.15 b shows the upper counterclockwise portion of the coiled muscle 10 . Fig.15 c and Fig.15 d show the corresponding counterclockwise and clockwise rotations of the coiled muscle 10 under RF heating, respectively.
[0092] Fig.16 A cross-sectional diagram is shown of the strain distribution of a coiled muscle 10. A detailed explanation of this diagram is as follows.
[0093] Fig.17 The performance of the coiled muscle in deionized water is shown. Fig.17 In a, the temperature change of the coiled muscle 10 under radio frequency heating can be seen. Fig.17 b and Fig.17 c shows the actuation strain and calculated work capacity of the coiled muscle 10 under different stretching forces. Fig.17 d shows the torsional torque of the coiled muscle 10 under RF heating. In this regard, it is noted that Fig.17 The underlying coiled muscle 10 consists of 4 wt % GO and an active sheath 14 200 μm thick.
[0094] Fig.18 The performance evaluation and application prospects of the coiled muscle 10 are shown. Fig.18 a shows a comparison of different types of soft actuators 100 , 200 , 300 , 400 in terms of functional capacity and power density. Fig.18 b includes schematic diagrams showing that the coiled muscle actuator is designed as a suturing device 100, a scissor device 200, a drill device 300, and a gripper device 400 for biomedical applications.
[0095] Fig.19 Force testing of suturing device 100 is included. Fig.19 a and 19b show photographs of pig skin wounds before and after being pulled closed by the Instron machine, respectively. Fig.19 c shows the pulling force during the pulling process.
[0096] Fig. 20 The design of a reversible gripper device 400 is shown, including a schematic diagram showing the reversible gripping process in coordination with muscle contraction and shape memory material (SMM) elongation.
[0097] Fig.21 The precursor fiber design of the multi-linked coiled muscle 500 is shown. The schematic diagram shows the cross-sectional structure of the precursor fiber 10 after being coated with the magnetized sheath 26.
[0098] Fig. 22 The surface walking motion of the multi-jointed coiled muscle 500 is shown. Fig. 22 a shows a multi-linked coiled muscle 500 wrapped around a cylindrical glass rod 506 and magnetized by a uniform 1.8T magnetic field. Fig. 22 b shows the corresponding distribution of magnetization directions. Fig. 22 c and 22d show the forward movement of the multi-jointed muscle 500 under an external magnetic field, while Fig. 22 22e and 22f show the backward movement of the multi-jointed muscle 500 under an external magnetic field.
[0099] Fig.23 A representation of the thickness of the active sheath 14 is shown, wherein the thickness of the active sheath 14 is plotted against the number of times the core 12 is coated using a droplet coating technique.
[0100] Fig.24 It is used to measure the tensile actuation force ( Fig.24 a) Torque Fig.24 b) and actuation strain ( Fig.24 c) Schematic diagram of the measurement device.
[0101] Fig.25The measurement results of the actuation strain measured by different methods are shown, as well as the comparison of the actuation strain of muscles coiled under various loads by heat gun heating and radio frequency heating.
[0102] Fig.26 Shown is a Matlab code for calculating the output force of the magnetic soft actuator 10. The Matlab code calculates the output force of the magnetic soft actuator 10 by using a numerical method.
[0103] Fig. 27 It is shown how the actuation strain and work capacity of a coiled muscle 10 can be calculated. The schematic diagram shows the length dependence on the load force of an actuated and a non-actuated coiled muscle 10.
[0104] Fig.28 A comparison of theoretical and experimentally coiled muscle 10 is shown, where Fig.28 A comparison of the actuation strain can be seen in a, while Fig.28 b shows a comparison of the work capacity results under different load forces. The theoretical calculation results are represented by the red dashed line, while the experimental measurement results are represented by the green solid line. It is noted in this regard that the experimental results are based on a coiled muscle 10 consisting of 4 wt % GO and 200 μm active sheath 14 thickness.
[0105] Fig.29 A gripper device 400 is shown comprising means for testing the gripping force of the bistable gripper device 400 .
[0106] Fig.30 shows the ratio between the output force and the input force as θ c / θ s Optimization results of the bistable design of the function.
[0107] Fig.31 The static clamping force and potential energy of the bistable clamp 400 are shown. Fig.31 a shows the relationship between the theoretical static clamping force and the joint rotation angle under different pre-stretching strains in the elastic body 404, and Fig.31 b shows the relationship between the theoretical potential energy and the joint rotation angle under different pre-stretching strains in the elastic body 404.
[0108] Fig.32 Included are characterizations of the pre-stretched elastomer 404 and tensile stress-strain curves of the elastomer 404 for the bistable gripper 400 .
[0109] The following is a detailed description of various embodiments of the present invention as well as the corresponding experimental devices, calculations and results.
[0110] Equipment design, manufacture and mechanism
[0111] The design of the proposed structure 10 (hereinafter referred to as muscle actuator 10) is as follows Figure 1 It consists of three layers: a high-strength nylon fiber as a muscle core 12 that provides restorative stiffness; an outermost protective sheath 16 that mechanically and thermally isolates the inner layer from the external environment (see the methods section below and Fig.11 ); and, an active sheath 14 between the core 12 and the protective sheath 16. The active sheath 14 is composed of three elements: Crystal Clear TM The matrix 20 (rigid polyurethane casting resin 20, which is a heat-cured commercial product), superparamagnetic Fe3O4 nanoparticles 22 and mechanical strength-enhancing GO flakes. The three-state structure is finally twisted to form a muscle structure 10, that is, a coiled muscle 10.
[0112] It is noted in this regard that the nylon fibers have a strength selected within the range of 1.0 GPa to 1.2 GPa.
[0113] The three-layer structure 10 is manufactured by a customized droplet coating technique ( Figure 1 b) In the first step, a nylon fiber 12 with a diameter of 0.45 mm is immersed in uncured Crystal Clear TM The resin 20 solution is mixed with Fe3O4 nanoparticles 22 and GO flakes to produce an active sheath 14. Next, a similar droplet coating process is used to coat with PDMS 24 to form a protective sheath 16. Fig.12 As shown in FIG. 1 , after the PDMS layer 16 is completely cured, its cross-sectional structure is characterized by scanning electron microscopy (SEM). The thickness of each sheath 14, 16 can be controlled by repeatedly applying the droplet coating method. Then, by continuously twisting the above-mentioned three-state structure 10, a rolled structure 10 is first formed, and then annealed and trained to obtain the final rolled structure 10. As shown in the optical microscopy image ( Figure 1 c) and zoomed SEM images ( Fig.12 As shown in b), the obtained muscle 10 has a coiled shape and a diameter of about 1 mm.
[0114] The coiled muscle 10 is wirelessly actuated by heating the embedded magnetic nanoparticles 22 with an external RF magnetic field generator. The coiled muscle 10 has two operating modes under wireless RF magnetic heating. First, it exhibits contraction actuation when both ends are allowed to move axially but restricted from rotation. Figure 1 d, it is possible to pull a target of 1.3 N at a strain of 30%. It is even possible to pull up to 12.6 N at a reduced strain (1%), which will be combined later Figure 2 a for discussion. Fig.13As shown, the tensile force output of the coiled muscle 10 at a constant strain of 0.1% may reach about 3.1 N.
[0115] Secondly, if Figure 1 As shown in Fig. 5, when one end of the coiled muscle 10 is fixed and rotated freely, it exhibits torsional actuation, and its torque may reach about 1.76 mN·m. In addition, the changes of actuation strain and torsional stroke in such contraction actuation and torsional actuation are characterized respectively ( Fig.14 ). It shows that contraction actuation is reversible actuation, while torsion actuation is only a one-time actuation. This is because there is no constraint during torsion actuation, which releases the strain energy generated during the twisting and coiling manufacturing process. In order to reverse the torsion actuation, the coiled muscle 10 is designed with two parts with different twisting directions. This design is shown in Fig.15 By actuating the lower part, the actuator rotates counterclockwise, as opposed to its clockwise design. By actuating the upper part, the actuator rotates clockwise.
[0116] The proposed coiled muscle 10 exhibits new characteristics that were not available with previous twisted muscles, including magnetic responsiveness, enhanced mechanical output, and better compatibility with biological tissues, enabling wireless medical device applications. Its actuation mechanism is due to the untwisting process of the fiber caused by thermal contraction in the longitudinal direction and thermal expansion in the radial direction. This mechanism was studied by recording the actuation process under optical microscopic imaging. Figure 1 As shown in Fig. 5, the coil spacing shrinks from 1.95 mm to 1.77 mm before and after RF magnetic heating. The length and diameter of the three-state structure 10 before the twisting and winding process at different temperatures are also characterized. Figure 1 As shown in Figure g, the axial contraction is 3.7% and the radial expansion is about 11.3%, which further verifies the actuation mechanism.
[0117] The main feature of this three-state design lies in the composition of the active sheath 14 (intermediate layer), which includes the resin matrix 20, magnetic nanoparticles 22 and GO flakes. TM The resin 20 serves as a matrix because of its inherent high toughness and large expansion ratio. Both are conducive to delivering high strokes and high mechanical outputs. Secondly, the Fe3O4 nanoparticles 22 enable a magnetocaloric effect, making it possible to actuate the muscle 10 wirelessly via a radio frequency magnetic field. It is also noted in this regard that the Fe3O4 nanoparticles 22 themselves also play a role in toughening the muscle 10. Furthermore, the GO flakes, due to their unique 2D geometry, greatly assist in fiber strain energy storage, especially when twisted much more than nanoparticles or carbon nanotubes as toughening agents. In this embodiment, GO flakes are introduced into the active layer 14 located near the outermost surface because the expansion forces are more effective when they act near the edges of the yarn ( Fig.16), where the strain energy is at its maximum value.
[0118] Performance Characterization
[0119] The performance of the magnetically heated coiled muscle 10, such as its actuation strain and work capacity as well as torque output, is highly dependent on the GO flake concentration and active sheath thickness. Figure 2 These two factors are systematically characterized. First, Figure 2 a- Figure 2 c shows the results of increasing the flake concentration from 1wt% to 4wt%, while keeping the active sheath thickness fixed at 200μm. The coiled muscle 10 with a 4wt% concentration delivered higher actuation strain. By adjusting the toughening agent from 1wt% to 4wt%, the load-optimized work capacity and torque increased from 2.46J / g and 0.66mN·m to 3.5J / g and 1.76mN·m, respectively. This is because the GO flakes exhibited obvious bending and twisting behavior inside the fiber, which improved the mechanical energy stored during twisting and coiling.
[0120] Secondly, Figure 2 d- Figure 2 f shows the results of increasing the sheath thickness from 100 to 200 μm while fixing the GO flake concentration at 4 wt%. Figure 2 d shows the results of the actuation strain. When the load is less than 2.1 N, the coiled muscle 10 with thicker sheath thickness has lower actuation strain. This is because of the coil-to-coil contact. When the load is higher than 2.1 N, the coiled muscle 10 with thicker active sheath 14 thickness has higher actuation strain. Figure 2 e and Figure 2 f shows that by increasing the active sheath thickness from 100 μm to 200 μm, the load-optimized work capacity and torque could be increased from 2.19 J / g and 1.01 mN·m to 3.5 J / g and 1.76 mN·m, respectively. Such results are consistent with previous literature findings, in which thickening the outer layer rather than the core is much more effective in improving the performance of artificial muscles. Note that when the flake (GO) concentration and the active sheath 14 thickness exceed 4% and 200 μm, respectively, the active sheath 14 tends to break in the experiment. Therefore, no further measurements of these parameters were performed. In addition, the coiled muscle 10 was characterized in deionized water. The results include surface temperature, tensile actuation strain, tensile work capacity, and torsional torque, as shown in Fig.17 As shown. Figure 2 By comparison, the output performance of the coiled muscle 10 in water is similar to that in air. This may be attributed to the insulating properties of the protective sheath 16.
[0121] Finally, the mechanical properties of the proposed coiled muscle 10 are further compared with other types of soft actuators, as summarized below. Fig.18a and Table 1, section “Calculation of force and work capacity of magnetic soft actuators”. The coiled muscle 10 has a higher work capacity than popular soft actuators, including skeletal muscle, McKibben actuator, liquid crystal elastomer (LCE), biohybrid actuator, hydraulically amplified self-healing electrostatic actuator (HASEL), ionic polymer metal composite (IPMC), and magnetic soft actuator (see section “Calculation of force and work capacity of magnetic soft actuators” below). In the category of magnetic soft actuators, the magnetically heated coiled muscle 10 shows a higher work capacity than previous magnetic soft actuators by about 2×10 5 times the actuation force output and about 1.75×10 4 times the work capacity, greatly increasing the mechanical performance of magnetic soft actuators and expanding their capabilities to medical device applications that require high force and high work density output.
[0122] Application Demo
[0123] Using the given magnetically heated coiled muscle prototype 10, several proof-of-concept demonstrations for wireless medical device applications are reported ( Fig.18 b). The first demonstration shows the suturing device 100 ( Figure 3 ). Suturing is a critical aspect of most surgeries. Traditional suturing relies on the physical manipulation of articulated tools and suturing devices. Due to the large footprint of the operating tools, traditional suturing usually requires a larger surgical incision, which can cause more tissue damage, longer recovery time or other associated infections. Here, a wireless suturing medical device 100 for suturing ex vivo wounds of pig skin is demonstrated. The device 100 is made possible by precise magnetic field control and the high output force of the coiled muscle 10.
[0124] like Figure 3 a- Figure 3 As shown in FIG. 1 , the suturing device 100 is composed of two rods 102 on both sides of the coiled muscle 100 and a magnetic component 104 located at the front, which is a cylindrical NdFeB magnet 104. The rod 102 is made of pure nylon fiber and is used to prevent the coiled muscle 10 from rotating under radio frequency magnetic heating. It also acts as an anchor to close the wound during the contraction of the coiled muscle 10. The NdFeB magnet 104 in the front is pulled by the gradient of an external permanent magnet to pull and guide the coiled muscle 10 around the wound. Please note that the Fe3O4 nanoparticles 22 used in the active sheath 14 are too weak to generate sufficient pulling force through the magnetic field generated by the permanent magnet.
[0125] The whole suture process is as follows Figure 3 c, which is divided into two steps. In the first step, the suture device 100 is wrapped around the wound under a magnetic field ( Figure 3IV in c), which demonstrates the flexibility (low bending stiffness) of the coiled muscle 10. Note in this regard that holes were previously punched in the pigskin to facilitate perforation. Due to the high stiffness of the pigskin, currently, even with the addition of a suture needle at one end of the actuator, it is not possible to penetrate the tissue. However, such penetration may be achieved by using a sharper needle or a larger magnetic gradient force. In a second step, the RF magnetic heating is turned on to contract the artificial muscle 10 for wound closure ( Figure 3 VI-VIII) in c, indicating that the coiled muscle 10 has a large output force.
[0126] A control experiment was performed by pulling the head of the device to close the wound using an Instron tensile measurement device. It required a force of 1.21 N and an actuation strain of 29.6% to achieve the same effect ( Fig.19 ). Therefore, the demonstration shows that the proposed coiled muscle 10 exhibits high flexibility and high output force. When the RF magnetic heating is turned off, the recovery of the contracted muscle 10 may reopen the wound. However, almost no reopening was observed. This may be due to the friction between the pigskin and the substrate to which the pigskin is attached. This problem of wound reopening can be solved by making appropriate knots at the end of the device 100 in the future or by designing an anchoring structure (such as a bistable structure). In addition, the device 100 is intended to remain in the body until the wound recovers. Currently, the outermost protective layer 16 of the device is composed of PDMS, which is a biocompatible material. However, further biocompatibility testing is needed to prove the overall biocompatibility of the device 100. Finally, how to release the device 100 after the wound heals deserves further study.
[0127] exist Figure 4 In the second demonstration shown, a scissor medical device 200 is designed. The scissor function is very important for cutting epidermal or internal biological tissues during surgery. Untethered scissors have the potential to reach confined areas within the body and achieve the above functions. Figure 4 a- Figure 4 As shown in FIG. 1 , a scissors medical device 200 is shown, which is composed of a circular printed frame 202, a magnetic component 204 (as a composite material of NdFeB particles embedded in a silicone elastomer (Ecoflex00-30) matrix) and two metal blades 206, which are assembled with a coiled muscle structure 10. The circular shape 202 and the NdFeB magnetic composite component 204 are used to achieve the rolling movement of the device 200 on the solid tissue under the control of an external permanent magnet, which is remotely operated. The blades 206 are carefully designed so as not to hinder the rolling movement and injure the surrounding tissue during the movement. Under radio frequency magnetic heating, the scissors device 200 exhibits cutting behavior based on the contraction of the coiled muscle 10 ( Figure 4 c).
[0128] like Figure 4 d, the cutting force of the scissors device 200 is quantitatively characterized. The force increases with the heating temperature, and the maximum force is about 2N. Figure 4 In e, the feasibility of the scissor device 200 for cutting tissue in future medical applications is demonstrated by cutting a synthetic gel column. By using an external NdFeB permanent magnet ( Figure 4 e), after manually rotating the magnetic field to roll the device 200 to the work site, the device 200 is carefully controlled to orient its blade on a gel column made of 5wt% agarose (a synthetic tissue-like material). Next, radio frequency magnetic heating is turned on to actuate the artificial muscle 10, and finally the column is cut in half ( Figure 4 e). After cutting, the scissor device 200 may be moved away from the agarose tissue under similar magnetic field control with a moving part ( Figure 4 e to leave the scene section).
[0129] Third, a wireless medical drill device 300 ( Figure 5 ). Wireless drills are promising devices for medical applications including navigation, clot removal, or tissue biopsy because the treatment procedure is untethered, precise, and minimally invasive. However, one challenge with these wireless drills is achieving large output torque. For example, the output torque of a previously reported magnetic drill was only 149 μN·m. The drill device 300 according to the present invention adopts a new mechanism to achieve large torque output by utilizing the high energy release capability of the coiled muscle structure 10 during the untwisting process to overcome these challenges. Figure 5 a- Figure 5 As shown in FIG. 1 , a screw 302 and a base plate 202 with a rectangular tail are assembled at the bottom end of the coiled muscle structure 10. The rectangular tail of the base plate 202 is tied to one side of the coiled muscle structure 10 to limit the rotation of one end of the muscle structure 10 during the drilling process. The device 300 may drill into a 5wt% agarose gel ( Figure 5 b) As a synthetic tissue-like material for drilling demonstration. Figure 5 As shown in ΔS in c, the drilling displacement is about 3 mm and the drilling torque can reach about 1.2 mN·m ( Figure 5 d) Currently, the device 300 relies on another structure to function because the tail chassis needs to counteract the torque applied by the screw drilling. By designing a larger tail, the reaction force can be distributed over a wider area, considering the maximum pressure that the target environment can support.
[0130] In a fourth case, a wireless bistable gripper device 400 ( Figure 6The gripper is used for wound gripping and tissue compression in surgical procedures. The gripper device 400 is constructed by combining the bistable coupling structures 402, 404 with the proposed magnetically heated coiled muscle structure 10. The bistable structure acts as a force amplifier, which can further enhance the output force, response speed and actuation strain performance of the twisted muscle structure 10. The design is as follows Figure 6 As shown in a, the actuating mechanism is as follows Figure 6 b. Fabrication details are shown in the Methods section. A theoretical model was developed to guide the gripper design (see below). The mechanical energy of the gripper is stored in a pre-stretched elastomer embedded in a rigid link ( Figure 6 a. Figure 6 b) By simple elastomer pretensioning 404 or setting a stop angle in the connecting rod, the energy storage capacity of the elastomer may be adjusted from low to high.
[0131] The pre-stretched elastic body 404 can enable the clamp 400 to achieve two stable states ( Figure 6 c). When the RF magnetic heating is turned on, the gripper 400 deforms toward the unstable state II where the elastic body 404 stores the most energy. Once it bypasses the unstable state, it quickly enters another stable state III. The coiled muscle structure 10 selected for this design has a force of 1N. Figure 6 d, with the proposed bistable design, the output force of the coiled muscle 10 may be amplified to 14 N. A more detailed explanation of the bistable design can be found in the "Modeling of the Bistable Gripper" section of this disclosure. By using this design enhanced by the bistable structure, it is possible to demonstrate ex vivo gripping of chicken skin wounds (see Figure 6 e). This process can be divided into two parts: muscle contraction and elastic body snap-through. When the RF magnetic heating is turned on, the muscle begins to contract, actuating the clamp 400 from stable state I to unstable state II, and then quickly enters stable state III within 2.7ms.
[0132] In addition, the bistable structure gives the design two additional capabilities. First, the bistable kick can be actuated faster than a coiled muscle structure alone. Second, the structure is also used to amplify the actuation strain of the muscle structure. Therefore, this combination can enable future micro (medical) device applications to have a wider design space. According to the illustrated embodiment, the clamp device is a disposable actuation device due to the presence of the bistable structure. However, the target function of the clamp device 400 is wound clamping and tissue compression. Therefore, in most cases, there is no need to reopen the clamp 400. Even commercial tethered clamps (such as SureClip TMHemoclips) will also exhibit one-time actuation. To achieve reversible functionality, additional actuators (such as shape memory materials) can be introduced to switch the device 400 back to the open state (such as Fig. 20 shown).
[0133] In a final embodiment, a multi-linked coiled muscle structure 500 is shown with both programmable magnetic deformation and high force output ( Figure 7 ). In order to encode the magnetization profile on the coiled muscle structure 10, first, an additional sheath 126 is coated on the outer surface of the precursor fiber. The magnetic sheath 26 is composed of PDMS and NdFeB particles. By this modification ( Fig.21 ), the artificial muscle structure 10 has three sheaths. In this regard, it is pointed out that the protective sheath 16 is indispensable because it is more than the active sheath 14 (Crystal Clear TM ) is better combined with the magnetized sheath 26. After the artificial muscle structure 10 is made, four of them (about 4 mm) are connected in series through the connector 504, such as Figure 7 a. The connector 504 is composed of PDMS and NdFeB particles. The connector 504 is softer than the artificial muscle structure 10 and can therefore amplify the magnetic deformation. Finally, two rods 502 are added on both sides of the multi-connected coiled muscle structure 500 to prevent the coiled muscle structure 10 from rotating under RF magnetic heating. Figure 7 a and Fig. 22 As shown, after magnetization, the multi-linked coiled muscle 500 is able to achieve deformation under an external magnetic torque.
[0134] like Figure 7 As shown in Fig. 2b, by using magnetic torque and magnetic gradient, the multi-linked coiled muscle 500 exhibits "walking" behavior. The movement direction of this multi-linked coiled device 500 can be controlled by an external magnetic field. It can move forward and backward ( Fig. 22 ). In addition, when both sides are constrained to rotate but allowed to move axially ( Figure 7 c), the multi-linked coiled muscle 500 also exhibited contraction behavior with an actuation strain (ΔL) of 19.5% under a load force of 0.2N. The maximum tensile force of the coiled muscle structure is about 1N, and the actuation strain is 17.3%. The maximum force is limited by the NdFeB-PDMS connector because it breaks when the tensile force exceeds 1N. With these capabilities, the coiled muscle can achieve more diverse operational behaviors and medical functions in addition to high force output and work capacity.
[0135] Discussion and Conclusion
[0136] The coiled muscle structure 10 according to the present invention can be improved in several directions. First, the core 12 currently used in the above experiments is a commercially available nylon filament. This limits the potential for making microactuators. To address this shortcoming, electrospinning can be used to reduce the diameter of the nylon core 12 used for the microactuator.
[0137] Secondly, the surface temperature of the coiled muscle structure 10 can be further adjusted for different applications. However, the effect of high temperature on specific applications is uncertain. For the current coiled muscle structure 10, a protective insulating sheath 16 located at the outermost layer of the precursor fiber is designed by using PDMS.
[0138] like Fig.11 As shown, the surface temperature is reduced by increasing the thickness of the protective sheath 16. The surface temperature of the wound muscle structure 10 is now reduced to below 60°C. In addition, the surrounding temperature decreases rapidly as the distance from the wound muscle structure 10 increases. Figure 3 As shown in c, at a distance of 2 mm from the coiled muscle structure 10, the temperature drops to 30°C.
[0139] Generally speaking, ordinary cells can withstand temperatures as high as 42° C. to 45° C. However, for the scissors 200 , the drill 300 , and the clamp 400 apparatus, due to the presence of the printing frame 202 , the coiled muscle structure 10 is not in direct contact with the tissue.
[0140] like Figure 4 , Figure 5 and Figure 6 As shown, for the scissors 200, drill 300 and clamp 400 devices, the distance between the coiled muscle structure 100 and the tissue is approximately 5 mm, 4 mm and 1 cm, respectively. Therefore, the temperature on the tissue is below 30°C and will not cause damage to the tissue. For the suturing device 100 and the multi-connection device 500, the target application is to close the wound so that the devices 100, 500 are in direct contact with the tissue. In this case, high temperature can be beneficial for closing the wound during the suturing process through thermal therapy. Such topics deserve further study in the future. Finally, if there is a demanding requirement to further reduce the surface temperature of the coiled muscle 10, it can be achieved by increasing the thermal insulation efficiency of the protective sheath 16. The thermal conductivity of PDMS elastomer is 0.16 W / mK, which can be replaced by cellulose (thermal conductivity is 0.04 W / mK) or polyurethane (thermal conductivity is 0.032 W / mK) (54).
[0141] Third, although fast response is not important in the proof-of-concept application demonstrations (such as suture 100, scissors 200, drill 300, gripper 400 and multi-link actuator 500), it may be desirable in certain future applications. For the current coiled muscle structure 10, the response speed can be increased by selecting a material with a lower glass transition temperature (such as polycaprolactone). For these materials, an outer insulating sheath (protective sheath) may no longer be required, thereby increasing heat dissipation efficiency.
[0142] Materials and methods
[0143] Precursor fiber manufacturing
[0144] The precursor fiber 10' can be and is manufactured by the so-called droplet coating technique. In detail, 640 mg of Fe3O4 nanoparticles 22 (50 to 100 nm in diameter, purchased from Sigma-Aldrich) and 63 mg of GO (Sigma-Aldrich) are first added to 1.5 g of mixed Crystal Clear TM 202 resin 20 (Smooth-On, initial modulus after annealing (ε=1%) measured as 1.04 GPa; volume expansion rate at 120°C 29.5%). The matrix and curing agent (weight ratio 10:9) were stirred for 1 minute. Then, the above mixture was degassed for 5 minutes. Then, nylon 6, fiber 12 (Goodfellow) was vertically immersed in the above mixture, then extracted from the uncured elastomer pool and rapidly heated and cured at about 100°C.
[0145] This step may be repeated multiple times to achieve the desired thickness / diameter of the active sheath 14 ( Fig.23 ). After drying the coated fiber at 30°C for 6 hours, the fiber was vertically immersed in a freshly mixed PDMS matrix and curing agent (weight ratio 10:1, Sylgard 184, Dow Corning) to form a protective sheath 16. The fiber was then pulled out of the uncured PDMS pool and heated at about 90°C for curing. Finally, the fiber was dried at 30°C for 8 hours to obtain a coated precursor fiber 10'.
[0146] Coiled muscle construct fabrication and characterization
[0147] The coiled muscle is obtained through a continuous twisting and winding process. In a typical experiment, a 200g weight is suspended under one end of the precursor fiber 10' and the other end is fixed to the shaft of a rotating motor. This configuration only allows the fiber 10' to rotate. After the fiber 10' has obtained a sufficient number of turns and can no longer withstand more twisting, the fiber 10' begins to coil around its axis. The coiled muscle structure 10 is then stretched with a pre-strain of 32%. The fully coiled structure 10 is then annealed above about 180°C for 4 hours and cooled to room temperature on average to obtain the resulting coiled shape.
[0148] Finally, the coiled muscle structure 10 was actuated at a temperature of 120°C with a load of 200 g until consistent actuation was obtained. SEM measurements were performed on a LEO-1530-VP scanning electron microscope. The RF magnetic heating system used in the current study was EASY HEAT 8310 (Ambrell Induction Heating Solutions). CCD images and videos were captured by using a SONY DSC-RX10III digital camera. A uniform magnetic field was provided by a vibrating sample magnetometer (VSM, EZ7, Microsense).
[0149] Thermal Characterization of Protective Layers
[0150] The temperature changes of the coiled muscle 10 with or without the outermost protective PDMS sheath 16 were recorded under radio frequency magnetic heating using a FLIR-A300 camera (FLIR Systems Inc.). Fig.11 It can be seen that before and after RF magnetic heating, the temperature of the coiled muscle structure 10 without the PDMS sheath 16 rises from 22.7°C to 121°C in air. This is due to the magnetically induced heating effect of the Fe3O4 nanoparticles 22. Fig.11 ), due to the thermal insulation effect of PDMS, the surface temperature decreases with the increase of the thickness of the PDMS sheath 16. Although there are breaks during the twisting and coiling process, the minimum surface temperature of the coiled muscle is 60°C if the PDMS sheath thickness is higher than 200 μm.
[0151] Measurement of muscle actuation force, torque and actuation strain
[0152] Fig.13 The contraction actuation force of the coiled muscle structure 10 shown was directly measured using an Instron tensile measurement machine (INSTRON 5942). Fig.24As shown in Fig. 1, the coiled muscle structure 10 is pre-stretched by about 0.1%, and its two ends are directly clamped on the bottom clamp and the top clamp of the Instron machine. The two clamps are fixed without further displacement. Therefore, it is possible to obtain the tensile actuation force caused by muscle contraction. Figure 2 c. Figure 2 The torsional torque shown in f is tested using a similar procedure.
[0153] like Fig.24 As shown in Fig. b, one side of the muscle structure 10 is fixed to the substrate. The other side is connected to the print bar and tethered to the Instron fixture. Since it is difficult to use the Instron machine and the RF magnetic heating system at the same time, a heat gun (HE20-600, Metabo) is placed to heat the coiled muscle structure 10, and a thermal imager is used to monitor the temperature. The actuation strain of the coiled muscle structure 10 when heated by a hot air gun and RF magnetic heating under various loads has been compared. Fig.25 As shown, the difference in actuation strain between the two methods is negligible. It shows that a heat gun can also be used to measure the performance of the coiled muscle structure 10 . Figure 2 a and Figure 2 The actuation strain results shown in d are characterized by applying a non-rotating load at the bottom end under RF magnetic heating ( Fig.24 c), where the tensile force is provided. Figure 2 a. Figure 2 Each point in d represents the maximum actuation strain of the coiled muscle 10 during contraction under the corresponding load force.
[0154] Calculate the power
[0155] Figure 2 b. Figure 2 The work capacity shown in e is defined as Figure 2 a. Figure 2 The product of the actuation strain and the stretching force in d is:
[0156]
[0157] Where l and m are the length and mass of the coiled muscle 10, respectively. The actuation strain is negatively correlated with the actuation stress. Therefore, the work capacity is Figure 2 b. Figure 2 e shows a peak value (called “load-optimized work capacity”).
[0158] Design of Bistable Gripper
[0159] The untethered bistable gripper 400 presented here is constructed by combining a bistable link structure with the proposed magnetically heated coiled muscle structure 10 ( Figure 6a). It consists of a bistable linkage structure with an embedded pre-stretched elastic body 404 and a coiled muscle structure 10. The 3D printed bistable gripper 400 consists of two rigid hinge links 402. Without the pre-stretched elastic body 404 connected, the gripping force of the gripper 400 was measured to be about 1N. The pre-stretched elastic body 404 connecting the two ends of the bistable mechanism can store and release potential strain energy.
[0160] Calculation of force and work capacity of magnetic soft actuators
[0161] In this section, we build a simplified model to study how much work a typical magnetic soft actuator can generate. Fig. 9 As shown, it is assumed that the actuator 10 has a residual flux density consistent with its longitudinal direction, one end of the beam is fixed and the other end is under a constant external load, and the beam applies a uniform magnetic field in the vertical direction. All these assumptions tend to generate relatively large magnetic torques, resulting in relatively large end-effector reaction forces. This helps predict the maximum capability of a typical magnetic soft actuator in mechanical output from a power perspective.
[0162] When no magnetic field is applied, an actuator with a free-end load (such as Fig. 9 The total potential energy of the convex shape shown is:
[0163]
[0164] Among them, the first term represents the bending energy in the soft actuator, and the second term represents the work done by the external force F. EI is the bending stiffness of the soft bending actuator, E is the Young's modulus of the magnetic soft composite material, is the second moment of inertia. is the approximate curvature in the soft actuator (where θ is the bending angle of the actuator). is the deflection of the beam at the free end. Note that to simplify the model, the deadweight of the actuator is neglected and linear elasticity of the soft composite is assumed. It is also assumed that the beam is in pure bending and has uniform curvature, which means that θ is a constant. The equilibrium bending angle θ0 of the beam under constant load can be numerically solved by minimizing the total potential energy, i.e.:
[0165]
[0166] When a magnetic field is applied, the actuator's magnetic moment ( Fig. 9 The concave shape shown) is:
[0167]
[0168] Among them B r is the residual magnetic flux density, μ0 is the magnetic permeability of vacuum, V mis the volume of the magnetic (NdFeB) particle 22. The potential energy induced by magnetic actuation is defined as:
[0169]
[0170] Where B is the external magnetic field. By substituting Equation 3 into Equation 4, we can obtain:
[0171]
[0172] where w, t and L are the width, thickness and length respectively. is the angle between the magnetic moment and the horizontal direction. The work done by the magnetic field to rotate the actuator from the loaded state (bending angle -θ0) to the actuated state (bending angle θ) is:
[0173]
[0174] Then the total potential energy of the actuator is:
[0175]
[0176] where K0 and d0 are the curvature and deflection of the soft actuator under load, respectively. K and d are the curvature and deflection of the soft actuator under actuation, respectively. The equilibrium bending angle of the beam when actuated can be expressed as Numerical solution. By obtaining θ eq , the work capacity of the actuator can be calculated as follows:
[0177]
[0178] Through this equation, the functional relationship between the actuator's work capacity and the magnetic field can be predicted, such as Fig.10 shown.
[0179] exist Fig.10 In the experiment, F = 60 μN, E = 200 kPa, L = 3 mm, w = 1 mm, t = 0.1 mm, B r = 0.84T, and V m / V=0.3 (NdFeB particle / Ecoflex volume ratio). The results show that the work capacity first increases monotonically with the magnetic field and then approaches a plateau at B=about 7.8 mT, showing a highly nonlinear behavior. Further increasing the magnetic field beyond B=about 7.8 mT does not significantly change the work capacity, which remains unchanged at about 2×10 -4kJ / kg. This plateau is due to the complete alignment of the magnetic moment with the magnetic field. It should be noted that E = 200 kPa was chosen because the Young's modulus (E) of the magnetic soft actuator is in the range of 6.6 to 200 kPa. In addition, F = 60 μN is used because an external load greater than 60 μN will cause the soft beam to deflect greatly or even collapse under load (according to the numerical results of Eq. 2), making it impossible for the actuator to operate and be used as designed. It should be noted that the output force is obtained by using a numerical method (the corresponding Matlab code is as follows Fig.26 It is obtained by solving the relationship between the output force and deflection of the magnetic soft actuator (as shown in Equation 2).
[0180] It is observed that despite the assumptions made for the model (large B r , homogeneous magnetic moment, magnetic field perpendicular to the remanent flux density, and saturated NdFeB-ecoflex volume ratio) tend to generate large torque (i.e., high force) in magnetic soft actuators, but their maximum work coefficient is still only about 2×10 -4 kJ / kg, which is about 10 weaker than skeletal muscle 2 , which is about 10 times weaker than the proposed magnetic artificial muscle 4 Unfortunately, in reality, magnetic soft actuators usually have heterogeneous magnetic moments, small angles between the magnetic moment and the magnetic field, small magnetic particle volumes, and different boundary conditions (e.g., both ends are free), all of which tend to generate smaller torques. Therefore, their "real" work-doing capacity is expected to be smaller than Fig.10 The results shown in are much smaller. As shown in Table 1, this explains why the magnetic soft actuator has a smaller work capacity.
[0181] Calculation of tensile actuation strain, work capacity, and torsional torque
[0182] In this section, a model is established to calculate the tensile actuation strain, work capacity, and torsional torque of the coiled muscle structure. For the three-state muscle structure 10, the coiled muscle core 12 (E core )、Active sheath 14(E active ) and protective sheath 16 (E protective ) are approximately 1.2 GPa, 1.04 GPa and 1.5 MPa, respectively, that is,
[0183]
[0184] Therefore, in order to simplify the model, the three-layer coiled muscle structure 10 is assumed to be a single-layer coil spring, and E core = 1.2 GPa was chosen as the Young's modulus. First, the dependence of the actuation strain (ε) and the work capacity (W) on the load force (F) can be obtained from Fig. 27The coiled muscle structure has four states (I-IV). States I and II represent non-actuated states, while III and IV are actuated states. Although states I and III are free states, meaning there is no load hanging at the bottom, states III and IV are loaded states. Fig. 27 In the experiment, the working capacity of actuation strain and load force can be obtained.
[0185]
[0186]
[0187] Where m, l, y0 and Δy are the mass, length, free actuation length and loaded actuation length of the coiled muscle structure, respectively. According to Hooke's law Therefore, Equation 10 and Equation 11 can be rewritten as:
[0188]
[0189]
[0190] where k1 and k2 represent the spring stiffness of the non-actuated coiled muscle structure and the actuated coiled muscle structure, respectively. Therefore, the actuation strain and work capacity are given by the free actuation strain and reverse spring rate changes To complete the calculation, the free actuation strain and spring stiffness must be derived. Based on the coiled actuation mechanism, the free actuation strain It can be obtained by the following formula:
[0191]
[0192] Where N is the number of coils of the wound muscle. ΔT is the torsional stroke and can be calculated by the following formula:
[0193]
[0194] Where n is the number of fiber turns used to make the spirally wound muscle structure; n0 and l0 are initial values. According to existing technical literature, the change of the wound muscle structure is caused by the expansion of the fiber volume during actuation. The relationship is:
[0195]
[0196] Where V and h are the volume and length of the constructed fiber, respectively. The zero subscript represents the corresponding initial value. It is assumed that the change in fiber length during the stretching actuation process is negligible. Equation 16 can be simplified to:
[0197]
[0198] where d is the diameter of the constructed fiber. Therefore, by substituting Eq. 15 and Eq. 17 into Eq. 14, the free actuation strain can be obtained:
[0199]
[0200] Furthermore, the spring stiffness of the coiled muscle is calculated by using Castigliano's theorem:
[0201]
[0202] where D is the diameter of the coil structure, which is assumed to change negligibly during actuation. G is the shear modulus, i.e.,
[0203]
[0204] Where δ is the Poisson's ratio of the fiber. By combining Eqs. 12, 13 with Eqs. 18, 19, 20, the actuation strain and work capacity can be calculated.
[0205]
[0206]
[0207] For the coiled muscle structure studied, the corresponding parameters are as follows: the number of coils (N) is N=80; the initial number of fiber turns (n0) is n0=278; the constructed fiber diameter (d) is d=0.73mm, and the initial value (d0) is d0=0.65mm; the length of the coiled muscle (L) is L=11cm; the diameter of the coil structure (D) is D=1mm. Here, in order to simplify the model, the Young's modulus (E) and Poisson's ratio (δ) of the nylon fiber core, i.e., E=1.2GPa and δ=0.39, are selected as the parameters of the constituent fibers in the model. Therefore, it is possible to predict the dependence of the actuation strain and work capacity on the load force by using equations 21, 22 and the above parameters. As Fig.28 As shown, it is possible to compare the theoretical results with the experimental results in order to prove the correctness of the above model.
[0208] The mismatch between the theoretical results and the experimental results can be explained as follows: First, the three-state structure 10 is assumed to be a single-layer structure of a wound structure, and the Young's modulus and Poisson's ratio of the nylon fiber are used as parameters of the entire constituent fiber 12. Then, in this model, the change of the Young's modulus of the fiber between the actuated and non-actuated states is not considered. In addition, only the diameter expansion of the constituent fiber is considered, and it is assumed that the fiber length and diameter changes of the wound structure are negligible. Finally, during the actuation process, if the load force is small, inter-coil contact will occur, which is not the case in this model.
[0209] In addition, according to the prior art literature, the torsional torque (τ) can be calculated by the following formula:
[0210]
[0211] Where J = πd 4 / 32 is the polar second moment of area; Δn=n-n0 is the number of fiber turns changed due to the fiber volume expansion during actuation. Combining equations 17, 20 and 23, the torsional torque can be obtained as:
[0212]
[0213] The equation shows that the torsional torque increases with the material Young's modulus and the fiber diameter, and its trend is similar to Figure 2 c. Figure 2 The experimental results of f are the same.
[0214] Modeling of a Bistable Gripper
[0215] like Figure 6 As shown in Fig. 2, the working principle of the bistable clamp 400 follows four steps. First, the elastic body 404 is pre-stretched and attached to both ends of the connecting rod 402 to achieve bistable state. The connecting rod-based structure with embedded pre-stretched elastic body 404 leads to an unstable state ( Figure 6 b) has the following characteristics: Figure 6 c schematically shows the maximum potential energy (state II) and the zero joint rotation angle θ of the energy profile. Secondly, after releasing the elastic body 404, the gripper rotates and deforms into a concave shape ( Figure 6 b) and in a stable state ( Figure 6 c) in state I, which is at θ = -θ s The local minimum energy is obtained at the position where the bistable mechanism has a local minimum energy (here the angular position limit of the bistable mechanism is set to a preset stop angle θ s Stop its rotation, such as Figure 6 c). Then, attach the stress-free coiled muscle structure 10 to connect the two arms of the clamp 400, such as Figure 6 b. Third, as the coiled muscle structure 10 contracts during magnetic heating, the gripper 400 deforms toward the unstable state, in which the elastic body 404 stores the most energy. Fourth, when the device bypasses the unstable state II, it quickly enters another stable state III, θ = θ c (θ c is the revolting angle of the target tissue. Figure 6 c) By setting θ c >>θ s, the potential energy of this stable state III is much lower than that of the other stable state I.
[0216] Figure 6 c schematically shows the energy situation of the bistable actuator as a function of the bending angle θ. It shows a peak energy state (unstable state II) and two local low energy states (stable states I and III). The difference between the peak and lower energy states defines the energy barrier. Here, the energy barrier from state I to state II is defined as ΔE1, and the energy released from state II to state III is defined as ΔE2. In order to achieve actuation from state I to state II, muscle actuation should provide sufficient energy input to trigger the sudden instability, i.e., U in ≥ΔE1. Once state II is bypassed, the bistable system will quickly enter another stable state III, during which the large amount of strain energy stored in the elastomer will be quickly released, resulting in a large energy output ΔE2. It is observed that by setting θ c >>θ s , the energy output of the system will be much greater than the input, that is, ΔE2>>U in ≥ΔE1, indicating energy / force amplification effect.
[0217] Energy-based theoretical model and evaluation of the clamping force
[0218] As shown below, an energy-based theoretical model is developed to understand the nonlinear behavior of the proposed bistable gripper 400, including the relationship between design parameters (e.g., link stop angle and pre-extension strain in the elastic body) and output (e.g., potential energy and output force). The total potential energy of the bistable gripper is:
[0219] U t =U muscle +U elastomer , (25)
[0220] Among them U muscle is the potential energy in the coiled artificial muscle structure 10, U elastomer is the potential energy in the pre-strained rubber 404. In this case, the rubber has a high modulus (about 2 MPa) and is pre-stretched at high strain. Therefore, its potential energy will be much greater than the potential energy of the twisted muscle structure, i.e., U elast omer>>U muscle In this case, the second term in Equation 25 can be ignored. Then Equation 25 can be rewritten as:
[0221]
[0222] Where E is the Young's modulus of the elastic body 404, and V is the volume of the elastic body 404. ε is the strain of the elastic body at a given joint rotation angle θ, as shown below:
[0223]
[0224] where ε pre is the pre-stretch strain of the elastic body 404 at the unstable state II. Then equation 26 can be rewritten as:
[0225]
[0226] It should be noted that although the elastic body has nonlinear deformation, an idealized linear elastic behavior in a homogeneous continuous material is assumed. Based on the total potential energy U of the system in Eq. t , the joint torque T of the bistable actuator 400 can be obtained by the following formula:
[0227]
[0228] The clamping force F of the bistable actuator 400 c Or the reaction force of the end effector can be obtained by the following formula:
[0229]
[0230] like Figure 6 d, where d is the distance between the gripper tip and the joint. Based on this equation, the gripping force can be plotted as a function of the joint rotation angle θ, as Figure 6 d. It shows that by setting θ s =4°, E = 2MPa and ε pre = 400%, the force required to bypass the energy barrier is about 1.46 N. Once the snap instability occurs, the structure will snap, and the corresponding output force is θ c =50° can reach about 18.09N, indicating that the output force is amplified by about 10.70 times. In order to verify the model, the static output force of the bistable gripper is experimentally checked as a function of the bending angle by a quasi-static indentation test. Fig.29 Similar to the trend captured by the model, the experimental results show that by increasing θ s and θ c The difference between, for example, θ s =4° and θ c = 50°, the system shows a huge force amplification of up to about 7.43 times (the mismatch between the model and the experiment will be explained in detail below). Fig.30 The corresponding output force / force input is plotted as θ c / θ sIt shows that the force improvement ratio of the bistable system increases with θ c / θ s increases monotonically, which means that we only need to change θ c / θ s Adjusting from 1 to 13 can easily increase the output force / input force from 1 to 7.43. Fig.31 As shown, in addition to the joint angle, the pre-extension strain ε in the elastic body can also be pre to adjust the energy and force situation of the bistable system, where the clamping force and energy output vary with ε pre And significantly increased.
[0231] The analytical model and experimental results only capture the static (or quasi-static) response of the bistable system. If the dynamic effects of the system during the snap-action process were included, the output forces would be much larger than those modeled (and measured) here, since fast snap-action instabilities typically result in much larger dynamic forces. Figure 6 The mismatch between the experimental results shown in d is explained as follows. First, in the model, the potential energy of the twisting muscle is neglected. In fact, at larger bending angles, the strain energy in the twisting muscle increases significantly. This explains why only a small mismatch between the model and the experiment is observed at small θ, while a large difference is observed at large θ. Next, in the model, the friction at the joint is assumed to be zero. In fact, the joint friction is not zero and varies with ε. pre Third, it is assumed that the elastic body used in the model is linear elastic. Fig.32 As shown, according to the measured stress-strain curve of the elastomer, although the slope is almost constant at a small strain, the stress-strain curve of the elastomer shows a high degree of nonlinearity.
Claims
1. A device consisting of one or more structures (10), each of the structures (10) comprising at least three layers: core(12); an active sheath (14); and a protective sheath (16); in, The core (12) is formed of nylon fibers (18); The active sheath (14) comprises a resin (20), and graphene oxide (GO) and a first type of magnetic particles (22) are respectively embedded in the resin (20); and The protective sheath (16) is formed of an elastic material (24), and the elastic material (24) protects the inner layer from being affected by the external environment.
2. The device according to claim 1, It also includes a fourth layer (24), which is a magnetization sheath (24).
3. The device according to claim 2, in, The magnetizing sheath (24) includes a combination of second type magnetic particles (28) and an elastomer (30), such as a combination of NdFeB and PDMS.
4. The device according to any one of the preceding claims, in, The resin (20) of the active sheath (14) comprises a polyurethane casting resin, such as Crystal Clear TM Or nylon.
5. The device according to any one of the preceding claims, in, The first type of magnetic particles (22) are formed of Fe3O4; The first type of magnetic particles (22) comprises a size selected in the range of 10 nm to 500 nm, in particular in the range of 20 nm to 200 nm, in particular in the range of 50 nm to 100 nm; And / or, the device further comprises a second type of magnetic particles (28) formed of NdFeB, the second type of magnetic particles (28) comprising a size selected in the range of 0.1 μm to 10 μm, in particular in the range of 2 μm to 6 μm.
6. The device according to any one of the preceding claims, in, The active sheath (14) comprises a thickness in the range of 50 μm to 300 μm, in particular in the range of 100 μm to 250 μm, in particular 200 μm.
7. The device according to any one of the preceding claims, in, The active sheath (14) comprises a GO concentration selected in the range of 1 wt% to 6 wt%, in particular in the range of 2 wt% to 4 wt%.
8. The device according to any one of the preceding claims, in, The active sheath (14) comprises a magnetic particle concentration of the first type of magnetic particles (22) selected in the range of 10 wt% to 30 wt%.
9. The device according to any one of the preceding claims, in, The device comprises a coiled shape.
10. The device according to any one of the preceding claims, in, The core (12), i.e. the nylon fiber (12), comprises a diameter selected in the range of 0.1 mm to 0.5 mm, in particular in the range of 0.2 mm to 0.5 mm, in particular 0.45 mm, and preferably, a length selected in the range of 1 cm to 100 cm, in particular in the range of 1 cm to 50 cm, in particular in the range of 5 cm to 40 cm.
11. The device according to any one of the preceding claims, in, The device comprises a diameter selected in the range of 0.1 mm to 10 mm, in particular in the range of 0.4 mm to 5 mm, and in particular in the range of 0.4 mm to 1.2 mm.
12. The device according to any one of the preceding claims, in, The device includes at least one functional component, such as a frame (202), a blade (206), a rod (502), a screw, a chassis (402, 102), a connector (504), a magnetic component (204), a pre-tensioning elastomer (404) and / or a combination of a frame (202), a blade (206), a rod (502), a screw, a chassis (402, 102), a connector (504), a magnetic component (204), a pre-tensioning elastomer (404).
13. A method of forming a device having one or more three-layer structures (10), the method comprising the steps of: providing fiber (12); The fiber (12) is coated with an active sheath (14) material, wherein the active sheath material comprises a resin (20), and graphene oxide (GO) and a first type of magnetic particles (22) are respectively embedded in the resin; further coating the fiber (12) with a protective sheath (16) material, wherein the protective sheath (16) material comprises an elastic material (24); Optionally, curing the coated fibers (10); and The coated fiber (10) is continuously twisted and wound to form the device.
14. The method according to claim 14, in, Prior to winding the coated fiber (10), the method further comprises the step of coating the fiber with an additional magnetic sheath (26).
15. The method according to claim 13 or 14, in, The step of winding the coated fiber (10) comprises at least 250 turns, preferably 300 to 400 turns.