Polycarbonates having phenolic structural units and low chlorine content
Polycarbonates derived from lignin-based bisphenols with aromatic terminators and low chlorine content address the limitations of existing lignin-derived polycarbonates, achieving high molecular weights and improved mechanical and optical properties for industrial applications.
Patent Information
- Application Number
- CN202380035865.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-20
- Publication Date
- 2024-12-03
AI Technical Summary
Existing polycarbonates derived from lignin-based bisphenols face challenges in achieving high molecular weights, low saponifiable chlorine content, and optimal mechanical and optical properties, limiting their industrial applicability and scalability due to yellowing and corrosiveness.
The development of polycarbonates terminated with aromatic groups and low chlorine content, using bisphenols derived from lignin, achieves high molecular weights (8000-20000 g/mol) and low saponifiable chlorine content (0.2-19 ppm), enhancing mechanical and optical properties and allowing industrial processing.
The resulting polycarbonates exhibit mechanical properties comparable to bisphenol A-based polycarbonates, reduced yellowing, and non-corrosiveness, enabling industrial-scale applications such as injection molding and extrusion.
Smart Images

Figure BDA0005098008340000031 
Figure BDA0005098008340000071 
Figure BDA0005098008340000081
Abstract
Description
[0001] The present invention relates to polycarbonates comprising specific phenolic structural units, molding compounds comprising the polycarbonates, molded articles comprising the polycarbonates, and a process for preparing the specific polycarbonates, wherein the polycarbonates are terminated with at least one aromatic group which may optionally be terminated with at least one C1-C6 alkyl group, have a saponifiable chlorine content of 0.2 ppm to 19 ppm and a number average molecular weight of 8000 g / mol to 20000 g / mol.
[0002] Polycarbonates, in particular aromatic polycarbonates, are known to exhibit a good profile of properties in terms of mechanical and optical properties, heat resistance and weathering resistance. Due to this profile of properties, they are used in a variety of indoor and outdoor applications. Typically, polycarbonates are prepared by an interphase phosgenation process or a melt transesterification process.
[0003] Lignocellulosic biomass has been recognized as having potential use in the production of chemicals and biomaterials. It contains cellulose, hemicellulose and lignin. Lignin is a highly cross-linked macromolecule consisting of different types of substituted phenols. The corresponding processing of lignin can provide various bisphenols, so lignin is expected to become a potential substitute for compounds used in petrochemicals, but based on natural and renewable sources at an affordable cost.
[0004] Some studies have been conducted focusing on the provision of bisphenols from lignin. For example, WO2019 / 002503A1 describes a method for producing o-alkoxy bisphenols that can be used as reactants for the preparation of biopolymers. The document mentions the reaction of these bisphenol compounds with phosgene to form polycarbonates. However, no such reaction was performed in the experimental section.
[0005] WO2018 / 134427A1 relates to the production of high-purity meta, meta-coupled bis(4-alkylphenol) derivatives from lignin-derived sources. The resulting bisphenols are said to be useful monomers for the production of polycarbonates, in particular using phosgene. However, polycarbonates are not prepared in this document either.
[0006] In Green Chem., 2017, 19, 2561-2570, polycarbonates are synthesized by standard laboratory scale procedures using m,m'-bis(4-alkylguaiacol) and triphosgene. In the paper, the end group content of the resulting polycarbonate is not indicated, but due to the procedure, the resulting saponifiable chlorine content is likely to be high. The resulting molecular weight given in the paper indicates that the reaction is incomplete. However, the chlorine content of the polycarbonate has an effect on the resulting optical properties. The higher the chlorine content, the higher the yellowness index and the tendency to yellowing. This limits the possible applications of polycarbonate. In addition, the chlorine content makes polycarbonate corrosive to pipes and reactors, and therefore, polycarbonates with high chlorine content cannot be processed in scale-up processes and / or diversified applications (such as injection molding, extrusion, etc.). Finally, the paper does not disclose the use of chain terminators.
[0007] The reaction of specific bisphenols with triphosgene is also described in CN105461912 A. In this prior art document no chain terminator is used and the document does not mention the resulting end groups. However, due to the reaction, the end groups are most likely -Cl or -OH. Both groups usually need to be reduced in polycarbonate resins. As mentioned above, the saponifiable chlorine content has an impact on the optical properties. High -OH content adversely affects the thermal stability of polycarbonates. Polycarbonates have a tendency to yellow when exposed to heat.
[0008] WO2015 / 183892A1 describes the synthesis of new reactive functionalized phenolic building blocks. The synthesis of bisguaiacol polycarbonate is described in Example 46. Bisguaiacol F is reacted with nitrochloroformate in acetonitrile. In this example, no chain terminator is used. Therefore, the resulting polycarbonate has -Cl or -OH end groups. In addition, the resulting polycarbonate has a weight average molecular weight of 13,200 g / mol relative to a polystyrene standard. This means that the resulting polycarbonate has a very low molecular weight, indicating that the mechanical properties of the polycarbonate may not be sufficient for any application where bisphenol A-based polycarbonates are typically used.
[0009] WO 2015 / 168225 A2 describes the reaction of alkoxybisphenols to polycarbonates by interphase phosgenation. In Example 5 of this document, a polycarbonate based on 4,4'-(2-isopropylidene-bis(2-methoxy)phenol (PBMP) is prepared using interphase phosgenation and p-cumylphenol as a capping agent. The resulting polycarbonate has a dry chloride content of 21 ppm and a number average molecular weight (M) of 6,600 g / mol. n) (measured by GPC and PC standards). Such a molecular weight is undesirable for the resulting mechanical properties. In addition, the resulting viscosity of the polycarbonate is not sufficient to meet the common market requirements based on the use of bisphenol A-based polycarbonates. In addition, the dry chloride content is still too high when considering market requirements and application possibilities.
[0010] This document describes a method for preparing polycarbonates, wherein a suspension (not a solution) of bisphenols is provided and phosgene is added to the suspension. The pH of the mixture is maintained at 9. Generally, polymerization reactions in suspensions are not easy to control (especially compared to polymerizations in solution). Generally, the resulting polymers have a high polydispersity and can lead to incomplete reactions. This can be seen, for example, from the relatively small molecular weights obtained in this document. Finally, it is obvious that any teaching on suspension polymerization cannot be directly transferred to solution polymerization due to the fundamentally different reaction systems.
[0011] As can be seen from the prior art described above, the skilled person knows how to prepare specific bisphenols from lignin. In the examples of these documents, clear indications of the facts on how these bisphenols are prepared can be found. For the provision of bisphenols from lignin, these examples are incorporated herein by reference. For example, the synthesis of 4,4'-propylenebis(2-methoxyphenol) is described in WO2019 / 002503A1.
[0012] Based on this prior art, there is a need to provide and prepare polycarbonates based on natural and renewable resources. In addition, there is a need to provide polycarbonates that can be prepared on an industrial scale. In addition, such polycarbonates should show properties comparable to standard bisphenol A-based polycarbonates on the market (e.g. with respect to processing properties, mechanical properties and optical properties, especially yellowing). Finally, there is a need for an efficient, economical and ecologically advantageous method for preparing such polycarbonates.
[0013] The present invention has addressed at least one, and preferably all, of the above objects.
[0014] Surprisingly, the inventors have found that when using the method according to the invention, polycarbonates with sufficiently high molecular weights can be obtained to ensure good mechanical properties, preferably mechanical properties comparable to polycarbonates based on bisphenol A with comparable molecular weights. In addition, the resulting polycarbonates exhibit good optical properties, especially in terms of yellowness index and / or yellowing. In addition, due to the method according to the invention, it is possible to obtain polycarbonates with saponifiable chlorine contents of 0.2 ppm to 19 ppm. Such a low saponifiable chlorine content leads to the fact that polycarbonates have a low tendency to yellowing. In addition, the polycarbonate itself is non-corrosive and can therefore be handled in pipelines and reactors on an industrial scale and further processed accordingly for applications such as injection molding, extrusion, etc. In addition, the fact that the polymer chain is terminated with at least one aromatic group reduces the amount of -OH end groups, and the aromatic group can optionally be terminated with at least one C1-C6 alkyl group. This positively affects the thermal stability of the polycarbonate. Finally, the polycarbonate of the present invention is a polycarbonate that can be obtained using bisphenols obtained from lignin. Therefore, the polycarbonate of the present invention can be based on natural and renewable bisphenols. The polycarbonates of the invention thus contain at least 30% by weight of specific structural units as defined below. This results in the fact that when the bisphenols used to obtain such specific structural units are based on natural and / or renewable bisphenols, the resulting polycarbonates contain a high content of structural units derived from natural and / or renewable bisphenols.
[0015] The present invention therefore provides a polycarbonate comprising, preferably comprising at least 30% by weight of structural units of the formula (1), wherein the % by weight is based on the total weight of the polycarbonate.
[0016]
[0017] in
[0018] Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus,
[0019] R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl,
[0020] R 2 and R 4each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and
[0021] p and q are each independently 1 or 2, preferably 1, and
[0022] n represents the average number of repeating units,
[0023] Characterized in that the polycarbonate is end-capped with at least one, optionally with at least one C1-C6-alkyl, preferably substituted aromatic group, has a total saponifiable chlorine content of 0.2 ppm to 19 ppm, relative to the mass of the polycarbonate, and a number average molecular weight of 8000 g / mol to 20000 g / mol as determined by gel permeation chromatography in dichloromethane by calibration with bisphenol A-polycarbonate.
[0024] The polycarbonate in the context of the present invention is a homopolycarbonate or a copolycarbonate.The polycarbonate may be linear or branched, depending on the type of monomer used in the process of the present invention.
[0025] Preferably, the polycarbonate according to the present invention is bio-based. For the purposes of the present invention, the expression "bio-based" is understood to mean that the relevant compound can be provided and / or obtained via renewable and / or sustainable raw materials on the application date. Renewable and / or sustainable raw materials are preferably understood to mean raw materials that are regenerated by natural processes at a rate comparable to their consumption rate (see CEN / TS16295:2012). This expression is particularly used to distinguish it from raw materials produced from fossil raw materials (also referred to as fossil-based according to the present invention). As an example, most bisphenol A-based polycarbonates represent commonly known fossil-based polycarbonates. Whether a raw material is bio-based or fossil-based can be determined by measuring the carbon isotopes in the raw materials, because the carbon isotopes C in fossil raw materials are 14 The relative amount of is low. This can be done, for example, according to ASTM D6866-18 (2018) or ISO 16620-1 to -5 (2015) or DIN SPEC 91236 2011-07. An exemplary bio-based material is bisphenol obtained from lignin.
[0026] Preferably, in formula (1),
[0027] Each X independently represents a substituted or unsubstituted C3-C 18 -cycloalkylidene; formula—C(R c )(R d )—C1-C 18 -alkylidene, wherein R c and Rd are independently hydrogen, C1-C 12 -alkyl, C1-C 12 -Cycloalkyl, C7-C 12 -Arylalkyl, C1-C 12 -heteroalkyl or cyclic C7-C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-valent C1-C 12 - a hydrocarbon group,
[0028] R 1 and R 3 Each independently represents C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl,
[0029] R 2 and R 4 each independently represents a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and
[0030] p and q are each independently 1 and n represents the average number of repeating units.
[0031] Preferably, X can be a substituted or unsubstituted C3-C 18 -cycloalkylidene; formula—C(R c )(R d )—C1-C 18 -alkylidene, where R c and R d are independently hydrogen, C1-C 12 -alkyl, C1-C 12 -Cycloalkyl, C7-C 12 -Arylalkyl, C1-C 12 -heteroalkyl or cyclic C7-C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-valent C1-C 12 -hydrocarbon group. More preferably, R 1 and R 3 Each independently represents C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl. Even more preferably, R 1 and R 3 Each independently represents a methyl group, an ethyl group, a propyl group, an octyl group, an isooctyl group, a benzyl group, an ethylphenyl group, a butylphenyl group, a propyldiphenyl group or a cyclohexylphenyl group.1 and R 3 Each is a methyl group.
[0032] Preferably, X represents methylene, cyclohexyl-methylene, 2-[2.2.1]-bicycloheptylidene, ethylidene, isopropylidene, neopentylidene, cyclohexylidene, cyclopentadecylidene, cyclododecylidene or adamantylidene. More preferably, X represents a group of the formula—C(R c )(R d )—C1-C 18 -alkylidene, where R c and R d are independently hydrogen, C1-C 12 -alkyl, C1-C 12 -Cycloalkyl, C7-C 12 -Arylalkyl, C1-C 12 -heteroalkyl or cyclic C7-C 12 -heteroarylalkyl, preferably hydrogen or C1-C 12 -alkyl. Even more preferably, R c and R d are each independently hydrogen or C1-C6 alkyl. Most preferably, R c is hydrogen and R d is methyl, ethyl, propyl or butyl. At the same time, most preferably, R 1 and R 3 Each is a methyl group.
[0033] Preferably, R 2 and R 4 Each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and even more preferably a hydrogen atom or a C1-C4-alkyl group.
[0034] Preferably, p and q are each 1. However, in this case it is most preferred that R 2 and R 4 They are all hydrogen atoms.
[0035] Preferably, each X in formula (1) independently represents the formula: c )(R d )—C1-C6-alkylidene, wherein R c and R dEach is independently hydrogen or C1-C5-alkyl.
[0036] More preferably, in formula (1), each X independently represents the formula: c )(R d )—C1-C4-alkylidene, wherein R c and R d are each independently hydrogen or C1-C3-alkyl, R 1 and R 3 Each independently represents a methyl group or an ethyl group, R 2 and R 4 Each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group, and n represents the average number of repeating units.
[0037] Formula (1) lists "n" as the number of repeating units. Preferably, if the polycarbonate of the present invention is a homopolycarbonate, n is 30 to 80, more preferably 35 to 75, even more preferably 40 to 70, even more preferably 45 to 65, and most preferably 50 to 60. The homopolycarbonate according to the present invention is a polymer having only one type of repeating unit of formula (1). This does not mean that such a homopolymer cannot contain any end groups or any other structures caused by impurities, etc. However, such a homopolymer is essentially composed of the structure of formula (1) and is composed of only one type of repeating unit of formula (1). If there are more than one type of repeating units of formula (1), the resulting polymer according to the present invention is a copolycarbonate. In this case, "n" in formula (1) may be different from the values given above. In the case where the copolycarbonate contains more than one type of structure of formula (1), n in formula (1) may have the values given above. In the case where the copolycarbonate has a comonomer with a structure different from that of formula (1), the value of n may be lower than the value given above. In any case, the skilled person is able to calculate "n" in formula (1) based on the number average molecular weight defined according to the present invention.
[0038] According to the present invention, polycarbonate has a number average molecular weight of 8000 g / mol to 20000 g / mol, preferably 8500 g / mol to 17000 g / mol, more preferably 9000 g / mol to 15000 g / mol as determined by gel permeation chromatography in dichloromethane using bisphenol A-polycarbonate calibration. Preferably, the gel permeation chromatography is calibrated using bisphenol A polycarbonate and dichloromethane as eluents. Typically, linear polycarbonates (obtained from bisphenol A and phosgene) with known molecular weight distribution from PSS Polymer Standards Service GmbH, Deutschland can be used for calibration. Most preferably, calibration is performed according to method 2301-0257502-09D (2009 German version) from Currenta GmbH & Co. OHG, Leverkusen. The eluent is dichloromethane. Preferably, a combination of columns based on crosslinked styrene divinylbenzene resins is used. More preferably, the analytical column has a diameter of 7.5 mm and a length of 300 mm. The particle size of the column material is preferably 3 μm to 20 μm. The concentration of the solution is preferably 0.2 wt %. The flow rate is preferably 1.0 ml / min. The temperature of the solution is preferably 30° C. Preferably, UV- and / or RI- detection is used.
[0039] The number average molecular weight as defined according to the invention ensures that the resulting polycarbonate exhibits good mechanical properties in terms of tensile strength and processing parameters. It has surprisingly been found that the resulting tensile strength is comparable to that of bisphenol A based polycarbonates of comparable number average molecular weight.
[0040] In particular, the glass transition temperature of the polycarbonate of the present invention is above 100° C., preferably above 110° C., more preferably above 116° C. Such a glass transition temperature ensures that the polycarbonate of the present invention can be used in all applications in which bisphenol A-based polycarbonates are also used. Preferably, the glass transition temperature can be determined by differential scanning calorimetry ISO 11357-2:2013-05 at a heating rate of 10° C. / min.
[0041] In addition, the saponifiable chlorine content of the polycarbonate according to the present invention is 0.2ppm to 19ppm, preferably 0.4ppm to 15ppm, more preferably 0.5ppm to 10ppm, even more preferably 0.8ppm to 8ppm, and most preferably 1ppm to 7.5ppm, relative to the mass of the polycarbonate. According to the present invention, ppm refers to parts by weight if there is no different indication. The technician understands "saponifiable chlorine content". Preferably, the chloride that forms saponifiable chlorine is covalently bonded to the polycarbonate. The technician knows how to determine the saponifiable chlorine content. Preferably, the saponifiable chlorine content is determined by UV absorption after reaction with 4-(4-nitrobenzyl)pyridine. The chlorine end groups react with 4-(4-nitrobenzyl)pyridine, and the UV absorption of the reaction product can be measured. Due to the reaction, a methine dye is formed. The intensity of this complex can be converted into the concentration of the saponifiable chlorine content of the polycarbonate. Such calibration is known to the technician. Preferably, the polycarbonate is dissolved in dichloromethane and the absorption of the methine dye is measured at 438nm.
[0042] The saponifiable chlorine content according to the invention leads to the fact that the polycarbonates according to the invention have a low tendency to yellowing. Furthermore, the polycarbonates themselves are non-corrosive and can therefore be handled on an industrial scale in pipelines and reactors.
[0043] Preferably, the polycarbonate of the invention is characterized in that the polycarbonate additionally comprises at least one structural unit selected from the structural units of the formulae (2) to (10), (IIa), (IIb), (IIc), (IId), (IIe) and (IIf
[0044]
[0045] Among them, X, R 2 To R 4 , p and q are as defined for formula (1), and m1 represents the average number of repeating units;
[0046]
[0047] wherein each Z independently represents a single bond, -S(=O)2-, -C(=O)-, -O-, -S-, -S(=O)-, -CH(CN)-, a straight-chain or branched C1-C6-alkylene group optionally containing at least one carbonyl group, optionally containing at least one halogen atom and / or optionally interrupted by at least one heteroatom, a C2-C6-alkylene group optionally containing at least one carbon-carbon double bond, optionally containing at least one carbonyl group and / or optionally containing at least one halogen atom 10 -alkylidene, C5-C6-alkylene ... 12-cycloalkylene, C5-C6-cycloalkylene, wherein the alicyclic group is optionally fused to at least one alicyclic and / or at least one aromatic ring 15 -cycloalkylidene, C7-C 20 -Arylalkylidene, C8-C 20 -aralkylene, a C6-C6-alkylene ring optionally fused to a further aromatic ring which may optionally contain at least one heteroatom 12 -arylene group, formula (B1-A), formula (B1-B), formula (B1-C) or formula (B1-D)
[0048]
[0049] wherein in formulae (B1-A), (B1-B) and (B1-C), each R' independently represents a linear C1-C4-alkyl group, a branched C3-C4-alkyl group, an aralkyl group or an aryl group, and "C*" represents a quaternary carbon atom at the position indicated as "Z" in formula (3), and
[0050] wherein in formula (B1-D), each R' independently represents a straight-chain C1-C4-alkyl group, a branched C3-C4-alkyl group, each R" independently represents a straight-chain C1-C4-alkylene group, a branched C3-C4-alkylene group, each R"' independently represents H or a straight-chain C1-C3-alkyl group, s is 0 to 2, and each s1 is independently 0 or 1, and "*" represents a bond connecting "Z" to the aromatic ring in formula (3),
[0051] R 5 and R 6 Each independently represents H, C1-C 18 -alkyl, C5-C6-cycloalkyl, C1-C5-alkenyl-, C1-C 18 -alkoxy, phenoxy, halogen atom, C6-C 18 -Aryl or C7-C 18 -aralkyl,
[0052] p1 and q1 are each 1 to 4, and
[0053] m2 represents the average number of repeating units;
[0054]
[0055] Wherein in formulas (4) to (6), m2 represents the average number of repeating units;
[0056]
[0057] Each R x independently represent a straight or branched C1-C6-alkyl, C1-C 12- aryl, C1-C8-aralkyl or halogen atom, t is 0 to 4, and m2 represents the average number of repeating units;
[0058]
[0059] Wherein in formulae (8) and (9), each Y1 independently represents oxygen, sulfur or NR y , where R y is H or -CH3, each Y2 independently represents a single bond, oxygen, sulfur or NR as defined above y , and m2 represents the average number of repeating units, and in formula (8), each R' independently represents a linear C1-C4-alkyl group, a branched C3-C4 alkyl group, an aralkyl group or an aryl group, and s is 0 to 2;
[0060]
[0061] Where m3 represents the average number of repeating units;
[0062]
[0063] Wherein "*" indicates the connection of the crosslinking point to the polycarbonate polymer chain, and wherein
[0064] R in formula (IIb) and (IIc) is independently selected from H and alkyl, preferably H and methyl,
[0065] X in formula (IIb) is selected from a linear or branched alkyl group and a single bond, preferably C(CH3)2 and a single bond,
[0066] R1 in formula (IId) is selected from H and alkyl, preferably H and methyl, and
[0067] R2 in formula (IId) is independently selected from H and alkyl, preferably H and methyl.
[0068] The resulting polycarbonate is a copolycarbonate according to the present invention. It is understood by the skilled person that there may be overlap between the structures of the chemical formulae (1) and (3). However, according to the present invention, in this preferred embodiment, the term "polycarbonate additionally comprises at least one structural unit of formula (3)" is preferably understood to mean that the structure of formula (1) must be different from the structure of formula (3). Only in this way can a copolycarbonate comprising two different structural units be obtained.
[0069] Preferably, the (co)polycarbonate of the present invention does not contain structural units of formula (100)
[0070]
[0071] wherein t represents the number of repeating units and is preferably 1 to 80, more preferably 2 to 75, even more preferably 40 to 70, even more preferably 45 to 65, and most preferably 50 to 60. However, this preferably does not exclude that structural units of formula (100) may be present in trace amounts in the polycarbonate of the present invention. Preferably, the amount of structural units of formula (100) in the polycarbonate of the present invention is less than 30% by weight, more preferably less than 20% by weight, and most preferably less than 10% by weight, wherein the % by weight is based on the total weight of the polycarbonate.
[0072] Preferably, the polycarbonate of the present invention further comprises at least one structural unit selected from the structural units of formulae (3), (4) and (7),
[0073] In formula (3), each Z independently represents a single bond, -S(=O)2-, -C(=O)-, -O-, -S-, -S(=O)-, a straight or branched C1-C6-alkylene group, a C2-C6-alkylene group optionally containing at least one carbon-carbon double bond, 10 -alkylidene, C5-C6-alkylidene, wherein the alicyclic group is optionally fused to at least one alicyclic and / or at least one aromatic ring 15 -cycloalkylidene, C7-C 15 -aralkylidene group, C8-C 15 -Arylene
[0074]
[0075] wherein in formula (B1-E), each R' independently represents a linear C1-C4-alkyl group, a branched C3-C4 alkyl group, each R" independently represents a linear C1-C4-alkylene group, a branched C3-C4 alkyl group, s is 0 to 2, and each s1 is independently 0 or 1, and "*" represents a bond connecting "Z" to the aromatic ring in formula (3),
[0076] Formula (B1-A), Formula (B1-B), Formula (B1-C),
[0077] R 5 and R 6 Each independently represents H, C1-C 18 -alkyl, C5-C6-cycloalkyl, C1-C 18 -alkoxy, phenoxy, C6-C 18 -Aryl or C7-C 18 -aralkyl,
[0078] p1 and q1 are each 1 to 4, and m2 represents the average number of repeating units.
[0079] More preferably, the polycarbonate of the present invention further comprises at least one structural unit selected from the structural units of formula (3), wherein each Z independently represents a single bond, a C2-C6-alkylidene group, a C5-C6-alkylidene group in which the alicyclic group is optionally fused to at least one aromatic ring. 12 - cycloalkylidene group,
[0080] Formula (B1-A), Formula (B1-B), Formula (B1-C),
[0081] R 5 and R 6 Each independently represents H, C1-C3-alkyl, C1-C 18 - alkoxy,
[0082] p1 and q1 are each 1 to 4, and m2 represents the average number of repeating units.
[0083] Most preferably, the polycarbonate of the present invention further comprises at least one structural unit selected from the structural units of formulae (3a) to (3k)
[0084]
[0085] In formulae (3h), (3i) and (3j), R' represents a methyl group or a phenyl group.
[0086] Most preferably, the polycarbonates of the present invention additionally comprise structural units of the formula (3b) or (3g).
[0087] Most preferably still, the polycarbonate of the present invention further comprises at least one structural unit of formula (2) and at least one structural unit of formula (3) to (10), (IIa), (IIb), (IIc), (IId), (IIe) and (IIf). All preferences given above for the individual formulas also apply to this preference. Even more preferably, the polycarbonate of the present invention further comprises at least one structural unit of formula (2) and at least one structural unit of formula (3), (10) and (IId). Most preferably, in this case, formula (3) is represented by formula (3b) and / or (3g).
[0088] "Alkyl" in the context of the present invention, for example and if not mentioned otherwise, refers to an alkane structure from which one hydrogen atom has been removed. An "alkyl" according to the present invention, which may be linear or branched, is saturated and therefore contains only single bonds between adjacent carbon atoms. Preferably, the alkyl group according to the present invention comprises methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, neopentyl, 1-ethylpropyl, n-hexyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 1,2-dimethylpropyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, 1,1,2-trimethylpropyl, 1,2,2-trimethylpropyl, 1-ethyl-1-methylpropyl, 1-ethyl-2-methylpropyl, 1-ethyl-2-methylpropyl, and the like. In the case where the carbon atoms of the alkyl group are defined in various ways in the present invention, these structures may be limited in selection.
[0089] "Alkylene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged alkane structure in which two hydrogen atoms are removed from different carbon atoms. In this article, the two carbon atoms from which the two hydrogen atoms are removed can be any carbon atoms present in the alkane structure. This means that the two carbon atoms can but do not necessarily have to be adjacent to each other. The alkylene structure can be straight or branched and is saturated. In the case where the alkylene comprises only one carbon atom, the alkylene is a methylene group (-CH2-) connected to the rest of the molecule by two single bonds. Preferably, the alkylene according to the present invention comprises methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, tert-butylene, n-pentylene, 1-methylbutylene, 2-methylbutylene, 3-methylbutylene, neopentylene, 1-ethylpropylene, n-hexylene, 1,1-dimethylpropylene, 1,2-dimethylpropylene, 1,2-dimethylpropylene, 1-methylpentylene, 2-methylpentylene, 3-methylpentylene, 4 ... -methylpentylene, 1,1-dimethylbutylene, 1,2-dimethylbutylene, 1,3-dimethylbutylene, 2,2-dimethylbutylene, 2,3-dimethylbutylene, 3,3-dimethylbutylene, 1-ethylbutylene, 2-ethylbutylene, 1,1,2-trimethylpropylene, 1,2,2-trimethylpropylene, 1-ethyl-1-methylpropylene, 1-ethyl-2-methylpropylene, 1-ethyl-2-methylpropylene, etc. In the case where the present invention defines the carbon atoms of the alkylene in different ways, these structures may be limited in selection. In addition, the alkylene according to the present invention optionally contains at least one carbonyl group, optionally contains at least one halogen atom and / or is optionally interrupted by at least one heteroatom. Examples of such alkylene groups are -C(=O)-(CH2)4-C(=O)-, -C(=O)-(CH2)3-C(=O)-, -C(=O)-(CH2)2-C(=O)-, -C(CF3)2, -O-(CH2)4-O-, -O-(CH2)3-O-, -O-(CH2)2-O-, and the like.
[0090] "Alkylidene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged alkane structure in which two hydrogen atoms are removed from the same carbon atom. The alkylidene optionally comprises at least one carbon-carbon double bond, optionally comprises at least one carbonyl group and / or optionally comprises at least one halogen atom. Preferably, the alkylidene according to the present invention and / or in formula (3) comprises CH2=C*, C(CH3)2=C*, isopropylidene, n-propylidene, isoheptidene, C*(CH3)(C(=O)CH3), C(Cl2)=C*, C(Br2)=C*, etc., wherein "C*" represents the carbon atom at the position indicated as "Z" in formula (3).
[0091] "Cycloalkylene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged cycloalkane structure in which two hydrogen atoms are removed from different carbon atoms in the ring. In this context, the two carbon atoms from which the two hydrogen atoms are removed can be any carbon atoms present in the cycloalkane structure. This means that the two carbon atoms can, but do not necessarily have to, be adjacent to each other. According to the present invention, the alicyclic radical of the cycloalkylene is fused to at least one further alicyclic ring. An example of such a cycloalkylene is adamantylene (tricyclo[3.3.1.13,7]decanediyl).
[0092] "Cycloalkylidene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged cycloalkane structure in which two hydrogen atoms are removed from the same carbon atom in the ring. The alicyclic radical of the cycloalkylidene is optionally fused with at least alicyclic and / or at least one aromatic ring. Examples of such cycloalkylidene are cyclopentylidene, cyclohexylidene, 3,3,5-trimethylcyclohexylidene, cyclodecylidene, cyclododecylidene, tetrahydrodicyclopentylidene, 9-fluorenylidene, etc.
[0093] "Aralkylidene" in the context of the present invention, for example and if not mentioned otherwise, refers independently in each case to a bridged straight, cyclic, branched or unbranched alkyl structure that has two hydrogen atoms removed from the same carbon atom and is monosubstituted, multiply or polysubstituted by an aryl group. At the same time, "aralkylene" refers independently in each case to a bridged straight, cyclic, branched or unbranched alkyl structure that has two hydrogen atoms removed from different carbon atoms and is monosubstituted, multiply or polysubstituted by an aryl group. "Aryl" in the context of the present invention, for example and if not mentioned otherwise, is a carbocyclic aromatic group. Examples of "aryl" are phenyl, o-, p-, m-tolyl, naphthyl, phenanthrenyl or anthracenyl. In particular, in formula (3), examples of such aralkylidene groups are phenyl-CH*, phenyl-C*(CH3), naphthyl-CH*, phenyl-C*-phenyl, etc., wherein "C*" represents the carbon atom at the position indicated as "Z" in formula (3). Examples of such aralkylene groups are m-diisopropylidene phenylene and p-diisopropylidene phenylene.
[0094] "Arylalkyl" in the context of the present invention, for example and if not mentioned otherwise, may be an aryl group as defined above having an alkyl, alkynyl or alkenyl group attached to an aromatic group.
[0095] "Alkoxy" in the context of the present invention, for example and if not mentioned otherwise, refers to a straight-chain, cyclic or branched alkyl group (-OR) which is singly bonded to oxygen. Preferably, the alkoxy group according to the invention has 1 to 6 carbon atoms and thus includes methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, tert-butoxy, n-pentoxy, 1-methylbutoxy, 2-methylbutoxy, 3-methylbutoxy, neopentoxy, 1-ethylpropoxy, cyclohexyloxy, cyclopentyloxy, n-hexyloxy, 1,1-dimethylpropoxy, 1,2-dimethylpropoxy, 1,2-dimethylpropoxy, 1-methylpentyloxy, 2-methylpentyloxy. In the case where the present invention defines the carbon atom of the alkoxy group in different ways, these structures may be limited in selection.
[0096] "Halogen atom" in the context of the present invention, if not mentioned otherwise, refers to fluorine (F), chlorine (Cl), bromine (Br) or iodine (I). Preferably, the halogen atom is F, Cl, Br or I, more preferably Cl or Br.
[0097] Based on the definitions given above, the skilled person knows how to understand further definitions not explicitly stated in the above paragraphs.
[0098] The term "average number of repeating units" is known to the skilled person. The skilled person knows how to determine this parameter. Typically, it is determined by using a GPC method. Preferably, it is determined using a GPC method as outlined in the present invention.
[0099] More preferably, the polycarbonate of the present invention is characterized in that the polycarbonate further comprises at least one structural unit selected from the structural units of formulae (2), (3) and (IId),
[0100] In formula (2), X independently represents the formula—C(R c )(R d )—C1-C4-alkylidene, wherein R c and R d are each independently hydrogen or C1-C3-alkyl, R 1 and R 3 Each independently represents a methyl group or an ethyl group, R 2 and R 4Each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group, and m1 represents the average number of repeating units,
[0101] In formula (3), Z independently represents a single bond, a C2-C5-alkylidene group or a C5-C 12 - cycloalkylidene, preferably single bond, isopropylidene or 3,3,5-trimethylcyclohexylidene, and
[0102] In formula (IId), R1 and R2 are each independently selected from H and alkyl, preferably H and methyl. The presence of comonomers can be used to effectively and finely adjust the resulting properties of the copolycarbonate. For example, the presence of a specific comonomer can affect the glass transition temperature or mechanical properties of the polycarbonate.
[0103] Preferably, the polycarbonate of the present invention comprises at least 30 wt %, more preferably at least 40 wt %, even more preferably at least 50 wt %, even more preferably at least 60 wt %, even more preferably at least 70 wt %, even more preferably at least 80 wt %, most preferably at least 90 wt % of the structure of formula (1), wherein the wt % is based on the total weight of the polycarbonate. More preferably, the polycarbonate comprises at least 30 wt %, more preferably at least 40 wt %, even more preferably at least 50 wt %, even more preferably at least 60 wt %, even more preferably at least 70 wt %, even more preferably at least 80 wt %, most preferably at least 90 wt % of the sum of the structures of formula (1), (2), (3), (4), (IIa), (IIb), (IIc), (IId), (IIe) and (IIf), wherein the wt % is based on the total weight of the polycarbonate. Most preferably, the polycarbonate consists essentially of the structure of formula (1) or consists of the structure of formula (1). Most preferably, the polycarbonate consists essentially of or consists of the structure of formula (1) and at least one other structure selected from the group consisting of the structures of formula (2), (3), (4), (IIa), (IIb), (IIc), (IId), (IIe) and (IIf). Obviously, the term "consisting of" in this case does not include the additionally present end groups.
[0104] In the case where the polycarbonate of the present invention further comprises at least one structural unit selected from the structural units of formula (2), (3) and / or (4), it is preferred that the molar ratio of the structural unit of formula (1) to the structural unit of formula (2), (3) and / or (4) (whichever is present) is 20:80 to 80:20, more preferably 30:70 to 70:30, most preferably 35:65 to 65:35. In the case where the polycarbonate of the present invention further comprises at least one structural unit selected from the structural units of formula (IIa), (IIb), (IIc), (IId), (IIe) and / or (IIf), it is preferred that the polycarbonate comprises 0.1 to 5 mol %, more preferably 0.5 to 3 mol %, most preferably 1.0 to 1.5 mol % of the structural unit selected from the structural units of formula (IIa), (IIb), (IIc), (IId), (IIe) and / or (IIf) (whichever is present).
[0105] Preferably, the polycarbonates of the invention are characterized in that the at least one polycarbonate chain-terminating and optionally end-capped with at least one C1-C6 alkyl, preferably substituted aromatic group is selected from the formula (5a), (6a), (7a), (8a) and (9a), wherein
[0106]
[0107] wherein each Y independently represents a halogen atom, a C1-C3-alkyl group, a C1-C3-alkoxy group, a C7-C 12 -Arylalkyl, C7-C 12 - alkylaryl or nitro,
[0108] y is 0 to 4, and c is 1 to 5, provided that y+c is 1 to 5,
[0109]
[0110] And each "*" represents the position at which the structure of formula (5a), (6a), (7a) or (8a) is attached to the polycarbonate.Most preferably, the polycarbonate of the present invention is characterized in that the polycarbonate chain comprises an end group of formula (7a).
[0111] According to the invention, the saponifiable chlorine content is very low. This is due to the fact that the polymerization reaction has a very high conversion rate. In addition, this is affected by the fact that in the polymerization process, a chain terminator is used to obtain a polycarbonate chain terminated with at least one aromatic group, which aromatic group can optionally be terminated with at least one C1-C6 alkyl group, preferably substituted. According to the invention, the correct process parameters are found so that the chain terminator does react with the polycarbonate chain ends. The technician knows that not every polycarbonate chain is terminated with an aromatic group (especially the preferred groups mentioned above). This can already be seen from the fact that the saponifiable chlorine content is not zero. In addition, some polycarbonate chains may be terminated with OH. The present invention preferably covers the situation in which not all generated polymer chains are terminated with the at least one optionally C1-C6 alkyl group, preferably substituted aromatic group. However, preferably at least 50 mol%, more preferably at least 75 mol%, most preferably at least 90 mol% of the polymer chains are terminated with the at least one optionally C1-C6 alkyl group, preferably substituted aromatic group (wherein the mol% refers to the number of moles of all polymer chains). It is advantageous to use chain terminators during the preparation of the polycarbonates of the invention in order to terminate the chain with groups other than chlorine atoms, more preferably with groups other than chlorine atoms or OH groups. However, as can be seen from experiments using only the process according to the invention, chain terminators do react with the chain ends.
[0112] Furthermore, it is preferred that the polycarbonate according to the invention has 0.5 to 10% by weight, more preferably 1 to 5% by weight, of aromatic end groups, relative to the total weight of the polycarbonate.
[0113] Finally, the use of chain terminators results in polycarbonate chains having a low -OH end group content. Preferably, the polycarbonates of the present invention have an -OH end group content of no more than 1000 ppm, more preferably less than 500 ppm, and most preferably less than 100 ppm. The skilled person knows how to determine the -OH end group content. For example, infrared spectroscopy or 1 H-NMR. According to the invention, the -OH end group content is preferably determined by infrared spectroscopy. The polycarbonate is dissolved preferably in dichloromethane. Preferably, a wavelength of 3583 cm -1 The content is determined by measuring the band at . The technician can perform the respective calibration. In another aspect of the present invention, a molding compound is provided, which comprises the polycarbonate of the present invention as given in each definition above. Such a molding compound can be obtained by adding additional thermoplastic polymers and / or additives. In addition, another aspect of the present invention provides a molded article, which comprises the polycarbonate of the present invention as given in each definition above. Such a molded article can be obtained by methods known to the technician, such as extrusion, injection molding, blow molding or thermoforming of sheets or plates.
[0114] In another aspect of the invention, there is provided a process for producing a polycarbonate having a low saponifiable chlorine content and a high number average molecular weight. Preferably, the process of the invention produces a polycarbonate of the invention as per the definitions given above.
[0115] Therefore, a process for preparing a polycarbonate is provided, which preferably comprises at least 30% by weight of structural units of the formula (1), the % by weight being based on the total weight of the polycarbonate.
[0116]
[0117] In formula (1)
[0118] Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus,
[0119] R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl,
[0120] R 2 and R 4 each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and
[0121] p and q are each independently 1 or 2, preferably 1, and
[0122] n represents the average number of repeating units,
[0123] wherein the method comprises
[0124] (a) dissolving at least one diol of formula (I) in an aqueous alkaline solution
[0125]
[0126] Wherein in formula (I),
[0127] Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus,
[0128] R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl,
[0129] R 2 and R 4 each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and
[0130] p and q are each independently 1 or 2, preferably 1, and
[0131] optionally adding at least one chain terminator,
[0132] Optionally, at least one catalyst and
[0133] optionally adding additional aqueous alkaline solution,
[0134] To obtain a solution,
[0135] (b) adding an organic solvent suitable for dissolving polycarbonate to the solution of step (a) to thereby obtain a mixture,
[0136] (c) adding phosgene to the mixture of step (b) and optionally adding additional aqueous base solution,
[0137] (d) reacting the mixture of step (c) for 2 to 30 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes,
[0138] (e) optionally adding at least one chain terminator to the mixture of step (d), with the proviso that in case no chain terminator is added in step (a), at least one chain terminator must be added in step (e), and
[0139] optionally adding at least one catalyst,
[0140] optionally adding additional aqueous alkaline solution,
[0141] and in case at least one chain terminator and / or at least one catalyst is added in this step, the resulting mixture is reacted for 2 to 60 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes,
[0142] (f) optionally adding at least one catalyst to the mixture of step (d) or step (e), depending on which step is performed last, provided that in case no catalyst is added in both step (a) and step (e), at least one catalyst must be added in step (f),
[0143] and in the case of adding at least one catalyst in this step, the resulting mixture is reacted for 2 to 60 minutes, preferably 10 to 50 minutes, more preferably 15 to 45 minutes, most preferably 25 to 35 minutes,
[0144] (g) determining the pH of the mixture obtained after step (d), (e) or (f), depending on which step is performed last, and, if necessary, adjusting the pH by adding additional aqueous base solution so that the resulting pH is at least 10.0,
[0145] And in case additional aqueous base solution is added in this step, the mixture is allowed to react for 2 to 30 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes.
[0146] In the present invention, aqueous alkaline solution is preferably understood as aqueous alkali metal hydroxide solution, and preferably refers to aqueous sodium hydroxide solution, potassium hydroxide solution or a mixture thereof, particularly preferably aqueous sodium hydroxide solution. Preferably, the pH of the aqueous alkaline solution is equal to or higher than 10.0, preferably equal to or higher than 10.5, more preferably equal to or higher than 10.7, most preferably equal to or higher than 10.8.
[0147] According to the invention, the pH is determined during the method. Preferably, the term "determining" according to the invention means (actively) measuring and / or calculating (e.g. based on the molar ratios of the educts and / or the reaction itself). In case the pH is measured, it is measured at room temperature or in the state in which the measured solution is at the moment - if there is no different indication. Due to the exothermic reaction, it is possible for the measured solution to have a temperature above room temperature.
[0148] Preferably, with respect to the diol of formula (I),
[0149] Each X independently represents a substituted or unsubstituted C3-C 18 -cycloalkylidene; formula—C(R c )(R d )—C1-C 18 -alkylidene, where R c and R d are independently hydrogen, C1-C12 -alkyl, C1-C 12 -Cycloalkyl, C7-C 12 -Arylalkyl, C1-C 12 -heteroalkyl or cyclic C7-C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-valent C1-C 12 - a hydrocarbon group,
[0150] R 1 and R 3 Each independently represents C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl,
[0151] R 2 and R 4 each independently represents a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and
[0152] p and q are each independently 1. It is to be understood that the skilled person sees that formula (1) and formula (I) differ from each other in that in formula (1), the OH groups of formula (I) react to form carbonates. Therefore, it is also to be understood that the skilled person can replace X, R given with respect to formula (1) with 1 To R 4 All preferred definitions of , p and q are transferred to formula (I). Therefore, all preferences given for formula (1) are also valid for formula (I). In addition, it is to be understood that if the polycarbonate comprises a specific structural formula (1), the corresponding diol of formula (I) needs to be of the same structural formula, but additionally has OH groups.
[0153] Preferably, the polycarbonate as obtained by the process according to the invention comprises at least 30% by weight, more preferably at least 40% by weight, even more preferably at least 50% by weight, even more preferably at least 60% by weight, even more preferably at least 70% by weight, even more preferably at least 80% by weight, most preferably at least 90% by weight of structures of formula (1), wherein the % by weight are based on the total weight of the polycarbonate. Furthermore, it is preferably understood that after the last process step according to the invention (e.g. process step (g)), a polycarbonate comprising at least 30% by weight, more preferably at least 40% by weight, even more preferably at least 50% by weight, even more preferably at least 60% by weight, even more preferably at least 70% by weight, even more preferably at least 80% by weight, most preferably at least 90% by weight of structures of formula (1) is obtained, wherein the % by weight are based on the total weight of the polycarbonate. Furthermore, all preferences as given for the polycarbonate according to the invention preferably apply.
[0154] Furthermore, the skilled person is aware of the fact that in principle the % by weight of the structural formula (1) in the resulting polycarbonate can be achieved by using corresponding amounts / ratios of the corresponding diols. This means that, for example, if two diols are used, the resulting polycarbonate will contain the corresponding structural units in a ratio comparable to if the two diols were originally used.
[0155] This means, for example, that in step (a) of the process according to the invention, preferably at least 30% by weight of at least one diol of the formula (I) is dissolved, wherein the weight % is based on the total weight of all diols and polyols used. Preferably, in step (a) of the process according to the invention, preferably at least 30% by weight, more preferably at least 40% by weight, even more preferably at least 50% by weight, even more preferably at least 60% by weight, even more preferably at least 70% by weight, even more preferably at least 80% by weight and most preferably at least 90% by weight of at least one diol of the formula (I) is dissolved. Preferably, in step (a), additional diols and / or triols and / or tetraols different from formula (I) are used. Preferably, in step (a) of the process according to the invention, additional polyols having structural units selected from the group consisting of formulae (II) to (X), (IIg), (IIh), (IIi), (IIj), (IIk) and (IIl) are used, wherein In formula (II), X, R 2 To R 4 , p and q are defined as for equation (2),
[0156] Wherein in formula (III), Z, R 5 , R 6 , p1 and q1 are each as defined for formula (3),
[0157] Wherein in formula (VII), each R x and each t is defined as in equation (7),
[0158] Wherein in formula (VIII), Y1, Y2, R' and s are each as defined for formula (8),
[0159] Wherein in formula (IX), Y1 and Y2 are each as defined for formula (9),
[0160]
[0161] wherein each R and X are as defined for formula (IIb),
[0162] wherein each R is as defined for formula (IIc),
[0163] wherein each R1 and R2 are as defined for formula (IId),
[0164]
[0165] The person skilled in the art will be able to see the relationship between the above polyols and the corresponding structures of formulae (2) to (10) and (IIa) to (IIf). Therefore, all preferences given for the polycarbonates of the present invention can also be transferred to the polyols as shown above. Furthermore, in the present invention, the term "polyol" or "additional polyol" preferably comprises a diol, a triol or a tetraol. Sometimes only a diol or an additional diol is mentioned. However, it is to be understood that this statement may also cover triols and tetraols of formulae (IIg) to (IIl). This is understandable to the skilled person in the context of the present invention.
[0166] Preferably, in the process of the present invention, no diol of formula (101) is used.
[0167]
[0168] This preferably does not exclude that structural units of the formula (101) may be present in trace amounts in the diols or polyols used. Preferably, the amount of diols of the formula (101) in the at least one diol and possible polyol used according to the invention is less than 30% by weight, more preferably less than 20% by weight, most preferably less than 10% by weight, wherein the weight % is based on the total weight of all diols and polyols used.
[0169] The solution of step (a) contains an aqueous alkaline solution, one or more diols of formula (I) and water, wherein the concentration of this aqueous solution is preferably between 1% and 30% by weight, particularly preferably between 3% and 25% by weight, very particularly preferably between 15% and 18% by weight, based on the total weight of the aqueous phase, with respect to the sum of the diols present (not calculated as alkali metal salts but as free diols). The alkali metal hydroxide used to dissolve the diols, for example sodium hydroxide or potassium hydroxide, can be used in solid form or as the corresponding aqueous alkali metal hydroxide solution. The concentration of the aqueous alkaline solution depends on the target concentration of the desired diol solution, but is generally between 5% and 25% by weight, preferably between 5% and 15% by weight, based on 100% by weight of the aqueous alkaline solution, or more concentrated and subsequently diluted with water. The method of subsequent dilution uses an optionally temperature-controlled aqueous alkaline solution with a concentration of between 15% and 75% by weight, preferably between 25% and 55% by weight. The alkali metal content depends on the structure of the diol. Preferably, the alkali metal content is adjusted so that the resulting pH of the solution of process step (a) is at least 12.0, more preferably at least 12.5, most preferably at least 12.7. If more than one diol is used, these can be dissolved together. This means that the comonomers, especially those of formula (II) to (X) or (IIg) to (IIl), are preferably added simultaneously with the diol of formula (I). In the case of adding trifunctional or tetrafunctional compounds / crosslinkers (e.g. structures of formula (IIg) to (IIl)), this is preferably added simultaneously with the diol of formula (I). This means that preferably all difunctional and (if present) trifunctional or tetrafunctional components are added simultaneously in process step (a). However, since the solubility of diols and / or polyols depends to a large extent on the amount of alkali metal used, it may be advantageous not to provide one solution comprising two diols, but to provide two solutions each comprising one diol dissolved in a suitable aqueous alkaline solution, which are then metered separately to form the correct mixing ratio. The dissolution process can be started from solid glycol, usually in the form of flakes or pellets, or from molten glycol. In the case of sodium hydroxide or aqueous sodium hydroxide solution, the aqueous alkaline solution used can be produced, for example, by the amalgam process or the so-called membrane process. Both methods have been used for a long time and are familiar to those skilled in the art. In the case of aqueous sodium hydroxide solution, it is preferred to use a solution produced by a membrane process.
[0170] In such aqueous solutions and / or aqueous phases, the diols are completely or partly in the form of the corresponding alkali metal salts / dialkaline metal salts.
[0171] According to the invention, method step (a) produces a solution. In the present invention, a "solution" differs from a "suspension" in particular in that solid particles can hardly be detected in a solution. A solution is a single-phase system. The state of the phases can be determined by methods known to the skilled person. For example, optical analysis, such as the refractive index, can distinguish between a single-phase or a two-phase system.
[0172] In step (a), the addition of at least one chain terminator, at least one catalyst and additional aqueous alkaline solution is optional. Preferably, no chain terminator is added in process step (a). More preferably, no catalyst is added in process step (a). More preferably, neither any chain terminator nor any catalyst is added in process step (a).
[0173] Preferably, the pH at the end of process step (a) is at least 12.0, more preferably at least 12.5, most preferably at least 12.7. In case the pH at the end of process step (a) is below this value, it is preferred to add additional aqueous alkaline solution to adjust the pH so that it is at least 12.0, more preferably at least 12.5, most preferably at least 12.7. In step (b), an organic solvent suitable for dissolving the polycarbonate is added to the solution of step (a) and a mixture is obtained. In principle, this mixture of step (b) is a dispersion comprising the aqueous phase of step (a) and the organic phase (solvent) added in step (b).
[0174] Dispersing the organic phase in the aqueous phase or the aqueous phase in the organic phase using, for example, a disperser can produce an oil-in-water (ow) dispersion or a water-in-oil dispersion (wo), wherein oil is understood to mean the organic phase. However, it is preferred according to the invention that process step (b) produces an oil-in-water dispersion. Preferably, during step (b), the organic phase is continuously dispersed into the aqueous phase of step (a) using a disperser.
[0175] By definition, an oil-in-water dispersion is a dispersion in which water forms the outer (continuous) phase and oil forms the inner (dispersed) phase, ie the oil droplets are distributed in the water. A water-in-oil dispersion is thus a dispersion in which oil forms the outer phase and water forms the inner phase.
[0176] Suitable organic solvents for dissolving polycarbonates are known to the skilled worker.
[0177] Suitable solvents are aromatic and / or aliphatic chlorinated hydrocarbons, preferably dichloromethane, trichloroethylene, 1,1,1-trichloroethane, 1,1,2-trichloroethane and chlorobenzene and mixtures thereof. However, aromatic hydrocarbons such as benzene, toluene, m / p / o-xylene or aromatic ethers such as anisole can also be used alone, in admixture, or together or in admixture with chlorinated hydrocarbons; preference is given to dichloromethane and chlorobenzene and mixtures thereof. Another embodiment of the process according to the invention uses solvents which do not dissolve the polycarbonate but only swell it. Thus, non-solvents for polycarbonate can also be used in combination with the solvent. If the solvent partner forms a second organic phase, solvents soluble in the aqueous phase such as tetrahydrofuran, 1,3- or 1,4-dioxane or 1,3-dioxolane can also be used as solvents.
[0178] In step (c) phosgene is added to the mixture of step (b). Its introduction can be achieved in gaseous form or in liquid form. The skilled person knows how to adjust the amount of phosgene relative to the diol used and (if used) trifunctional or tetrafunctional crosslinking agent. Usually, phosgene is used in a molar excess relative to the diol used and (if used) trifunctional or tetrafunctional crosslinking agent. However, for economic and ecological reasons, this excess should be as low as possible. Preferably, the molar ratio of phosgene to diol (and if used, trifunctional or tetrafunctional crosslinking agent) is 1.05 to 1.6.
[0179] In addition, an additional aqueous alkaline solution is optionally added. In the present invention, an aqueous alkaline solution is already used in method step (a). This is why any further actively added aqueous alkaline solution is referred to as "additional", which means that an aqueous alkaline solution is further added. It is usually added to adjust the pH. Preferably, throughout the entire process of the method of the present invention, the pH is at least 8. In the case of adding an additional aqueous alkaline solution, the amount is preferably selected so that the resulting pH is at least 10.8, more preferably 11. The method of the present invention includes several optional possibilities for adding additional aqueous alkaline solutions. However, it is preferred that the number of additional additions of aqueous alkaline solutions is as low as possible. Most preferably, if necessary, additional aqueous alkaline solutions are added only in steps (g) and / or (c).
[0180] Any step of adding additional aqueous alkaline solution is an exothermic reaction. According to the invention, the step is preferably carried out in a temperature range of -5°C to 100°C, particularly preferably 15°C to 80°C, very particularly preferably 25°C to 65°C, wherein, depending on the solvent or solvent mixture, it can be carried out under positive pressure. Depending on the reactor used, different pressures can be used. For example, pressures of 0.5 to 20 bar (absolute) can preferably be used.
[0181] According to the invention, it is preferred to add additional aqueous alkaline solution in process step (c). In process step (a), the alkali metal is usually used in a stoichiometric amount or in a small molar excess relative to the diol. It is preferred to add additional aqueous alkaline solution in process step (c) to compensate for the excess phosgene. Preferably, the pH after process step (c) is at least 10.8, more preferably at least 11.0, most preferably at least 11.5.
[0182] In process step (d), the mixture of step (c) is reacted for 2 to 30 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes. The skilled person knows how to carry out this "reaction". For example, the two phases can be mixed so that the two phases do not separate. At the same time, the reaction is preferably carried out in a manner that no solid precipitates.
[0183] The process step (e) comprises optionally adding at least one chain terminator to the mixture of step (d), with the proviso that in case no chain terminator is added in step (a), at least one chain terminator must be added in step (e), and
[0184] optionally adding at least one catalyst,
[0185] optionally adding additional aqueous alkaline solution,
[0186] And in case at least one chain terminator and / or at least one catalyst is added in this step, the resulting mixture is reacted for 2 to 60 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes.
[0187] This means that in case at least one chain terminator has been added in process step (a), process step (e) can be optional. However, if no chain terminator has been added in step (a), process step (e) must be carried out. This is due to the fact that according to the invention, the use of chain terminators is necessary in order to obtain polycarbonates with a low saponifiable chlorine content.
[0188] The at least one chain terminator is usually monofunctional. The at least one chain terminator is preferably selected from monocyclic phenols, C1-C 22Alkyl-substituted phenols, monoethers of diphenols, alkyl-substituted phenols with branched alkyl substituents containing 8 to 9 carbon atoms, 4-substituted 2-hydroxybenzophenones, aryl salicylates, monoesters of diphenols, 2-(2-hydroxyaryl)-1,3,5-triazines, aromatic monocarboxylic acid chlorides, aromatic polycyclics and monocarboxylic acid chlorides. More preferably, the at least one chain terminator is selected from phenols, alkylphenols and their chlorocarbonates or acid chlorides of monocarboxylic acids, most preferably from phenol, tert-butylphenol and isooctylphenol, cumylphenol. Any desired mixture of the listed chain terminators can be used. The at least one chain terminator can be added to the aqueous phase and / or the organic phase. Preferably, the at least one chain terminator is dissolved in the organic phase. Preferably, 0.5 to 10 mol %, more preferably 1 to 5 mol % of the at least one chain terminator is used in the process of the invention relative to the molar number of the sum of all diols. The skilled person knows that, in the case of trifunctional hydroxy compounds, the amount of the at least one chain terminator can be adjusted so that theoretically every chain end can be terminated by the at least one chain terminator.
[0189] Preferably, the process of the present invention is characterized in that step (e) and / or step (f) must be performed. In case step (e) is performed, at least one chain terminator is added in step (e). This means that preferably step (e) must be performed and the at least one chain terminator is added. More preferably, at least one chain terminator is added only in step (e) (and not in step (a)). It is preferred that no additional aqueous alkaline solution is added in step (e) of the process.
[0190] Process step (f) comprises the optional addition of at least one catalyst to the mixture of step (d) or step (e), whichever step is performed last, provided that in case no catalyst is added in step (a) and step (e), at least one catalyst must be added in step (f) and, in case at least one catalyst is added in this step, the resulting mixture is reacted for 2 to 60 minutes, preferably 10 to 50 minutes, more preferably 15 to 45 minutes, most preferably 25 to 35 minutes. In parallel with step (e), process step (f) may be optional in case at least one catalyst has been added in process steps (a) and / or (e). However, process step (f) must be performed if at least one catalyst is not added in step (a) and step (e). This is due to the fact that, according to the invention, a catalyst must be used in order to obtain polycarbonates having a sufficiently high molecular weight within a reasonable reaction time.
[0191] However, preferably step (f) must be performed. More preferably, at least one catalyst is added only in step (f) (and not in steps (a) and / or (e)).
[0192] Preferably, the at least one catalyst is selected from tertiary amines, quaternary ammonium salts, quaternary phosphonium salts and mixtures thereof, regardless of the time of its addition. The at least one catalyst is very particularly preferably a tertiary amine or a mixture of at least two tertiary amines. The tertiary amine is also preferably triethylamine, tributylamine, trioctylamine, N-ethylpiperidine, N-methylpiperidine or N-iso / n-propylpiperidine; these compounds are described in the literature as typical interfacial catalysts, are commercially available and are well known to those skilled in the art. The catalyst can also be added to the synthesis individually, mixed or simultaneously or successively. The metered addition of one or more catalysts can be carried out in pure form, in an inert solvent (preferably the solvent or one of the solvents of the organic phase of process step (b)) or as an aqueous solution. When a tertiary amine is used as a catalyst, its metered addition can be carried out, for example, as its ammonium salt with an acid, preferably an inorganic acid, in particular hydrochloric acid, in an aqueous solution. It is to be appreciated that when two or more catalysts are used or when a sub-amount of the total catalyst amount is metered, different metered addition modes can be adopted at different locations or at different times. The total amount of catalyst used, based on the moles of diol used, is preferably between 0.001 and 10 mol %, preferably between 0.01 and 8 mol %, particularly preferably between 0.05 and 5 mol %.
[0193] In step (g) of the process according to the invention, the pH of the mixture obtained after step (d), (e) or (f) (whichever step is carried out last) is determined and, if necessary, adjusted by adding additional aqueous alkaline solution so that the resulting pH is at least 10.0, preferably at least 10.1, more preferably at least 10.2, even more preferably at least 10.3, even more preferably at least 10.4, even more preferably at least 10.5, even more preferably at least 10.6, even more preferably at least 10.7, even more preferably at least 10.8, and in the case of adding additional aqueous alkaline solution in this step, the mixture is reacted for 2 to 30 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes.
[0194] The determination, in particular the measurement of the pH, can be carried out in a manner known to the person skilled in the art. However, it is also possible to calculate the pH in method step (g).
[0195] According to the invention, it has been found that the pH at the end of the addition of all mandatory components plays a crucial role. Only when the pH is sufficiently high, i.e. at least 10.0, preferably at least 10.1, more preferably at least 10.2, even more preferably at least 10.3, even more preferably at least 10.4, even more preferably at least 10.5, even more preferably at least 10.6, even more preferably at least 10.7, even more preferably at least 10.8, can the chain terminator react with the polymer chain ends and thereby reduce the saponifiable chlorine content. This means that the determination of the pH during process step (g) is important in order to know whether it is high enough and to decide whether an additional aqueous alkaline solution must be added. According to the invention, additional aqueous alkaline solution can also be added in process steps (a), (c) and / or (e). This means that in step (g) the pH may already have a value of at least 10.0 (or any preferred pH value as given above). In this case, no additional addition of an aqueous alkaline solution is necessary. However, even if additional aqueous alkaline solution has been added in steps (a), (c) and / or (e), or if additional aqueous alkaline solution has not been added in any of these steps, the pH of the resulting solution may be lower than 10.0 (or any preferred pH value given above). In this case, additional aqueous alkaline solution must be added to ensure the quality of the resulting polycarbonate. Preferably, additional aqueous alkaline solution is added only in steps (c) and (g) of the present invention.
[0196] Preferably, in at least one of steps (a), (c) or (e), the pH is determined before the optional addition of additional aqueous base solution and, if necessary, adjusted by adding additional aqueous base solution so that the resulting pH is at least 10.0, preferably at least 10.1, more preferably at least 10.2, even more preferably at least 10.3, even more preferably at least 10.4, even more preferably at least 10.5, even more preferably at least 10.7, most preferably at least 10.8. More preferably, the pH after each of process steps (a) to (g) is at least 10.0, preferably at least 10.1, more preferably at least 10.2, even more preferably at least 10.3, even more preferably at least 10.4, even more preferably at least 10.5, even more preferably at least 10.7, most preferably at least 10.8.
[0197] Preferably, the polycarbonate of the present invention is obtained by the method of the present invention. Therefore, all preferences as given for the polycarbonate of the present invention are preferably applicable to the polycarbonate obtained as the method according to the present invention. After the method of the present invention, the polycarbonate can be separated. Post-treatment includes sedimentation of the at least two-phase reaction mixture of the reaction containing at most trace amounts, preferably less than 2ppm of chlorocarbonate to separate the phases. Optionally, the alkaline aqueous phase is fully or partially recycled to the polycarbonate synthesis as the aqueous phase, or is sent to the wastewater post-treatment, where the solvent and catalyst fraction are separated and optionally recycled to the polycarbonate synthesis. In another variant of post-treatment, after separating organic impurities, particularly solvents and polymer residues and optionally adjusting to a specific pH (e.g., by adding sodium hydroxide solution), salts are separated, which can be sent to, for example, chlor-alkali electrolysis, and the aqueous phase is optionally sent back to the polycarbonate synthesis.
[0198] The organic phase containing the polycarbonate may then be purified in a variety of ways known to those skilled in the art for removing alkali metal, ion or catalyst contamination.
[0199] Isolation of the polycarbonate from solution can be accomplished by evaporating the solvent using temperature, vacuum, or heated entraining gas. Other isolation methods include, for example, crystallization and precipitation.
[0200] The process of the present invention can be carried out continuously or in a batch process. Preferably, the process of the present invention is carried out continuously.
[0201] Preferably, no emulsifier is used throughout the entire process according to the invention. The skilled person is familiar with emulsifiers. One emulsifier commonly used in the production of polycarbonates is sodium gluconate. Without the use of such an emulsifier, post-processing is easier and therefore less effort is required to obtain polycarbonate. Example
[0202] Size exclusion chromatography was performed using a PSS SECurity System; polycarbonate calibration (according to method 2301-0257502-09D of Currenta GmbH & Co. OHG, Leverkusen), dichloromethane as eluent, column 1 (PL-PC5), concentration 2 g / l, flow rate 1.0 ml / min, at a temperature of 30°C, using UV and / or RI detection.
[0203] The saponifiable chlorine content was determined by UV absorption after reaction with 4-(4-nitrobenzyl)pyridine. A Perkin Elmer Lambda 365 spectrophotometer was used. Bisphenol A bis(chloroformate) was used as a calibration substance due to its known chlorine content. Polycarbonate was dissolved in dichloromethane and reacted with a dichloromethane solution of 4-(4-nitrobenzyl)pyridine. The saponifiable chlorine content (mg / kg) was determined by measuring the absorption at 438nm compared to the absorption at 600nm. In order to determine the OH groups, polycarbonate was dissolved in dichloromethane (2g / 50mL; 1mm quartz cuvette) and analyzed with a Fourier transform infrared spectrometer Nicolet iS20 from Thermo Fisher Scientific. The 3583cm -1 The content of phenolic OH groups can be determined by observing the band at
[0204] The glass transition temperature was determined by DSC using ISO 11357-2:2013-05 at a heating rate of 10°C / min.
[0205] abbreviation:
[0206] BPL1: 4,4'-propylenebis(2-methoxyphenol), recrystallized from toluene
[0207] BPL2: a mixture of 67 mol% of 4,4'-propylenebis(2-methoxyphenol) and 33 mol% of the corresponding meta- and para-isomers
[0208] BPA: Bisphenol A
[0209] DOD:4,4'-dihydroxybiphenyl
[0210] BP-TMC:1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane
[0211] THPE: Tris(4-hydroxyphenyl)ethane
[0212] General procedure for polymerization:
[0213] The laboratory batch reaction was carried out in a stirred glass reactor. The diol or diol mixture (or THPE) was added to demineralized water in which NaOH had been dissolved (2.6 mol NaOH / mol diol) to obtain a 5 wt % diol solution. Subsequently, dichloromethane was added to the diol solution in an amount calculated to provide a 15 wt % PC solution after the reaction was completed. The stirrer was set to a fixed speed to produce an oil-in-water dispersion. Phosgene was added to the stirred solution in a semi-batch feed via a dip tube using a mass flow meter over the course of 12 minutes. 1.28 mol phosgene was added per mole of diol (and if necessary, THPE) to ensure complete conversion of the bisphenol. After the addition of phosgene was complete, 0.035 mol p-tert-butylphenol / mol diol was added as a chain terminator. After a reaction time of 5 minutes, further NaOH was added together with 0.015 mol N-ethylpiperidine / mol diol to bring the pH to a value of 11. It is normal for the pH to drop during the post-reaction time. pH was measured using a Mettler Toledo DG 111-SC pH electrode.
[0214] The comparative example was stopped after a post-reaction time of 30 minutes. The sample was washed once with 10% HCl and then with demineralized water until the conductivity of the separated water was below 100 μS. The sample was dried with Na2SO4 and filtered through a folded paper filter (Whatman 113V, φ320 nm). The polymer was dried overnight in a vacuum oven at 120°C, 20 mbar.
[0215] For embodiments of the present invention, the reaction is completed (Cl end groups are completely converted) by further adding NaOH to raise the pH back to at least 10.0. After the pH remains stable, the solution is stirred for a post-reaction time of 30 minutes. The total time from the beginning of addition to the end of the post-reaction time is approximately 2 hours. Use phosgene leak detection paper to check residual chlorine end groups, and at the end of the reaction, the sample is washed once with 10% HCl, then washed with demineralized water, until the conductivity of the separated water is less than 100 μS. The sample is dried with Na2SO4 and filtered through a folded paper filter (Whatman 113V, φ320nm). The polymer is dried overnight at 120°C, 20 mbar in a vacuum oven.
[0216] Table 1:
[0217]
[0218]
[0219] As can be seen from the table above, if the pH at the end of the reaction is below 10.0, the saponifiable chlorine content is quite high (Example 1). This is independent of the fact that additional comonomers are used (see Examples 2 to 4 and Example 7). Furthermore, it can be seen from the high saponifiable chlorine content and the amount of OH end groups that the chain terminators used in these comparative examples have not reacted completely with the polymer chain ends.
[0220] Raising the pH at the end of the reaction to at least 10.0 results in a reduction in the saponifiable chlorine content (see Examples 5, 6, 8, 9 and 12). In many cases, high molecular weights are simultaneously obtained. In addition, the OH end group content is also at an acceptable level. This data indicates that the chain terminator reacts effectively with the polymer chain ends. In addition, the polymerization itself is close to completion. These effects exist for homopolymers as well as copolymers, including branched copolymers.
[0221] Furthermore, the polymerization of BPA at a pH of 9.3 appears to have resulted in polycarbonate of good quality, as can be seen from Comparative Examples 10 and 11. Increasing the pH to 11.1 (Comparative Example 11) shows that the properties of the polycarbonate containing BPA do not become better, if not slightly worse.
Claims
1. A polycarbonate comprising at least 30% by weight of structural units of the formula (1), wherein the % by weight is based on the total weight of the polycarbonate, in Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus, R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl, R 2 and R 4 each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and p and q are each independently 1 or 2, preferably 1, and n represents the average number of repeating units, Features The polycarbonate is end-capped with at least one aromatic group which may optionally be substituted with at least one C1-C6 alkyl group, has a total saponifiable chlorine content of 0.2 ppm to 19 ppm relative to the mass of the polycarbonate and a number average molecular weight of 8000 g / mol to 20000 g / mol as determined by gel permeation chromatography in dichloromethane by calibration with bisphenol A-polycarbonate.
2. The polycarbonate according to claim 1, characterized in that In formula (1) Each X independently represents a substituted or unsubstituted C3-C 18 -cycloalkylidene; formula—C(R c )(R d )—C1-C 18 -alkylidene, where R c and R d are independently hydrogen, C1-C 12 -alkyl, C1-C 12 -Cycloalkyl, C7-C 12 -Arylalkyl, C1-C 12 -heteroalkyl or cyclic C7-C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-valent C1-C 12 - a hydrocarbon group, R 1 and R 3 Each independently represents C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl, R 2 and R 4 each independently represents a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and p and q are each independently 1, and n represents the average number of repeating units.
3. The polycarbonate according to claim 1 or 2, characterized in that In formula (1) Each X independently represents the formula -C(R c )(R d )—C1-C6-alkylidene, wherein R c and R d Each is independently hydrogen or C1-C5-alkyl.
4. The polycarbonate according to any one of claims 1 to 3, characterized in that In formula (1) Each X independently represents the formula -C(R c )(R d )—C1-C4-alkylidene, wherein R c and R d are each independently hydrogen or C1-C3-alkyl, R 1 and R 3 each independently represents a methyl group or an ethyl group, R 2 and R 4 each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group, and n represents the average number of repeating units.
5. The polycarbonate according to any one of claims 1 to 4, characterized in that The polycarbonate further comprises at least one structural unit selected from the structural units of formulae (2) to (10), (IIa), (IIb), (IIc), (IId), (IIe) and (IIf) Among them, X, R 2 To R 4 , p and q are as defined in any one of claims 1 to 4, and m1 represents the average number of repeating units; wherein each Z independently represents a single bond, -S(=O)2-, -C(=O)-, -O-, -S-, -S(=O)-, -CH(CN)-, a straight-chain or branched C1-C6-alkylene group optionally containing at least one carbonyl group, optionally containing at least one halogen atom and / or optionally interrupted by at least one heteroatom, a C2-C6-alkylene group optionally containing at least one carbon-carbon double bond, optionally containing at least one carbonyl group and / or optionally containing at least one halogen atom 10 -alkylidene, C5-C6-alkylene ... 12 -cycloalkylene, C5-C6-cycloalkylene, wherein the alicyclic group is optionally fused to at least one alicyclic and / or at least one aromatic ring 15 -cycloalkylidene, C7-C 20 -Arylalkylidene, C8-C 20 -aralkylene, a C6-C6-alkylene ring optionally fused to a further aromatic ring which may optionally contain at least one heteroatom 12 -arylene group, formula (B1-A), formula (B1-B), formula (B1-C) or formula (B1-D) wherein in formulae (B1-A), (B1-B) and (B1-C), each R' independently represents a linear C1-C4-alkyl group, a branched C3-C4-alkyl group, an aralkyl group or an aryl group, and "C*" represents a quaternary carbon atom at the position indicated as "Z" in formula (3), and wherein in formula (B1-D), each R' independently represents a straight-chain C1-C4-alkyl group, a branched C3-C4-alkyl group, each R" independently represents a straight-chain C1-C4-alkylene group, a branched C3-C4-alkylene group, each R"' independently represents H or a straight-chain C1-C3-alkyl group, s is 0 to 2, and each s1 is independently 0 or 1, and "*" represents a bond connecting "Z" to the aromatic ring in formula (3), R 5 and R 6 Each independently represents H, C1-C 18 -alkyl, C5-C6-cycloalkyl, C1-C5-alkenyl-, C1-C 18 -alkoxy, phenoxy, halogen atom, C6-C 18 -Aryl or C7-C 18 -aralkyl, p1 and q1 are each 1 to 4, and m2 represents the average number of repeating units; Wherein in formulas (4) to (6), m2 represents the average number of repeating units; Each R x independently represent a straight or branched C1-C6-alkyl, C1-C 12 - aryl, C1-C8-aralkyl or halogen atom, t is 0 to 4, and m2 represents the average number of repeating units; In formulae (8) and (9), each Y1 independently represents oxygen, sulfur or NR y , where R y is H or -CH3, each Y2 independently represents a single bond, oxygen, sulfur or NR as defined above y , and m2 represents the average number of repeating units, and in formula (8), each R' independently represents a linear C1-C4-alkyl group, a branched C3-C4 alkyl group, an aralkyl group or an aryl group, and s is 0 to 2; Where m3 represents the average number of repeating units; Wherein "*" indicates the connection of the crosslinking point to the polycarbonate polymer chain, and wherein R in formula (IIb) and (IIc) is independently selected from H and alkyl, preferably H and methyl, X in formula (IIb) is selected from a linear or branched alkyl group and a single bond, preferably C(CH3)2 and a single bond, R1 in formula (IId) is selected from H and alkyl, preferably H and methyl, and R2 in formula (IId) is independently selected from H and alkyl, preferably H and methyl.
6. The polycarbonate according to any one of claims 1 to 5, wherein the at least one aromatic group terminating the polycarbonate chain and optionally substituted with at least one C1-C6 alkyl group is selected from the formulae (5a), (6a), (7a), (8a) and (9a), wherein wherein each Y independently represents a halogen atom, a C1-C3-alkyl group, a C1-C3-alkoxy group, a C7-C 12 -Arylalkyl, C7-C 12 - alkylaryl or nitro, y is 0 to 4, and c is 1 to 5, provided that y+c is 1 to 5, And each "*" represents a position where the structure of formula (5a), (6a), (7a) or (8a) is attached to the polycarbonate.
7. A molding compound comprising the polycarbonate according to any one of claims 1 to 6.
8. A molded article comprising the polycarbonate according to any one of claims 1 to 6.
9. A process for preparing a polycarbonate, said polycarbonate comprising at least 30% by weight of structural units of the formula (1), wherein the % by weight is based on the total weight of the polycarbonate, In formula (1) Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus, R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl, R 2 and R 4 each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and p and q are each independently 1 or 2, preferably 1, and n represents the average number of repeating units, The method comprises (a) dissolving at least one diol of formula (I) in an aqueous alkaline solution Wherein in formula (I), Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus, R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl, R 2 and R 4each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and p and q are each independently 1 or 2, preferably 1, and optionally adding at least one chain terminator, Optionally, at least one catalyst and optionally adding additional aqueous alkaline solution, To obtain a solution, (b) adding an organic solvent suitable for dissolving polycarbonate to the solution of step (a) to thereby obtain a mixture, (c) adding phosgene to the mixture of step (b) and optionally adding additional aqueous base solution, (d) reacting the mixture of step (c) for 2 to 30 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes, (e) optionally adding at least one chain terminator to the mixture of step (d), with the proviso that in case no chain terminator is added in step (a), at least one chain terminator must be added in step (e), and optionally adding at least one catalyst, optionally adding additional aqueous alkaline solution, and in case at least one chain terminator and / or at least one catalyst is added in this step, the resulting mixture is reacted for 2 to 60 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes, (f) optionally adding at least one catalyst to the mixture of step (d) or step (e), whichever step is performed last, provided that in case no catalyst is added in both step (a) and step (e), at least one catalyst must be added in step (f), and in the case of adding at least one catalyst in this step, the resulting mixture is reacted for 2 to 60 minutes, preferably 10 to 50 minutes, more preferably 15 to 45 minutes, most preferably 25 to 35 minutes, (g) determining the pH of the mixture obtained after step (d), (e) or (f), whichever step is performed last, and, if necessary, adjusting the pH by adding additional aqueous base solution so that the resulting pH is at least 10.0, And in case additional aqueous base solution is added in this step, the mixture is allowed to react for 2 to 30 minutes, preferably 2 to 20 minutes, most preferably 2 to 5 minutes.
10. The method according to claim 9, characterized in that Step (e) and / or step (f) must be performed.
11. The method according to any one of claims 9 or 10, characterized in that It is imperative to carry out step (e) and to add the at least one chain terminator.
12. The method according to any one of claims 9 to 11, characterized in that In at least one of steps (a), (c) or (e), the pH is measured prior to the optional addition of additional aqueous base solution and, if necessary, adjusted by adding additional aqueous base solution so that the resulting pH is at least 10.
0.
13. The method according to any one of claims 9 to 12, characterized in that The at least one catalyst is selected from tertiary amines, quaternary ammonium salts, quaternary phosphonium salts, and mixtures thereof.
14. The method according to any one of claims 9 to 13, characterized in that The at least one chain terminator is selected from monocyclic phenols, C1-C 22 Alkyl substituted phenols, monoethers of diphenols, alkyl substituted phenols having branched alkyl substituents containing 8 to 9 carbon atoms, 4-substituted 2-hydroxybenzophenones, aryl salicylates, monoesters of diphenols, 2-(2-hydroxyaryl)-1,3,5-triazines, aromatic monocarboxylic acid chlorides, aromatic polycyclic and monocarboxylic acid chlorides.
15. The method according to any one of claims 9 to 14, characterized in that In formula (1) and (I) Each X independently represents a substituted or unsubstituted C3-C 18 -cycloalkylene; formula—C(R c )(R d )—C1-C 18 -alkylidene, where R c and R d are independently hydrogen, C1-C 12 -alkyl, C1-C 12 -Cycloalkyl, C7-C 12 -Arylalkyl, C1-C 12 -heteroalkyl or cyclic C7-C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-valent C1-C 12 - a hydrocarbon group, R 1 and R 3 Each independently represents C1-C 26 -alkyl, C7-C 26 Alkyl aryl or C7-C 26 -aralkyl, R 2 and R 4 each independently represents a hydrogen atom, a C1-C6-alkoxy group or a C1-C6-alkyl group, and p and q are each independently 1.