Method of forming a composite substrate

Through the mixed gas plasma activation and ultraviolet surface modification process, the piezoelectric material is directly combined with the substrate, solving the band conduction deviation and electrostatic charge problems of surface acoustic wave devices during annealing and thinning, achieving efficient The combination of piezoelectric materials improves the temperature stability and propagation efficiency of the device.

CN119072769APending Publication Date: 2024-12-03佐尔坦·奇格勒
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280094049.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2022-11-15
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the annealing and thinning process, existing surface acoustic wave devices have problems such as conduction band offset, thermal micropores, damage to high electrostatic charges and insufficient binding strength, resulting in increased propagation losses and affecting the performance and stability of the device.

Method used

Using mixed gas plasma activation and ultraviolet surface modification processes, piezoelectric materials such as lithium tantalate and lithium niobate are directly combined with substrates such as silicon, silicon oxide, silicon carbide, etc. to form a high-quality composite substrate, and through low temperatures Thermal annealing and mechanical alignment technology improves bond strength and temperature stability.

Benefits of technology

The bonding interface without macroscopic or microscopic voids is realized, which enhances the electromechanical coupling coefficient and temperature stability of the piezoelectric material, reduces electrostatic charge damage, and improves the frequency characteristics and propagation efficiency of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072769A_ABST
    Figure CN119072769A_ABST
Patent Text Reader

Abstract

A method of forming a composite substrate is provided. The method includes a mixed gas plasma activation process using oxygen and nitrogen, including exposing the surface of the wafer and the surface of the piezoelectric material wafer to a plasma system; exposing the plasma activated surface of the wafer and the plasma activated surface of the piezoelectric material wafer to ultraviolet radiation in an oxygen and nitrogen atmosphere; placing the surface of the wafer on the surface of the piezoelectric material wafer; applying a mechanical load to the wafer and the piezoelectric material wafer; performing thermal annealing on the combined wafer and the piezoelectric material wafer; wherein the wafer is configured to support the wafer of piezoelectric material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present disclosure relates generally to the field of composite substrate formation including wafer bonding processes.

[0002] A surface acoustic wave (SAW) device is known in which a supporting substrate and a piezoelectric substrate for propagating surface acoustic waves are combined together. By attaching a supporting substrate having a smaller thermal expansion coefficient than the piezoelectric substrate in this manner, it is known that the dimensional change of the piezoelectric substrate when the temperature changes is suppressed and the frequency characteristic change of the surface acoustic wave device is reduced.

[0003] WO2017163722A1 discloses a surface acoustic wave device having a structure in which a piezoelectric substrate and a silicon substrate are bonded together using a multi-step process, wherein in a first step, a so-called bonding layer of a set of different specified materials is deposited on at least one of the bonding pairs, and in a second step, the layer and the surface of the other bonding pair are activated by a plasma process, followed by a direct bonding step and subsequent thermal annealing.

[0004] CN109786229B discloses a surface acoustic wave device, in which a piezoelectric wafer is bonded to different substrate materials using a wet chemical wafer bonding surface process followed by Ar / O2 mixed gas plasma activation for a limited wafer size of 0.051 μm to 0.102 μm.

[0005] CN109166793B discloses a two-step surface activation before the direct bonding step. Here, the first activation step is: placing the lithium niobate wafer and the silicon wafer to be bonded under a vacuum ultraviolet light source and activating them under a humidity condition of 20-80%. The second activation step is: placing the vacuum ultraviolet light activated wafer in N2 plasma under a pressure of 10-80Pa.

[0006] Known wafer bonding methods for bonding piezoelectric materials to supporting wafers typically exhibit the following problems and / or technical issues in the final production of RF filter devices: conduction band shift of SAW devices with substrate temperature during annealing and thinning, thermal microvoiding (e.g., outgassing), damage to high electrostatic charges (e.g., warping and high bowing), and insufficient bonding strength for further processing of the bonded wafers (e.g., thinning, dicing), and increased SAW propagation losses.

[0007] It is an object of the present invention to provide a method for forming a composite substrate having improved properties, said method comprising a wafer bonding process.

[0008] The method for forming the composite substrate may comprise the features of claim 1. Further embodiments are listed in the dependent claims. The method provides for efficient manufacturing of thin film surface acoustic wave (also known as TF-SAW) and other related devices by effectively forming a stable bond between the piezoelectric wafer and the supporting wafer.

[0009] For example, the method considers a process flow to improve the wafer bonding of a piezoelectric crystal on a supporting wafer material, which occurs in known wafer bonding processes and SAW device manufacturing. For example, the following characteristics can be improved by the method: conduction band shift of the SAW device with substrate temperature during annealing and thinning, thermal microvoids (such as degassing), damage to high electrostatic charges (such as warping and high bowing), and insufficient bonding strength of the bonded wafer pair to cope with further processing (such as thinning, cutting), and SAW propagation losses. In this way, a piezoelectric material with a large electromechanical coupling coefficient and excellent temperature stability can be provided.

[0010] In the accompanying drawings, the same reference numerals generally refer to the same parts / components in different views. The drawings are not necessarily drawn to scale, but are generally intended to emphasize the principles of the invention. In the following description, various aspects of the invention are described with reference to the following drawings, in which:

[0011] Figure 1 A schematic cross-sectional view of a composite substrate is shown.

[0012] Figure 2 A flow chart of a method for producing a composite substrate is shown.

[0013] FIG. 3A to FIG. 3F A schematic illustration of a method for producing a composite substrate is shown.

[0014] Figure 4 A schematic plasma system for a method of producing a composite substrate is shown.

[0015] FIG. 5A to FIG. 5D An atomic force microscope image of the surface of a substrate constituting the composite substrate is shown.

[0016] Figures 6 to 10B A surface acoustic microscopy image (SAM) and an infrared transmission image (IR) of the surface of the substrate constituting the composite substrate are shown.

[0017] FIG. 11A to FIG. 12B A schematic cross-sectional view of a composite substrate during a substrate thinning process is shown.

[0018] The following detailed description refers to the accompanying drawings that show, by way of illustration, specific details and aspects in which the invention may be practiced.

[0019] Exemplarily, a method is described for bonding a piezoelectric material wafer to a support substrate produced using mixed gas plasma activation. Exemplarily, the method includes: mixed gas plasma activation of oxygen (O2) and nitrogen (N2), ultraviolet light (UV) surface modification of a mixed gas including O2 and N2 (e.g., by using an excimer lamp), a bonding process under low vacuum, and low temperature thermal annealing below 200°C.

[0020] The method achieves high bonding quality of piezoelectric substrates such as lithium tantalate (LT) and lithium niobate (LN) on silicon (Si), silicon oxide, silicon carbide (SiC), cubic boron nitride (c-BN) and diamond. The resulting bonded material (also referred to as a composite substrate) may be free of or substantially free of macroscopic voids and microscopic voids at the bonding interface. Alternatively or additionally, the composite substrate may be free of creaking / cracking and warping of the bonded wafer. The initial pre-bonded state (also referred to as a precursor composite substrate) may show a higher bonding strength than using known bonding techniques. The composite structure can be used to realize thin film surface acoustic wave (also referred to as TF-SAW) devices for various applications, such as as filtering devices in communications, or pumps or mixing devices in fluid handling devices.

[0021] Piezoelectric materials in the material group such as lithium tantalate (LT) and lithium niobate (LN) have a large electromechanical coupling coefficient, which is conducive to achieving broadband filter characteristics. However, these materials have the disadvantage of poor temperature stability. The method provides a permanent wafer direct bonding method (also known as melt bonding) by using a mixed gas plasma activation process and UV surface modification to provide a composite substrate with strong bonding (also known as cohesive composite substrate) or strong adhesion between the wafer and the piezoelectric material. For the following different material combinations, the composite substrate can have no microvoids at the bonding interface: for example, LT / / Si, LN / / Si, LN / / SiO2, LT / / SiO2, quartz / / Si, LN / SiC, LT / / SiC, LN / / BN, LT / / BN, LT / / diamond and LN / / diamond.

[0022] The method can be configured so that the plasma activation process and the UV modification process form an intermediate film (also referred to as a bonding layer) at a predetermined level. The properties of the intermediate film can be controlled by the parameters of the UV modification process and the parameters of the plasma activation process that have an impact on the bonding surface of the piezoelectric substrate and the support substrate. The bonding layer can include the same components from the plasma gas used (e.g., oxygen and nitrogen) and the two substrate materials to be bonded (e.g., a wafer and a piezoelectric material wafer).

[0023] The intermediate layer may include one or more amorphous oxides and one or more amorphous nitrides. The amorphous oxides may improve the bonding quality, and the amorphous nitrides may improve the bonding strength.

[0024] The plasma activation process and the mixed gas UV surface modification process can be configured to remove impurities and organic contaminants from the substrate surface to clean the surface to be bonded. This improves the bonding quality and bonding strength between the piezoelectric substrate and the support substrate at low temperatures.

[0025] The bonding process can be performed under a low vacuum (preferably at most 0.1 Pa). In this way, water film residues are removed from the surfaces of both substrates.

[0026] For example, the bonding process is direct wafer bonding of different material combinations. Thus, high bonding strength and high efficiency bonding of Si / / Si, Si / / SiO2, LT / / SiO2, LT / / Si, LT / / quartz and LT / / sapphire (Al2O3) can be achieved at room temperature through material-dependent optimized plasma activation parameters. The plasma activation parameters may include: plasma power, plasma gas pressure, plasma duration, gas flow ratio (N2 to O2), pre-bonding process conditions (e.g. vacuum environment and mechanical pressure) as well as mixed gas UV surface modification and (post) thermal annealing processes.

[0027] The method provides surface activation using plasma surface activation of a gas mixture of O2 and N2, and mixed gas UV surface modification of two wafers to be bonded (e.g., a piezoelectric wafer (also referred to as a second substrate) and a supporting substrate wafer (also referred to as a first substrate)).

[0028] The first substrate (support substrate) includes or is formed of materials such as silicon (Si), silicon oxide (SiO2), sapphire (Al2O3), silicon carbide (SiC), cubic boron nitride (c-BN), and diamond. The second substrate (piezoelectric substrate) includes or is formed of materials such as lithium niobate (LN), lithium tantalate (LT), and quartz (SiO2). The first substrate is directly bonded to the second substrate after a plasma activation process and a UV modification process. The mixed gas plasma surface activation process and the mixed gas UV radiation modification process can bond the piezoelectric lithium niobate (LN) surface or the piezoelectric lithium tantalate (LT) surface to the support substrate. The bonding process can be used to bond different materials of the LN wafer or LT wafer to any one of Si, SiO2, c-BN, SiC, and diamond wafers under vacuum environment conditions and at room temperature.

[0029] The plasma activation process can be carried out in a plasma chamber, which encloses the first electrode and the second electrode in a housing and has an adjustable gas flow between the first electrode and the second electrode. The power at the first electrode and the second electrode can be adjusted independently of each other (also referred to as individually). The potential between the first electrode and the second electrode can form a plasma by the flow of gas molecules between the first electrode and the first electrode. Therefore, the electric power supplied to the first electrode and the second electrode can also be expressed as plasma power. For example, the plasma power of the first electrode (which can be the top electrode of the plasma chamber) can be in the range of 10W to 150W. For example, the plasma power of the second electrode (which can be the bottom electrode of the plasma chamber) can be in the range of 10W to 75W.

[0030] The treatment time (also referred to as plasma activation time) of the plasma activation process of the first substrate and / or the second substrate may be in a range of about 5 seconds to about 180 seconds, for example, in a range of about 10 seconds to about 120 seconds, respectively.

[0031] The plasma operating pressure of the plasma activation process of the first substrate and / or the second substrate may be in a range of about 10 Pa (Pa) to about 300 Pa, for example, in a range of about 20 Pa to about 100 Pa, respectively.

[0032] The bonded precursor composite substrate may be thermally annealed in a forming gas atmosphere at a temperature in a range of about 80°C to about 190°C, such as in a range of about 100°C to about 175°C.

[0033] Direct covalent bonding between the crystalline piezoelectric material of the second substrate and the material of the first substrate can achieve approximately 0.5 J / m 2 About 2.5 J / m 2 Adjustable bonding strength, e.g. 0.5 J / m 2 , 0.8J / m 2 , 1.0J / m 2 , 1.2J / m 2 , 1.5J / m 2 , 1.8J / m 2 or 2.0 J / m 2 .

[0034] The composite substrate can be one of various material combinations having covalent bonds and high bonding strength, such as LT / / Si, LT / / SiO2, LT / / SiC, LT / / c-BN and LT / / diamond, LN / / Si, LN / / SiO2, LN / / SiC, LN / / c-BN, LN / / diamond or any combination thereof.

[0035] The bonding interface of the composite substrates may be a high-quality bond, for example, the interface may be free of microvoids, outgassing, and surface structural damage.

[0036] The bonding interface of the composite substrate can have excellent thermal stability at high temperatures up to 200°C.

[0037] The method may allow for combining the first substrate and the second substrate in various commercially available wafer formats, for example supporting wafer sizes of 0.051 m, 0.102 m, 0.153 m, and 0.204 m, or even larger.

[0038] Figure 1 A schematic cross-sectional view of a composite substrate 100 is shown, comprising a first substrate 102 bonded to a second substrate 106 via a bonding layer 104. The second substrate 106 may include or may be formed of a piezoelectric material as described above. The first substrate 102 and the second substrate 106 are directly bonded. Thus, the bonding layer 104 may include a material combination of the first substrate, the second substrate 106, oxygen, and / or nitrogen.

[0039] Exemplarily, in the direct bonding interface and the sub-bonding interface, the bonding layer 104 may be divided into an oxide amorphous domain, a nitride amorphous domain, and a metal amorphous domain.

[0040] For example, the composite substrate 100 may be used to form a TF-SAW device.

[0041] The method for forming the composite substrate 100 can be improved or optimized by changing the plasma conditions: plasma power, plasma duration, plasma gas pressure below 200 Pa, mixed gas flow rate and the ratio of the two gas flow rates, and exposure to UV light (e.g., in the range of about 150nm-500nm) at low power in a mixed gas (O2+N2) atmosphere.

[0042] The composite substrates 100 of various material combinations include high bond strength, no or substantially no thermal degassing, low electrostatic charge (e.g., the bow of the composite substrate 100 may be less than 20 μm), no cracking of the bonded first and second substrates during thermal annealing at temperatures up to 200° C. and during optional mechanical thinning of the LT / LN bonded wafer portion from about 250 μm to about 2 μm film thickness without causing any damage to different wafer sizes (e.g., up to 0.153 μm wafers for the first substrate 102 and the second substrate 106).

[0043] Figure 2 It shows the use for forming Figure 1Flow chart of method 200 for preparing composite substrate 100. Method 200 may include: plasma activation process 202, which includes exposing a first surface of a first substrate to a plasma system. The plasma is a mixed gas plasma of oxygen and nitrogen at a first ambient pressure. The first ambient pressure may be lower than atmospheric pressure.

[0044] The method 200 may include a plasma activation process 204, which includes exposing a second surface of a second substrate. The plasma system may be a radio frequency system (e.g., a plasma chamber including a radio frequency or microwave generator, such that a gas plasma is generated by a gas flowing through the plasma chamber) having a plasma between a first electrode and a second electrode. The first electrode and the second electrode may be configured to be powered and controlled separately. The plasma is a mixed gas plasma of oxygen and nitrogen at a first ambient pressure. The first ambient pressure may be lower than atmospheric pressure.

[0045] Figure 4 The plasma system is described in more detail.

[0046] The method 200 may further include a surface modification process including exposing the plasma activated first surface 206 to ultraviolet radiation in an oxygen and nitrogen atmosphere at atmospheric pressure. The method 200 may further include a surface modification process including exposing 208 the plasma activated second surface 208 to ultraviolet radiation in an oxygen and nitrogen atmosphere at atmospheric pressure.

[0047] The method 200 may also include a process 210 of forming a precursor composite substrate by placing the first surface of the first substrate on the second surface of the second substrate.

[0048] The method 200 may also include a process 212 of bonding the first substrate to the second substrate by applying a mechanical load to the precursor composite substrate at a second ambient pressure.

[0049] The method may also include a process 214 of thermally annealing the bonded precursor composite substrate.

[0050] Here, the first substrate is a wafer configured to support the second substrate, which is single crystal and amorphous. The second substrate is a piezoelectric material wafer.

[0051] FIG. 3A to FIG. 3F The method for producing composite substrates is shown Figure 2 Schematic diagram of the method. Exemplarily, the method includes a general process flow for directly wafer bonding the second substrate 106 to the first substrate 102. The method may generally include the following process: exposing the first substrate 102 and the second substrate 106 to excimer light 306, 308 emitted by excimer lamps 302, 304 in an atmospheric air environment, such as Figure 3AAs shown. Excimer lamps 302, 304 can provide electromagnetic radiation (also referred to as light) having a wavelength or spectrum in the wavelength range of about 150nm to about 500nm (also referred to as ultraviolet (UV) light). Excimer light 306, 308 can be the same or different for the first substrate 102 and the second substrate 106. Therefore, organic contaminants and non-organic contaminants can be reduced or even removed.

[0052] Figure 3B It is shown that the first substrate 102 can be exposed to the mixed gas plasma activation 310 at room temperature, and the second substrate 106 can be exposed to the mixed gas plasma activation 312 at room temperature. In this way, the surface materials of the first substrate material and the second substrate material can be reduced, respectively, and the bonding layer 104 can be formed on the first surface and the second surface.

[0053] The method may include: rinsing processes 314, 316 of the plasma activated first substrate 102 and the plasma activated second substrate 106, such as Figure 3C As shown. The rinsing processes 314, 316 may include megasonic assisted deionized (DI) water rinsing, and drying the rinsed first substrate and the rinsed second substrate. In this way, particles and organic contaminants may be removed from the first surface and the second surface.

[0054] In other words, after surface activation, the first substrate 102 and the second substrate 106 can be cleaned by using a megasonic cleaning nozzle (herein, megasonic can correspond to an acoustic signal with a frequency of 700kHz to 5MHz) and a DI water cleaning nozzle, for example, in this order. The cleaned substrates 102, 106 can be placed in a spinner. The spinner can rotate the cleaned substrates to dry the substrates. Cleaning using a megasonic cleaning nozzle, a DI water cleaning nozzle, and a spinner can be integrated in a single wafer cleaning system.

[0055] like Figure 3DThe surface modification process of the method shown may include exposing the first substrate 102 and the second substrate 106 to light 318, 320 emitted by one or more excimer lamps 322, 324. The excimer light 318, 320 may be the same or different for the first substrate 102 and the second substrate 106. During the UV irradiation, the first surface of the first substrate 102 and the second surface of the second substrate 106 may be exposed to a mixture 334 of free radicals of N2 and O2 and other reactive atomic or molecular particles. The mixtures 332, 334 may be the same or different for the first substrate 102 and the second substrate 106. During the UV irradiation, the first surface of the first substrate 102 and the second surface of the second substrate 106 may be exposed to low temperatures (e.g., below 100°C). In this way, any contaminants may be removed from the first surface and the second surface. In addition, the surface energy and polarity of the first surface and the second surface may be adjusted to perform chemical reactions at the atomic or molecular level. In this way, the functional groups on the dangling bonds / side bonds are enhanced. Therefore, an increase in bonding strength at room temperature may be achieved.

[0056] The process of forming the precursor composite substrate 330 may include mechanical alignment, such as flat-to-flat or recess-to-recess alignment of the first surface with the second surface, such as Figure 3E As shown. The bonding process can be performed at room temperature in a vacuum environment at a process gas pressure of less than 0.1 Pa. The bonding process can be performed under a mechanical pressure of up to 5 kN. The mechanical pressure is directed to squeeze / compress the first substrate and the second substrate. In other words, the mechanical pressure is directed to press the first substrate into the second substrate, or vice versa.

[0057] In other words, in the process of forming the precursor composite substrate, the first substrate 102 and its first surface and the second substrate 106 and its second surface can be placed face to face in a mechanical alignment 326 (e.g., the wafer plane of the first substrate with the wafer plane of the second substrate) in a standard wafer bonder system. A standard wafer bonder system can use mechanical force pressures of up to 5 kN in a vacuum environment close to 0.1 Pa. Thus, the van der Waals forces pull the first substrate into contact with the second substrate, thereby obtaining a mechanical force of up to 0.8 J / m at room temperature. 2 A thermal annealing at a preselected temperature of 100°C to 190°C for several hours can be used to improve the bonding strength to greater than 1.2 J / m 2 .

[0058] The thermal annealing process 328 (also referred to as post thermal annealing) may be performed in a standard forming gas environment furnace and / or on a hot plate, in one or more temperature cycles, at one or more temperatures up to 200° C., such as Figure 3F In this way, the bonding strength can be improved, for example, the bonding layer 104 (see Figure 1 )’s cohesion.

[0059] A surface modification process including ambient UV light exposure may be an additional process applied to clean most organic contaminants of the first and second surfaces. The UV light exposure may include, for example, excimer light having a wavelength below 400 nm.

[0060] UV light exposure can be performed under normal air atmosphere. UV light exposure may destroy or be configured to destroy the molecular bonds of organic substances. In this way, UV light exposure can reduce various hydrocarbons at the first surface and / or the second surface, for example, before plasma activation.

[0061] Figure 4 A schematic diagram of a dual RF capacitively coupled plasma system 400 that can be used for mixed gas plasma activation of a wafer surface is shown.

[0062] The plasma system 400 can have a conventional horizontal capacitor parallel dual electrode, which includes a first electrode 404 and a second electrode 406. The first electrode 404 and the second electrode 406 can be powered and / or controlled by one or more RF power supplies 408 and 410 and one or more controllers (not shown), respectively. The RF power supplies 408 and 410 can provide RF power to the electrodes 404, 406 at different frequencies in the kHz range. For the first electrode and the second electrode, the plasma power can be in the range of about 10W to about 300W. The plasma power may vary slightly depending on the different process gas mixtures.

[0063] As an example, a single wafer of the first substrate 102 and the second substrate 106 can be placed on the second electrode 406, for example, the bottom electrode 406 of the plasma system 400 within the plasma chamber 402. A mixture 418 of gaseous oxygen 412 and gaseous nitrogen 414 is provided to the plasma chamber through an adjustable valve system 416, which provides flow rate control for each of the oxygen 412 and nitrogen 414. The RF power at the electrodes 404, 406 is adjustable to form the plasma 310 and / or 312 from the gas mixture 418. The surfaces to be bonded of the substrates 102, 106 (e.g., the first surface of the first substrate or the second surface of the second substrate) can be exposed to the plasma mixture 310 and / or 312 of oxygen 412 and nitrogen 414 for a short time. The duration of this time period can be from about 5 seconds to about 120 seconds. The duration may depend on the best known method formulation (BKM).

[0064] The mixing of gases (e.g., oxygen 412 and nitrogen 414) in the plasma chamber 402 can be performed by controlling the flow rates of the respective gases 412, 414 forming the gas mixture 418 via the valve system 416. The flow rates of the oxygen 412 and the nitrogen 414 can be about 5 standard cubic centimeters per minute (sccm) to about 100 sccm. At the same time, the gas pressure in the plasma chamber 402 can be controlled during plasma activation, for example, by a suction capacity throttle valve (not shown) in a vacuum pumping system. The gas pressure can be about 10 Pa to about 300 Pa. Depending on the materials of the first substrate and the second substrate, the concentration flow rate ratio of the N2 gas to the O2 gas can be about 5% to about 95%, for example, 10%, 15%, 20%, 25%, 30%, 50%, 75%, 95%, respectively.

[0065] UV light exposure in a mixed gas environment 318 can be used to improve the bonding strength at room temperature and reduced annealing temperatures. Exposure to UV light (e.g., with a wavelength of about 150 nm to about 500 nm) (e.g., using an excimer lamp) can be performed under normal pressure and a mixed gas N2 / O2 (e.g., 50% / 50% - it should be noted that this ratio can vary depending on the situation) atmosphere. In this case, the mixed gas can provide oxygen and nitrogen as reagents in the reaction between the piezoelectric material of the second substrate and the material of the first substrate. Therefore, activated groups, such as hydroxyl groups (-OH), can be generated on the surfaces of the first substrate and the second substrate. Therefore, the polarity and surface energy of the first surface of the first substrate and the second surface of the second substrate can be increased. UV light exposure can be performed in a processing chamber at atmospheric pressure.

[0066] Infrared analysis and scanning acoustic microscopy of the bonded precursor composite substrates show a bond interface, such as the bond layer described above, that is generally free of detectable voids (also referred to as microvoids) that are typically caused by thermal outgassing.

[0067] FIG. 5A to FIG. 5D AFM images 500, 502, 508, 510 are shown, including Figure 3B The linear scan height distributions 504, 506, 512, 514 of the materials shown after mixed gas (O2+N2) plasma activation 310 or 312, for example, BKM activation is performed on each material using a BKM formulation, and after mixed gas (O2+N2) plasma activation Figure 5A The silicon (Si) surface shown, Figure 5B Thermal silicon dioxide (SiO2) film (0.5 μm thick) on the Si wafer shown, Figure 5C The lithium tantalate surface and Figure 5DLinear scan height distribution of a quartz surface is shown. Despite the presence of individual scratches, the RMS roughness of all substrates may be well below 0.5 nm, as shown in linear scan height distributions 504, 506, 512, 514. Smooth surfaces with a root mean square (RMS, Rq) roughness of about 0.5 nm or less may be preferred for bonding.

[0068] Figure 6 Scanning acoustic microscope (SAM) images of a first example of a composite substrate are shown. The first example includes Si / / Si wafer bonding of a 0.204 μm wafer. Here, Si / / Si wafer bonding is performed using plasma activation with a mixed gas concentration by using a BKM recipe, a gas flow rate of less than 100 sccm, a gas pressure of up to 100 Pa, and a plasma power of the first electrode and the second electrode of less than 50 W. The process before the bonding process (also called a pre-bonding process) can be performed under the same conditions (mechanical pressure of 5 kN (piston downward)) in a vacuum at room temperature, followed by a 2-hour post-bonding annealing at 300°C. Figure 6 The SAM image of the composite wafer pre-bonded in vacuum is shown. This may be contrasted with the pre-bonding in atmospheric pressure environment, the high-quality bonding interface does not have any micro voids or any thermal degassing across the bonding interface, and the bond strength can be increased to 2.0 J / m 2 .

[0069] Figure 7 A scanning acoustic microscope (SAM) image of a second example of a composite substrate is shown. The second example includes: bonding Si / / SiO2 wafers (both with a diameter of 0.204 μm) by using a mixed gas plasma activation process using a BKM formulation, a plasma treatment gas pressure of less than 50 Pa, a low plasma power of less than 100 W for the first electrode and the second electrode, respectively, and a pre-bonding process in vacuum under the same conditions at room temperature, followed by post-annealing at 300°C for 2 hours. Except for some small treatment particles in the edge bonding area, there is basically no micro-void or thermal degassing on the interface of the two bonded wafers (e.g., the first substrate and the second substrate). After post-thermal annealing, the bonding strength can be increased to 1.6 J / m 2 .

[0070] Figure 8A scanning acoustic microscope (SAM) image of a third example of a composite substrate is shown. The composite substrate includes LiTaO3(LT) as a second substrate and Si as a first substrate. The picture shown shows the composite substrate after thermal annealing at 175°C. The composite substrate can be produced and evaluated according to the same procedure as Example 1. The precursor composite substrate can be bonded under a mechanical pressure of 2.0 kN in a vacuum environment at 0.1 Pa at room temperature. The entire area of ​​LiTaO3(LT) can be fully bonded. After annealing at 175°C for 2 hours, a void-free interface can be observed. After annealing at 175°C for 5 hours, the bonding strength can be 1.27 J / m 2 The second substrate may be thinned from a thickness of about 250 μm to about 400 μm to a thinned thickness of about 1 μm to 250 μm, for example, about 2 μm to 10 μm.

[0071] Fig. 9 A scanning acoustic microscope (SAM) image of a fourth example of a composite substrate 900 is shown. The composite substrate includes an LT wafer as a second substrate, a Si wafer as a first substrate, and has a thermal oxide (e.g., 500 nm thickness) after thermal annealing at 150°C. In the fourth example, a 0.153 μm wafer combining the first substrate and the second substrate can be produced and evaluated according to the same procedure as Example 2. Here, the material of the piezoelectric single crystal substrate (second substrate) can be lithium tantalate (LT), and the Si handle wafer can be covered with 500 nm of thermal oxide (first substrate) to prepare it for use as an RF speed layer as a support material. Fig. 9 Scanning acoustic microscopy (SAM) images of the bonding interface of LT / / SiO2 bonding at room temperature (RT) and after thermal annealing at 150°C for 2 hours are shown. The entire area of ​​the wafer pair can be fully bonded. The measured bonding strength can be 1.1 J / m 2 . Numerous small microbubbles were observed from the inspection of the bonding interface by SAM measurements, which also occurred when thermal oxide wafer bonding was performed in vacuum. However, it was observed that in the case of Si wafers with sputter-deposited oxide (100nm-1000nm thickness), there was no degassing and bubbles after thermal annealing at 150°C for 5 hours. The second substrate can be thinned from a thickness of about 250μm to about 400μm to a thickness of about 1μm to 250μm after thinning, for example about 2μm to 10μm.

[0072] Fig. 10A and Fig. 10B shows an infrared (IR) transmission image of a bonded composite substrate comprising a quartz wafer ( Fig. 10A ) and sapphire wafers ( Fig. 10B) includes a LiTaO3 wafer as a second substrate. The bonded 0.102m wafer can be produced and evaluated according to the same procedure as Example 3. In this example, the piezoelectric material of the second substrate can be a 0.204m single crystal lithium tantalate (LT) wafer, and the first substrate can be 0.204m quartz (fused silica) and 0.204m sapphire (Al2O3), respectively. The composite substrate has been pre-bonded in a vacuum environment, at room temperature, under a mechanical pressure of 2kN, and then thermally annealed at a temperature of <200°C for 5 hours. The bonded composite substrate shows high bonding quality, without macroscopic voids and thermal microscopic voids formed before and after annealing. The bonding strength can be 1.3J / m 2 The second substrate may be thinned from a thickness of about 250 μm to about 400 μm to a thinned thickness of about 1 μm to 250 μm, for example, about 2 μm to 10 μm.

[0073] Fig.11A and Fig. 11B shows the thinning and polishing process 1120 ( Fig.11A ) is a schematic diagram of a method for producing a piezoelectric material as a SiC wafer composite substrate. Here, the second substrate 106 has a first thickness 1110. Fig. 11B As shown, by thinning and polishing process 1120, the thickness 1110 of the second substrate 106 can be reduced to a second thickness 1112. The second thickness 1112 can be about 1 μm to about 250 μm, for example, about 2 μm to about 10 μm. The thinned composite substrate 1100 may include a piezoelectric material of silicon carbide (SiC), and its bonding surface may include a Si surface. Wafer bonding can be produced and evaluated according to the same procedure as in Example 3 described above. However, the material of the piezoelectric single crystal substrate may include a lithium tantalate (LT) single crystal, and the material of the first substrate 102 may include a 4H-SiC substrate.

[0074] Fig. 12A and Fig. 12B shows the thinning and polishing process 1120 ( Fig. 12A ) is a schematic diagram of a method for producing a piezoelectric material as a thin film c-BN or diamond wafer composite substrate (e.g., including a first substrate made of silicon and a thin layer of c-BN or diamond). Here, the second substrate 106 has a first thickness 1210. Fig. 12B As shown, through the thinning and polishing process 1210, the thickness 1210 of the second substrate 106 can be reduced to a second thickness 1212. The second thickness 1212 can be about 1 μm to about 250 μm, for example, about 2 μm to about 10 μm.

[0075] The composite substrate 100 may include a piezoelectric material of a second substrate 106, the piezoelectric material of the second substrate 106 being bonded to a first substrate, the first substrate also having, for example, a c-BN layer 1204 or a thin diamond layer 1204 (e.g., with a thickness of less than 1 μm). In other words, the composite substrate 100 may include a thin film of a c-boron nitride layer 1204 or a diamond layer 1204. The c-BN layer 1204 may also be deposited using a physical vapor deposition (PVD) method, wherein the c-BN layer 1204 may be deposited by radio frequency magnetron sputtering (RFMS). A c-BN film having a thickness of about 1.1 μm may be deposited on a first substrate 102 having a very smooth surface, such as a Si substrate. The composite substrate 100 may be produced and evaluated according to the same procedure as in Example 2, the mixed gas plasma may be activated based on a high plasma power in a nitrogen / oxygen mixture at a ratio of 1:1 (O2:N2), and the total gas flow rate is less than 50 sccm. The bonding layer 104 can be very uniform and can be in the range of 10.0 nm in thickness. The bonding layer 104 can include a large portion of amorphous nitride from the mixed gas activation process and mixed gas UV surface modification, thereby increasing the bonding strength to 0.8 J / m 2 Here, post-heat annealing at temperatures above 200°C increased the bond strength to 1.8 J / m 2 .

[0076] The diamond layer 1204 can also be deposited on the silicon substrate 102 by a PVD method. The layer thickness of the diamond film 1204 can be about 2.0 μm at most. The diamond layer 1204 can be polished using ion beam trimming to achieve a surface roughness (RMS) below 0.5 nm. Wafer bonding can be produced and evaluated according to the same procedure as the above-mentioned embodiment. The mixed gas plasma can be activated based on the following conditions: high plasma power, long-term plasma activation in a nitrogen / oxygen mixture at a ratio of 1:1 (O2:N2), and a total gas flow rate of less than 75 sccm, the "long time" is less than 120 seconds, and mixed gas UV surface modification is used. The bonding layer 104 can be very uniform and the thickness can be about 15.0 nm at most. According to the mixed gas plasma activation of the first surface and the second surface to be bonded, the bonding layer 104 can include a large part of amorphous nitride, thereby improving the bonding strength without using any heating. Here, post-thermal annealing at a temperature above 200° C. can be used to improve the bonding strength.

[0077] Exemplarily, lithium tantalate and lithium niobate single crystal substrates can be used for acoustic wave filters that can have low thermal conductivity. The present invention provides a surface activation process by using mixed gas (O2+N2) plasma and UV surface modification under a mixed gas atmosphere (O2+N2), which can show an excellent bonding layer between bonded wafers of a composite substrate, and provides a method for preparing a thin film bonded wafer. The plasma activation method and the UV surface modification method can be used to directly bond a first substrate such as silicon (Si), silicon oxide (SiO2), sapphire (Al2O3), silicon carbide (SiC), cubic boron nitride (c-BN) and diamond to a second substrate such as lithium niobate (LN), lithium tantalate (LT), quartz (SiO2).

[0078] Plasma surface activation processes can be used to bond lithium tantalate (LT) and lithium niobate (LN) surfaces to a variety of substrates.

[0079] The bonding method can be used to bond different materials of LN wafers and LT wafers to Si, SiO2, sapphire, c-BN and SiC substrates (e.g., diameters of 0.051m, 0.102m, 0.153m and 0.204m) in a vacuum environment at room temperature.

[0080] The mixed gas plasma process can be used for surface activation of all second substrates and the first substrate, and the plasma power of the first electrode of the plasma system is 10W to 150W, and the plasma power of the second electrode of the plasma system is 10W to 150W.

[0081] The mixed gas plasma process for surface activation can be used for all the second substrates and the first substrate, and the plasma duration (time) is 5 seconds to 180 seconds.

[0082] The mixed gas plasma process for surface activation of the second substrate and the first substrate may be used with a gas pressure plasma of 10 Pa to 200 Pa.

[0083] The mixed gas plasma process for surface activation of all second substrates and first substrates may be used for post thermal annealing in a forming gas atmosphere at 100° C. to 200° C.

[0084] The method provides a composite substrate having a high quality bonding interface without macro-voids and micro-voids, strong bonding, no thermal degassing, and no surface structural damage.

[0085] The composite substrate can have excellent thermal stability at high temperatures up to 250° C. Therefore, a thin film surface acoustic wave (TF-SAW) device that can be manufactured efficiently can be provided.

[0086] The method can provide bonding for wafers of different sizes, for substantially the entire wafer of the first substrate and the second substrate. In other words, the method for forming the composite substrate can include: a plasma activation process, which can include exposing the first surface of the first substrate and the second surface of the second substrate to a plasma system, respectively, wherein the plasma system can be a radio frequency system, the radio frequency system having a plasma between the first electrode and the second electrode which can be powered separately, and the plasma can be a mixed gas plasma of oxygen and nitrogen at a first ambient pressure which can be lower than atmospheric pressure; a surface modification process can include exposing the plasma activated first surface and the plasma activated second surface to ultraviolet radiation in an oxygen and nitrogen atmosphere at atmospheric pressure; a process of forming a precursor composite substrate by placing the first surface of the first substrate on the second surface of the second substrate, a process of bonding the first substrate to the second substrate by applying a mechanical load on the precursor composite substrate at a second ambient pressure; and a process of thermally annealing the bonded precursor composite substrate. The first substrate can be a wafer configured to support the second substrate, which can be single crystal and amorphous, and wherein the second substrate can also be a piezoelectric material wafer.

[0087] The second ambient pressure may be atmospheric pressure. The second ambient pressure may be about 0.1 Pa to about 10 -3 Pa vacuum pressure.

[0088] The method may further include polishing the first surface and the second surface to ensure that their root mean square roughness is less than 0.5 nm respectively.

[0089] The method may include a plasma power for the first electrode of about 10 W to about 300 W. The method may include a plasma power for the second electrode of about 10 W to about 300 W. The one or more time periods of plasma activation time period may be a time period of about 5 seconds to about 180 seconds.

[0090] The mixed gas plasma may include a gas flow ratio of nitrogen flow to oxygen flow of about 0.01 to about 0.99. The gas flow of the mixed gas plasma may be about 5 sccm to about 100 sccm. The first ambient pressure may be about 10 Pa to about 200 Pa. The method may also include a rinsing process, which may include megasonic assisted deionized (DI) water rinsing and drying the first and second surfaces of the plasma activation. The surface modification process may include a rinsing process. Exposure to ultraviolet radiation may be performed before the rinsing process. Alternatively, exposure to ultraviolet radiation may be performed after the rinsing process.

[0091] Ultraviolet radiation may include electromagnetic radiation having a wavelength within a wavelength range of about 150 nm to about 500 nm.

[0092] During the ultraviolet radiation, the temperature of the first surface and the second surface may be less than about 100°C.

[0093] Mechanical loading may include piston downforce of up to 5 kN.

[0094] The thermal annealing process may include one or more temperature cycles of the bonded precursor composite substrate at temperatures of 100°C, 120°C, 150°C, 175°C, 190°C, and 250°C.

[0095] The piezoelectric material wafer of the second substrate may include a piezoelectric single crystal selected from the group consisting of lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof.

[0096] In addition to the second substrate, the method may further include: a third substrate bonded to the first substrate, wherein the third substrate may be a piezoelectric material wafer different from the piezoelectric material of the second substrate. The piezoelectric material wafer of the third substrate may include a piezoelectric single crystal selected from the group consisting of lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof.

[0097] The wafer of the first substrate may include a material substrate selected from the group consisting of silicon (Si), silicon dioxide (SiO2), silicon carbide (SiC), cubic boron nitride (c-BN), sapphire, diamond, and any combination thereof.

[0098] The term "exemplary" is used herein to mean "serving as an example, instance, or illustration." Any aspect or design described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other aspects or designs. The term "exemplary" is used herein to mean "serving as an example, instance, or illustration." Any example or design described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other examples or designs.

[0099] "Multiple" and "plurality" in the specification or claims clearly refer to a quantity greater than one. The terms "group", "set", "series", "sequence", "combination", etc. in the specification or claims refer to a quantity equal to or greater than 1, i.e., one or more. Any term expressed in plural form without explicitly indicating "multiple" and "plurality" also refers to a quantity equal to or greater than 1.

[0100] For example, the term "processor" or "controller" used herein can be understood as any type of technical entity that allows processing data. Data can be processed according to one or more specific functions performed by a processor or controller. In addition, the processor or controller used herein can be understood as any type of circuit, such as any type of analog or digital circuit. Therefore, the processor or controller can be as follows or include the following: analog circuit, digital circuit, mixed signal circuit, logic circuit, processor, microprocessor, central processing unit (CPU), graphics processing unit (GPU), digital signal processor (DSP), field programmable gate array (FPGA), integrated circuit, application specific integrated circuit (ASIC), etc. or any combination thereof. Any other type of implementation of each function can also be understood as a processor, controller or logic circuit. It should be understood that any two (or more) of the processors, controllers or logic circuits described in detail herein can be regarded as a single entity with equivalent functions, etc., on the contrary, any single processor, controller, or logic circuit described in detail herein can be regarded as two (or more) separate entities with the same functions, etc.

[0101] The term "connected" may be understood as, for example, directly or indirectly connected and / or interacting (e.g., mechanically and / or electrically). For example, multiple components / elements may be connected together mechanically [so that they are physically held (e.g., a plug connected to a socket)] and electrically [so that they have a conductive path (e.g., a signal path exists along a communication link)].

[0102] Although the above description and drawings may describe electronic device components as separate components / elements, those skilled in the art will appreciate the various possibilities of combining or integrating discrete components / elements into a single component / element. This may include: combining two or more circuits in a single circuit together; mounting two or more circuits onto a common chip or chassis to form an integrated component / element; executing discrete software components on a common processor core, etc. On the contrary, those skilled in the art will recognize the possibility of dividing a single component / element into two or more discrete components / elements, such as dividing a single circuit into two or more separate circuits, dividing a chip or chassis into discrete components / elements originally provided thereon, dividing a software component into two or more parts, and executing each part on a separate processor core, etc. In addition, it should be understood that the specific implementation of the hardware and / or software components is merely illustrative, and other combinations of hardware and / or software for performing the methods described herein are also within the scope of the present disclosure.

[0103] It should be understood that the implementation of the methods described in detail herein is exemplary in nature and is therefore understood to be implemented in the corresponding devices. Similarly, it should be understood that the implementation of the devices described in detail herein is understood to be implemented as the corresponding methods. Therefore, it is understood that the devices corresponding to the methods described in detail herein may include one or more components that are configured to perform each aspect of the related methods.

[0104] All abbreviations defined in the above description also apply to all claims contained herein.

[0105] Although the present disclosure has been specifically shown and described with reference to specific embodiments, it will be understood by those skilled in the art that various changes may be made in form and detail without departing from the spirit and scope of the present disclosure as defined in the appended claims. Therefore, the scope of the present disclosure is indicated by the appended claims, and therefore it is intended to include all variations that fall within the equivalent meaning and scope of the claims.

Claims

1. A method for forming a composite substrate, the method comprising: A mixed gas plasma activation process of oxygen and nitrogen, which includes exposing the surface of the wafer and the surface of the piezoelectric material wafer to a plasma system; exposing the plasma activated surface of the wafer and the plasma activated surface of the piezoelectric material wafer to ultraviolet radiation in an oxygen and nitrogen atmosphere; placing a surface of the wafer on a surface of a wafer of piezoelectric material; applying a mechanical load to the wafer and the piezoelectric material wafer; and thermally annealing the bonded wafer and the piezoelectric material wafer; Wherein, the wafer is configured to support the piezoelectric material wafer.

2. The method of claim 1, further comprising: The surface of the wafer and the surface of the piezoelectric material wafer are polished so that the root mean square roughness of the wafer surface and the surface of the piezoelectric material wafer is less than 0.5 nm respectively.

3. The method according to any one of claims 1 to 2, wherein: The gas flow ratio of the nitrogen gas flow rate to the oxygen gas flow rate in the atmosphere is 0.01 to 0.

99.

4. The method according to any one of claims 1 to 3, wherein: The gas flow rate of the atmosphere is about 5 sccm to 100 sccm.

5. The method according to any one of claims 1 to 4, wherein: Plasma activation includes an ambient pressure of about 10Pa to 200Pa.

6. The method according to any one of claims 1 to 5, further comprising: A rinsing process including a megasonic-assisted deionized (DI) water rinse; and drying the plasma activated surface of the wafer and the plasma activated surface of the piezoelectric material wafer.

7. The method of claim 6, wherein: Surface modification includes a rinsing process.

8. The method according to claim 6 or 7, wherein: The exposure to UV radiation is performed prior to the rinsing process.

9. The method according to claim 6 or 7, wherein: The exposure to UV radiation is performed after the rinsing process.

10. The method according to any one of claims 1 to 9, wherein: Ultraviolet radiation includes electromagnetic radiation having a wavelength in the range of about 150 nm to 500 nm.

11. The method according to any one of claims 1 to 10, wherein: During the UV light irradiation, the temperature of the wafer surface and the piezoelectric material wafer surface is lower than 100°C.

12. The method according to any one of claims 1 to 11, wherein: The mechanical load consists of a piston downforce of up to 5 kN.

13. The method according to any one of claims 1 to 12, wherein: The piezoelectric material wafer includes a piezoelectric single crystal selected from the group consisting of lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof.

14. The method of any one of claims 1 to 13, further comprising bonding another piezoelectric material wafer to the wafer, wherein: The piezoelectric material of the another piezoelectric material wafer is different from the piezoelectric material of the piezoelectric material wafer.

15. The method of claim 14, wherein: The piezoelectric material of the another piezoelectric material wafer includes a piezoelectric single crystal selected from the group consisting of lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof.

16. The method according to any one of claims 1 to 15, wherein: The wafer includes a material selected from the group consisting of silicon (Si), silicon dioxide (SiO2), silicon carbide (SiC), cubic boron nitride (c-BN), sapphire, diamond, and any combination thereof.

Citation Information

Patent Citations

  • A method for directly bonding lithium niobate and silicon wafers using a two-step activation process: vacuum ultraviolet light followed by nitrogen plasma.

    CN109166793B

  • A wafer bonding method and a corresponding method for fabricating heterostructure substrates.

    CN109786229B

  • Bonding method

    WO2017163722A1