Carbon material and preparation method thereof, and secondary battery and electric device containing carbon material

CN119072801AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280095093.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-12-03
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

Existing secondary batteries have deficiencies in balancing high first Coulombic efficiency, cycle performance and storage performance. In particular, high-capacity graphite is difficult to meet these requirements at the same time, resulting in irreversible capacity loss and poor battery performance.

Method used

Provide a carbon material with a specific pore structure and Raman spectrum ratio (0.150≤ID/IG≤0.280). By adjusting the pore area ratio and layer spacing of the inner and outer regions of the carbon material, the risk of particle breakage and side effects are reduced. reaction, improving the stability of the electrolyte and the transmission performance of active ions.

Benefits of technology

It effectively reduces the irreversible capacity loss of secondary batteries, improves the first Coulomb efficiency and cycle performance, enhances storage performance, and enables batteries to take into account high energy density and long life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072801A_ABST
    Figure CN119072801A_ABST
Patent Text Reader

Abstract

The invention provides a carbon material and a preparation method thereof, and a secondary battery and an electric device containing the carbon material, the carbon material comprises a pore structure, the carbon material satisfies the condition that ID / IG is greater than or equal to 0.150 and less than or equal to 0.280, ID represents the D peak intensity of the Raman spectrum of the carbon material at 1350 + / -50 cm <-1 >, and IG represents the G peak intensity of the Raman spectrum of the carbon material at 1580 + / -50 cm <-1 >. According to the carbon material provided by the invention, the secondary battery can give consideration to high initial coulombic efficiency, high energy density and good cycle performance and storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

Carbon material and preparation method thereof, as well as secondary battery and electric device containing the same Technical Field

[0001] The present application belongs to the field of battery technology, and specifically relates to a carbon material and a preparation method thereof, as well as a secondary battery and an electrical device containing the same. Background Art

[0002] In recent years, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. As the application scope of secondary batteries becomes wider and wider, people have put forward severe challenges to the performance of secondary batteries, such as requiring secondary batteries to take into account various performance factors such as energy density and service life. The negative electrode active material is an important component of the secondary battery, which affects the performance of the secondary battery. At present, the negative electrode active material mainly includes graphite. However, the problem faced in the existing technology is that it is difficult for high-capacity graphite to take into account high first coulomb efficiency, and it is also difficult for the secondary battery to take into account good cycle performance and storage performance.

[0003] Summary of the Invention

[0004] The purpose of the present application is to provide a carbon material and a preparation method thereof, as well as a secondary battery and an electrical device containing the same, which can enable the secondary battery to have high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0005] In a first aspect, the present application provides a carbon material, wherein the carbon material comprises a pore structure and the carbon material satisfies 0.150≤I D / I G ≤0.280, I D The Raman spectrum of the carbon material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the carbon material is 1580±50cm -1 The G peak intensity at .

[0006] The carbon material provided in this application can effectively reduce the irreversible capacity loss of secondary batteries and improve the capacity utilization characteristics of secondary batteries, so that the secondary batteries can have high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0007] In any embodiment of the present application, 0.152≤I D / I G ≤0.280, optionally, 0.155≤I D / I G ≤0.220. When further adjusting the I D / IG Within the above range, the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0008] In any embodiment of the present application, the carbon material comprises one or more pores with an area greater than or equal to 0.15 μm 2 The pore structure may include one or more pores with an area of ​​0.15 μm 2 -2.0μm 2 When the carbon material includes a pore structure with the above-mentioned pore area, the pore structure can reserve the required expansion space for the volume change of the carbon material particles, thereby further reducing the risk of carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance and storage performance of the secondary battery.

[0009] In any embodiment of the present application, the carbon material includes an external region and an internal region located inside the external region, the external region refers to the region extending from the particle surface of the carbon material to the interior of the particle by a distance of 0.25L, L refers to the short axis length of the carbon material particle, the total pore area of ​​the external region is recorded as S1, the total pore area of ​​the internal region is recorded as S2, and S2>S1.

[0010] In any embodiment of the present application, 1.5≤S2 / S1≤450, optionally, 2≤S2 / S1≤400.

[0011] When S2 / S1 is within the above range, the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0012] In any embodiment of the present application, 0.01 μm 2 ≤S1≤5.0μm 2 , optionally, 0.02 μm 2 ≤S1≤4.5μm 2 When the total pore area of ​​the outer region of the carbon material is within the above range, on the one hand, the carbon material particles can have a more stable structure, and the electrolyte can be prevented from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions and reducing the consumption of active ions by the formation of the SEI film inside the carbon material particles. On the other hand, it will not affect the transmission performance of active ions and electrons.

[0013] In any embodiment of the present application, 2.5 μm 2 ≤S2≤25.0μm 2 , optionally, 3.0 μm 2 ≤S2≤22.5μm2 When the total pore area of ​​the internal region of the carbon material is within the above range, on the one hand, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, reducing the risk of carbon material particles breaking to produce new interfaces, reducing the occurrence of side reactions on the new interface surface, and reducing the consumption of active ions by the formation of the SEI film on the new interface surface. On the other hand, it can also improve the capacity and first coulombic efficiency of the carbon material.

[0014] In any embodiment of the present application, L≥4 μm, optionally, 4 μm≤L≤20 μm.

[0015] In any embodiment of the present application, the area of ​​the pore structure in the outer region of the carbon material is less than or equal to 0.15 μm 2 , can be selected to be less than or equal to 0.10μm 2 By controlling the area of ​​the pore structure in the outer region of the carbon material within the above range, the outer region of the carbon material can have a dense structure, thereby effectively improving the structural stability of the carbon material and preventing the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby effectively improving the cycle performance and storage performance of the secondary battery.

[0016] In any embodiment of the present application, the inner region of the carbon material includes one or more areas greater than or equal to 0.15 μm 2 The pore structure may optionally include one or more pores with an area of ​​0.15 μm 2 -2.0μm 2 By making the internal area of ​​the carbon material include a pore structure of the above area, on the one hand, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, reducing the risk of carbon material particle breakage, and on the other hand, the compaction density of the carbon material can be increased.

[0017] In any embodiment of the present application, the interlayer spacing of the outer region of the carbon material is denoted as d1, and the interlayer spacing of the inner region of the carbon material is denoted as d2, and the carbon material satisfies d1 ≥ d2, and optionally, d1 > d2. The larger interlayer spacing of the outer region of the carbon material is more conducive to the rapid insertion and extraction of active ions, thereby further improving the kinetic performance of the secondary battery; the smaller interlayer spacing of the inner region of the carbon material is conducive to improving the gram capacity and compaction density of the carbon material, thereby further improving the energy density of the secondary battery.

[0018] In any embodiment of the present application, d1 is 0.33565 nm-0.33620 nm.

[0019] In any embodiment of the present application, d2 is 0.33557 nm-0.33589 nm.

[0020] In any embodiment of the present application, the specific surface area of ​​the carbon material is ≤2.1m 2 / g, optional 0.7m 2 / g-1.8m 2 The carbon material of the present application has a low specific surface area and low surface activity, thereby reducing the consumption of active ions in SEI film formation, improving the first coulombic efficiency of the carbon material, and also improving the cycle performance and storage performance of the secondary battery.

[0021] In any embodiment of the present application, the volume distribution particle size Dv50 of the carbon material is 6.0 μm-30.0 μm, and can be optionally 8.0 μm-25.0 μm.

[0022] In any embodiment of the present application, the volume distribution particle size Dv90 of the carbon material is 16.0 μm-45.0 μm, and can be optionally 17.0 μm-42.0 μm.

[0023] When the volume distribution particle size Dv50 and / or Dv90 of the carbon material is within the above range, it is beneficial to improve the transport performance of active ions and electrons, thereby further improving the cycle performance and kinetic performance of the secondary battery.

[0024] In any embodiment of the present application, the particle size distribution of the carbon material (Dv90-Dv10) / Dv50 is ≤1.55, and can be optionally 0.5-1.50, which is beneficial to improving the compaction density of the carbon material, thereby further improving the energy density of the secondary battery.

[0025] In any embodiment of the present application, the powder resistivity of the carbon material at a pressure of 8 MPa is 0.006 Ω.cm-0.051 Ω.cm, and optionally 0.010 Ω.cm-0.040 Ω.cm. When the powder resistivity of the carbon material is within the above range, it is beneficial to improve the electron transport performance, thereby further improving the cycle performance and kinetic performance of the secondary battery.

[0026] In any embodiment of the present application, the powder compaction density of the carbon material under a pressure of 20000N is 1.70g / cm 3 -1.95g / cm 3 , optional 1.72g / cm 3 -1.92g / cm 3 When the compaction density of the carbon material powder is within the above range, the compaction density of the negative electrode sheet can be increased, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.

[0027] In any embodiment of the present application, the tap density of the carbon material is 0.80 g / cm 3 -1.35g / cm 3 , optional 0.85g / cm 3 -1.30g / cm 3 When the tap density of the carbon material is within the above range, it can increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.

[0028] In any embodiment of the present application, the gram capacity of the carbon material is 350 mAh / g-372 mAh / g, and optionally 353 mAh / g-371 mAh / g. When the gram capacity of the carbon material is within the above range, the energy density of the secondary battery can be improved.

[0029] In any embodiment of the present application, the graphitization degree of the carbon material is 92.0%-98.0%, and optionally 92.5%-97.6%. When the graphitization degree of the carbon material is within the above range, it is beneficial for the secondary battery to have high energy density and good cycle performance, storage performance, and dynamic performance.

[0030] In any embodiment of the present application, the morphology of the carbon material includes one or more of block, spherical and quasi-spherical.

[0031] The second aspect of the present application provides a method for preparing a carbon material, comprising the following steps: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and a filler material in a predetermined proportion, and then maintaining the mixture at a first temperature T1 for a first time t1 to obtain an intermediate; step 3, maintaining the obtained intermediate at a second temperature T2 for a second time t2 to obtain a carbon material, wherein the carbon material includes a pore structure and satisfies 0.150≤I D / I G ≤0.280, I D The Raman spectrum of the carbon material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the carbon material is 1580±50cm -1 The G peak intensity at .

[0032] In any embodiment of the present application, the raw material includes natural graphite. Optionally, the natural graphite includes one or more of flake graphite, natural spherical graphite and microcrystalline graphite.

[0033] In any embodiment of the present application, the volume distribution particle size Dv50 of the raw material is 6.0 μm-30.0 μm, and can be optionally 8.0 μm-25.0 μm.

[0034] In any embodiment of the present application, the specific surface area of ​​the raw material is ≥2.5m 2 / g, optional 2.5m 2 / g-10.0m 2 / g.

[0035] In any embodiment of the present application, the softening point temperature of the filling material is 100°C-180°C, and can be optionally 120°C-160°C.

[0036] In any embodiment of the present application, the coking value of the filler material is 25%-50%, and optionally 30%-42%.

[0037] In any embodiment of the present application, the volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be optionally 1 μm-5 μm.

[0038] In any embodiment of the present application, the filling material includes one or more of coal tar, petroleum asphalt, polymer compounds and resins, and can optionally include one or more of coal tar and petroleum asphalt.

[0039] In any embodiment of the present application, the mass ratio of the filler material to the raw material is (10-32):100, and can be optionally (15-25):100.

[0040] By adjusting the type, softening point, coking value, addition amount and other parameters of the filling material within the above range, the viscosity of the filling material is not high after being heated and melted, and good fluidity is maintained. At the same time, it is not easy to adhere to the raw material particles, which can reduce the agglomeration of the raw material particles in the subsequent preparation process, thereby reducing problems such as increased surface defects of carbon material particles and increased surface active sites due to the depolymerization process.

[0041] In any embodiment of the present application, the heating process of uniformly mixing the raw material and the filling material in a predetermined ratio and then heating to the first temperature T1 is a staged heating process, which may optionally include a first heating process, a second heating process and a third heating process.

[0042] In any embodiment of the present application, the first temperature raising process is to raise the temperature to 200° C.-250° C. and keep the temperature at this temperature for 1 hour-2 hours.

[0043] In any embodiment of the present application, the second temperature rising process is to raise the temperature to 450° C.-550° C. and keep the temperature at this temperature for 1 hour-2 hours.

[0044] In any embodiment of the present application, the third temperature raising process is to raise the temperature to the first temperature T1 and keep the temperature at the first time t1.

[0045] In any embodiment of the present application, the temperature is increased to the first temperature T1 at a rate of 1°C / min-10°C / min.

[0046] In any embodiment of the present application, the first temperature T1 is 700°C-1200°C, and can be optionally 720°C-1100°C.

[0047] In any embodiment of the present application, the first time t1 is 1 hour to 5 hours, and can be optionally 2 hours to 4 hours.

[0048] By adjusting one or more of the heating rate, the first temperature, the first time, the heating process, etc. within the above range, it is beneficial to prepare a carbon material with a desired structure.

[0049] In any embodiment of the present application, the second temperature T2 is 1800°C-2600°C, and can be optionally 1900°C-2450°C.

[0050] In any embodiment of the present application, the second time t2 is 1.5 hours to 6 hours, and can be optionally 2 hours to 5 hours.

[0051] By adjusting one or more of the second temperature and the second time within the above range, it is beneficial to adjust the content of disordered carbon in the carbon material within a suitable range, which is beneficial to making the I D / I G Within a suitable range, it is also beneficial for the carbon material to satisfy S2 / S1 within a suitable range.

[0052] A third aspect of the present application provides a secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises the carbon material of the first aspect of the present application or the carbon material prepared by the method of the second aspect of the present application.

[0053] A fourth aspect of the present application provides an electrical device comprising the secondary battery of the third aspect of the present application.

[0054] The carbon materials provided herein can effectively reduce the irreversible capacity loss of secondary batteries and improve their capacity utilization characteristics, enabling them to achieve high initial coulombic efficiency, high energy density, and good cycling and storage performance. The electrical device of this application includes the secondary battery provided herein and thus has at least the same advantages as the aforementioned secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.

[0056] FIG1 is a Raman spectrum diagram of one embodiment of the carbon material of the present application.

[0057] FIG2 is a schematic diagram of a cross-sectional image of a particle of the carbon material of the present application.

[0058] FIG3 is a schematic diagram of an embodiment of a secondary battery of the present application.

[0059] FIG. 4 is an exploded schematic diagram of an embodiment of a secondary battery of the present application.

[0060] FIG5 is a schematic diagram of an embodiment of a battery module of the present application.

[0061] FIG6 is a schematic diagram of an embodiment of a battery pack of the present application.

[0062] FIG. 7 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 6 .

[0063] FIG8 is a schematic diagram of an embodiment of an electric device including the secondary battery of the present application as a power source.

[0064] In the accompanying drawings, which are not necessarily drawn to scale, reference numerals are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 housing, 52 electrode assembly, 53 cover plate, 100 carbon material, 101 external region, 102 internal region. DETAILED DESCRIPTION

[0065] Below, the carbon material and its preparation method, as well as the embodiments of the secondary battery and the electrical device containing the carbon material of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0066] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0067] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.

[0068] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.

[0069] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0070] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0071] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0072] Unless otherwise specified, the terms used in this application have the common meanings generally understood by those skilled in the art.

[0073] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in this application.

[0074] Unless otherwise specified, in this application, the term "active ions" refers to ions that can be intercalated and extracted back and forth between the positive electrode and the negative electrode of a secondary battery, including but not limited to lithium ions.

[0075] In this application, the terms "plurality" and "multiple" refer to two or more.

[0076] Graphite can be divided into artificial graphite and natural graphite based on its preparation process or source. Artificial graphite generally requires a high-temperature graphitization process, which is energy-intensive and costly, resulting in a higher cost. Natural graphite, derived from nature, offers the advantage of being relatively inexpensive. It also has the advantage of high capacity.

[0077] Natural graphite mainly includes flake graphite, natural spherical graphite and microcrystalline graphite. Unlike artificial graphite, natural graphite has a large number of pores and defects inside and outside the particles. During the first charging process of a secondary battery, the electrolyte produces many side reactions with the pores on the surface and inside the particles, resulting in a high first irreversible capacity loss of the secondary battery, a low first coulombic efficiency, and poor cycle performance and storage performance. In particular, flake graphite and natural spherical graphite have high crystallinity and high graphitization degree, and their microstructure is mostly layered. This structure causes the volume of natural graphite to change significantly during the extraction and insertion of active ions, which easily leads to the breakage of the graphite layered structure and the breakage of particles. After the particles are broken, the exposed fresh surface will continue to react with the electrolyte, thereby further increasing the irreversible capacity loss of the secondary battery.

[0078] Currently, the properties of natural graphite are mainly improved by surface coating treatment of particles and / or internal filling treatment of particles.

[0079] The particle surface coating treatment mainly involves mixing natural graphite with a coating agent (such as asphalt, polymer compounds, etc.) and then heat-treating it to coat the surface of the natural graphite particles with an amorphous carbon layer, which slightly repairs the defects on the particle surface. However, the inventors of this application found during the research process that the surface-coated amorphous carbon layer will cause the gram capacity and / or compaction density of natural graphite to decrease, affecting the energy density of the secondary battery; at the same time, the surface defects of the particles are still relatively large after the surface-coated amorphous carbon layer; in addition, the surface-coated amorphous carbon layer cannot effectively prevent the electrolyte from penetrating into the pore structure inside the particles, resulting in limited improvement in the first coulombic efficiency, cycle performance and / or storage performance of the secondary battery.

[0080] The particle internal filling process mainly involves mixing natural graphite with a filler (such as asphalt, a polymer compound, etc.), and filling the filler into the particle internal pores by means of preset pressure, vacuuming, and heating, so as to obtain natural graphite without pores in the particle interior. However, the inventors of the present application have found in the course of research that a large amount of carbon filled in the particle interior, particularly soft carbon, causes the gram capacity and compacted density of natural graphite to decrease, affecting the energy density of the secondary battery. Simultaneously, since the pores in the natural graphite particles are all filled with carbon, the volume change of natural graphite produced during the active ion escape and embedding process is larger, and the particles are more easily broken, thereby causing the SEI film on the particle surface to be repeatedly destroyed and reconstructed, further increasing the irreversible consumption of active ions, increasing the irreversible capacity loss of the secondary battery, and shortening the service life of the secondary battery. Prior art also continues to coat a layer of amorphous carbon layer on the natural graphite surface without pores in the above-mentioned particles interior, which causes the gram capacity and / or compacted density of natural graphite to further decrease, and at this time, the particle surface defects are still more, thus the service life of the secondary battery can not be effectively improved.

[0081] Therefore, after modifying natural graphite through the above-mentioned particle surface coating treatment and / or particle internal filling treatment, although the irreversible capacity loss of the secondary battery can be reduced to a certain extent and the first coulombic efficiency of the secondary battery can be improved, its improvement effect on the first coulombic efficiency of the secondary battery is limited, and the energy density of the secondary battery will also be lost. In addition, the capacity utilization characteristics of the secondary battery during long-term cycling and storage are still poor.

[0082] In view of this, the inventors of this application have, after extensive research, proposed a new type of carbon material, which has a higher gram capacity, a higher first coulombic efficiency and a smaller volume change, and can also enable secondary batteries to have a high first coulombic efficiency, a high energy density and good cycle performance and storage performance.

[0083] carbon materials

[0084] A first aspect of the embodiments of the present application provides a carbon material, wherein the carbon material comprises a pore structure and the carbon material satisfies 0.150≤I D / I G ≤0.280, I D The Raman spectrum of the carbon material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the carbon material is 1580±50cm -1 The G peak intensity at .

[0085] The carbon materials provided in this application can effectively reduce the irreversible capacity loss of secondary batteries and improve the capacity utilization characteristics of secondary batteries, enabling secondary batteries to achieve high initial coulombic efficiency, high energy density, and good cycle performance and storage performance. Possible reasons for this include at least the following:

[0086] The carbon material provided in the present application includes a pore structure. In the present application, "the carbon material includes a pore structure" means that the carbon material has a pore structure that can be directly observed from a cross-sectional image (for example, a scanning electron microscope image with a magnification of 1000 times), that is, the pore structure in the raw material used to prepare the carbon material is not completely filled. Thus, the pore structure in the carbon material can reserve the required expansion space for the volume change of the carbon material particles, thereby reducing the risk of the carbon material particles breaking and producing new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance and storage performance of the secondary battery.

[0087] The carbon material provided in this application satisfies 0.150≤I D / I G ≤0.280. I D / I G It can reflect the disorder of the carbon material surface, I D / I G The smaller it is, the less disordered carbon content on the surface of the carbon material particles, the fewer active sites on the particle surface, and the less irreversible consumption of active ions. However, the inventors of this application found in the course of research that the less disordered carbon content is not necessarily better. When its content is too low, the crystallinity and graphitization degree of the carbon material are very high, which is not conducive to the rapid escape and embedding of active ions. At the same time, the volume change of the carbon material during the charge and discharge process of the secondary battery is still large, thereby increasing the risk of carbon material particle breakage, and further causing the SEI film on the surface of the particles to be easily destroyed and rebuilt repeatedly, further increasing the irreversible consumption of active ions, increasing the irreversible capacity loss of the secondary battery, and shortening the service life of the secondary battery. The inventors found in further research that when the carbon material satisfies 0.150≤I D / I GWhen ≤0.280, on the one hand, it can effectively reduce the content of disordered carbon, reduce the surface activity of carbon materials, and reduce the consumption of active ions by SEI film formation on the particle surface; on the other hand, it can also make the carbon material have a stable structure and avoid particle breakage as much as possible.

[0088] Therefore, when the carbon material satisfies the conditions including the pore structure and 0.150≤I D / I G When ≤0.280, the carbon material has small volume expansion, high structural stability and low surface activity, thereby having a higher gram capacity, a higher first coulombic efficiency and a smaller volume change, and can also enable the secondary battery to have a high first coulombic efficiency, a high energy density and good cycle performance and storage performance.

[0089] FIG1 is a Raman spectrum diagram of an embodiment of the carbon material of the present application. D The Raman spectrum of carbon materials is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of carbon materials is 1580±50cm -1 The G peak intensity at D / I G It can be expressed by the ratio of the D peak height to the G peak height in the Raman spectrum.

[0090] In some embodiments, I D / I G It can be 0.155, 0.160, 0.170, 0.180, 0.190, 0.200, 0.210, 0.220, 0.230, 0.240, 0.250, 0.260, 0.270, 0.280 or any range thereof. Optionally, 0.152≤I D / I G ≤0.280, 0.152≤I D / I G ≤0.260,0.155≤I D / I G ≤0.240,0.155≤I D / I G ≤0.220,0.155≤I D / I G ≤0.200,0.155≤I D / I G ≤0.180. The inventors found in further research that when the I D / I G Within the above range, the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0091] In some embodiments, the carbon material comprises at least one pore with an area greater than or equal to 0.15 μm 2 The pore structure may include one or more pores with an area of ​​0.15 μm 2 -2.0μm 2 When the carbon material includes a pore structure with the above-mentioned pore area, the pore structure can reserve the required expansion space for the volume change of the carbon material particles, thereby further reducing the risk of carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance and storage performance of the secondary battery.

[0092] In some embodiments, the carbon material includes an external region and an internal region located inside the external region, wherein the external region refers to a region extending a distance of 0.25L from the particle surface of the carbon material to the interior of the particle, L refers to the short axis length of the carbon material particle, the total pore area of ​​the external region is recorded as S1, the total pore area of ​​the internal region is recorded as S2, and S2>S1.

[0093] When the carbon material also satisfies S2>S1, the carbon material particles further have the following characteristics: the number of pores in the inner region is large and / or the pore size is large, while the number of pores in the outer region is small and / or the pore size is small. The pore structure in the inner region of the carbon material can reserve the required expansion space for the volume change of the carbon material particles, thereby reducing the risk of the carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance and storage performance of the secondary battery; the number of pores in the outer region of the carbon material is small and / or the pore size is small, thereby making the carbon material particles have a more stable structure and avoiding the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions, reducing the consumption of active ions by the SEI film formation inside the particles, thereby improving the first coulombic efficiency of the carbon material, and further improving the cycle performance and storage performance of the secondary battery.

[0094] Optionally, 1.5≤S2 / S1≤450, 2≤S2 / S1≤400, 2.5≤S2 / S1≤300, 2.5≤S2 / S1≤250, 2.5≤S2 / S1≤200, 2.5≤S2 / S1≤150, 2.5≤S2 / S1≤100, and 2.5≤S2 / S1≤50. The inventors found in further research that when S2 / S1 is also within the above range, the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0095] In some embodiments, 0.01 μm 2≤S1≤5.0μm 2 , optionally, 0.02 μm 2 ≤S1≤4.5μm 2 , 0.03μm 2 ≤S1≤4μm 2 , 0.04μm 2 ≤S1≤3.5μm 2 , 0.05μm 2 ≤S1≤3μm 2 , 0.05μm 2 ≤S1≤2.5μm 2 , 0.05μm 2 ≤S1≤2μm 2 When the total pore area of ​​the outer region of the carbon material is within the above range, on the one hand, the carbon material particles can have a more stable structure, and the electrolyte can be prevented from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions and reducing the consumption of active ions by the formation of the SEI film inside the carbon material particles. On the other hand, it will not affect the transmission performance of active ions and electrons.

[0096] In some embodiments, 2.5 μm 2 ≤S2≤25.0μm 2 , optionally, 3.0 μm 2 ≤S2≤22.5μm 2 , 3.0μm 2 ≤S2≤20μm 2 , 3.0μm 2 ≤S2≤18μm 2 , 3.0μm 2 ≤S2≤16μm 2 , 3.0μm 2 ≤S2≤14μm 2 , 3.0μm 2 ≤S2≤12μm 2 , 3.0μm 2 ≤S2≤10μm 2 , 3.0μm 2 ≤S2≤8μm 2 When the total pore area of ​​the internal region of the carbon material is within the above range, on the one hand, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, reducing the risk of carbon material particles breaking to produce new interfaces, reducing the occurrence of side reactions on the new interface surface, and reducing the consumption of active ions by the formation of the SEI film on the new interface surface. On the other hand, it can also improve the capacity and first coulombic efficiency of the carbon material.

[0097] In the present application, the total pore area S1 of the outer region and the total pore area S2 of the inner region of the carbon material can be obtained by testing a cross-sectional image of the carbon material.

[0098] In the present application, the cross-sectional image of the carbon material includes a cross-sectional image passing through the center of the carbon material particle. "Particle center" refers to the range within a radius of 0.1 μm extending from the geometric center of the particle to the particle surface.

[0099] In this application, the minor axis length of a particle refers to the minimum value when a line connecting two points on the particle surface passes through the geometric center of the particle.

[0100] FIG2 is a schematic diagram of a cross-sectional image of a particle of the carbon material 100 of the present application, and the cross-sectional image passes through the center of the particle of carbon material 100. As shown in FIG2 , L represents the minor axis length of the particle of carbon material 100, and the region extending from the surface of the particle of carbon material 100 to the interior of the particle by a distance of 0.25L is the outer region 101, and the region inside the outer region 101 is the inner region 102.

[0101] The cross-section of the carbon material can be prepared using a cross-section polisher (e.g., the IB-09010CP argon ion cross-section polisher from JEOL, Japan); then, referring to JY / T010-1996, a scanning electron microscope (e.g., the Sigma 300 scanning electron microscope from ZEISS, Germany) is used to scan the cross-section of the carbon material; finally, the total pore area S1 of the outer region and the total pore area S2 of the inner region of the carbon material are calculated using image processing software (e.g., AVIZO).

[0102] In some embodiments, the minor axis length L of the carbon material particles satisfies L≥4μm, optionally, 4μm≤L≤25μm, 4μm≤L≤20μm, 6μm≤L≤20μm, 8μm≤L≤20μm, 8μm≤L≤18μm, 8μm≤L≤16μm.

[0103] In some embodiments, the area of ​​the pore structure in the outer region of the carbon material is less than or equal to 0.15 μm 2 , can be selected to be less than or equal to 0.10μm 2 In further research, the inventors also found that by controlling the area of ​​the pore structure in the outer region of the carbon material within the above range, the outer region of the carbon material can have a dense structure, thereby effectively improving the structural stability of the carbon material and preventing the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby effectively improving the cycle performance and storage performance of the secondary battery. Of course, this application does not intend to limit the area of ​​all pore structures in the outer region of the carbon material to be less than or equal to 0.15 μm 2For example, the area of ​​the pore structure can be controlled to be less than or equal to 0.15 μm by more than 95%, or more than 99%. 2 , can be selected to be less than or equal to 0.10μm 2 .

[0104] In some embodiments, the inner region of the carbon material includes one or more carbon atoms with an area greater than or equal to 0.15 μm 2 The pore structure may optionally include one or more pores with an area of ​​0.15 μm 2 -2.0μm 2 The inventors further discovered that by including a pore structure of the aforementioned area in the internal region of the carbon material, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, thereby reducing the risk of carbon material particle breakage. Furthermore, the compaction density of the carbon material can be increased.

[0105] In some embodiments, the interlayer distance of the outer region of the carbon material is denoted as d1, and the interlayer distance of the inner region of the carbon material is denoted as d2. The carbon material satisfies d1≥d2, and optionally, d1>d2.

[0106] The interlayer spacing in the outer region of the carbon material is larger, which is more conducive to the rapid embedding and extraction of active ions, thereby further improving the kinetic performance of the secondary battery; the interlayer spacing in the inner region of the carbon material is smaller, which is conducive to improving the gram capacity and compaction density of the carbon material, thereby further improving the energy density of the secondary battery.

[0107] In some embodiments, d1 is 0.33565 nm-0.33620 nm.

[0108] In some embodiments, d2 is 0.33557 nm - 0.33589 nm.

[0109] The interlayer spacing of different regions of the carbon material can be measured using instruments and methods known in the art. For example, a high-resolution transmission electron microscope (HRTEM) can be used for testing. The testing instrument can be a Thermo Fisher Scientific Spectra S / TEM scanning transmission electron microscope.

[0110] In some embodiments, the carbon material has a morphology of one or more of block, spherical, and quasi-spherical, which is beneficial for increasing the compaction density of the negative electrode sheet and thus improving the energy density of the secondary battery.

[0111] In some embodiments, the carbon material includes primary particles. Optionally, the primary particles in the carbon material account for ≥50%, for example, 55%-95%, 60%-100%, 65%-90%, 65%-80%, 70%-100%, 75%-90%, 80%-100%, 90%-100%, or 95%-100%. The carbon material containing an appropriate proportion of primary particles can provide it with higher structural stability and reduce the occurrence of side reactions. In addition, it can also increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the secondary battery.

[0112] In some embodiments, the carbon materials may all be primary particles, that is, the number of the primary particles in the carbon materials accounts for 100%.

[0113] Primary particles and secondary particles are both well-known in the art. Primary particles refer to non-agglomerated particles. Secondary particles refer to agglomerated particles formed by the aggregation of two or more primary particles. Primary particles and secondary particles can be distinguished using scanning electron microscopy (SEM) images.

[0114] In the present application, the number ratio of primary particles in the carbon material can be tested according to the following method: randomly select a test sample in the negative electrode film layer, randomly select multiple test areas in the test sample, use a scanning electron microscope to obtain images of the multiple test areas, and count the proportion of the number of carbon material particles with primary particle morphology in each image to the total number of carbon material particles. The average value of multiple statistical results is the number ratio of primary particles in the carbon material.

[0115] In some embodiments, the graphitization degree of the carbon material is 92.0%-98.0%, optionally 92.5%-97.6%. When the graphitization degree of the carbon material is within the above range, it is beneficial for the secondary battery to have high energy density and good cycle performance, storage performance and dynamic performance.

[0116] The graphitization degree of carbon materials is well known in the art and can be measured using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for measurement. The measurement can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain the average interlayer spacing d of the (002) crystal plane in the carbon material crystal structure. 002 Then according to the formula g=(0.344-d 002 ) / (0.344-0.3354)×100% to calculate the degree of graphitization. In the above formula, d 002 It is the average interlayer distance between (002) planes in the carbon material crystal structure expressed in nanometers (nm).

[0117] In some embodiments, the specific surface area of ​​the carbon material is ≤2.1 m 2 / g, optional 0.7m 2 / g-1.8m 2 / g,0.7m 2 / g-1.7m 2 / g,0.7m 2 / g-1.6m 2 / g,0.7m 2 / g-1.5m 2 / g,0.7m 2 / g-1.4m 2 / g,0.7m 2 / g-1.3m 2 / g,0.7m 2 / g-1.25m 2 The carbon material of the present application has a low specific surface area and low surface activity, thereby reducing the consumption of active ions in SEI film formation, improving the first coulombic efficiency of the carbon material, and also improving the cycle performance and storage performance of the secondary battery.

[0118] The specific surface area of ​​a carbon material is well known in the art and can be measured using instruments and methods known in the art. For example, the specific surface area can be measured using the nitrogen adsorption specific surface area analysis test method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed using a Micromeritics Tri-Star 3020 specific surface area pore size analyzer.

[0119] In some embodiments, the volume distribution particle size Dv50 of the carbon material is 6.0 μm-30.0 μm, optionally 8.0 μm-25.0 μm.

[0120] In some embodiments, the volume distribution particle size Dv90 of the carbon material is 16.0 μm-45.0 μm, optionally 17.0 μm-42.0 μm.

[0121] When the volume distribution particle size Dv50 and / or Dv90 of the carbon material is within the above range, it is beneficial to improve the transport performance of active ions and electrons, thereby further improving the cycle performance and kinetic performance of the secondary battery.

[0122] In some embodiments, the carbon material has a particle size distribution (Dv90-Dv10) / Dv50 of ≤1.55, and can optionally be 0.5-1.50. A particle size distribution (Dv90-Dv10) / Dv50 of the carbon material within the above range is beneficial for increasing the compaction density of the carbon material, thereby further increasing the energy density of the secondary battery. It also facilitates the formation of a reasonable pore structure between the particles of the negative electrode film layer, thereby improving the cycling performance and kinetic performance of the secondary battery.

[0123] In this application, the volume distribution particle sizes Dv10, Dv50, and Dv90 of the carbon material are well-known in the art and represent the particle sizes corresponding to the cumulative volume distribution percentages of the material reaching 10%, 50%, and 90%, respectively. They can be measured using instruments and methods known in the art. For example, they can be conveniently measured using a laser particle size analyzer with reference to GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.

[0124] In some embodiments, the powder resistivity of the carbon material at a pressure of 8 MPa is 0.006 Ω.cm-0.051 Ω.cm, and optionally 0.010 Ω.cm-0.040 Ω.cm. When the powder resistivity of the carbon material is within the above range, it is beneficial to improve the electron transport performance, thereby further improving the cycle performance and kinetic performance of the secondary battery.

[0125] The powder resistivity of carbon materials is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder resistivity tester (e.g., Suzhou Jingge ST2722, Sansi Zongheng UTM7305) using the four-probe method, with reference to GB / T 30835-2014. An exemplary test method is as follows: a certain amount of sample powder to be tested is weighed and placed in a dedicated mold. A test pressure is set to obtain the powder resistivity at different pressures. In this application, the test pressure can be set to 8 MPa.

[0126] In some embodiments, the powder compaction density of the carbon material under a pressure of 20,000 N is 1.70 g / cm 3 -1.95g / cm 3 , optional 1.72g / cm 3 -1.92g / cm 3 When the compaction density of the carbon material powder is within the above range, the compaction density of the negative electrode sheet can be increased, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.

[0127] In this application, the compacted density of carbon material powder is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured by an electronic pressure testing machine (for example, a UTM7305 electronic pressure testing machine) with reference to GB / T 24533-2009. An exemplary test method is as follows: 1g of carbon material powder is weighed and added to a container with a bottom area of ​​1.327cm 2 The mold was pressurized to 2000 kg (equivalent to 20000 N), maintained for 30 seconds, then released and maintained for 10 seconds, and then the powder compaction density of the carbon material under a pressure of 20000 N was recorded and calculated.

[0128] In some embodiments, the tap density of the carbon material is 0.80 g / cm 3 -1.35g / cm 3 , optional 0.85g / cm 3 -1.30g / cm 3 When the tap density of the carbon material is within the above range, it can increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.

[0129] The tap density of carbon materials is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder tap density tester in accordance with GB / T 5162-2006. A suitable tester is the Dandong Better BT-301.

[0130] In some embodiments, the gram capacity of the carbon material is 350 mAh / g-372 mAh / g, optionally 353 mAh / g-371 mAh / g. When the gram capacity of the carbon material is within the above range, the energy density of the secondary battery can be increased.

[0131] The gram capacity of carbon materials is a well-known meaning in the art and can be tested using methods known in the art. An exemplary test method is as follows: a carbon material sample is thoroughly stirred and mixed with a binder of styrene-butadiene rubber (SBR), a thickener of sodium carboxymethyl cellulose (CMC), and a conductive agent of carbon black in a mass ratio of 96.2:1.8:1.2:0.8 in an appropriate amount of solvent deionized water to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil and dried in an oven for later use; ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L; a metal lithium sheet is then used as a counter electrode and a polyethylene (PE) film is used as an isolation membrane to assemble a CR2430 button cell in an argon-protected glove box. At 25°C, the prepared button cell was first discharged at a constant current of 0.15 mA to 0.005 V, allowed to stand for 5 minutes, and then discharged at a constant current of 10 μA to 0.005 V. The first-cycle discharge capacity of the button cell was recorded. The cell was then charged at a constant current of 0.3 mA to 2.0 V, and the charge capacity of the button cell was recorded. The ratio of the charge capacity of the button cell to the mass of the carbon material sample is the gram capacity of the carbon material.

[0132] Preparation method

[0133] A second aspect of the embodiments of the present application provides a method for preparing a carbon material, which can prepare the carbon material of the first aspect of the embodiments of the present application.

[0134] The preparation method of the carbon material comprises the following steps: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and a filler material in a predetermined ratio, and then keeping the mixture at a first temperature T1 for a first time t1 to obtain an intermediate; step 3, keeping the obtained intermediate at a second temperature T2 for a second time t2 to obtain a carbon material, wherein the carbon material comprises a pore structure and satisfies 0.150≤I D / I G ≤0.280, I D The Raman spectrum of the carbon material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the carbon material is 1580±50cm -1 The G peak intensity at .

[0135] In some embodiments, the raw material for preparing the carbon material includes natural graphite. Optionally, the natural graphite includes one or more of flake graphite, natural spherical graphite, and microcrystalline graphite, and more preferably includes natural spherical graphite.

[0136] "Natural spherical graphite" refers to natural graphite with a spherical or quasi-spherical shape, and not all natural graphite particles are controlled to be ideal spheres. In some embodiments, natural spherical graphite with a desired particle size and morphology can be obtained by pre-treating flake graphite. Optionally, the pre-treatment includes crushing, classification, spheroidization, purification, and other processes.

[0137] In some embodiments, the raw material has a morphology comprising one or more of a spherical shape or a spheroidal shape.

[0138] In some embodiments, the volume distribution particle size Dv50 of the raw material is 6.0 μm-30.0 μm, and optionally 8.0 μm-25.0 μm.

[0139] In some embodiments, the specific surface area of ​​the raw material is ≥2.5m 2 / g, optional 2.5m 2 / g-10.0m 2 When the specific surface area of ​​the raw material is within the above range, it is beneficial to carry out subsequent filling processing and obtain a carbon material with a desired specific surface area, and it is also beneficial for the carbon material to have both high capacity and high first coulombic efficiency. In addition, it is also beneficial for the carbon material to have better kinetic properties.

[0140] By adjusting the particle size of the raw materials (e.g., volume distribution particle size Dv50 and / or specific surface area) within the above range, agglomeration of the raw materials during the subsequent preparation process can be avoided as much as possible, thereby minimizing problems such as increased surface defects and increased surface active sites caused by particle breakage.

[0141] In some embodiments, the volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be selected from 1 μm-6 μm, 1 μm-5 μm, 2 μm-5 μm, and 3 μm-5 μm. This facilitates the filler material to be melted and filled into the pore structure of the raw material after heating, and also helps to improve the uniformity of the dispersion of the filler material and the raw material.

[0142] In some embodiments, the softening point temperature of the filler material is 100° C.-180° C. For example, the softening point temperature of the filler material can be 100° C., 110° C., 120° C., 125° C., 130° C., 135° C., 140° C., 145° C., 150° C., 155° C., 160° C., 165° C., 170° C., 175° C., 180° C., or any range thereof. Optionally, the softening point temperature of the filling material may be 100℃-160℃, 100℃-150℃, 100℃-140℃, 110℃-180℃, 110℃-170℃, 110℃-160℃, 110℃-150℃, 110℃-140℃, 120℃-180℃, 120℃-170℃, 120℃-160℃, 120℃-150℃, 120℃-140℃, 125℃-180℃, 125℃-170℃, 125℃-160℃, 125℃-150℃, 125℃-140℃, 130℃-180℃, 130℃-170℃, 130℃-160℃, 130℃-150℃, 130℃-140℃.

[0143] During the research process, the inventors found that when the softening point temperature of the filling material is within the above range, it is beneficial to adjust the number of pores and / or pore size in the outer region and the inner region of the carbon material to be within a suitable range. And it can effectively avoid the following situations: when the softening point temperature of the filling material is too high, the filling material is not easy to flow and fill into the pore structure of the raw material after being heated and melted, thereby failing to effectively modify the internal defects of the particles, and failing to effectively prevent the electrolyte from penetrating into the pore structure inside the obtained carbon material particles, thereby affecting the initial coulombic efficiency, cycle performance and storage performance of the secondary battery; when the softening point temperature of the filling material is too low, the filling material contains more small molecules, which are easily volatilized when heated. Therefore, although the filling material is easy to flow and fill into the pore structure of the raw material after being heated and melted, when step 2 and / or step 3 are heat treated, the small molecules in the filling material volatilize, thereby resulting in the actual residual carbon in the filling area failing to effectively fill the pore structure of the raw material, failing to achieve an effective filling effect, or the actual residual carbon in the filling area has more pore structures, thereby failing to reduce the consumption of active ions by SEI film formation and reduce the irreversible capacity loss of the secondary battery, and at the same time affecting the cycle performance and storage performance of the secondary battery.

[0144] In some embodiments, the coking value of the filler material is 25%-50%, and optionally 30%-42%. The inventors found during research that when the coking value of the filler material is within the above range, it is beneficial to adjust the number and / or pore size of the pores in the outer region and the inner region of the carbon material to be within a suitable range.

[0145] In some embodiments, the filler material simultaneously meets the requirements of a softening point temperature of 120° C. to 160° C. and a coking value of 30% to 42%.

[0146] In this application, the coking value of the filler material has a well-known meaning in the art and can be measured using instruments and methods known in the art, for example, according to GB / T 8727-2008.

[0147] In some embodiments, the filling material includes one or more of coal tar, petroleum asphalt, polymer compounds and resins, and may optionally include one or more of coal tar and petroleum asphalt.

[0148] In some embodiments, the mass ratio of the filler material to the raw material is (10-32):100, optionally (12-30):100, (14-28):100, or (15-25):100. This facilitates adjusting the number and / or size of pores in the outer and inner regions of the carbon material within a suitable range. It can also effectively avoid the following situations: when the mass ratio of the filling material to the raw material is too small, the dispersion uniformity of the filling material and the raw material is poor. At this time, the filling material is not easy to flow and fill into the pore structure of the raw material after being heated and melted, thereby failing to effectively modify the internal defects of the particles, nor effectively preventing the electrolyte from penetrating into the pore structure inside the obtained carbon material particles, thereby affecting the initial coulombic efficiency, cycle performance and storage performance of the secondary battery; when the mass ratio of the filling material to the raw material is too large, it is easy to cause the internal pore structure of the raw material to be completely filled. At this time, the volume of the obtained carbon material changes greatly, the particles are more easily broken, the consumption of active ions for SEI film formation increases, and the irreversible capacity loss of the secondary battery increases; in addition, when the mass ratio of the filling material to the raw material is too large, a large amount of filling material may remain on the surface of the particles. At this time, the particles are more likely to agglomerate, which not only increases the depolymerization process, but also reduces the gram capacity and compaction density of the obtained carbon material.

[0149] By adjusting the type, softening point, coking value, addition amount and other parameters of the filling material within the above range, the viscosity of the filling material is not high after being heated and melted, and good fluidity is maintained. At the same time, it is not easy to adhere to the raw material particles, which can reduce the agglomeration of the raw material particles in the subsequent preparation process, thereby reducing problems such as increased surface defects of carbon material particles and increased surface active sites due to the depolymerization process.

[0150] In some embodiments, in step 2, the heating process of uniformly mixing the raw material and the filling material in a predetermined proportion and then heating the temperature to the first temperature T1 is a staged heating process, which may optionally include a first heating process, a second heating process, and a third heating process.

[0151] In some embodiments, the first temperature raising process is to raise the temperature to 200° C.-250° C. and keep the temperature at this temperature for 1 hour-2 hours.

[0152] In some embodiments, the second temperature raising process is to raise the temperature to 450° C.-550° C. and keep the temperature at this temperature for 1 hour-2 hours.

[0153] In some embodiments, the third temperature raising process is to raise the temperature to the first temperature T1 and keep the temperature at the first time t1.

[0154] In the staged heating process, the temperature is first raised to 200℃-250℃. Since the heating temperature is higher than the softening point of the filling material, the filling material is melted and softened by the heat. Keeping it warm for 1h-2h allows it to flow and fill into the pore structure of the raw material; then the temperature is raised to 450℃-550℃. At this time, the melted and softened filling material undergoes a carbonization reaction, gradually forming a semi-coke state and turning into a viscous liquid or solid, thereby preventing the filling material from entering the entire pore structure of the raw material; finally, the temperature is raised to the first temperature. At this time, the filling material undergoes a carbonization reaction, thereby enabling the pore structure occupied by the filling material to be effectively filled.

[0155] In some embodiments, in step 2, the temperature is increased to the first temperature T1 at a rate of 1°C / min-10°C / min. For example, the temperature increase rate can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, or any range thereof.

[0156] During the research process, the inventors found that when the heating rate is within the above range, it is beneficial to adjust the number of pores and / or pore size in the outer region and the inner region of the carbon material to be within a suitable range.

[0157] In some embodiments, the heating rate of the first heating process may be 1° C. / min-10° C. / min.

[0158] In some embodiments, the heating rate of the second heating process may be 1° C. / min-10° C. / min.

[0159] In some embodiments, the heating rate of the third heating process may be 1° C. / min-10° C. / min.

[0160] In some embodiments, in step 2, the first temperature T1 is 700° C.-1200° C. For example, the first temperature T1 can be 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1200° C., or any range thereof. Optionally, the first temperature T1 is 720° C.-1100° C.

[0161] During the research process, the inventors found that when the first temperature is within the above range, it is beneficial to adjust the number and / or pore size of pores in the outer and inner regions of the carbon material within an appropriate range. It can also effectively avoid the following situations: when the first temperature is too low, the filling material may not be completely converted into carbon, and will continue to decompose into small molecules during the subsequent heat treatment in step 3, resulting in the actual residual carbon in the filling area having a large porous structure, failing to effectively modify the internal defects of the particles, and failing to effectively prevent the electrolyte from penetrating into the pore structure inside the obtained carbon material particles, thereby affecting the initial coulombic efficiency, cycle performance and storage performance of the secondary battery; when the first temperature is too high, the energy consumption in the carbon material preparation process will increase.

[0162] In some embodiments, the first time t1 is 1 hour to 5 hours. For example, the first time t1 can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, or any range thereof. Alternatively, the first time t1 is 2 hours to 4 hours.

[0163] During their research, the inventors discovered that a first time within the aforementioned range is beneficial for regulating the number and / or pore size of pores in the outer and inner regions of the carbon material within an appropriate range. This can also effectively avoid the following situations: When the first time is too short, the filler cannot effectively fill the carbon material particles, resulting in the residual carbon in the filled region having a relatively large porous structure, failing to effectively modify the internal defects of the particles and failing to effectively prevent the electrolyte from penetrating into the pore structure within the obtained carbon material particles, thereby affecting the initial coulombic efficiency, cycling performance, and storage performance of the secondary battery; and when the first time is too long, energy consumption during the carbon material preparation process increases.

[0164] In some embodiments, in step 2, the heat treatment may be performed in a medium frequency furnace, a roller kiln, a rotary kiln, or a pusher kiln.

[0165] In some embodiments, in step 2, the heat treatment atmosphere may be a protective gas atmosphere, which may include one or more of nitrogen, argon, and helium.

[0166] In step 2, adjusting one or more of the heating rate, the first temperature, the first time, and the heating process within the above-mentioned ranges facilitates the preparation of a carbon material with a desired structure. For example, the carbon material is advantageously configured to satisfy S2>S1, and may optionally satisfy 1.5≤S2 / S1≤450 and 2≤S2 / S1≤400.

[0167] In some embodiments, the second temperature T2 is 1800° C.-2600° C. For example, the second temperature can be 1800° C., 1900° C., 2000° C., 2100° C., 2200° C., 2300° C., 2400° C., 2500° C., 2600° C., or any range thereof. Optionally, the second temperature T2 is 1860°C-2560°C, 1860°C-2520°C, 1860°C-2480°C, 1860°C-2450°C, 1860°C-2410°C, 1860°C-2370°C, 1860°C-2330°C, 1900°C-2560°C, 1900°C-2520°C, 1900°C-2480°C, 1900°C-2450°C, 1900°C-2410°C, 1900°C-2370°C, 1900°C -2330℃,1970℃-2560℃,1970℃-2520℃,1970℃-2480℃,1970℃-2450℃,1970℃-2410℃,1970℃-2370℃,1970℃-2330℃,2030℃-2560℃,2030℃-2520℃,2030℃-2480℃,2030℃-2450℃,2030℃-2410℃,2030℃-2370℃,2030℃-2330℃.

[0168] During their research, the inventors discovered that when the second temperature is within the above range, it is beneficial to regulate the disorder of the carbon material, and it is also beneficial for the carbon material to have a stable structure, thereby minimizing particle breakage. This can effectively avoid the following situations: when the second temperature is too low, the obtained carbon material contains a high content of disordered carbon, which leads to a high content of defects in the carbon material, especially a high content of surface defects, which affects the initial coulombic efficiency and storage performance of the carbon material; when the second temperature is too high, the obtained carbon material contains too little disordered carbon, and the carbon material has a high degree of crystallinity and graphitization, which is not conducive to the rapid extraction and embedding of active ions. At the same time, the volume change of the carbon material during charge and discharge is also large, thereby increasing the risk of carbon material particle breakage, thereby affecting the cycle performance and storage performance of the secondary battery.

[0169] In some embodiments, the second time t2 is 1.5 hours to 6 hours. For example, the second time t1 can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, or any range thereof. Alternatively, the second time t2 is 2 hours to 5 hours.

[0170] During the research process, the inventors found that when the second time is within the above range, it is beneficial to adjust the disorder of the carbon material, and it is also beneficial for the carbon material to have a stable structure, thereby minimizing particle breakage. It can also effectively avoid the following situations: when the second time is too short, the content of disordered carbon in the obtained carbon material is relatively high, resulting in a high content of defects in the carbon material, especially a high content of surface defects, which affects the gram capacity and initial coulombic efficiency of the carbon material; when the second time is too long, the content of disordered carbon in the obtained carbon material is too low, and the crystallinity and graphitization degree of the carbon material are both very high, which is not conducive to the rapid extraction and embedding of active ions. At the same time, the volume change of the carbon material during the charge and discharge process is also relatively large, thereby increasing the risk of carbon material particle breakage, thereby affecting the cycle performance and storage performance of the secondary battery.

[0171] In some embodiments, in step 3, the heat treatment may be performed in a medium frequency furnace, a box-type graphitization furnace, an Acheson graphitization furnace, a continuous graphitization furnace, or an inner-string graphitization furnace.

[0172] In some embodiments, in step 3, the medium frequency furnace and the continuous graphitization heat treatment atmosphere may be a protective gas atmosphere. The protective gas may include one or more of nitrogen, argon, and helium.

[0173] By adjusting one or more of the second temperature and the second time within the above range, it is beneficial to adjust the content of disordered carbon in the carbon material within a suitable range, which is beneficial to making the I D / I G Within a suitable range, it is also beneficial for the carbon material to satisfy S2 / S1 within a suitable range.

[0174] The carbon material preparation method of the present application is simple and highly safe, does not require a preset pressure or vacuum treatment, and does not require an additional depolymerization step during the heat treatment process. The carbon material prepared in the present application has low volume expansion, high structural stability, and low surface activity, thereby achieving a high gram capacity, a high first coulombic efficiency, and a small volume change. It also enables secondary batteries to have high first coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0175] The preparation method of the present application is low-cost, highly practical, and suitable for large-scale production.

[0176] secondary batteries

[0177] A third aspect of the embodiments of the present application provides a secondary battery.

[0178] The present application has no particular restrictions on the type of secondary battery. For example, the secondary battery can be a lithium-ion battery, etc. In general, a secondary battery includes a positive electrode plate, a negative electrode plate, and an electrolyte, etc. During the charge and discharge process of the secondary battery, active ions are embedded and released back and forth between the positive electrode plate and the negative electrode plate, and the electrolyte plays a role in conducting active ions between the positive electrode plate and the negative electrode plate. The present application has no particular restrictions on the type of the electrolyte, and it can be selected according to actual needs. For example, the electrolyte can be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte). Secondary batteries using electrolytes and some secondary batteries using solid electrolytes can also include an isolation membrane, which is arranged between the positive electrode plate and the negative electrode plate to play an isolation role.

[0179] [Negative electrode]

[0180] In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces that are opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.

[0181] In some embodiments, the negative electrode film layer comprises the carbon material of the first aspect of the embodiment of the present application or the carbon material prepared by the method described in the second aspect of the embodiment of the present application. This enables the secondary battery to have high initial coulombic efficiency, high energy density, and good cycle performance and storage performance.

[0182] In some embodiments, the negative electrode film layer may further include other negative electrode active materials in addition to the above-mentioned carbon materials. In some embodiments, the other negative electrode active materials include, but are not limited to, one or more of conventional natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy materials. The tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials.

[0183] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. As examples, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0184] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As examples, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0185] In some embodiments, the negative electrode film layer may further include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.

[0186] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0187] The negative electrode film layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring until uniformly mixed. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.

[0188] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode plate described in the present application further includes a protective layer covering the surface of the negative electrode film layer.

[0189] [Positive electrode]

[0190] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces that are opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0191] The positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0192] The positive electrode film layer generally comprises a positive electrode active material, an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating a positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is generally formed by dispersing a positive electrode active material, an optional conductive agent, an optional binder and any other components in a solvent and stirring them evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited to this. As an example, the binder for the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. As an example, the conductive agent for the positive electrode film layer includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0193] The positive electrode active material may be a positive electrode active material for a secondary battery known in the art.

[0194] When the secondary battery of the present application is a lithium-ion battery, the positive electrode active material may include, but is not limited to, one or more of lithium-containing transition metal oxides, lithium-containing phosphates, and their respective modified compounds. Examples of the lithium transition metal oxide may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of the lithium-containing phosphate may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

[0195] In some embodiments, in order to further improve the energy density of the secondary battery, the positive electrode active material for the lithium ion battery may include a general formula of Li a Nib Co c M d O e A f One or more of lithium transition metal oxides and their modified compounds thereof. 0.8 ≤ a ≤ 1.2, 0.5 ≤ b < 1, 0 < c < 1, 0 < d < 1, 1 ≤ e ≤ 2, 0 ≤ f ≤ 1, M is selected from one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A is selected from one or more of N, F, S and Cl.

[0196] In some embodiments, by way of example, the positive electrode active material for a lithium ion battery may include one or more of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), LiNi 0.85 Co 0.15 Al 0.05 O2, LiFePO4 and LiMnPO4.

[0197] In the present application, the modified compounds of the above positive electrode active materials may be doping modification and / or surface coating modification of the positive electrode active materials.

[0198] [Electrolyte]

[0199] In some embodiments, the electrolyte uses an electrolyte solution, and the electrolyte solution includes an electrolyte salt and a solvent.

[0200] The type of the electrolyte salt is not specifically limited and can be selected according to actual needs.

[0201] When the secondary battery of the present application is a lithium ion battery, as an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0202] The type of the solvent is not specifically limited and can be selected according to actual needs. In some embodiments, for example, the solvent may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE). One or more.

[0203] In some embodiments, the electrolyte may further optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives capable of improving certain properties of the secondary battery, such as additives that improve the overcharge performance of the secondary battery, additives that improve the high-temperature performance of the secondary battery, and additives that improve the low-temperature power performance of the secondary battery.

[0204] [Isolation film]

[0205] The present application has no particular limitation on the type of the isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected.

[0206] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different.

[0207] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process.

[0208] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0209] In some embodiments, the outer packaging can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0210] The present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. FIG3 shows a secondary battery 5 with a square structure as an example.

[0211] In some embodiments, as shown in FIG4 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.

[0212] The preparation method of the secondary battery of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The secondary battery is then vacuum packaged, allowed to stand, formed, and shaped.

[0213] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.

[0214] Figure 5 is a schematic diagram of an exemplary battery module 4. As shown in Figure 5 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured using fasteners.

[0215] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0216] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0217] Figures 6 and 7 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 6 and 7, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0218] Electrical devices

[0219] The present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.

[0220] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.

[0221] Figure 8 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.

[0222] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.

[0223] Example

[0224] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.

[0225] Example 1

[0226] (1) Preparation of carbon materials

[0227] Step 1: Mechanically crush, classify, spheroidize and purify 100 mesh flake graphite to obtain natural spherical graphite with a volume distribution particle size Dv50 of 11 μm and a BET specific surface area of ​​7 m 2 / g.

[0228] Step 2: The obtained natural spherical graphite and petroleum asphalt (softening point temperature of 148 ° C, volume distribution particle size Dv50 of 4.5 μm, coking value of 40%) are mixed in a VC mixer at a mass ratio of 100:20 for 30 minutes, and then the mixed material is placed in a roller kiln, heated to 220 ° C at a rate of 5 ° C / min and kept warm for 1 hour (first heating process), then heated to 500 ° C at a rate of 5 ° C / min and kept warm for 2 hours (second heating process), and finally heated to 1000 ° C at a rate of 5 ° C / min and kept warm for 2 hours (third heating process), and then cooled to room temperature to obtain an intermediate.

[0229] Step 3: Place the obtained intermediate in an Acheson graphitization furnace, heat it to 2400°C and keep it warm for 2 hours. After the graphitization is completed, demagnetize and sieve to obtain the carbon material.

[0230] According to GB / T 19587-2017, the specific surface area of ​​the carbon material was calculated to be 1.07 m by nitrogen adsorption specific surface area analysis test method and BET (Brunauer Emmett Teller) method. 2 The testing instrument can be a Tri-Star 3020 specific surface area pore size analyzer produced by Micromeritics, USA.

[0231] The powder resistivity of the carbon material was measured using a four-probe method with a powder resistivity tester according to GB / T 30835-2014. The powder resistivity of the carbon material at a pressure of 8 MPa was found to be 0.0110 Ω.cm. The test instrument can be a Suzhou Jingge ST2722 powder resistivity tester.

[0232] Referring to JIS K 0131-1996 and JB / T 4220-2011, the average interlayer spacing d of the (002) plane in the carbon material crystal structure was obtained. 002 Then according to the formula g=(0.344-d 002 ) / (0.344-0.3354)×100%, the graphitization degree of the carbon material is 97.3%. The testing instrument can be a Bruker D8 Discover X-ray diffractometer.

[0233] (2) Preparation of button cells (half-cells)

[0234] The carbon material prepared above was thoroughly stirred and mixed with the binder styrene-butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC), and the conductive agent carbon black in an appropriate amount of deionized water at a mass ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry. The negative electrode slurry was evenly coated on the surface of the negative electrode current collector copper foil and dried in an oven for later use. Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed at a volume ratio of 1:1:1 to obtain an organic solvent, and LiPF6 was dissolved in the organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L. A metal lithium sheet was then used as the counter electrode and a polyethylene (PE) film as the separator to assemble a CR2430 button cell in an argon-protected glove box.

[0235] (3) Preparation of secondary batteries (full batteries)

[0236] The carbon material prepared above, the conductive agent carbon black (Super P), the binder styrene-butadiene rubber, and the thickener sodium carboxymethyl cellulose were thoroughly stirred and mixed in an appropriate amount of deionized water at a weight ratio of 96:1:1:2 to form a negative electrode slurry. The negative electrode slurry was coated on both surfaces of the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.

[0237] LiFePO4 was mixed with conductive carbon black and polyvinylidene fluoride in a weight ratio of 96:2.5:1.5. An appropriate amount of NMP solvent was added and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on both surfaces of the positive electrode current collector aluminum foil. After drying and cold pressing, a positive electrode sheet was obtained.

[0238] A polypropylene film with a thickness of 12 μm is used as an isolation membrane, and is placed in order with the positive electrode sheet and the negative electrode sheet prepared above, so that the isolation membrane is located between the positive electrode sheet and the negative electrode sheet to play an isolation role, and then the electrode assembly is obtained by winding; the electrode assembly is placed in an outer package, dried, and then injected with the same electrolyte as the button battery prepared above, and after vacuum packaging, standing, formation, capacity and other processes, a secondary battery is obtained.

[0239] Comparative Example 1

[0240] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.

[0241] The 100 mesh flake graphite was mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 11 μm and a BET specific surface area of ​​7 m 2 / g, and then half-cells and full cells were prepared using the obtained natural spherical graphite as carbon material.

[0242] Comparative Example 2

[0243] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.

[0244] The 100 mesh flake graphite was mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 11 μm and a BET specific surface area of ​​7 m 2 The obtained natural spherical graphite and petroleum asphalt (softening point temperature of 148°C, volume distribution particle size Dv50 of 4.5μm, and coking value of 40%) were mixed in a VC mixer at a mass ratio of 100:20 for 30 minutes. The mixed material was then graphitized at 3200°C for 10 hours and then cooled to room temperature to obtain a carbon material.

[0245] Comparative Example 3

[0246] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.

[0247] The 100 mesh flake graphite was mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 11 μm and a BET specific surface area of ​​7 m 2 The obtained natural spherical graphite was mixed with petroleum pitch (softening point temperature of 148°C, volume distribution particle size Dv50 of 4.5 μm, and coking value of 40%) at a mass ratio of 100:20 in a VC mixer for 30 minutes. The mixed material was then carbonized at 1300°C for 2 hours and then cooled to room temperature to obtain a carbon material.

[0248] Comparative Example 4

[0249] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.

[0250] Raw graphite ore is processed into small particles through mechanical treatment. It is then treated with a strong alkaline solution and a strong acid solution at high temperature to remove impurities. After washing and drying at high temperature, it is screened to produce plate-like natural graphite. To sphericalize the plate-like natural graphite, primary and secondary grinding, i.e., mechanical processing, is performed. Subsequently, after acid treatment, washing, and drying, purification is performed to obtain high-purity spherical natural graphite. The mechanical crushing and grinding process damages the surface of the resulting spherical natural graphite, and chemically reactive groups are formed after strong alkaline / strong acid cleaning. During spheroidization, defects are introduced into the natural graphite due to mechanical processing. Carbon coating is achieved by dry-coating the damaged, high-purity solid-phase natural graphite with pitch (softening point temperature of 148°C, volume distribution particle size Dv50 of 4.5 μm, and coking value of 40%) onto the surface. The carbon coating is then performed at 1200°C for 24 hours in an inert gas atmosphere. The carbon material is then crushed, screened, and iron removed.

[0251] Comparative Example 5

[0252] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.

[0253] The 100 mesh flake graphite was mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 11 μm and a BET specific surface area of ​​7 m 2 / g. The obtained natural spherical graphite was mixed with powdered medium-temperature pitch (quinoline insoluble content of 1%, softening point of 80°C) and toluene accounting for 0.5% of the asphalt mass in a mass ratio of 1:1. The mixture was then added to a sealed reactor and heated to 200°C at a rate of 3°C / min. The temperature was maintained at this temperature for 4 hours, with the pressure maintained at 0.1 MPa. The sample was then removed and, after cooling, loaded into a furnace for graphitization at 3000°C. The graphitized sample was crushed and classified to obtain a carbon material.

[0254] Comparative Example 6

[0255] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.

[0256] The 100 mesh flake graphite was mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 11 μm and a BET specific surface area of ​​7 m 2 / g.

[0257] The obtained natural spherical graphite and petroleum asphalt (softening point temperature of 148 ° C, volume distribution particle size Dv50 of 4.5 μm, coking value of 40%) were mixed in a VC mixer for 30 minutes. The mixed materials were then put into a reactor, and the reactor was gradually heated at a heating rate of 2 ° C / min. While heating, the reactor was kept in a uniform stirring state, and the temperature was raised to 190 ° C. The reactor was pumped to a pressure of -0.1 MPa, and then kept warm for 2 hours. After the insulation was completed, the reactor was heated to 650 ° C and kept warm for 2 hours. After that, the reactor was cooled to about 160 ° C, and then petroleum asphalt was slowly added to the reactor. The mass ratio of the amount of petroleum asphalt added this time to the previous petroleum asphalt was 1:1. After that, the reactor was heated to 190 ° C again, the reactor was pumped to a pressure of -0.1 MPa, and then kept warm for 2 hours. After that, the reactor was heated to 650 ° C and kept warm for 2 hours. After that, the temperature was cooled by condensation cooling. Finally, the material processed by the above process was heat-treated at 1300°C for 2 hours, and the heat-treated sample was crushed and sieved to obtain a carbon material with no pores inside.

[0258] Examples 2-7 and Comparative Example 7

[0259] The preparation methods of half cells and full cells are similar to those in Example 1, except that the preparation process parameters of the carbon material are adjusted. See Table 1 for details.

[0260] Table 1

[0261]

[0262] Examples 8-13

[0263] The preparation methods of half cells and full cells are similar to those in Example 1, except that the parameters of the filling material in the preparation process of the carbon material are adjusted. See Table 2 for details.

[0264] Table 2

[0265]

[0266] Examples 14-23

[0267] The preparation methods of half cells and full cells are similar to those in Example 3, except that the parameters of step 2 in the preparation process of the carbon material are adjusted. See Table 3 for details.

[0268] Table 3

[0269]

[0270] Examples 24-28

[0271] The preparation methods of half cells and full cells are similar to those in Example 1, except that the parameters of step 1 in the preparation process of the carbon material are adjusted. See Table 4 for details.

[0272] Table 4

[0273]

[0274] Performance Testing

[0275] (1) Total pore area test in the outer and inner regions of carbon materials

[0276] Mix the sample preparation binder and carbon material powder evenly, then apply the mixture to copper foil and dry at 60°C for 30 minutes. Cut the sample into 6mm x 6mm pieces and affix them to the sample stage of a CP-type argon ion cross-section polisher. Use a plasma beam to cut the sample to obtain a cross section of the carbon material, with the cross section passing through the center of the carbon material particle. The testing instrument can be the IB-09010CP-type argon ion cross-section polisher from JEOL, Japan.

[0277] The cross section of the carbon material was scanned using a scanning electron microscope. The test may refer to JY / T010-1996. The testing instrument may be a Sigma 300 scanning electron microscope from the German ZEISS company.

[0278] The area extending 0.25L from the particle surface of the carbon material to the interior of the particle is recorded as the outer area, and the area inside the outer area is recorded as the inner area, where L represents the minor axis length of the carbon material particle. The total pore area S1 of the outer area of ​​the carbon material and the total pore area S2 of the inner area of ​​the carbon material are calculated using image processing software. The image processing software can be AVIZO.

[0279] (2) Raman spectroscopy test of carbon materials

[0280] The Raman spectrometer was used under the following test conditions: excitation wavelength of 532 nm, grating of 600 lines, objective lens of 50 times, integration time of 10 s, accumulation times of 3 times, surface scanning, and the D peak and G peak intensities of 100 points were obtained. The I of 100 points was calculated. D / I G , remove the largest and smallest 30 I D / I G The average value of the remaining 40 points is the I D / I G The testing instrument may be a Horiba LabRAM HR800 Raman spectrometer.

[0281] (3) The first coulombic efficiency test of carbon materials

[0282] At 25°C, the button cell prepared above was first discharged at a constant current of 0.15 mA to 0.005 V, allowed to stand for 5 minutes, and then discharged at a constant current of 10 μA to 0.005 V, and the first-cycle discharge capacity of the button cell was recorded. Thereafter, the button cell was charged at a constant current of 0.3 mA to 2.0 V, and the first-cycle charge capacity of the button cell was recorded.

[0283] The first coulombic efficiency of the carbon material (%) = the first cycle charging capacity of the button cell / the first cycle discharging capacity of the button cell × 100%.

[0284] (4) Cycle performance test of secondary batteries

[0285] At 45°C, the prepared secondary battery was charged at a constant current of 1C to the upper cutoff voltage (corresponding to 100% SOC), then charged at a constant voltage to a current of 0.05C. After standing for 5 minutes, the secondary battery was discharged at a constant current of 1C to the lower cutoff voltage (corresponding to 0% SOC). The discharge capacity at this point was recorded as the first cycle discharge capacity. The secondary battery was subjected to a cyclic charge and discharge test according to the above method, and the discharge capacity after each cycle was recorded. Capacity retention rate (%) of the secondary battery after 1000 cycles at 45°C = discharge capacity after 1000 cycles / discharge capacity after 1 cycle × 100%.

[0286] (5) Storage performance test of secondary batteries

[0287] At 25°C, the secondary battery prepared above was charged at a constant current of 1C to the upper cutoff voltage (corresponding to 100% SOC), and then charged at a constant voltage to a current of 0.05C. After standing for 5 minutes, the secondary battery was discharged at a constant current of 1C to the lower cutoff voltage (corresponding to 0% SOC), and the discharge capacity at this time was recorded, which was the discharge capacity before storage.

[0288] At 25°C, the prepared secondary battery was charged at a constant current of 1C to the upper cutoff voltage (corresponding to 100% SOC), and then charged at a constant voltage to a current of 0.05C. The secondary battery was then stored in a thermostat at 60°C for 150 days. Capacity retention (%) of the secondary battery after 150 days of storage at 60°C = discharge capacity after storage / discharge capacity before storage × 100%.

[0289] Table 5

[0290]

[0291]

[0292] The parameters such as specific surface area, volume distribution particle size, powder resistivity, powder compaction density, tap density, and degree of graphitization of the carbon materials prepared in Examples 1-28 are all within the ranges described in the specification of this application.

[0293] The Raman spectra of the carbon materials prepared in the examples of this application all meet the requirement of 0.150≤I D / I G ≤0.280. At this point, on the one hand, it can effectively reduce the content of disordered carbon, reduce the surface activity of the carbon material, and reduce the consumption of active ions by the SEI film formation on the particle surface. On the other hand, it can also make the carbon material have a stable structure and avoid particle breakage as much as possible. Therefore, the carbon material provided in this application has small volume expansion, high structural stability and low surface activity, and can enable the battery to have high gram capacity, high initial coulombic efficiency, high capacity retention rate after cycling, and high capacity retention rate after storage.

[0294] The Raman spectra of the carbon materials prepared in Comparative Examples 1-7 do not satisfy 0.150≤I D / I G ≤0.280, and none of them can make the battery have high gram capacity, high initial coulombic efficiency, high capacity retention rate after cycle and high capacity retention rate after storage. D / I G are all greater than 0.280. In this case, the disordered carbon content in the carbon material is high, the surface active sites of the carbon material are many, and the surface defect content is high, thereby causing a large irreversible consumption of active ions, and thus failing to achieve a high gram capacity, a high initial coulombic efficiency, a high capacity retention rate after cycling, and a high capacity retention rate after storage for the battery. D / I G Both are less than 0.150. At this time, the content of disordered carbon on the surface of the carbon material particles is relatively low, and the active sites on the particle surface are relatively few. However, the ability of active ions to quickly escape and embed is deteriorated, and the volume change of the carbon material during the charge and discharge process of the battery is still relatively large. As a result, the carbon material particles are more easily broken, and the battery cannot take into account high gram capacity, high first coulombic efficiency, high capacity retention rate after cycle, and high capacity retention rate after storage.

[0295] From the test results in Table 5, it can be seen that when the carbon material further satisfies S2>S1, optionally satisfies 1.5≤S2 / S1≤450, and more optionally satisfies 2≤S2 / S1≤400, the carbon material can further improve the battery's gram capacity, first coulombic efficiency, capacity retention rate after cycling, and capacity retention rate after storage. At this time, the carbon material particles further have the following characteristics: the number of pores in the inner region is large and / or the pore size is large, while the number of pores in the outer region is small and / or the pore size is small. The pore structure in the inner region of the carbon material can reserve the required expansion space for the volume change of the carbon material particles, thereby reducing the risk of carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions and reducing the irreversible capacity loss of the secondary battery. The number of pores in the outer region of the carbon material is small and / or the pore size is small, thereby making the carbon material particles have a more stable structure and avoiding the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions and reducing the consumption of active ions by the SEI film formation inside the particles. This can further improve the battery's gram capacity, initial coulombic efficiency, capacity retention rate after cycling, and capacity retention rate after storage.

[0296] The carbon materials prepared in Comparative Examples 1-6 also do not satisfy S2>S1.

[0297] Comparative Example 1 uses untreated natural spherical graphite as the carbon material, which has relatively many pores both inside and outside.

[0298] The carbon materials prepared in Comparative Examples 2-4 form a carbon layer coating on the surface of natural spherical graphite, but the carbon layer only exists on the surface of natural spherical graphite and fails to achieve a filling effect. Moreover, the carbon layer cannot effectively prevent the electrolyte from penetrating into the pore structure inside the particles, which leads to limited improvement in the battery's first coulombic efficiency, cycle performance and storage performance.

[0299] When preparing the carbon material in Comparative Example 5, the softening point temperature of the filling material used is relatively low, and the small molecular substances in the filling material will volatilize during the graphitization treatment, resulting in the actual residual carbon in the filling area being unable to effectively fill the pore structure of the natural spherical graphite, failing to achieve an effective filling effect, and failing to effectively prevent the electrolyte from penetrating into the pore structure inside the particles, which in turn leads to limited improvement in the battery's cycle performance and storage performance.

[0300] When preparing the carbon material in Comparative Example 6, the filling material is filled into all the pore structures inside the natural spherical graphite particles by vacuum extraction, and there is no pore structure inside the carbon material particles obtained at this time. As a result, the volume change of the carbon material during the extraction and embedding of active ions is large, and the particles are more easily broken, which in turn leads to limited improvement in the cycle performance and storage performance of the battery.

[0301] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A carbon material, wherein The carbon material includes a pore structure, and the carbon material satisfies 0.150≤I D / I G ≤0.280, I D The Raman spectrum of the carbon material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the carbon material is 1580±50cm -1 The G peak intensity at .

2. The carbon material according to claim 1, wherein 0.152 ≤ I D / I G ≤0.280, selectable area, 0.155≤I D / I G ≤0.

220.

3. The carbon material according to claim 1 or 2, wherein The carbon material includes at least one pore with an area greater than or equal to 0.15 μm 2 The pore structure may include one or more pores with an area of ​​0.15 μm 2 -2.0μm 2 pore structure.

4. The carbon material according to any one of claims 1 to 3, wherein The carbon material includes an external region and an internal region located inside the external region. The external region refers to the region extending from the particle surface of the carbon material to the interior of the particle by a distance of 0.25L, and L refers to the short axis length of the carbon material particle. The total pore area of ​​the external region is recorded as S1, and the total pore area of ​​the internal region is recorded as S2, and S2>S1.

5. The carbon material according to claim 4, wherein 1.5≤S2 / S1≤450, optionally, 2≤S2 / S1≤400.

6. The carbon material according to claim 4 or 5, wherein 0.01μm 2 ≤S1≤5.0μm 2 , optionally, 0.02 μm 2 ≤S1≤4.5μm 2 and / or, 2.5μm 2 ≤S2≤25.0μm 2 , optionally, 3.0 μm 2 ≤S2≤22.5μm 2 .

7. The carbon material according to any one of claims 4 to 6, wherein L≥4μm, optionally, 4μm≤L≤20μm.

8. The carbon material according to any one of claims 4 to 7, wherein The area of ​​the pore structure in the outer region of the carbon material is less than or equal to 0.15 μm 2 , can be selected to be less than or equal to 0.10μm 2 and / or, The inner region of the carbon material includes at least one area greater than or equal to 0.15 μm 2 The pore structure may optionally include one or more pores with an area of ​​0.15 μm 2 -2.0μm 2 pore structure.

9. The carbon material according to any one of claims 4 to 8, wherein The interlayer spacing of the outer region of the carbon material is recorded as d1, and the interlayer spacing of the inner region of the carbon material is recorded as d2, and the carbon material satisfies d1≥d2; Optionally, d1>d2; Optionally, d1 is 0.33565nm-0.33620nm; Optionally, d2 is 0.33557nm-0.33589nm.

10. The carbon material according to any one of claims 1 to 9, wherein The carbon material satisfies at least one of the following: (1) The specific surface area of ​​the carbon material is ≤2.1m 2 / g, optional 0.7m 2 / g-1.8m 2 / g; (2) The volume distribution particle size Dv50 of the carbon material is 6.0 μm-30.0 μm, and can be optionally 8.0 μm-25.0 μm; (3) The volume distribution particle size Dv90 of the carbon material is 16.0 μm-45.0 μm, and can be optionally 17.0 μm-42.0 μm; (4) The particle size distribution of the carbon material (Dv90-Dv10) / Dv50 is ≤1.55, and can be optionally 0.5-1.

50.

11. The carbon material according to any one of claims 1 to 10, wherein The carbon material satisfies at least one of the following: (1) The powder resistivity of the carbon material under a pressure of 8 MPa is 0.006 Ω.cm-0.051 Ω.cm, and can be optionally 0.010 Ω.cm-0.040 Ω.cm; (2) The powder compaction density of the carbon material under a pressure of 20,000 N is 1.70 g / cm 3 -1.95g / cm 3 , optional 1.72g / cm 3 -1.92g / cm 3 ; (3) The tap density of the carbon material is 0.80 g / cm 3 -1.35g / cm 3 , optional 0.85g / cm 3 -1.30g / cm 3 ; (4) The gram capacity of the carbon material is 350 mAh / g-372 mAh / g, and can be optionally 353 mAh / g-371 mAh / g; (5) The graphitization degree of the carbon material is 92.0%-98.0%, and can be optionally 92.5%-97.6%; (6) The morphology of the carbon material includes one or more of block, spherical and quasi-spherical shapes.

12. A method for preparing a carbon material, comprising the following steps: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and a filler material in a predetermined ratio, and then maintaining the mixture at a first temperature T1 for a first time t1 to obtain an intermediate; step 3, maintaining the obtained intermediate at a second temperature T2 for a second time t2 to obtain a carbon material, wherein: The carbon material includes a pore structure, and the carbon material satisfies 0.150≤I D / I G ≤0.280, I D The Raman spectrum of the carbon material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the carbon material is 1580±50cm -1 The G peak intensity at .

13. The method according to claim 12, wherein: The raw materials satisfy at least one of the following: (1) The raw material includes natural graphite, and optionally, the natural graphite includes one or more of flake graphite, natural spherical graphite and microcrystalline graphite; (2) The volume distribution particle size Dv50 of the raw material is 6.0 μm-30.0 μm, and can be optionally 8.0 μm-25.0 μm; (3) The specific surface area of ​​the raw material is ≥2.5m 2 / g, optional 2.5m 2 / g-10.0m 2 / g.

14. The method according to claim 12 or 13, wherein: The filling material satisfies at least one of the following: (1) The softening point temperature of the filling material is 100°C-180°C, and can be optionally 120°C-160°C; (2) The coking value of the filler material is 25%-50%, and can be optionally 30%-42%; (3) The volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be optionally 1 μm-5 μm.

15. The method according to claim 14, wherein The filling material includes one or more of coal tar, petroleum tar, polymer compound and resin, and can be selected to include one or more of coal tar and petroleum tar.

16. The method according to any one of claims 12 to 15, wherein: The mass ratio of the filling material to the raw material is (10-32):100, and can be optionally (15-25):

100.

17. The method according to any one of claims 12 to 16, wherein: The heating process of uniformly mixing the raw material and the filling material in a predetermined ratio and then heating the mixture to the first temperature T1 is a staged heating process, which may optionally include a first heating process, a second heating process and a third heating process.

18. The method according to claim 17, wherein The first heating process is heating to 200-250°C and keeping the temperature at this temperature for 1-2 hours; and / or, The second temperature raising process is to raise the temperature to 450°C-550°C and keep the temperature at this temperature for 1h-2h; and / or, The third temperature raising process is to raise the temperature to the first temperature T1 and keep the temperature at the first time t1.

19. The method according to any one of claims 12 to 18, wherein: The temperature is raised to the first temperature T1 at a rate of 1°C / min-10°C / min.

20. The method according to any one of claims 12 to 19, wherein: The first temperature T1 is 700° C.-1200° C., optionally 720° C.-1100° C.; and / or, The first time t1 is 1 hour to 5 hours, and can be optionally 2 hours to 4 hours.

21. The method according to any one of claims 12 to 20, wherein: The second temperature T2 is 1800° C.-2600° C., optionally 1900° C.-2450° C.; and / or, The second time t2 is 1.5 hours to 6 hours, and can be optionally 2 hours to 5 hours.

22. A secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises the carbon material according to any one of claims 1 to 11 or the carbon material prepared by the method according to any one of claims 12 to 21.

23. An electric device comprising the secondary battery according to claim 22.

Citation Information

Patent Citations

  • Negative electrode material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery using same

    CN102362380A

  • Graphite particles for nonaqueous secondary battery and method for producing same, negative electrode and nonaqueous secondary battery

    CN103443977A

  • Negative electrode active material and secondary battery

    CN112310352A

  • Starting material of negative electrode material for nonaqueous secondary batteries, negative electrode material for nonaqueous secondary batteries, negative electrode for nonaqueous secondary batteries, and nonaqueous secondary battery

    CN113646920A

  • Porous carbon material

    JP2020114804A