Binder for electric storage device, electrode for electric storage device, electric storage device, polymer composite, and method for producing binder for electric storage device
By using the polymer complex of polyimide precursor and cyclic molecules as the binder, the problem of insufficient mechanical characteristics of the lithium-ion battery electrode is solved, and the charge and discharge cycle characteristics are significantly improved, which enhances the battery's Coulomb efficiency and stability.
Patent Information
- Application Number
- CN202480001531.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-22
- Publication Date
- 2024-12-03
AI Technical Summary
The mechanical properties of the existing binder for lithium-ion battery electrodes are insufficient, and the effect of improving the charge and discharge cycle characteristics is insufficient.
A polymer complex composed of a polyimide precursor and a cyclic molecule having multiple ether bonds is used as a binder, and an amide bond is formed by reacting the tetracarboxylic acid component with the diamine component at a high temperature. , thereby improving the breaking energy and charge and discharge cycle characteristics of the binder.
The mechanical characteristics and charge and discharge cycle characteristics of the lithium-ion battery electrode are significantly improved, and the Coulomb efficiency and charge and discharge stability of the battery are enhanced.
Smart Images

Figure CN119072804A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a binder for a storage device having excellent mechanical properties and capable of improving charge-discharge cycle properties, an electrode for a storage device and a storage device obtained using the binder for a storage device, and a method for producing the binder for a storage device. In addition, the present invention also relates to a polymer composite having excellent mechanical properties. Background Art
[0002] Polyimide is widely used in electrical and electronic equipment such as flexible wiring boards and TAB (Tape Automated Bonding) tapes due to its excellent heat resistance, solvent resistance (chemical resistance), mechanical properties, and electrical properties. For example, polyimide obtained from aromatic tetracarboxylic dianhydride and aromatic diamine, particularly polyimide obtained from 3,3',4,4'-biphenyltetracarboxylic dianhydride and p-phenylenediamine, is preferably used.
[0003] In addition, polyimide has also been studied as a binder for storage devices such as a binder for electrodes of lithium ion batteries. For example, Patent Document 1 discloses a binder for lithium ion battery electrodes, which includes a polyimide precursor obtained using a specified aromatic tetracarboxylic dianhydride and a specified diamine, a polyimide or polyamide-imide, and a lithium salt. In addition, Patent Document 1 discloses a negative electrode obtained by mixing a polyamic acid and 12-crown ether-4 obtained by using an aromatic tetracarboxylic dianhydride and a diamine with a negative electrode active material.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2013-89437 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, the binder for lithium ion battery electrodes disclosed in Patent Document 1 has insufficient mechanical properties and insufficient effect of improving charge and discharge cycle characteristics.
[0009] An object of the present invention is to provide a binder for an electrical storage device which has excellent mechanical properties and can improve charge and discharge cycle characteristics.
[0010] Means for solving problems
[0011] In order to solve the above-mentioned problems, the inventors conducted intensive research and found that the binder based on a polymer composite formed by compounding a polyimide precursor and a cyclic molecule having multiple ether bonds has a particularly high fracture energy among mechanical properties, and can improve the charge and discharge cycle characteristics when applied to storage devices, thereby completing the present invention.
[0012] That is, the present invention provides the following [1] to
[11] .
[0013] [1] A binder for an electric storage device, comprising a polymer composite, wherein the polymer composite is a composite of a polyimide precursor comprising a reaction product of a tetracarboxylic acid component and a diamine component and / or a polyimide obtained by imidizing a part or all of the polyimide precursor, and a cyclic molecule having a plurality of ether bonds.
[0014] [2] The binder for a power storage device according to [1], wherein the cyclic molecule is at least one selected from the group consisting of cyclodextrin, crown ether, and thiocrown ether.
[0015] [3] A binder for a storage device as described in [1] or [2], wherein the content ratio of the above-mentioned cyclic molecules in the above-mentioned binder is 4 mol% to 25 mol% relative to 100 mol% of the total of the amic acid groups and imide groups contained in the above-mentioned polyimide precursor and / or the polyimide obtained by imidizing a part or all of the above-mentioned polyimide precursor.
[0016] [4] The binder for an electrical storage device according to any one of [1] to [3], wherein the ratio of the alicyclic tetracarboxylic dianhydride in 100 mol % of the tetracarboxylic acid component is 35 mol % or more.
[0017] [5] The binder for an electrical storage device according to any one of [1] to [4], wherein the polymer composite is obtained by reacting the tetracarboxylic acid component and the diamine component in the presence of the cyclic molecule.
[0018] [6] A varnish comprising the binder for an electric storage device according to any one of [1] to [5].
[0019] [7] An electrode for an electricity storage device, comprising the binder for an electricity storage device according to any one of [1] to [5] and an active material.
[0020] [8] The electrode for an electric storage device according to [7], wherein the active material is a negative electrode active material containing silicon.
[0021] [9] An electricity storage device comprising the electrode described in [7] or [8].
[0022]
[10] A method for producing a binder for a power storage device, which is a method for producing the binder for a power storage device according to any one of [1] to [5], wherein:
[0023] The production method includes a step of reacting a tetracarboxylic acid component and a diamine component in the presence of a cyclic molecule having a plurality of ether bonds to prepare a polyimide precursor.
[0024]
[11] A polymer composite comprising a polyimide precursor comprising a reaction product of a tetracarboxylic acid component and a diamine component and / or a polyimide obtained by imidizing a part or all of the polyimide precursor, and a cyclic molecule having a plurality of ether bonds, wherein:
[0025] The ratio of the alicyclic tetracarboxylic dianhydride in 100 mol % of the said tetracarboxylic acid component is 35 mol % or more.
[0026] Effects of the Invention
[0027] According to the present invention, there can be provided a binder for a storage device having excellent mechanical properties and capable of improving charge-discharge cycle characteristics, an electrode for a storage device and a storage device obtained by using the binder for a storage device, and a method for producing the binder for a storage device. In addition, the present invention can also provide a polymer composite having excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 IR spectra of Example 1 and Comparative Example 2.
[0029] Figure 2 IR spectra of Example 2 and Comparative Example 4. DETAILED DESCRIPTION
[0030] <Binder for power storage devices>
[0031] The binder for a storage battery device of the present invention is a binder for a storage battery device, which contains a polymer composite, wherein the polymer composite is a composite of a polyimide precursor containing a reaction product of a tetracarboxylic acid component and a diamine component and / or a polyimide obtained by imidizing a part or all of the polyimide precursor, and a cyclic molecule having multiple ether bonds (including a substance in which a part or all of the ether bonds are thioether bonds, the same applies hereinafter).
[0032] In addition, below, first, the case where the polymer composite is a composite of a polyimide precursor containing a reaction product of a tetracarboxylic acid component and a diamine component and a cyclic molecule having a plurality of ether bonds will be described.
[0033] The binder for a storage device of the present invention may contain a polyimide precursor (hereinafter also referred to as "polyimide precursor") containing a reaction product of a tetracarboxylic acid component and a diamine component and a cyclic molecule having a plurality of ether bonds (hereinafter also referred to as "cyclic molecule"), and may contain a substance in which at least a portion of such a polyimide precursor is complexed with at least a portion of such a cyclic molecule to form a polymer complex. That is, the binder for a storage device of the present invention may contain a non-complexed polyimide precursor and a non-complexed cyclic molecule in addition to a substance in which at least a portion of a polyimide precursor is complexed with at least a portion of a cyclic molecule to form a polymer complex. In addition, the binder for the storage device of the present invention may contain, in addition to the polyimide precursor, a polyimide in which a part or all of the polyimide precursor is imidized (that is, it may contain a partially imidized polyimide in which a part of the amic acid structure constituting the polyimide precursor is imidized, or a fully imidized polyimide in which all of the amic acid structure constituting the polyimide precursor is imidized).
[0034] In the present invention, the term "complexation of a polyimide precursor and a cyclic molecule" means that the polyimide precursor and the cyclic molecule are physically or chemically complexed. For example, it means that even when the binder for a storage battery device of the present invention is heated at a temperature 50°C or higher than the boiling point of the cyclic molecule (i.e., (boiling point of the cyclic molecule + 50)°C or higher) for 5 minutes or more (more specifically, when heated at 350°C for 5 minutes or more), out of 100% by weight of the total amount of cyclic molecules contained in the binder for a storage battery device of the present invention, 10% by weight or more of the cyclic molecules remain without volatilization. For example, in the case of containing 18-crown-6 (boiling point: 190° C.) as a cyclic molecule, it means that when the binder is heated at a certain rate from room temperature to a temperature of 240° C. or higher for 5 minutes or more (more specifically, when heated at 350° C. or higher for 5 minutes or more), 10% or more of 18-crown-6 remains without volatilization out of 100% by weight of the total amount of 18-crown-6 contained in the binder for a storage device. When the binder for a storage device of the present invention is heated at a high temperature of (the boiling point of the cyclic molecule + 50)° C. or higher for 5 minutes or more, the amount of the cyclic molecules remaining without volatilization is preferably 15 to 100% by weight, more preferably 20 to 100% by weight out of 100% by weight of the total amount of the cyclic molecules contained in the binder for a storage device of the present invention. It should be noted that the above measurement can be performed in the state of a varnish prepared by dissolving or dispersing the binder for a storage device of the present invention in a solvent. In addition, in the present invention, at least a portion of the polyimide precursor and at least a portion of the cyclic molecule can be composited by forming a rotaxane structure. It should be noted that, depending on the type of cyclic molecule, when heated at a high temperature of (the boiling point of the cyclic molecule + 50) ° C or more for more than 5 minutes, in addition to the volatile components, there are uncompounded and carbonized components, the proportion of the carbonized components when the cyclic molecules are heated alone is calculated in advance, and the amount obtained by subtracting the amount of the carbonized components is interpreted as the amount of the cyclic molecules that are not volatilized and remain. For example, for α-cyclodextrin, the proportion of the carbonized components is about 10% by weight, so this value can be subtracted.
[0035] In the present invention, the reason why the fracture energy is high and the charge-discharge cycle characteristics can be improved by compounding at least a part of the polyimide precursor with at least a part of the cyclic molecule is not necessarily clear, but it is believed that this is because: by compounding them, high strength can be achieved while maintaining high flexibility, thereby effectively showing a tracking or mitigation effect on the expansion and contraction caused by charging and discharging of the active material used in the storage device.
[0036] The polyimide precursor is obtained by reacting a tetracarboxylic acid component with a diamine component to form an amide bond (-CONH-). The polyimide precursor preferably contains a repeating unit represented by the following formula (1), more preferably 50 mol% or more, further preferably 75 mol% or more, and still more preferably 90 mol% or more.
[0037] [Chemistry 1]
[0038]
[0039] In the above formula (1), A is one or more selected from tetravalent groups obtained by removing a carboxyl group from an aromatic tetracarboxylic acid or an aliphatic tetracarboxylic acid, and B is one or more selected from divalent groups obtained by removing an amino group from an aromatic diamine or an aliphatic diamine.
[0040] As a tetracarboxylic acid component, aromatic tetracarboxylic dianhydride, aliphatic tetracarboxylic dianhydride, etc. are mentioned, for example. These may be used individually or in combination of 2 or more types.
[0041] As the aromatic tetracarboxylic dianhydride, tetracarboxylic dianhydride having an aromatic ring can be preferably used. Specific examples of the aromatic tetracarboxylic dianhydride include 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), pyromellitic dianhydride (hereinafter also referred to as "PMDA"), 2,3,3',4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, diphenylsulfone-3,4,3',4'-tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride (also known as 4,4'-(hexafluoroisopropylidene)diphthalic anhydride), 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl) )methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylenebis(trimellitic acid monoester anhydride), p-biphenylenebis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride, and the like. These may be used alone or in combination of two or more.
[0042] As the aliphatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride (a tetracarboxylic dianhydride having an alicyclic structure and no aromatic ring) can be preferably used. Specific examples of alicyclic tetracarboxylic dianhydrides include (1R, 2S, 4S, 5R)-cyclohexanetetracarboxylic dianhydride (hereinafter referred to as "H'-PMDA"), (1S, 2R, 4S, 5R)-cyclohexanetetracarboxylic dianhydride, (1S, 2S, 4R, 5R)-cyclohexanetetracarboxylic dianhydride (hereinafter referred to as "H'-PMDA"), bicyclo [2.2.2] octane-2,3,5,6-tetracarboxylic dianhydride, bicyclo [2.2.2] oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (hereinafter referred to as "BTA"), 4-(2 ,5-dioxotetrahydrofuran-3-yl)-tetrahydronaphthalene-1,2-dicarboxylic anhydride, tetrahydrofuran-2,3,4,5-tetracarboxylic dianhydride, bicyclo-3,3',4,4'-tetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride (hereinafter also referred to as "CBDA"), 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,4-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclohexanetetracarboxylic dianhydride, pentacyclic [8.2.1.1 4,7 .0 2,9 .0 3,8 ]tetradecane-5,6,11,12-tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, cyclohex-1-ene-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride, etc. These may be used alone or in combination of two or more.
[0043] In the present invention, from the perspective of further improving the fracture energy, further improving the charge-discharge cycle characteristics, and the effect of improving the charge-discharge characteristics such as the coulomb efficiency, it is preferred to use at least alicyclic tetracarboxylic dianhydride as the tetracarboxylic acid component, and the proportion of alicyclic tetracarboxylic dianhydride in 100 mol% of the tetracarboxylic acid component is preferably 35 mol% or more, more preferably 50 mol% or more, further preferably 70 mol% or more, still more preferably 90 mol% or more, and particularly preferably 100 mol% of the alicyclic tetracarboxylic dianhydride.
[0044] From the perspective of improving the charge-discharge cycle characteristics, coulomb efficiency and other charge-discharge characteristics, as alicyclic tetracarboxylic dianhydrides, H"-PMDA, CBDA, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride (CpODA), [1,1'-bis(cyclohexane)]-3,3',4,4'-tetracarboxylic acid (H-BPDA), H"-PMDA, BTA are preferred. In order to further improve the charge-discharge cycle characteristics, H"-PMDA and CBDA are more preferred. In addition, as aromatic tetracarboxylic dianhydrides, s-BPDA and PMDA are preferred. In order to further improve the charge-discharge cycle characteristics, PMDA is more preferred.
[0045] Examples of the diamine compound as the diamine component include 4,4'-diaminodiphenyl ether (hereinafter also referred to as "ODA"), 2,2'-dimethylbenzidine, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, p-phenylenediamine (PPD), m-phenylenediamine, 2,4-diaminotoluene, 1,3-bis(4-aminophenoxy)benzene (hereinafter also referred to as "TPE-R"), 1,4-bis(4-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, m-phenylenediamine, Aromatic diamines having an aromatic group, such as methylamine, p-phenylenediamine, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-methylenebis(2,6-xylidine), α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, 2,2'-dimethyl-4,4'-aminobiphenyl, 3,3'-dimethyl-4,4'-aminobiphenyl, 2,2'-ethylenedianiline, and 4,4'-diaminobenzanilide (hereinafter also referred to as "DABAN"); 1,4-diaminocyclohexane, 1,4 -diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,2-diaminocyclohexane, 1,3-diaminocyclobutane, 1,4-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, Alicyclic diamines having an alicyclic structure such as diaminobicycloheptane, diaminomethylbicycloheptane, diaminooxybicycloheptane, diaminomethyloxybicycloheptane, isophoronediamine, diaminotricyclodecane, diaminomethyltricyclodecane, bis(aminocyclohexyl)methane, bis(aminocyclohexyl)isopropylidene, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, and 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane;2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,3,5,6-tetrafluoro-1,4-diaminobenzene, 2,4,5,6-tetrafluoro-1,3-diaminobenzene, 2,3,5,6-tetrafluoro-1,4-benzene(dimethylamine), 2,2'-difluoro-(1,1'-biphenyl)-4,4'-diamine, 2,2',6,6'-tetrafluoro-(1,1'-biphenyl)-4,4'-diamine, 4,4'-diaminooctafluorobiphenyl, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-oxygen Fluorine-containing diamines such as 2,3,5,6-tetrafluoroaniline, 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether, 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene, 2,2-bis[4-[4-amino-2-(trifluoromethyl)phenoxy]hexafluoropropane, 3,5-diaminotrifluorinated benzene, 4,4-diamino-2-(trifluoromethyl)diphenyl ether; ester-bonded diamines such as 4-aminobenzoic acid 4-aminophenyl ester and terephthalic acid bis(4-aminophenyl). These can be used alone or in combination of two or more. ;
[0046] From the viewpoint of improving the charge-discharge cycle characteristics and coulombic efficiency, the diamine compound as the diamine component is preferably ODA, TPE-R, or DABAN, and more preferably ODA alone or a combination of ODA and TPE-R or DABAN.
[0047] As a cyclic molecule, as long as it is a compound having multiple ether bonds and a cyclic molecular structure, it is not particularly limited. From the aspect of further improving the fracture energy and the aspect of further improving the improvement effect of the charge-discharge cycle characteristics, it is preferably selected from at least one of cyclodextrin, crown ether and thiocrown ether, more preferably cyclodextrin, crown ether, and more preferably crown ether. As cyclodextrin, α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, etc. can be cited, as crown ether, 12-crown ether-4, 15-crown ether-5, 18-crown ether-6, dibenzo-18-crown ether-6, diaza-18-crown ether-6, etc. can be cited, wherein, from the aspect of its high effect, 18-crown ether-6 is preferred.
[0048] The content ratio of the cyclic molecules in the binder for storage devices of the present invention is preferably 4 mol% to 25 mol%, more preferably 10 mol% to 20 mol%, relative to the total 100 mol% of the amic acid group and the imide group contained in the polyimide precursor and / or the polyimide obtained by imidizing a part or all of the polyimide precursor. In addition, the content ratio of the cyclic molecules in the binder for storage devices of the present invention, calculated on a weight basis, is preferably 5 wt% to 25 wt%, more preferably 10 wt% to 20 wt%, relative to the total 100 wt% of the polyimide precursor and the cyclic molecules.
[0049] <Method for producing a binder for an electric storage device>
[0050] The method for producing a binder for an electricity storage device of the present invention includes the step of reacting a tetracarboxylic acid component and a diamine component in the presence of a cyclic molecule to form an amide bond, thereby forming a polyimide precursor.
[0051] According to the present invention, when the tetracarboxylic acid component and the diamine component are reacted, the presence of cyclic molecules allows at least a portion of the polyimide precursor to be complexed with at least a portion of the cyclic molecules, thereby forming a polymer complex of the complexed molecules.
[0052] As a method for reacting a tetracarboxylic acid component with a diamine component in the presence of a cyclic molecule, there is no particular limitation. For example, by reacting approximately equimolar tetracarboxylic acid components and diamine components in the presence of a cyclic molecule in a solvent at a relatively low temperature of 100°C or below, preferably 80°C or below, in a manner such that an imidization reaction does not proceed or does not proceed excessively, a polymer composite can be obtained in a state where the polymer composite is dissolved in the solvent, i.e., in a state of a polymer composite solution. It should be noted that in the polymer composite solution thus obtained, in addition to the polyamic acid as a polyimide precursor, a polyimide formed by an imidization reaction may also be included. At this time, as a polyimide, it may be a polyimide in which a part of the amic acid structure of the polyimide precursor is imidized, or it may be a polyimide that is fully imidized. In addition, at this time, in addition to at least a part of the polyimide precursor, at least a part of the polyimide may also be in a state of being compounded with a cyclic molecule.
[0053] The polymerization temperature when obtaining the polyimide precursor is preferably 25°C or more and 100°C or less, more preferably 40°C or more and 80°C or less, and further preferably 50°C or more and 80°C or less. The polymerization time is preferably 0.1 hours or more and 24 hours or less, and more preferably 2 hours or more and 12 hours or less. By making the polymerization temperature and the polymerization time within the above range, a high molecular weight polyimide precursor can be easily obtained with good production efficiency. The polymerization can also be carried out in an air atmosphere, usually in an inert gas, preferably nitrogen atmosphere. The molar ratio of the tetracarboxylic acid component and the diamine component is approximately equimolar, specifically, 0.90 or more and 1.10 or less, preferably 0.95 or more and 1.05 or less, more preferably more than 0.98 and 1.04 or less, and more preferably more than 0.98 and 1.03 or less. In addition, in this specification, "substantially equimolar" means that the above-mentioned molar ratio exceeds the range of 0.99 to 1.01, and "equimolar" means a significant figure of 1.00 for the molar ratio.
[0054] When the tetracarboxylic acid component and the diamine component are reacted in the presence of a cyclic molecule, a method of adding the cyclic molecule and the diamine component to a polymerization apparatus filled with a solvent, confirming that the cyclic molecule and the diamine component are dissolved, and then adding the tetracarboxylic acid component can be preferably used.
[0055] As the solvent used when the tetracarboxylic acid component and the diamine component are reacted in the presence of a cyclic molecule, any solvent may be used as long as the polyimide precursor can be polymerized and the polyimide precursor can be dissolved, and the solvent may be an aqueous solvent or an organic solvent. The solvent may be a mixture of two or more organic solvents, or a mixed solvent of two or more organic solvents or a mixed solvent of water and one or more organic solvents may be used. The organic solvent is not particularly limited, and examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, hexamethylphosphoric triamide, 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, tetrahydrofuran, bis[2-(2-methoxyethoxy)ethyl]ether, 1,4-dioxane, dimethyl sulfoxide, dimethyl sulfone, diphenyl ether, sulfolane, diphenyl sulfone, tetramethyl urea, anisole, m-cresol, phenol, and γ-butyrolactone.
[0056] The binder for storage devices of the present invention can be produced by removing the solvent used for polymerization from the polymer complex solution obtained as described above. There is no particular limitation on the method for removing the solvent, and examples include a method of drying the solvent. In addition, the binder for storage devices of the present invention can be dissolved or dispersed in a solvent to form a varnish containing the binder for storage devices. As a solvent for the varnish constituting the binder for storage devices, the solvent used when polymerizing the polyimide precursor in the presence of cyclic molecules can be directly used as a solvent for the varnish of the binder for storage devices, or a solvent different from the solvent used in the polymerization can also be used. In the case of using a solvent different from the solvent used in the polymerization, the solvent used in the polymerization can be removed by drying, etc., and then dissolved or dispersed in other solvents, or it can be replaced with other solvents.
[0057] The solid content concentration of the polymer complex in the varnish of the binder for storage devices is not particularly limited, but is preferably 5 mass % to 45 mass %, more preferably 5 mass % to 40 mass %, and further preferably more than 10 mass % and 30 mass % relative to the total amount of the polymer complex and the solvent.
[0058] To the varnish of the binder for storage devices, known additives such as amine compounds and dehydrating agents that promote imidization reaction, organic phosphorus compounds, the above-mentioned fillers, surfactants, silane coupling agents, and leveling agents may be added as necessary.
[0059] As the amine compound, there can be mentioned substituted or unsubstituted nitrogen-containing heterocyclic compounds, N-oxide compounds of the nitrogen-containing heterocyclic compounds, substituted or unsubstituted amino acid compounds, aromatic hydrocarbon compounds or aromatic heterocyclic compounds having hydroxyl groups, etc. Specific examples of the imidization catalyst include imidazole derivatives such as 1,2-dimethylimidazole, N-methylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 5-methylbenzimidazole, and N-benzyl-2-methylimidazole, and substituted pyridine derivatives such as isoquinoline, 3,5-lutidine, 3,4-lutidine, 2,5-lutidine, 2,4-lutidine, and 4-n-propylpyridine. The amount of the imidization catalyst used is preferably 0.01 equivalent or more and 2 equivalents or less, more preferably 0.02 equivalent or more, and more preferably 1 equivalent or less, relative to the amic acid unit of the polyamide precursor. By using an imidization catalyst, the physical properties of the resulting binder for a power storage device, particularly the elongation and edge tearing resistance, may be improved.
[0060] Examples of other amine compounds include aliphatic tertiary amines such as trimethylamine and triethylenediamine, aromatic tertiary amines such as dimethylaniline, and heterocyclic tertiary amines such as isoquinoline, pyridine, α-picoline, and β-picoline, and they can be added as needed.
[0061] Examples of the dehydrating agent include aliphatic carboxylic anhydrides such as acetic anhydride, propionic anhydride, and butyric anhydride, and aromatic carboxylic anhydrides such as benzoic anhydride.
[0062] Examples of the organic phosphorus-containing compound include phosphoric acid esters such as monocaproyl phosphate, monooctyl phosphate, monolauryl phosphate, monomyristyl phosphate, monocetyl phosphate, monostearyl phosphate, monophosphate of triethylene glycol monotridecyl ether, monophosphate of tetraethylene glycol monolauryl ether, monophosphate of diethylene glycol monostearyl ether, dicaproyl phosphate, dioctyl phosphate, didecanoyl phosphate, dilauryl phosphate, dimyristyl phosphate, dicetyl phosphate, distearyl phosphate, diphosphate of tetraethylene glycol mononeopentyl ether, diphosphate of triethylene glycol monotridecyl ether, diphosphate of tetraethylene glycol monolauryl ether, and diphosphate of diethylene glycol monostearyl ether, and amine salts of these phosphoric acid esters. Examples of the amine include ammonia, monomethylamine, monoethylamine, monopropylamine, monobutylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, monoethanolamine, diethanolamine, and triethanolamine.
[0063] In addition, in the present invention, by imidizing the polyimide precursor contained in the polymer composite constituting the binder for storage devices, a polymer composite formed by imidizing the polyimide precursor containing the reactant of the tetracarboxylic acid component and the diamine component and a cyclic molecule having multiple ether bonds can be prepared. In this case, it is sufficient to form a substance in a state where at least a portion of the polyimide is composited with at least a portion of the cyclic molecule to form a polymer composite. That is, the binder for storage devices of the present invention can be a substance containing uncomplexed polyimide and uncomplexed cyclic molecules in addition to a substance in a state where at least a portion of the polyimide is composited with at least a portion of the cyclic molecule.
[0064] The polyimide preferably has a polyimide containing a repeating unit represented by the following formula (2) as a main component (50 mol % or more), more preferably 75 mol % or more, and further preferably 90 mol % or more. That is, the polyimide may be a partially imidized polyimide in which a part of the amic acid structure contained in the polyimide precursor is imidized, or a fully imidized polyimide in which all the amic acid structures contained in the polyimide precursor are imidized, or a polyimide mixed with these.
[0065] [Chemistry 2]
[0066]
[0067] In the above formula (2), X1 is one or more tetravalent groups obtained by removing carboxyl groups from aromatic or aliphatic tetracarboxylic acids, and Y1 is one or more divalent groups obtained by removing amino groups from aromatic or aliphatic diamines.
[0068] In the present invention, the polyimide and the cyclic molecule are composited as long as the polyimide and the cyclic molecule are composited physically or chemically. For example, it means that even when the binder for a storage device of the present invention is heated at a temperature higher than the boiling point of the cyclic molecule by 50°C or more (i.e., (the boiling point of the cyclic molecule + 50)°C or more) for 5 minutes or more (more specifically, when heated at 350°C for 5 minutes or more), 10% or more of the cyclic molecules in the total amount of 100% by weight of the cyclic molecules contained in the binder for a storage device of the present invention remain without volatilization. When the binder for a storage device of the present invention is heated at a high temperature higher than (the boiling point of the cyclic molecule + 50)°C for 5 minutes or more, the amount of the cyclic molecules remaining without volatilization is preferably 15 to 100% by weight, and more preferably 20 to 100% by weight, in the total amount of 100% by weight of the cyclic molecules contained in the binder for a storage device of the present invention. It should be noted that the above measurement can be performed in the state of a varnish containing the binder for a storage device of the present invention. In the present invention, at least a part of the polyimide and at least a part of the cyclic molecule may be composited by constituting a rotaxane structure.
[0069] The method for imidizing the polyimide precursor is not particularly limited, and examples thereof include a method of chemically imidizing / or thermally imidizing a polymer composite containing a polyimide precursor and a cyclic molecule. When chemically imidizing / or thermally imidizing, the method may be performed in the state of a solution of the polymer composite containing a polyimide precursor and a cyclic molecule, or in a state where the solvent has been removed by drying or the like.
[0070] In the present invention, chemical imidization and / or thermal imidization can be carried out by heat treatment. If thermal imidization is used as an example, the maximum heating temperature in the heat treatment is usually 150°C or more, preferably 200°C or more, more preferably 250°C or more, and more preferably 350°C or more. The upper limit of the heat treatment temperature is preferably 450°C or less, more preferably 430°C or less, and more preferably 400°C or less as long as the characteristics are not reduced. It should be noted that the heat treatment can also be carried out in an air atmosphere, and is usually suitable for an inert gas, preferably a nitrogen atmosphere. Chemical imidization depends on the type of additives such as a chemical imidization catalyst, and milder heat treatment conditions than thermal imidization can be applied. For example, it is usually 100°C or more, preferably 120°C or more, more preferably 150°C or more, and more preferably 200°C or more, usually 360°C or less, preferably 300°C or less, more preferably 250°C or less, and more preferably 220°C or less.
[0071] The heat treatment of chemical imidization and / or thermal imidization can be carried out in stages. For example, it is preferred to carry out the first heat treatment at a relatively low temperature of 100°C to 170°C for more than 0.5 minutes and less than 30 minutes, followed by a second heat treatment at a temperature of more than 170°C and less than 220°C for more than 0.5 minutes and less than 30 minutes, and then, at a high temperature of more than 220°C and less than 350°C, a third heat treatment is carried out for more than 0.5 minutes and less than 30 minutes, and then a fourth high-temperature heat treatment can be carried out from more than 350°C to the highest heating temperature. The heat treatment is preferably carried out continuously. For example, it is preferred to carry out the heat treatment from a relatively low temperature of 100°C to 170°C to the highest heating temperature. There is no particular restriction on the heating rate, and it is preferably more than 1°C / minute and less than 30°C / minute, and particularly preferably more than 2°C / minute and less than 20°C / minute. If it is in the above range, the foaming caused by the rapid temperature increase can be suppressed, so it is preferred.
[0072] <Electrodes for power storage devices>
[0073] The electrode for the storage device of the present invention contains the above-mentioned storage device binder and active material. The active material can be any one of a negative electrode active material and a positive electrode active material. That is, the electrode for the storage device of the present invention can be a negative electrode or a positive electrode.
[0074] When the electrode for the electrical storage device of the present invention is a negative electrode, examples of the negative electrode active material, particularly the negative electrode active material for a lithium secondary battery, include lithium metal, lithium alloy, carbon materials capable of occluding and releasing lithium [easily graphitizable carbon, hardly graphitizable carbon with an interplanar spacing of the (002) plane of 0.37 nm or more, graphite with an interplanar spacing of the (002) plane of 0.34 nm or less, etc.], tin (elemental), tin compounds, silicon (elemental), silicon compounds, Li4Ti5O 12 and lithium titanate compounds such as the like. They can be used alone or in combination of two or more. As the negative electrode active material, since the effect of improving the charge-discharge cycle characteristics brought by using the binder for the electrical storage device of the present invention is great, silicon (elemental) or a silicon-containing negative electrode active material such as a silicon compound is preferred. The silicon (elemental) or a silicon-containing negative electrode active material such as a silicon compound has a much larger theoretical capacity than graphite. On the other hand, the volume expansion rate of the negative electrode active material itself during charging is relatively large. On the other hand, according to the binder for the electrical storage device of the present invention, since the fracture energy is high, it is considered that such volume expansion can be appropriately alleviated, and thus the charge-discharge cycle characteristics can be more appropriately improved.
[0075] The silicon-containing negative electrode active material is not particularly limited. For example, it may include silicon (elemental), silicon compounds, partial substituents of silicon, partial substituents of silicon compounds, solid solutions of silicon compounds, etc. As a specific example of the silicon compound, SiO x silicon oxides represented by (0.05 < x < 1.95), SiC y silicon carbides represented by (0 < y < 1), SiN z silicon nitrides represented by (0 < z < 4 / 3), and silicon alloys such as silicon alloys with a foreign element M1. In the silicon alloy, as the foreign element M1, at least one element selected from the group consisting of Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, and Ti is preferably used.
[0076] In addition, the partial substituent of silicon is a compound in which a part of the silicon contained in silicon (elemental) and silicon compounds is replaced by a foreign element M2. Specific examples of the foreign element M2 include, for example, B, Mg, Ni, Ti, Mo, Co, Ca, Cr, Cu, Fe, Mn, Nb, Ta, V, W, Zn, C, N, and Sn. Among these silicon-containing negative electrode active materials, silicon (elemental), silicon oxides, or silicon alloys are preferred, and silicon (elemental) or silicon oxides are more preferred.
[0077] When the electrode used in the storage device of the present invention is a negative electrode, in addition to the negative electrode active material, a conductive material may also be contained. As a conductive material, there is no particular restriction as long as it is an electronic conductive material that does not cause chemical changes. Preferably, metal powders such as copper, nickel, titanium or aluminum, carbon materials, etc. are used. As carbon materials, graphites such as natural graphite (flake graphite, etc.), artificial graphite, one or more carbon blacks selected from acetylene black, ketjen black, channel black, furnace black, lamp black and thermal black, fibrous carbon powders such as carbon nanotubes and carbon fibers, etc. can be cited.
[0078] When the electrode for the power storage device of the present invention is a positive electrode, as a positive electrode active material, in particular as a positive electrode active material for a lithium secondary battery, a composite metal oxide containing one or more selected from cobalt, manganese and nickel and lithium can be cited. Examples of such lithium composite metal oxides include LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x Ni x O2(0.01 <x<1)、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、LiNi 1 / 2 Mn 3 / 2 O4、LiCo 0.98 Mg 0.02 O2, etc. In addition, LiCoO2 and LiMn2O4, LiCoO2 and LiNiO2, LiMn2O4 and LiNiO2 can also be used in combination.
[0079] When the electrode used in the storage device of the present invention is a positive electrode, it may contain a conductive material in addition to the positive electrode active material. As the conductive material, there is no particular limitation as long as it is an electronic conductive material that does not cause chemical changes. For example, graphite such as natural graphite (flaky graphite, etc.), artificial graphite, one or more carbon blacks selected from acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black, carbon nanotubes, fibrous carbon powders such as carbon fibers can be preferably cited.
[0080] The electrode for the storage device of the present invention can be prepared by mixing the storage device binder of the present invention, the negative electrode active material or the positive electrode active material, and the conductive material used as needed to obtain an electrode mixture, and molding it into a sheet shape. When the storage device binder of the present invention, the negative electrode active material or the positive electrode active material, and the conductive material used as needed are mixed, a solvent can be used to make a slurry. In addition, at this time, as the storage device binder of the present invention, when a varnish-state binder is used, the negative electrode active material or the positive electrode active material is mixed with the conductive material used as needed in the varnish state to make a slurry. At this time, in order to adjust the solid content concentration, a solvent can be further added.
[0081] The electrode for the storage device of the present invention can be formed into a sheet by, for example, casting or coating a slurry containing the storage device binder of the present invention, the negative electrode active material or the positive electrode active material, and the conductive material used as needed on a conductive collector such as aluminum foil or copper foil, performing a heat treatment to remove the solvent, and performing a pressure treatment as needed to form an active material layer on the collector. As the storage device binder of the present invention, when a binder containing a polymer composite formed by a polyimide precursor and a cyclic molecule is used, the imidization reaction can be carried out by heating when the active material layer is formed on the collector, and the polyimide precursor can be made into a polyimide.
[0082] The thickness of the active material layer of the present invention can be appropriately determined according to the application and the desired capacity. Although not limited, it is preferably used in a range of 0.1 μm or more and 500 μm or less. It is more preferably 1 μm or more, further more preferably 10 μm or more, further more preferably 20 μm or more, more preferably 300 μm or less, further more preferably 100 μm or less, further more preferably 50 μm or less.
[0083] <Electrical Storage Devices>
[0084] The power storage device of the present invention comprises the electrode for the power storage device of the present invention. The power storage device includes power storage devices such as lithium batteries, electric double layer capacitors, and lithium ion capacitors. Among them, lithium batteries using lithium salts as electrolyte salts are preferred, and lithium secondary batteries are preferred.
[0085] The lithium secondary battery includes a positive electrode, a negative electrode, a non-aqueous electrolyte, other separators, etc., and the known structure required for the lithium secondary battery can be adopted. In the present invention, as the positive electrode and / or the negative electrode, the electrode for the storage device of the present invention is used. In addition, the lithium secondary battery can be a lithium polymer battery using a gel electrolyte as an electrolyte, or an all-solid-state battery using an inorganic solid electrolyte such as an oxide system or a sulfide system.
[0086] The non-aqueous electrolyte solution is prepared by dissolving an electrolyte salt in a non-aqueous solvent. The non-aqueous electrolyte solution is not particularly limited, and various non-aqueous electrolyte solutions can be used.
[0087] As the electrolyte salt, an electrolyte salt dissolved in a non-aqueous electrolyte is used, for example, inorganic lithium salts such as LiPF6, LiBF4, LiPO2F2, LiN(SO2F)2, LiClO4, lithium salts containing chain fluorinated alkyl groups such as LiN(SO2CF3)2, LiN(SO2C2F5)2, LiCF3SO3, LiC(SO2CF3)3, LiPF4(CF3)2, LiPF3(C2F5)3, LiPF3(CF3)3, LiPF3(iso-C3F7)3, LiPF5(iso-C3F7), lithium salts containing cyclic fluorinated alkylene chains such as (CF2)2(SO2)2NLi and (CF2)3(SO2)2NLi, and lithium salts having oxalate complexes as anions such as lithium bis[oxalate-O,O']borate or lithium difluoro[oxalate-O,O']borate.
[0088] The concentration of all these electrolyte salts dissolved in the nonaqueous solvent is preferably 0.3 M or more, more preferably 0.5 M or more, and even more preferably 0.7 M or more. The upper limit is preferably 2.5 M or less, more preferably 2.0 M or less, and even more preferably 1.5 M or less.
[0089] As the non-aqueous solvent, cyclic carbonate, chain carbonate, chain ester, ether, amide, phosphoric acid ester, sulfone, lactone, nitrile, S=O bond-containing compound etc. can be cited, preferably including cyclic carbonate. It should be noted that the term "chain ester" is used as a concept including chain carbonate and chain carboxylic acid ester.
[0090] As cyclic carbonate, one or more selected from ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 4-fluoro-1,3-dioxolane-2-one (FEC), trans- or cis-4,5-difluoro-1,3-dioxolane-2-one (hereinafter both are collectively referred to as "DFEC"), vinylene carbonate (VC), vinylethylene carbonate (VEC) and 4-ethynyl-1,3-dioxolane-2-one (EEC) can be cited. The proportion of cyclic carbonates having an alkylene chain in all cyclic carbonates is preferably 55% to 100% by volume, more preferably 60% by volume or more, and more preferably 90% by volume or less.
[0091] In addition, in order to achieve appropriate physical properties, non-aqueous solvents are preferably used in a mixed manner. Its combination, for example, can include a combination of cyclic carbonates and chain esters. As chain esters, preferably, one or more asymmetric chain carbonates selected from ethyl methyl carbonate (MEC), methyl propyl carbonate (MPC), methyl isopropyl carbonate (MIPC), methyl butyl carbonate and ethyl propyl carbonate can be included; one or more symmetrical chain carbonates selected from dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate and dibutyl carbonate; pivalic acid esters such as methyl pivalate, ethyl pivalate, and propyl pivalate; one or more chain carboxylic acid esters selected from methyl propionate, ethyl propionate, propyl propionate, methyl acetate and ethyl acetate (EA); etc.
[0092] Example
[0093] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.
[0094] The abbreviations of the compounds used in the following examples are as follows.
[0095] H"-PMDA: (1R,2S,4S,5R)-cyclohexanetetracarboxylic dianhydride
[0096] CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride
[0097] PMDA: pyromellitic dianhydride
[0098] ODA: 4,4'-diaminodiphenyl ether
[0099] DABAN: 4,4'-diaminobenzanilide
[0100] TPE-R: 1,3-bis(4-aminophenoxy)benzene
[0101] α-CD: α-cyclodextrin
[0102] <Example 1>
[0103] [Production of polymer composite solution]
[0104] Into a reaction container equipped with a stirrer and a nitrogen inlet tube, 193.9311 g of NMP (N-methylpyrrolidone), 11.0689 g of 18-crown-6, 16.7726 g of ODA, and 4.7585 g of DABAN were added, and stirred at 50° C. for 2 hours under a nitrogen atmosphere. Then, 23.4689 g of H″-PMDA was added and reacted to form a polyimide precursor, thereby obtaining a polymer composite solution. At this time, H″-PMDA:ODA:DABAN (molar ratio)=100:80:20, and the amount of 18-crown-6 was 20 mol% relative to the total of 100 mol% of the amic acid group and the imide group contained in the polyimide precursor.
[0105] [TGA measurement]
[0106] The obtained polymer complex solution was heated from room temperature to 500°C at a heating rate of 20°C / min using a thermogravimetric measuring apparatus (product name "TG-DTA2000S", manufactured by Bruker AXS), and the weight was measured when the temperature reached 350°C. It should be noted that the residual rate of 18-crown-6 as a cyclic molecule relative to the input amount of 18-crown-6 when the temperature reached 350°C was calculated according to the following formula. The results are shown in Table 1.
[0107] Residual rate [weight %] = ((weight at 350°C [g]) - (theoretical value of weight when all 18-crown-6 is volatilized [g])) / ((theoretical value of weight when all 18-crown-6 is not volatilized [g]) - (theoretical value of weight when all 18-crown-6 is volatilized [g])) × 100
[0108] [IR measurement]
[0109] The polymer complex solution obtained above was spin-coated on an alkali-free glass wafer, and heated at 120°C, 150°C, 200°C, 250°C, and 300°C for 10 minutes each to remove the solvent and imidize to obtain a polymer complex film with a thickness of 10 μm. Then, the obtained polymer complex film was used to perform IR measurement using an IR measuring device (product name "FT / IR-4100", manufactured by JASCO Corporation). The results are shown in Figure 1 .
[0110] [Mechanical strength measurement]
[0111] The polymer composite solution obtained above was spin-coated on an alkali-free glass wafer, and heated at 120°C, 150°C, 200°C, 250°C, and 350°C for 10 minutes each to remove the solvent and imidize to obtain a polymer composite film with a thickness of 10 μm. Then, the obtained polymer composite film was used to measure the elastic modulus, elongation, and breaking energy using a tensile test device (product name "Tensilon (registered trademark) RTG-1350", manufactured by A&D Co., Ltd.). The results are shown in Table 2.
[0112] [Manufacturing of negative electrode sheet]
[0113] The polymer composite solution, silicon (Si) and acetylene black obtained above were mixed in a ratio of silicon (Si): polymer composite: acetylene black = 60:30:10 (weight ratio) to prepare a negative electrode mixture paste. The negative electrode mixture paste was applied to one side of a nickel-plated steel foil (collector), dried at 110°C for 1 minute, and then pressurized. The temperature was raised from room temperature to 360°C at a constant speed over 1.5 hours, heated at 360°C for 1.5 hours, and then naturally cooled to remove the solvent and imidize. The mixture was punched into a specified size to prepare a collector of 10 μm and a negative electrode sheet with a thickness of 20 μm.
[0114] [Battery production]
[0115] The negative electrode sheet obtained above was placed opposite to the metal lithium through a glass filter (GA-100 manufactured by ADVANTEC), and a non-aqueous electrolyte was added and sealed to produce a 2032-type button battery. It should be noted that as the non-aqueous electrolyte, a non-aqueous electrolyte in which LiPF6 as an electrolyte salt was dissolved in a non-aqueous solvent with ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1 (volume ratio) and 1% by weight of vinylene carbonate was added to form a 1M concentration was used.
[0116] [Evaluation of battery characteristics]
[0117] In a constant temperature chamber at 30°C, for the button-type batteries produced above, the charging was carried out in the direction in which Li was enclosed in the negative electrode sheet, and the constant current charging was performed at 0.1C to 0.001V, and the constant current discharge was performed at 0.1C to 1V, and the initial efficiency was calculated according to "initial efficiency [%] = discharge capacity [mAh] / charge capacity [mAh] × 100". Then, the charge and discharge were repeated under the above conditions to carry out a cycle test. The results of the cycle test were calculated as a ratio relative to the initial discharge capacity. The results are shown in Table 3. It should be noted that 0.1C C represents the current value during charging and discharging. For example, 1C refers to the current value that can fully discharge (or fully charge) the theoretical capacity in 1 / 1 hour, and 0.1C refers to the current value that can fully discharge (or fully charge) the theoretical capacity in 1 / 0.1 hour.
[0118] <Comparative Example 1>
[0119] Into a reaction container equipped with a stirrer and a nitrogen inlet tube, 205.0000 g of NMP (N-methylpyrrolidone), 16.7726 g of ODA, and 4.7585 g of DABAN were added, and after stirring at 50° C. for 30 minutes under a nitrogen atmosphere, 23.4689 g of H″-PMDA was added and reacted to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, H″-PMDA:ODA:DABAN (molar ratio)=100:80:20. Next, 11.0689 g of 18-crown ether-6 was added to the obtained polyimide precursor solution, and the mixture was mixed under air at room temperature to obtain a mixed solution of the polyimide precursor and 18-crown ether-6. It should be noted that the amount of 18-crown ether-6 was 20 mol% relative to 100 mol% of the total of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained mixed solution, TGA measurement was performed in the same manner as in Example 1 to measure the residual rate of 18-crown-6 as a cyclic molecule at 350° C. The results are shown in Table 1.
[0120] <Comparative Example 2>
[0121] Into a reaction container equipped with a stirrer and a nitrogen inlet tube, 205.0000 g of NMP (N-methylpyrrolidone), 16.7726 g of ODA, and 4.7585 g of DABAN were added, and after stirring at 50°C for 30 minutes under a nitrogen atmosphere, 23.4689 g of H"-PMDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, H"-PMDA:ODA:DABAN (molar ratio) = 100:80:20. Then, using the obtained polyimide precursor solution, IR measurement, mechanical strength measurement and battery characteristics evaluation were carried out in the same manner as in Example 1. The results are shown in Figure 1 , Table 2, 3.
[0122] <Example 2>
[0123] Into a reaction vessel equipped with a stirrer and a nitrogen inlet tube, 206.2725 g of NMP (N-methylpyrrolidone), 8.7275 g of 18-crown-6, 7.2400 g of TPE-R, and 11.5716 g of ODA were added, and stirred at 50° C. for 2 hours under a nitrogen atmosphere, and then 16.1883 g of CBDA was added to react to form a polyimide precursor, thereby obtaining a polymer composite solution. At this time, CBDA:TPE-R:ODA (molar ratio) = 100:30:70, and the amount of 18-crown-6 was 20 mol% relative to the total of 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained polymer composite solution, TGA measurement was performed in the same manner as in Example 1 to measure the residual rate of 18-crown-6 as a cyclic molecule at 350° C. In addition, IR measurement, mechanical strength measurement and battery characteristics evaluation were performed in the same manner as in Example 1. The results are shown in Table 1. Figure 2 , Table 2, 3.
[0124] <Comparative Example 3>
[0125] Into a reaction vessel equipped with a stirrer and a nitrogen inlet pipe, 215.0000 g of NMP (N-methylpyrrolidone), 7.2400 g of TPE-R, and 11.5716 g of ODA were added, and after stirring at 50° C. for 30 minutes under a nitrogen atmosphere, 16.1883 g of CBDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, CBDA: TPE-R: ODA (molar ratio) = 100: 30: 70. Next, 8.7275 g of 18-crown ether-6 was added to the obtained polyimide precursor solution, and mixed at room temperature under the atmosphere to obtain a mixed solution of the polyimide precursor and 18-crown ether-6. It should be noted that the amount of 18-crown ether-6 is 20 mol% relative to the total 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained mixed solution, TGA measurement was performed in the same manner as in Example 1 to measure the residual rate of 18-crown-6 as a cyclic molecule at 350° C. The results are shown in Table 1.
[0126] In addition, in Comparative Example 3, the polyimide precursor solution obtained above (solution before adding 18-crown ether-6), silicon element (Si) and acetylene black were mixed in a ratio of silicon element (Si): polyimide precursor: acetylene black = 60:30:10 (weight ratio), and then 18-crown ether-6 was added and mixed under the atmosphere at room temperature to obtain a negative electrode mixture paste. It should be noted that the amount of 18-crown ether-6 was 20 mol% relative to the total of 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained negative electrode mixture paste, the battery characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3. It should be noted that using the obtained negative electrode mixture paste, TGA measurement was performed in the same manner as in Example 1, and the residual rate of 18-crown ether-6 as a cyclic molecule at 360°C was measured, and the result was 8.79 weight%.
[0127] <Comparative Example 4>
[0128] Into a reaction vessel equipped with a stirrer and a nitrogen inlet pipe, 215.0000 g of NMP (N-methylpyrrolidone), 7.2400 g of TPE-R, and 11.5716 g of ODA were added, and after stirring at 50°C for 30 minutes under a nitrogen atmosphere, 16.1883 g of CBDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, CBDA:TPE-R:ODA (molar ratio) = 100:30:70. Then, using the obtained polyimide precursor solution, IR measurement, mechanical strength measurement and battery characteristics evaluation were performed in the same manner as in Example 1. The results are shown in Figure 2 , Table 2, 3.
[0129] <Example 3>
[0130] Into a reaction vessel equipped with a stirrer and a nitrogen inlet tube, 215.0000 g of NMP (N-methylpyrrolidone), 8.8448 g of 18-crown ether-6, and 16.7530 g of ODA were added, and after stirring at 50 ° C for 2 hours under a nitrogen atmosphere, 18.2470 g of PMDA was added to react to form a polyimide precursor, thereby obtaining a polymer composite solution. At this time, PMDA: ODA (molar ratio) = 100: 100, and the amount of 18-crown ether-6 was 20 mol% relative to the total of 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained polymer composite solution, TGA measurement was performed in the same manner as in Example 1 to measure the residual rate of 18-crown ether-6 as a cyclic molecule at 350 ° C. In addition, mechanical strength measurement and battery characteristics evaluation were performed in the same manner as in Example 1. The results are shown in Tables 1, 2, and 3. It should be noted that in Example 3, when manufacturing the negative electrode sheet, silicon element (Si): polymer composite: acetylene black = 60:25:15 (weight ratio). In addition, in the cycle test for evaluating battery characteristics, the charging and discharging of the first and second cycles were carried out at 0.1C, and the charging and discharging after the third cycle were carried out at 0.5C.
[0131] <Comparative Example 5>
[0132] Into a reaction vessel equipped with a stirrer and a nitrogen inlet tube, 215.0000 g of NMP (N-methylpyrrolidone) and 16.7530 g of ODA were added, and after stirring at 50 ° C for 30 minutes under a nitrogen atmosphere, 18.2470 g of PMDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, PMDA: ODA (molar ratio) = 100: 100. Next, 8.8448 g of 18-crown ether-6 was added to the obtained polyimide precursor solution, and mixed at room temperature under the atmosphere to obtain a mixed solution of the polyimide precursor and 18-crown ether-6. It should be noted that the amount of 18-crown ether-6 is 20 mol% relative to the total 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained mixed solution, TGA measurement was performed in the same manner as in Example 1 to measure the residual rate of 18-crown-6 as a cyclic molecule at 350° C. The results are shown in Table 1.
[0133] <Comparative Example 6>
[0134] Into a reaction vessel equipped with a stirrer and a nitrogen inlet pipe, 215.0000 g of NMP (N-methylpyrrolidone) and 16.7530 g of ODA were added, and after stirring at 50 ° C for 30 minutes under a nitrogen atmosphere, 18.2470 g of PMDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, PMDA: ODA (molar ratio) = 100: 100. Then, using the obtained polyimide precursor solution, mechanical strength measurement and battery characteristics were evaluated in the same manner as in Example 1. The results are shown in Tables 2 and 3. It should be noted that in Comparative Example 6, as in Example 3, when manufacturing the negative electrode sheet, the ratio of silicon element (Si): polymer composite: acetylene black was set to 60:25:15 (weight ratio). In addition, in the cycle test for evaluating the battery characteristics, charging and discharging were carried out at 0.1C in the first and second cycles, and at 0.5C after the third cycle.
[0135] <Example 4>
[0136] Into a reaction vessel equipped with a stirrer and a nitrogen inlet pipe, 187.4648 g of NMP (N-methylpyrrolidone), 12.5352 g of 18-crown-6, and 23.7610 g of ODA were added, and stirred at 50° C. for 2 hours under a nitrogen atmosphere. Then, 13.2990 g of H″-PMDA and 12.9400 g of PMDA were added and reacted to form a polyimide precursor, thereby obtaining a polymer composite solution. At this time, H″-PMDA:PMDA:ODA (molar ratio)=50:50:100, and the amount of 18-crown-6 was 20 mol% relative to 100 mol% of the total of amic acid groups and imide groups contained in the polyimide precursor. Then, using the obtained polymer composite solution, TGA measurement was performed in the same manner as in Example 1 to measure the residual rate of 18-crown-6 as a cyclic molecule at 350° C. In addition, mechanical strength measurement and battery characteristics evaluation were performed in the same manner as in Example 1. The results are shown in Tables 1, 2, and 3.
[0137] <Comparative Example 7>
[0138] Into a reaction container equipped with a stirrer and a nitrogen inlet tube, 200.0000 g of NMP (N-methylpyrrolidone) and 23.7610 g of ODA were added. After stirring at 50°C for 0.5 hour under a nitrogen atmosphere, 13.2990 g of H"-PMDA and 12.9400 g of PMDA were added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, H"-PMDA:PMDA:ODA (molar ratio) = 50:50:100. Then, using the obtained polyimide precursor solution, mechanical strength measurement and battery characteristics evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 2 and 3.
[0139] <Example 5>
[0140] Into a reaction vessel equipped with a stirrer and a nitrogen inlet tube, 198.9388 g of NMP (N-methylpyrrolidone), 16.0612 g of α-CD, 7.2400 g of TPE-R, and 11.5716 g of ODA were added, and after stirring at 50° C. for 2 hours under a nitrogen atmosphere, 16.1883 g of CBDA was added to react to form a polyimide precursor, thereby obtaining a polymer composite solution. At this time, CBDA:TPE-R:ODA (molar ratio) = 100:30:70, and the amount of α-CD was 10 mol% relative to the total of 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained polymer composite solution, TGA measurement was performed in the same manner as in Example 1. In addition, the battery characteristics were evaluated in the same manner as in Example 1. The results are shown in Tables 1 and 3.
[0141] It should be noted that in Example 5, in the TGA measurement, the residual amount of α-CD was determined at 350°C, similarly to the case of using 18-crown-6 as the cyclic molecule. On the other hand, when α-CD was measured alone at 600°C, the TGA measurement showed that there was about 10% by weight of carbonized components that were not volatilized. In Example 5, the TGA measurement at 350°C was estimated to be about 10% by weight lower than the measurement results shown in Table 1. In addition, regarding the evaluation of battery characteristics, in Example 5, when manufacturing the negative electrode sheet, silicon oxide: polymer composite: acetylene black = 80:15:5 (weight ratio), and in the cycle test, the discharge voltage was set to 1.5V.
[0142] <Comparative Example 8>
[0143] Into a reaction vessel equipped with a stirrer and a nitrogen inlet pipe, 215.0000 g of NMP (N-methylpyrrolidone), 7.2400 g of TPE-R, and 11.5716 g of ODA were added, and stirred at 50° C. for 0.5 hours under a nitrogen atmosphere, and then 16.1883 g of CBDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, CBDA:TPE-R:ODA (molar ratio) = 100:30:70. Next, the obtained polyimide precursor solution, silicon oxide and acetylene black were mixed in a ratio of silicon oxide:polyimide precursor:acetylene black = 80:15:5 (weight ratio), and α-CD was added, and mixed under air and at room temperature to obtain a negative electrode mixture paste. It should be noted that the amount of α-CD was 10 mol% relative to the total of 100 mol% of the amic acid group and the imide group contained in the polyimide precursor. Then, using the obtained negative electrode mixture paste, the battery characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3. It should be noted that in Comparative Example 8, the discharge voltage was set to 1.5V in the cycle test in the evaluation of battery characteristics.
[0144] <Comparative Example 9>
[0145] Into a reaction container equipped with a stirrer and a nitrogen inlet pipe, 215.0000 g of NMP (N-methylpyrrolidone), 7.2400 g of TPE-R, and 11.5716 g of ODA were added, and after stirring at 50°C for 0.5 hours under a nitrogen atmosphere, 16.1883 g of CBDA was added to react to form a polyimide precursor, thereby obtaining a polyimide precursor solution. At this time, CBDA:TPE-R:ODA (molar ratio) = 100:30:70. Then, using the obtained polyimide precursor solution, the battery characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3. It should be noted that in Comparative Example 8, when manufacturing the negative electrode sheet, silicon oxide: polymer composite: acetylene black = 80:15:5 (weight ratio), and in the cycle test in the evaluation of battery characteristics, the discharge voltage was set to 1.5 V.
[0146] [Table 1]
[0147] Table 1
[0148]
[0149]
[0150]
[0151] <Evaluation of TGA Measurement>
[0152] As can be seen from the results in Table 1, in Examples 1 to 5 in which a polyimide precursor is formed by reacting a tetracarboxylic acid component with a diamine component in the presence of 18-crown-6 as a cyclic molecule, a considerable amount of 18-crown-6 (boiling point: 190°C) or α-CD remains even when heated to 350°C, and the polyimide precursor or polyimide is complexed with at least a portion of 18-crown-6 or α-CD as a cyclic molecule to form a polymer complex.
[0153] On the other hand, in Comparative Examples 1, 3, and 5 in which 18-crown ether-6 as a cyclic molecule was mixed with the polyimide precursor, almost no 18-crown ether-6 remained when heated to 350°C, indicating that the polyimide precursor and the cyclic molecule 18-crown ether-6 were not complexed.
[0154] As described above, when 18-crown-6 as a cyclic molecule is mixed with the polyimide precursor as in Comparative Examples 1, 3, and 5, almost no 18-crown-6 as a cyclic molecule remains when the imidization reaction is carried out at a temperature of 300 to 350° C., and therefore, regarding the mechanical strength measurement and battery characteristics, it is appropriate to evaluate the state of the polyimide precursor solution without mixing 18-crown-6 as a cyclic molecule as in Comparative Examples 2, 4, 6, and 7. That is, it is considered that even if 18-crown-6 as a cyclic molecule is mixed with the polyimide precursor as in the above Comparative Examples 1, 3, and 5, the same results are obtained when 18-crown-6 as a cyclic molecule is not mixed, and therefore, as in Comparative Examples 2, 4, 6, and 7, 18-crown-6 as a cyclic molecule is not mixed, and the evaluation is performed in the state of the polyimide precursor solution.
[0155] <Evaluation of IR Measurement>
[0156] Figure 1 The IR spectra of Example 1 and Comparative Example 2 are shown in Figure 1 (A) is 750~800cm -1 The spectrum of Figure 1 (B) is 1680~1730cm -1 spectrum), Figure 2 The IR spectra of Example 2 and Comparative Example 4 are shown in Figure 2 (A) is 770~820cm -1 The spectrum of Figure 2 (B) is 1680~1730cm -1 Spectrum of ). Figure 1 , Figure 2 It is understood that the polyimide precursor or the polyimide is complexed with at least a part of the cyclic molecule 18-crown-6, and thus the shift of the peaks specific to the polyimide precursor and the polyimide is observed.
[0157] <Evaluation of Mechanical Strength Measurement>
[0158] As can be seen from the results in Table 2, according to Examples 1 to 4, the polyimide precursor or polyimide is complexed with at least a part of 18-crown-6 which is a cyclic molecule to form a polymer complex, and as a result, the fragmentation energy becomes high.
[0159] <Evaluation of Battery Characteristics>
[0160] As can be seen from the results in Table 3, according to Examples 1 to 5, the polyimide precursor or polyimide is complexed with at least a portion of 18-crown ether-6 or α-CD as a cyclic molecule to form a polymer complex, thereby achieving excellent charge and discharge cycle characteristics compared to the case where no polymer complex is formed.
[0161] On the other hand, in Comparative Examples 3 and 8 in which 18-crown ether-6 or α-CD as a cyclic molecule was mixed with the polyimide precursor, the results showed poorer charge-discharge cycle characteristics than in Comparative Examples 4 and 9 in which the cyclic molecule was not mixed. Based on this result, in Comparative Example 8 in which α-CD was mixed, it can be said that the cyclic molecule was not compounded, similarly to Comparative Example 3 in which 18-crown ether-6 as a cyclic molecule was mixed.
[0162] Industrial Applicability
[0163] The binder for a power storage device of the present invention is suitable for use in the production of a power storage device.
Claims
1. A binder for an electric storage device, comprising a polymer composite, wherein the polymer composite is a composite of a polyimide precursor containing a reaction product of a tetracarboxylic acid component and a diamine component and / or a polyimide obtained by imidizing a part or all of the polyimide precursor, and a cyclic molecule having a plurality of ether bonds.
2. The binder for an electrical storage device according to claim 1, wherein The cyclic molecule is at least one selected from cyclodextrin, crown ether and thiocrown ether.
3. The binder for an electrical storage device according to claim 1 or 2, wherein The content ratio of the cyclic molecules in the binder is 4 mol % to 25 mol % based on 100 mol % of the total of amic acid groups and imide groups contained in the polyimide precursor and / or a polyimide obtained by imidizing a part or all of the polyimide precursor.
4. The binder for an electrical storage device according to claim 1 or 2, wherein The ratio of the alicyclic tetracarboxylic dianhydride in 100 mol % of the tetracarboxylic acid component is 35 mol % or more.
5. The binder for an electrical storage device according to claim 1 or 2, wherein The polymer complex is obtained by reacting the tetracarboxylic acid component and the diamine component in the presence of the cyclic molecule. A varnish comprising the binder for an electric storage device according to claim 1 or 2. 7 . An electrode for an electricity storage device, comprising the binder for an electricity storage device according to claim 1 or 2 and an active material.
8. The electrode for an electric storage device according to claim 7, wherein The active material is a negative electrode active material containing silicon. 9 . An electricity storage device comprising the electrode according to claim 7 .
10. A method for producing a binder for a power storage device, which is a method for producing the binder for a power storage device according to claim 1 or 2, wherein: The production method includes a step of reacting a tetracarboxylic acid component and a diamine component in the presence of a cyclic molecule having a plurality of ether bonds to prepare a polyimide precursor.
11. A polymer composite, the polymer composite being a composite of a polyimide precursor comprising a reaction product of a tetracarboxylic acid component and a diamine component and / or a polyimide obtained by imidizing a part or all of the polyimide precursor, and a cyclic molecule having a plurality of ether bonds, wherein: The ratio of the alicyclic tetracarboxylic dianhydride in 100 mol % of the tetracarboxylic acid component is 35 mol % or more.
Citation Information
Patent Citations
Binder for lithium ion battery electrode, paste for lithium ion battery negative electrode using the same and manufacturing method of lithium ion battery negative electrode
JP2013089437A
Crown ether modified polyimide hybrid membrane and preparation method thereof
CN104356647A
Method for producing composite polymer, and composite polymer composition
JP2007046013A