Cylindrical lithium secondary battery
By using core type electrode assembly and specific electrolyte system in large-size cylindrical lithium secondary batteries, the problem of increased heat and explosion risks during fast charging is solved, and excellent output characteristics and life characteristics are achieved, which improves the battery's Safety and energy density.
Patent Information
- Application Number
- CN202380035889.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-29
- Filing Date
- 2023-06-29
- Publication Date
- 2024-12-03
AI Technical Summary
Large-size cylindrical lithium secondary batteries have problems such as increased heat, risk of explosion and reduced output during fast charging, and the precipitation of lithium at high voltages leads to rapid deterioration of the battery.
Using core-type electrode assembly and specific electrolyte systems, including lithium salts, organic solvents, lithium difluorophosphate, vinylene carbonate and 1,3-propanesulfonolide, to meet specific additive ratios and form factor ratios to form excellent Organic and inorganic membranes improve high temperature life characteristics and fast charging characteristics.
The excellent output characteristics and life characteristics of large-capacity cylindrical lithium secondary batteries are realized, which reduces the amount of gas generated and improves safety and energy density.
Smart Images

Figure CN119072812A_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Korean Patent Application No. 10-2022-0079872, filed on June 29, 2022, the disclosure of which is incorporated herein by reference. Technical Field
[0004] The invention relates to a cylindrical lithium secondary battery. Background Art
[0005] As technology of electric vehicles and portable electronic devices advances, demand for lithium secondary batteries as energy sources has significantly increased.
[0006] In particular, with the recent technological advancement of electric vehicles, the demand for high-capacity batteries has increased, and it is necessary to develop large-sized cylindrical batteries with large volume. For the small cylindrical batteries commonly used in the past, (that is, cylindrical batteries with a form factor of 1865 or 2170), high fast charging performance is not required.
[0007] However, for large-sized cylindrical batteries, since they are used in electric vehicles, fast charging characteristics become very important. Since the increase in the normal cross-sectional area of large-sized cylindrical batteries is not as large as the increase in volume, the heat generated in the battery increases as the size of the battery increases, and, as a result, the risk of explosion increases and problems such as reduced output occur. In addition, in the case of fast charging at high voltage, a situation may occur in which the battery deteriorates rapidly due to the precipitation of lithium from the negative electrode, and a problem may also occur in which the battery deteriorates or catches fire while a large amount of heat is generated around the electrode joint in a short period of time.
[0008] Therefore, there is a need to develop a cylindrical type battery having excellent lifespan characteristics and fast charging characteristics as well as a large volume in order to achieve high capacity. Summary of the invention
[0009] Technical issues
[0010] One aspect of the present invention provides a large-capacity cylindrical lithium secondary battery having excellent overall performance such as output characteristics, life characteristics, and rapid charging characteristics.
[0011] Technical Solution
[0012] According to one embodiment, the present invention provides a cylindrical lithium secondary battery, which includes: a core-wound electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator disposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is accommodated; an electrolyte injected into the battery can; and a seal that seals an open end of the battery can, wherein the electrolyte includes a lithium salt, an organic solvent, and lithium difluorophosphate, vinylene carbonate, and 1,3-propane sultone as additives, and satisfies formula (1).
[0013] Formula (1): 3.5 ≤ W LiDFP / (W VC +W PS )×Ф / H×100≤20
[0014] In formula (1), W LiDFP is the weight ratio of lithium difluorophosphate to the total electrolyte (%), W VC is the weight ratio of vinylene carbonate to the total electrolyte (%), W PS is the weight ratio (%) of 1,3-propane sultone to the total electrolyte, Φ is the diameter of the battery can (mm), and H is the height of the battery can (mm).
[0015] Beneficial Effects
[0016] The cylindrical lithium secondary battery according to the present invention is a large-capacity cylindrical lithium secondary battery, in which an electrolyte system different from a conventional electrolyte system used in a 1865 cell or a 2170 cell is required to be used. Therefore, the cylindrical lithium secondary battery according to the present invention has the effects of excellent high temperature life characteristics and fast charging characteristics by using an additive ratio according to an increased shape factor ratio.
[0017] Specifically, vinylene carbonate and 1,3-propane sultone are additives for forming an organic film on the surface of the negative electrode and the positive electrode during the initial activation process, and lithium difluorophosphate is an additive for forming an inorganic film containing fluorine (F) and phosphorus (P) on the electrode during the initial activation process. In the present invention, by allowing the required organic film and inorganic film to be formed according to the form factor related to the size of the cylindrical lithium secondary battery, the effect of excellent high temperature life characteristics and fast charging characteristics is achieved.
[0018] Furthermore, the cylindrical type lithium secondary battery according to the present invention may include a silicon-based negative electrode active material having a large capacity as a negative electrode active material, and in this case, a higher energy density may be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a diagram illustrating a stacked state of an electrode assembly according to the present invention before winding.
[0020] Figure 2 is a cross-sectional view illustrating a structure of an electrode plate of an electrode assembly according to one embodiment of the present invention.
[0021] Figure 3 is a cross-sectional view illustrating the structure of a cylindrical type battery having a tabless structure according to one embodiment of the present invention.
[0022] Figure 4 is a cross-sectional view illustrating the structure of a cylindrical type battery having a tabless structure according to another embodiment of the present invention.
[0023] Figure 5 is a diagram for explaining the structure of an electrode assembly according to one example of the present invention.
[0024] Figure 6 is a diagram for explaining a battery pack according to the present invention.
[0025] Figure 7 is a diagram for explaining a vehicle including a battery pack according to the present invention. DETAILED DESCRIPTION
[0026] Hereinafter, the present invention will be described in more detail.
[0027] It will be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in general dictionaries, and it will be further understood that the words or terms should be interpreted as having meanings consistent with their meanings in the context of the relevant art and the technical concept of the present invention based on the principle that the inventor can appropriately define the meanings of the words or terms to best interpret the present invention.
[0028] In the present invention, the expression "primary particle" means a particle unit in which no grain boundary exists in appearance when observed by using a scanning electron microscope having a field of view of 5,000 to 20,000 times. The expression "average particle size of primary particles" means the arithmetic mean of particle sizes calculated after measuring the particle sizes of primary particles observed in a scanning electron microscope image.
[0029] In the present invention, the expression "secondary particle" is a particle formed by aggregation of a plurality of primary particles. In the present invention, a secondary particle in which 10 or less primary particles are aggregated is referred to as a pseudo single particle in order to distinguish it from a conventional secondary particle formed by aggregation of tens to hundreds of primary particles.
[0030] The expression "average particle size D" in the present invention is 50" represents a particle size based on 50% in the volume cumulative particle size distribution of the positive electrode active material powder, which can be measured by using a laser diffraction method. For example, after the positive electrode active material powder is dispersed in a dispersion medium, the dispersion medium is introduced into a commercially available laser diffraction particle size measuring instrument (e.g., Microtrac MT3000), and then irradiated with an ultrasonic wave of about 28 kHz at an output of 60 W to obtain a volume cumulative particle size distribution diagram, and the average particle size D can then be measured by obtaining a particle size corresponding to 50% of the volume cumulative amount. 50 .
[0031] The expression "consisting essentially of A" in the present invention indicates that component A is included as a main component, wherein, for example, it means that the content of component A is 95 wt% to 100 wt%, preferably 98 wt% to 100 wt% and more preferably 99 wt% to 100 wt%.
[0032] A cylindrical lithium secondary battery according to the present invention includes: a core-wound electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator disposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is housed; and a sealing body that seals an open end of the battery can.
[0033] The electrolyte included in the cylindrical lithium secondary battery of the present invention is characterized in that it includes a lithium salt, an organic solvent, and lithium difluorophosphate, vinylene carbonate, and 1,3-propane sultone as additives, and satisfies the following formula (1).
[0034] Formula (1): 3.5 ≤ W LiDFP / (W VC +W PS )×Ф / H×100≤20
[0035] In formula (1), W LiDFP is the weight ratio of lithium difluorophosphate to the total electrolyte (%), W VC is the weight ratio of vinylene carbonate to the total electrolyte (%), W PS is the weight ratio (%) of 1,3-propane sultone to the total electrolyte, Φ is the diameter of the battery can (mm), and H is the height of the battery can (mm).
[0036] W LiDFP / (W VC +W PS The value of )×Φ / H×100 may be in the range of 3.5 to 20, preferably 5 to 15, and more preferably 10 to 15.
[0037] Vinylene carbonate and 1,3-propane sultone are additives for forming an organic film on the surface of the negative electrode and the positive electrode during the initial activation process, and lithium difluorophosphate is an additive for forming an inorganic film containing fluorine (F) and phosphorus (P) on the electrode during the initial activation process. In the present invention, by allowing the required organic and inorganic films to be formed according to the form factor related to the size of the cylindrical lithium secondary battery, the effects of excellent high temperature life characteristics and fast charging characteristics are achieved.
[0038] The electrolyte used in the cylindrical lithium secondary battery of the present invention includes a lithium salt, an organic solvent, and an additive.
[0039] Lithium difluorophosphate (LiPO2F2) used as an additive is reduced during the initial activation process to form an inorganic film including F and P on the electrode, and the inorganic film can inhibit the decomposition of the electrode film even at high temperatures by improving the durability of the solid electrolyte interface (SEI) film.
[0040] The electrolyte may include LiPO 2 F 2 in an amount of 0.01 wt % to 1 wt %, preferably 0.1 wt % to 1 wt %, and more preferably 0.2 wt % to 0.8 wt %, based on the total weight of the electrolyte.
[0041] Vinylene carbonate used as an additive is an additive for forming a stable organic-based negative electrode film by being reduced at a low potential during an initial activation process.
[0042] The electrolyte may include vinylene carbonate in an amount of 0.1 wt % to 10 wt %, preferably 1 wt % to 5 wt %, and more preferably 2 wt % to 4 wt %, based on the total weight of the electrolyte.
[0043] 1,3-Propane sultone used as an additive is an additive for forming a stable sulfur (S)-based organic film on the surface of the negative electrode and the positive electrode during an initial activation process.
[0044] The electrolyte may include 1,3-propane sultone in an amount of 0.1 wt % to 2 wt %, preferably 0.1 wt % to 1.5 wt %, and more preferably 0.2 wt % to 0.5 wt %, based on the total weight of the electrolyte.
[0045] The organic solvent may include at least one organic solvent selected from the group consisting of a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, a linear ester-based organic solvent, and a cyclic ester-based organic solvent.
[0046] Specifically, the organic solvent may include a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, or a mixed organic solvent thereof.
[0047] The cyclic carbonate-based organic solvent is an organic solvent that is a high-viscosity organic solvent and can well dissociate lithium salts in the electrolyte due to its high dielectric constant, wherein a specific example of the cyclic carbonate-based organic solvent can be at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate, and wherein the cyclic carbonate-based organic solvent can include ethylene carbonate.
[0048] The content of cyclic carbonate (e.g., ethylene carbonate) may be 15 vol% to 30 vol%, preferably 15 vol% to 25 vol%, and most preferably 15 vol% to 20 vol%, based on the total organic solvent. When ethylene carbonate is included within the above range, it may help LiPO2F2 form a uniform SEI film.
[0049] In addition, the linear carbonate-based organic solvent is an organic solvent with low viscosity and low dielectric constant, wherein a typical example of the linear carbonate-based organic solvent can be at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate and ethyl propyl carbonate, and the linear carbonate-based organic solvent can specifically include ethyl methyl carbonate (EMC).
[0050] In addition, the organic solvent further includes at least one ester-based organic solvent selected from the group consisting of linear ester-based organic solvents and cyclic ester-based organic solvents and at least one carbonate-based organic solvent selected from the group consisting of cyclic carbonate-based organic solvents and linear carbonate-based organic solvents to prepare an electrolyte having high ionic conductivity.
[0051] Specific examples of the linear ester-based organic solvent may be at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0052] Furthermore, the cyclic ester-based organic solvent may include at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0053] If necessary, the organic solvent may be used by adding an organic solvent generally used in a non-aqueous electrolyte without limitation. For example, the organic solvent may further include at least one organic solvent selected from an ether-based organic solvent, an ethylene glycol dimethyl ether-based solvent, and a nitrile-based organic solvent.
[0054] As the ether-based solvent, any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL) and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL) or a mixture of two or more thereof may be used, but the ether-based solvent is not limited thereto.
[0055] The glycol dimethyl ether-based solvent is a solvent having a higher dielectric constant, a lower surface tension, and a lower reactivity with metals than a linear carbonate-based organic solvent, wherein the glycol dimethyl ether-based solvent may include at least one selected from the group consisting of dimethoxyethane (ethylene glycol dimethyl ether, DME), diethoxyethane, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (tri-glyme) and tetraethylene glycol dimethyl ether (TEGDME), but is not limited thereto.
[0056] The nitrile-based solvent may be at least one selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorobenzene acetonitrile, and 4-fluorobenzene acetonitrile, but is not limited thereto.
[0057] Lithium salt is used as an electrolyte salt in lithium secondary batteries, where it acts as a medium for transferring ions. Generally, for example, lithium salts may include Li + as cations, and may include a group consisting of F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - , B 10 Cl 10 - 、AlCl4 - 、AlO2 - PF6 - CF3SO3 - 、CH3CO2 - CF3CO2 - 、AsF6 - 、SbF6 - 、CH3SO3 - 、(CF3CF2SO2)2N - 、(CF3SO2)2N - 、(FSO2)2N - 、BF2C2O4 - , BC4O8 - PF4C2O4- PF2C4O8 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - 、C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - CF3(CF2)7SO3 - and SCN - At least one of the group consisting of is used as an anion.
[0058] Specifically, the lithium salt may include a lithium salt selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2(lithium bis(fluorosulfonyl)imide; LiFSI), LiN(SO2CF2CF3)2(lithium bis(perfluoroethanesulfonyl)imide; LiBETI) and LiN(SO2CF3)2(lithium bis(trifluoromethanesulfonyl)imide; LiTFSI) or a mixture of two or more thereof. In addition to these materials, lithium salts commonly used in electrolytes of lithium secondary batteries can be used without restriction.
[0059] The lithium salt may be appropriately changed within the range of normal use, but may be included in the electrolyte at a concentration of 0.1 M to 4.0 M, preferably 0.5 M to 3.0 M, and more preferably 0.8 M to 2.0 M, to obtain the best effect of forming a film for preventing corrosion of the electrode surface. In the case where the concentration of the lithium salt satisfies the above range, since the effect of improving the cycle characteristics during high temperature storage of the lithium secondary battery is sufficient and the viscosity of the nonaqueous electrolyte is appropriate, the electrolyte impregnation ability can be improved.
[0060] In addition, the non-aqueous electrolyte of the present invention may also include electrolyte additives to prevent the occurrence of negative electrode collapse due to decomposition of the non-aqueous electrolyte under high output conditions, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, prevent overcharging, and inhibit battery expansion at high temperatures.
[0061] Typical examples of the electrolyte additive may include at least one additive for forming a SEI film selected from the group consisting of cyclic carbonate-based compounds, halogen-substituted carbonate-based compounds, sultone-based compounds, sulfate-based compounds, phosphate-based compounds, borate-based compounds, nitrile-based compounds, phenyl compounds, amine-based compounds, silane-based compounds and lithium salt-based compounds.
[0062] The cyclic carbonate-based compound may include vinyl ethylene carbonate.
[0063] The halogen-substituted carbonate-based compound may include fluoroethylene carbonate (FEC).
[0064] The sultone-based compound may include at least one compound selected from the group consisting of 1,4-butane sultone, ethane sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.
[0065] The sulfate-based compound may include ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyltrimethylene sulfate (MTMS).
[0066] The phosphate-based compound may include at least one compound selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tetramethyltrimethylsilyl phosphate, trimethylsilyl phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.
[0067] Borate-based compounds may include tetraphenylborate, lithium oxalyldifluoroborate (LiODFB), and lithium bis(oxalato)borate (LiB(C2O4) 2、 LiBOB).
[0068] The nitrile-based compound may include at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanecarbonitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide.
[0069] The phenyl compound may include fluorobenzene, the amine compound may include triethanolamine or ethylenediamine, and the silane compound may include tetravinylsilane.
[0070] The lithium salt-based compound is a compound different from the lithium salt included in the non-aqueous electrolyte, wherein the lithium salt-based compound may include LiBF 4 .
[0071] The electrolyte may further include a compound selected from the group consisting of succinonitrile, 1H-imidazole-1-carboxylate and methyl-prop-2-ynyl carbonate. In the case of further including such an additive, a more solid SEI film may be formed on the surface of the negative electrode during the initial activation process of the secondary battery, and the high temperature stability of the secondary battery may be improved by suppressing the generation of gas that may be generated due to the decomposition of the electrolyte at high temperature.
[0072] The cylindrical lithium secondary battery according to the present invention may be a large-sized cylindrical battery having a shape factor ratio (defined as a value obtained by dividing the diameter of a cylindrical battery by its height, that is, a ratio of the diameter (Φ) to the height (H)) of 0.4 or more. Here, the shape factor refers to a value representing the diameter and height of a cylindrical battery.
[0073] The cylindrical battery according to the present invention can be, for example, a 46110 cell (46 mm in diameter, 110 mm in height, and a shape factor ratio of 0.418), a 4875 cell (48 mm in diameter, 75 mm in height, and a shape factor ratio of 0.640), a 48110 cell (48 mm in diameter, 110 mm in height, and a shape factor ratio of 0.436), a 4880 cell (48 mm in diameter, 80 mm in height, and a shape factor ratio of 0.600), a 4680 cell (46 mm in diameter, 80 mm in height, and a shape factor ratio of 0.575), or a 4695 cell (46 mm in diameter, 95 mm in height, and a shape factor ratio of 0.484). In the numbers representing the shape factor, the first two numbers represent the diameter of the cell, and the next two or three numbers represent the height of the cell.
[0074] The cylindrical lithium secondary battery according to the present invention significantly reduces the amount of gas generation compared to conventional cases, and therefore, excellent safety can be achieved even in a large-sized cylindrical battery having a shape factor ratio of 0.4 or more.
[0075] The electrode assembly included in the cylindrical lithium secondary battery of the present invention is a jellyroll-type electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator disposed between the positive electrode plate and the negative electrode plate are wound in one direction.
[0076] exist Figure 1 The stacked structure before winding the electrode assembly according to the present invention is illustrated in Figure 2 exemplifies the cross-sectional structure of the electrode plate (positive electrode plate or negative electrode plate) according to the present invention.
[0077] Reference Figure 1and Figure 2 The electrode assembly A of the present invention may be prepared by winding a laminated body formed by sequentially laminating the separator 12, the positive electrode plate 10, the separator 12, and the negative electrode plate 11 at least once in one direction X.
[0078] In this case, the positive electrode plate 10 and the negative electrode plate 11 have a structure in which the active material layer 21 is formed on the long sheet-like current collector 20 , and may include an uncoated portion 22 in which the active material layer 21 is not formed in a partial region of the current collector 20 .
[0079] If positive and negative plates 10 and 11 including non-coating portions 22 as described above are used, a battery having a jointless structure in which a separate electrode tab is not included and at least a portion of the non-coating portions of positive and negative plates 10 and 11 defines an electrode tab can be realized.
[0080] Specifically, the uncoated portion 22 may be formed longer along the winding direction X on one side end of the current collector 20 , and a battery having a jointless structure may be realized by joining a current collecting plate to each of the positive and negative electrode plate uncoated portions and connecting the current collecting plate to the electrode terminals.
[0081] For example, a battery with a jointless structure can be prepared by the following method. First, a separator, a positive plate, a separator and a negative plate are sequentially stacked so that the uncoated portions 22 of the positive plate 10 and the negative plate 11 are arranged in opposite directions to each other, and then wound in one direction to prepare a core-wound electrode assembly. Then, after the uncoated portions 22 of the positive plate and the negative plate are bent toward the winding center C, the current collector is welded and joined to the uncoated portion of the positive plate and the uncoated portion of the negative plate, respectively, and a battery with a jointless structure can be prepared by connecting the current collector to the electrode terminal. Since the current collector has a larger cross-sectional area than a strip electrode joint, and the resistance is inversely proportional to the cross-sectional area of the channel through which the current flows, when a secondary battery is formed with the above structure, the cell resistance can be significantly reduced.
[0082] The uncoated portions of the positive electrode plate and the negative electrode plate may be processed into the form of a plurality of independently bendable segments, and at least a portion of the plurality of segments may be bent toward a winding center C of the electrode assembly.
[0083] The current collectors of the positive and negative plates may be processed to form segments by metal foil cutting processes such as laser slotting, ultrasonic cutting, and punching.
[0084] When the uncoated portions of the positive and negative electrode plates are processed into a plurality of segments, deformation or damage of the uncoated portions can be prevented by reducing stress applied to the uncoated portions during bending, and welding characteristics with the current collecting plates can be improved.
[0085] The current collector and the uncoated portion are usually joined by welding, wherein, in order to improve the welding characteristics, it is necessary to apply strong pressure to the welding area of the uncoated portion to bend the uncoated portion as flatly as possible. However, the shape of the uncoated portion may be irregularly distorted and deformed during the bending process, and the deformed portion may contact the electrode of the opposite polarity, thereby causing an internal short circuit or causing microcracks in the uncoated portion. However, if the uncoated portion of the positive plate and the negative plate is processed into the form of multiple independently bendable segments, the stress applied to the uncoated portion during bending is alleviated, so that deformation and damage of the uncoated portion can be minimized.
[0086] In addition, in the case where the uncoated portion is processed into the form of a segment as described above, overlap occurs between the plurality of segments during bending, and, as a result, the welding strength relative to the current collecting plate is increased, and wherein, when the latest technology such as laser welding is used, the problem of the laser beam penetrating into the electrode assembly and ablating the diaphragm or active material can be prevented. Preferably, at least a portion of the plurality of bent segments may overlap at the upper and lower ends of the electrode assembly, and the current collecting plate may be joined to the overlapping plurality of segments.
[0087] The cylindrical type battery according to the present invention may preferably be a battery having a tabless structure not including an electrode tab, but is not limited thereto.
[0088] A battery with a jointless structure may, for example, have a structure in which the positive plate and the negative plate each include an uncoated portion on which an active material layer is not formed, the positive plate uncoated portion and the negative plate uncoated portion are respectively arranged at the upper end and the lower end of the electrode assembly, the current collector is bonded to each of the positive plate uncoated portion and the negative plate uncoated portion, and the current collector is connected to the electrode terminal. The cylindrical lithium secondary battery according to the present invention may have a structure in which the uncoated portions of the positive plate and the negative plate are used as electrode joints without forming a separate electrode joint (e.g., a jointless structure). With respect to conventional cylindrical batteries in which electrode joints are formed, a large amount of heat is generated around the electrode joints during charging as a large amount of current is concentrated on the electrode joints. In particular, since this phenomenon is strengthened during fast charging, there is a risk of battery fire or explosion. In contrast, the cylindrical lithium secondary battery with a jointless structure according to the present invention may be formed into a structure in which the uncoated portions without active material layers are formed at the ends of the positive plate and the negative plate, respectively, and the uncoated portions are connected to the electrode terminals by welding them to a current collector having a large cross-sectional area. Since a battery having a tab-free structure has a smaller current concentration than a conventional battery having an electrode tab, it can effectively reduce heat generation in the battery, and thus, can improve thermal stability of the battery to suppress deterioration of output characteristics.
[0089] Figure 3A cross-sectional view of a cylindrical battery having a jointless structure according to an embodiment of the present invention is illustrated. Figure 3 A cylindrical battery according to an embodiment of the present invention is described. However, Figure 3 Only one embodiment of the present invention is shown, and the structure of the cylindrical battery of the present invention is not limited to Figure 3 The scope disclosed in.
[0090] The cylindrical type battery 140 according to one embodiment of the present invention includes the jellyroll type electrode assembly 141 as described above, the battery can 142 accommodating the electrode assembly 141 therein, and the sealing body 143 sealing the open end of the battery can 142 .
[0091] In this case, the positive electrode plate and the negative electrode plate of the electrode assembly may each include an uncoated portion on which an active material layer is not formed, and may be stacked and wound so that the positive electrode uncoated portion and the negative electrode uncoated portion are respectively disposed at the upper end and the lower end of the electrode assembly. Since the electrode assembly has been described above, only components other than the electrode assembly will be described below.
[0092] The battery can 142 is a cylindrical container having an upper opening, wherein it is formed of a conductive metal material such as aluminum or steel, etc. The battery can can accommodate the electrode assembly 141 in an inner space through the upper end opening, and also accommodate an electrolyte (not shown) together.
[0093] The battery can 142 is electrically connected to the non-coating portion 146 b of the negative electrode plate, and serves as a negative terminal that contacts an external power source to transfer current applied from the external power source to the negative electrode plate.
[0094] If necessary, a curling portion 147 and a crimping portion 148 may be included at the upper end of the battery can 142. The curling portion 147 may be formed by pressing the outer peripheral surface of the battery can 142 by a distance D1. The curling portion 147 prevents the electrode assembly 141 accommodated inside the battery can 142 from escaping through the upper end opening of the battery can 142, and may serve as a support member on which the sealing body 143 is stably placed.
[0095] The crimping portion 148 may be formed on an upper portion of the beading portion 147 and have an extended and bent shape to surround an outer circumferential surface of the cap plate 143 a disposed on the beading portion 147 and a portion of an upper surface of the cap plate 143 a .
[0096] Next, the sealing body 143 is used to seal the open end of the battery can 142, wherein the sealing body 143 includes a cap plate 143a and a first gasket 143b that provides airtightness between the cap plate 143a and the battery can 142 and has insulating properties, and, if necessary, may also include a connecting plate 143c that is electrically and mechanically bonded to the cap plate 143a. The cap plate 143a may be pressed onto a crimping portion 147 formed in the battery can 142 and may be fixed by a crimping portion 148.
[0097] The cap plate 143a is a component formed of a conductive metal material, wherein it covers the upper end opening of the battery can 142. The cap plate 143a is electrically connected to the positive plate of the electrode assembly 141 and is electrically insulated from the battery can 142 by the first gasket 143b. Therefore, the cap plate 143a can be used as a positive terminal of a cylindrical secondary battery. The cap plate 143a may include a protrusion 143d protruding upward from the center C, and the protrusion 143d may contact an external power source to allow current to be applied from the external power source.
[0098] The first gasket 143 b may be disposed between the cap plate 143 a and the crimping portion 148 to ensure airtightness of the battery can 142 and to electrically insulate the battery can 142 and the cap plate 143 a .
[0099] If necessary, the cylindrical battery 140 according to the present invention may further include current collecting plates 144 and 145. The current collecting plates are respectively joined to the uncoated portions 146a and 146b of the positive and negative plates and connected to electrode terminals (ie, positive and negative terminals).
[0100] Specifically, the cylindrical type battery 140 according to the present invention may include a first current collecting plate 144 coupled to an upper portion of the electrode assembly 141 and a second current collecting plate 145 coupled to a lower portion of the electrode assembly 141 .
[0101] A first current collecting plate 144 and / or a second current collecting plate 145 may also be included.
[0102] The first current collecting plate 144 is joined to the upper portion of the electrode assembly 141. The first current collecting plate 144 is formed of a conductive metal material such as aluminum, copper, and nickel, and is electrically connected to the uncoated portion 146a of the positive electrode plate. A lead 149 may be connected to the first current collecting plate 144. The lead 149 may extend upward from the electrode assembly 141 and may be joined to the connection plate 143c or may be directly joined to the lower surface of the cap plate 143a. The lead 149 and other components may be joined by welding. Preferably, the first current collecting plate 144 may be integrally formed with the lead 149. In this case, the lead 149 may have a long plate shape extending outward from the center of the first current collecting plate 144.
[0103] The first current collecting plate 144 is joined to the end of the non-coating portion 146 a of the positive electrode plate, and, for example, the joining may be performed by a method such as laser welding, resistance welding, ultrasonic welding, and brazing.
[0104] The second current collecting plate 145 is joined to the lower portion of the electrode assembly 141. The second current collecting plate 145 is formed of a conductive metal material such as aluminum, copper, and nickel, and is electrically connected to the uncoated portion 146b of the negative electrode plate. One surface of the second current collecting plate 145 may be joined to the uncoated portion 146b of the negative electrode plate, and the opposite surface may be joined to the inner bottom surface of the battery can 142. In this case, the joining may be performed by methods such as laser welding, resistance welding, ultrasonic welding, and brazing.
[0105] If necessary, the cylindrical battery 140 according to the present invention may further include an insulator 146. The insulator 146 may be provided to cover the upper surface of the first current collecting plate 144. Since the insulator 146 covers the first current collecting plate 144, direct contact between the first current collecting plate 144 and the inner circumferential surface of the battery can 142 may be prevented.
[0106] The insulator 146 includes a lead hole 151 so that the lead 149 extending upward from the first current collecting plate 144 can be led out. The lead 149 is led out upward through the lead hole 151 and is bonded to the lower surface of the connection plate 143c or the lower surface of the cap plate 143a.
[0107] The insulator 146 may be formed of an insulating polymer resin, for example, a polymer resin material such as polyethylene, polypropylene, polyimide, or polybutylene terephthalate.
[0108] If necessary, the cylindrical battery 140 according to the present invention may further include a vent 152 formed on the lower surface of the battery can 142. The vent 152 corresponds to an area in the lower surface of the battery can 142 having a thickness thinner than the surrounding area. Since the vent 152 is thin, it is structurally weaker than the surrounding area. Therefore, if the pressure in the cylindrical battery 140 increases to a certain level or higher, the vent 152 ruptures and the gas in the battery can 152 can be discharged to the outside to prevent the battery from exploding.
[0109] Figure 4 A cross-sectional view of a cylindrical battery having a jointless structure according to another embodiment of the present invention is illustrated. Figure 4 A cylindrical battery according to another embodiment of the present invention is described. However, Figure 4 Only one embodiment of the present invention is shown, and the structure of the cylindrical battery of the present invention is not limited to Figure 4 The scope disclosed in.
[0110] Reference Figure 4 ,and Figure 3 Compared to the cylindrical battery 140 shown in FIG. 1 , a cylindrical battery 170 according to another embodiment of the present invention has a different structure of a battery can and a sealing body, and has substantially the same configuration of an electrode assembly and an electrolyte.
[0111] Specifically, the cylindrical battery 170 includes a battery can 171 through which a riveted terminal 172 is installed. The riveted terminal 172 is installed on a partially closed closed surface (upper surface in the figure) at one end of the battery can 171. The riveted terminal 172 is riveted to a through hole (first opening of the first end) of the battery can 171 in a state where an insulating second gasket 173 is provided therebetween. The riveted terminal 172 is exposed to the outside in a direction opposite to the direction of gravity.
[0112] The riveted terminal 172 includes a terminal exposure portion 172a and a terminal insertion portion 172b. The terminal exposure portion 172a is exposed outside the closed surface of the battery can 171. The terminal exposure portion 172a may be located at approximately the center of the partially closed surface of the battery can 171. The maximum diameter of the terminal exposure portion 172a may be formed to be larger than the maximum diameter of the through hole formed in the battery can 171. The terminal insertion portion 172b may be electrically connected to the uncoated portion 146a of the positive plate through approximately the center of the closed surface of the battery can 171. The terminal insertion portion 172b may be riveted on the inner surface of the battery can 171. That is, the end of the terminal insertion portion 172b may have a shape bent toward the inner surface of the battery can 171. The maximum diameter of the end of the terminal insertion portion 172b may be larger than the maximum diameter of the through hole of the battery can 171.
[0113] The lower end surface of the terminal insertion portion 172b may be welded to the first current collecting plate 144 connected to the uncoated portion 146a of the positive electrode plate. An insulating cap 174 formed of an insulating material may be disposed between the first current collecting plate 144 and the inner surface of the battery can 171. The insulating cap 174 covers the upper portion of the first current collecting plate 144 and the upper edge portion of the electrode assembly 141. Therefore, it may prevent a short circuit caused by contact between the peripheral uncoated portion B3 of the electrode assembly 141 and the inner surface of the battery can 171 having different polarities. The terminal insertion portion 172b of the riveted terminal 172 may pass through the insulating cap 174 to be welded to the first current collecting plate 144.
[0114] The second gasket 173 is disposed between the battery can 171 and the rivet terminal 172 to prevent electrical contact between the battery can 171 and the rivet terminal 172 having opposite polarities. Therefore, the upper surface of the battery can 171 having a substantially flat shape can be used as a positive terminal of the cylindrical battery 170.
[0115] The second gasket 173 includes a gasket exposure portion 173a and a gasket insertion portion 173b. The gasket exposure portion 173a is disposed between the terminal exposure portion 172a of the riveted terminal 172 and the battery can 171. The gasket insertion portion 173b is disposed between the terminal insertion portion 172b of the riveted terminal 172 and the battery can 171. The gasket insertion portion 173b can be tightly attached to the inner surface of the battery can 171 by deforming together during riveting of the terminal insertion portion 172b. The second gasket 173 can be formed of, for example, a polymer resin having insulating properties.
[0116] The gasket exposed portion 173a of the second gasket 173 may have an extended shape to cover the outer peripheral surface of the terminal exposed portion 172a of the riveted terminal 172. In the case where the second gasket 173 covers the outer peripheral surface of the riveted terminal 172, a short circuit may be prevented from occurring during the process of joining an electrical connection component such as a bus bar to the upper surface of the battery can 171 and / or the riveted terminal 172. Although not shown in the drawings, the gasket exposed portion 173a may have an extended shape to cover not only the outer peripheral surface of the terminal exposed portion 172a but also a portion of the upper surface thereof.
[0117] In the case where the second gasket 173 is formed of a polymer resin, the second gasket 173 may be joined to the battery can 171 and the riveted terminal 172 by heat fusion. In this case, airtightness at the joining interface between the second gasket 173 and the riveted terminal 172 and at the joining interface between the second gasket 173 and the battery can 171 may be enhanced. In the case where the gasket exposed portion 173a of the second gasket 173 has a shape extending to the upper surface of the terminal exposed portion 172a, the riveted terminal 172 may be integrally joined to the second gasket 173 by insert injection molding.
[0118] An area 175 other than the area occupied by the rivet terminal 172 and the second gasket 173 in the upper surface of the battery can 171 corresponds to a negative terminal having a polarity opposite to that of the rivet terminal 172 .
[0119] The second current collecting plate 176 is coupled to the lower portion of the electrode assembly 141. The second current collecting plate 176 is formed of a conductive metal material such as aluminum, steel, copper, and nickel, and is electrically connected to the non-coating portion 146b of the negative electrode plate.
[0120] Preferably, the second current collecting plate 176 is electrically connected to the battery can 171. To this end, at least a portion of the edge portion of the second current collecting plate 176 may be fixed by being disposed between the inner surface of the battery can 171 and the first gasket 178b. In one example, at least a portion of the edge portion of the second current collecting plate 176 may be fixed to the curling portion 180 by welding while being supported on the lower end surface of the curling portion 180 formed at the lower end of the battery can 171. In a modified example, at least a portion of the edge portion of the second current collecting plate 176 may be directly welded to the inner wall surface of the battery can 171.
[0121] The second current collecting plate 176 may have a plurality of irregularities (not shown) radially formed on a surface facing the non-coating portion 146b. In the case where the irregularities are formed, the second current collecting plate 176 may be pressed to press the irregularities into the non-coating portion 146b.
[0122] Preferably, the end portion of the non-coating portion 146 b and the second current collecting plate 176 may be joined by welding (eg, laser welding).
[0123] The sealing body 178 that seals the lower open end of the battery can 171 includes a cap plate 178a and a first gasket 178b. The first gasket 178b electrically separates the cap plate 178a and the battery can 171. The crimping portion 181 fixes the edge of the cap plate 178a and the first gasket 178b together. The exhaust portion 179 is included in the cap plate 178a. The configuration of the exhaust portion 179 is substantially the same as that of the exhaust portion of the above-mentioned embodiment.
[0124] Preferably, the cap plate 178a is formed of a conductive metal material. However, since the first gasket 178b is disposed between the cap plate 178a and the battery can 171, the cap plate 178a does not have an electrical polarity. The seal 178 is used to seal the lower open end of the battery can 171 and discharge gas when the internal pressure of the battery cell 170 increases above a critical value.
[0125] Preferably, the rivet terminal 172 electrically connected to the uncoated portion 146a of the positive electrode plate is used as the positive terminal. In addition, a portion 175 other than the rivet terminal 172 in the upper surface of the battery can 171 electrically connected to the uncoated portion 146b of the negative electrode plate through the second current collecting plate 176 is used as the negative terminal. As described above, in the case where two electrode terminals are provided at the upper portion of the cylindrical battery, an electrical connection component such as a bus bar may be provided only on one side of the cylindrical battery 170.
[0126] This can lead to simplification of the battery pack structure and improvement of energy density. In addition, since the portion 175 serving as the negative terminal has a substantially flat shape, a sufficient bonding area can be ensured for bonding an electrical connection component such as a bus bar. Therefore, the cylindrical battery 170 can reduce the resistance at the bonding portion of the electrical connection component to a desired level.
[0127] The cylindrical lithium secondary battery of the present invention as described above can be used to prepare a battery pack. Figure 6 The configuration of a battery pack according to one embodiment of the present invention is schematically illustrated in FIG. Figure 6 , a battery pack 3 according to one embodiment of the present invention includes an assembly in which a cylindrical secondary battery 1 is electrically connected and a battery pack case 2 accommodating the assembly. The cylindrical secondary battery 1 is a battery cell according to the above-mentioned embodiment. In the drawings, for the convenience of illustration, components such as bus bars for electrically connecting the cylindrical secondary batteries 1, a cooling unit, and external terminals are omitted.
[0128] The battery pack 3 may be installed in a vehicle. For example, the vehicle may be an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The vehicle includes a four-wheel vehicle or a two-wheel vehicle.
[0129] Figure 7 It is used to explain Figure 6 Figure 3. A diagram of a battery pack for a vehicle.
[0130] Reference Figure 7 , a vehicle 5 according to an embodiment of the present invention includes the battery pack 3 according to an embodiment of the present invention, and operates by receiving electric power from the battery pack 3 .
[0131] like Figure 5 As shown, the electrode assembly according to the present invention may be formed in a structure in which an insulating layer 24 is additionally formed on the positive electrode plate 10. Specifically, the insulating layer 24 may be formed to cover a portion of the positive active material layer and a portion of the uncoated portion in a direction parallel to the winding direction of the electrode assembly.
[0132] For a battery having a jointless structure in which the uncoated portion 22c of the positive electrode plate 10 and the uncoated portion 22a of the negative electrode plate 11 are used as electrode joints, the electrode assembly is formed so that the positive electrode plate 10 protrudes above the separator 12 and the negative electrode plate 11 protrudes below the separator 12, and the protruding positive electrode plate 10 and / or negative electrode plate 11 is bent and then joined to the current collector plate. In the case where the positive electrode plate 10 or the negative electrode plate 11 is bent as described above, the current collector of the positive electrode plate 10 or the negative electrode plate 11 passes over the separator and is disposed close to the electrode having the opposite polarity, and as a result, there is a possibility that the positive electrode plate and the negative electrode plate are electrically contacted to cause an internal short circuit. However, as Figure 5As shown, when the insulating layer 24 is formed to cover the positive electrode active material layer and a portion of the uncoated portion, since the electrical contact between the positive electrode plate 10 and the negative electrode plate 11 can be prevented by the insulating layer 24, a short circuit in the battery can be prevented from occurring.
[0133] Preferably, the insulating layer 24 may be disposed on at least one side of the current collector of the positive electrode plate 10 , and preferably, may be disposed on both sides of the positive electrode plate 10 .
[0134] In addition, the insulating layer 24 may be formed in a region of the positive electrode plate 10 that may face the active material layer 21a of the negative electrode plate 11. For example, on the surface of the uncoated portion 22c of the positive electrode plate 10 that faces the negative electrode plate 11 after bending, the insulating layer 24 may be formed by extending to the end of the uncoated portion 22c. However, relative to the surface opposite to the surface facing the negative electrode plate 11 after bending, it is desirable that the insulating layer 24 is formed only on a portion of the uncoated portion 22c (e.g., before the bending point of the uncoated portion 22c). The reason for this is that, in the case where the insulating layer 24 is formed on the entire region of the uncoated portion of the surface opposite to the surface facing the negative electrode plate 11, it cannot be used as an electrode tab because electrical contact with the current collector is impossible.
[0135] As long as the insulating layer 24 can be attached to the positive plate while ensuring insulation performance, it can be used, and its material or component is not particularly limited. For example, the insulating layer can be an insulating coating layer or an insulating tape, and the insulating coating layer can include an organic binder and inorganic particles. In this case, the organic binder can be, for example, styrene-butadiene rubber (SBR), and the inorganic particles can be alumina, but are not limited thereto.
[0136] Next, each component of the electrode assembly of the present invention will be described in more detail.
[0137] (1) Positive plate
[0138] The positive electrode plate may be formed in a structure in which a positive electrode active material layer is formed on one side or both sides of a long sheet-shaped positive electrode collector, and the positive electrode active material layer may include a positive electrode active material, a conductive agent, and a binder.
[0139] Specifically, the positive electrode plate may be prepared by a method in which a positive electrode slurry prepared by dispersing a positive electrode active material, a conductive agent, and a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, and water is applied to one or both sides of a long sheet of positive electrode collector, the solvent of the positive electrode slurry is removed by a drying process, and rolling is performed. The positive electrode plate including the uncoated portion may be prepared by a method in which, when applying the positive electrode slurry, the positive electrode slurry is not applied to a partial region of the positive electrode collector (e.g., one end of the positive electrode collector).
[0140] As the positive electrode current collector, various positive electrode current collectors used in the art can be used. For example, as the positive electrode current collector, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc. can be used. The positive electrode current collector can generally have a thickness of 3 μm to 500 μm, and microscopic irregularities can be formed on the surface of the current collector to improve the adhesion of the positive electrode active material. The positive electrode current collector can be used in various shapes such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.
[0141] As the positive electrode active material, a positive electrode active material commonly used in the art may be used.
[0142] Preferably, the positive electrode active material may include a lithium nickel-based oxide, and specifically, may include a lithium nickel-based oxide containing 85 mol% or more of nickel (Ni) based on the total molar number of the transition metal. Preferably, the lithium nickel-based oxide may include Ni in an amount of 85 mol% or more to less than 100 mol%, 86 mol% or more to less than 100 mol%, or 88 mol% or more to less than 100 mol%. In the case of using a lithium nickel-based oxide with a high Ni content as described above, a high capacity can be achieved.
[0143] More specifically, the positive electrode active material may include a lithium nickel-based oxide represented by the following [Formula 1].
[0144] [Formula 1]
[0145] Li a Ni b Co c M 1 d M 2 e O2
[0146] In Formula 1, M 1 It may be manganese (Mn), aluminum (Al), or a combination thereof, and may be preferably Mn or Mn and Al.
[0147] M 2 It may be at least one selected from the group consisting of zirconium (Zr), tungsten (W), yttrium (Y), barium (Ba), calcium (Ca), titanium (Ti), magnesium (Mg), tantalum (Ta) and niobium (Nb), and may preferably be at least one selected from the group consisting of Zr, Y, Mg and Ti, and may more preferably be Zr, Y or a combination thereof. Element M 2 It is not necessarily included, however, when the element M is included in an appropriate amount 2In this case, it can play a role in promoting grain growth or improving the crystal structure stability during sintering.
[0148] a represents the molar ratio of lithium in the lithium nickel-based oxide, where a can satisfy 0.8 ≤ a ≤ 1.2, 0.85 ≤ a ≤ 1.15, or 0.9 ≤ a ≤ 1.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be formed stably.
[0149] b represents the molar ratio of nickel among all the metals except lithium in the lithium nickel-based oxide, where b can satisfy 0.85 ≤ b < 1, 0.86 ≤ b < 1, or 0.88 ≤ b < 1. When the molar ratio of nickel satisfies the above range, a high energy density can be exhibited to achieve a high capacity.
[0150] c represents the molar ratio of cobalt among all the metals except lithium in the lithium nickel-based oxide, where c can satisfy 0 < c < 0.15, 0 < c < 0.14, or 0.01 ≤ c ≤ 0.12. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be achieved.
[0151] d represents the molar ratio of element M among all the metals except lithium in the lithium nickel-based oxide 1 where d can satisfy 0 < d < 0.15, 0 < d < 0.14, or 0.01 ≤ d ≤ 0.12. When the molar ratio of element M 1 satisfies the above range, the structural stability of the positive electrode active material is excellent.
[0152] e represents the molar ratio of element M among all the metals except lithium in the lithium nickel-based oxide 2 where e can satisfy 0 ≤ e ≤ 0.1 or 0 ≤ e ≤ 0.05.
[0153] If necessary, the positive electrode active material according to the present invention may further include a coating layer on the surface of the particles of the lithium nickel-based oxide, and the coating layer includes at least one coating element selected from the group consisting of Al, Ti, W, boron (B), F, P, Mg, Ni, cobalt (Co), iron (Fe), chromium (Cr), vanadium (V), copper (Cu), Ca, zinc (Zn), Zr, niobium (Nb), molybdenum (Mo), strontium (Sr), antimony (Sb), bismuth (Bi), silicon (Si), and sulfur (S). Preferably, the coating element may be Al, B, Co, or a combination thereof, and most preferably, the coating element may be B.
[0154] When the coating layer is present on the surface of the lithium nickel-based oxide particles, the contact between the electrolyte and the lithium composite transition metal oxide is inhibited by the coating layer, and as a result, the effect of reducing the dissolution of the transition metal or the generation of gas due to the side reaction with the electrolyte can be obtained.
[0155] The positive electrode active material may be included in an amount of 80 wt % to 99 wt %, preferably 85 wt % to 99 wt %, and more preferably 90 wt % to 99 wt %, based on the total weight of the positive electrode active material layer.
[0156] The form of the positive electrode active material is not particularly limited, and the positive electrode active material may be in the form of secondary particles in which a plurality of primary particles are aggregated, in the form of a single particle composed of one primary particle, or a combination thereof.
[0157] Preferably, the positive electrode active material may include a single particle consisting of one primary particle and / or a pseudo single particle as an aggregate of 10 or less primary particles. By using a positive electrode active material consisting of a single particle consisting of one primary particle and / or a pseudo single particle as an aggregate of 10 or less primary particles, a large-sized cylindrical battery with high capacity and excellent safety can be obtained.
[0158] Conventionally, spherical secondary particles in which tens to hundreds of primary particles are gathered are generally used as positive electrode active materials for lithium secondary batteries. However, for positive electrode active materials in the form of secondary particles in which many primary particles are gathered as described above, there is a problem in that the particle rupture in which the primary particles fall off in the calendering process during the preparation of the positive electrode is likely to occur, and cracks appear in the particles during charging and discharging. In the case of particle rupture or cracking of the positive electrode active material, due to the increase in the contact area with the electrolyte solution, there is a problem of increased gas generation due to the side reaction with the electrolyte solution. If the gas generation in the cylindrical battery increases, there is a risk of battery explosion due to the increase in pressure in the battery. In particular, in the case of an increase in the volume of the cylindrical battery, since the amount of active material in the battery increases with the increase in volume, and as a result, the amount of gas generated also increases significantly, the risk of fire and / or explosion of the battery is further increased.
[0159] On the contrary, since the positive electrode active material in the form of a single particle composed of one primary particle or a pseudo single particle in which 10 or less primary particles are aggregated has a higher particle strength than the conventional positive electrode active material in the form of a secondary particle in which tens to hundreds of primary particles are aggregated, particle breakage hardly occurs during rolling. In addition, for the positive electrode active material in the form of a single particle or a pseudo single particle, since the number of primary particles constituting the particle is small, the change caused by the volume expansion and contraction of the primary particles during charging and discharging is small, and thus the occurrence of cracks in the particles is significantly reduced.
[0160] Therefore, in the case where a positive electrode active material composed of single particles and / or pseudo single particles is used, the amount of gas generated due to particle breakage and the occurrence of internal cracks can be significantly reduced, and thus, excellent safety can be achieved even in large-sized cylindrical batteries.
[0161] Based on the weight of the total positive electrode active material included in the positive electrode active material layer, it is desirable that the positive electrode active material composed of single particles and / or pseudo single particles is included in an amount of 95wt% to 100wt%, preferably 98wt% to 100wt%, more preferably 99wt% to 100wt%, and even more preferably 100wt%. When the amount of the single particles and / or pseudo single particles satisfies the above range, sufficient safety can be obtained when the positive electrode active material is used in a large-sized cylindrical battery.
[0162] The positive electrode active material in the form of a single particle and / or a pseudo single particle according to the present invention may have an average particle size D of 5 μm or less, 4 μm or less, 3 μm or less, or 2 μm or less (e.g., 0.5 μm to 5 μm, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm). 50 When the average particle size D of the positive electrode active material 50 When the above range is satisfied, the increase in resistance can be minimized.
[0163] Since the positive electrode active material in the form of a single particle and / or a pseudo single particle has fewer interfaces between primary particles as diffusion paths for lithium ions in the particles, its lithium mobility is lower than that of the positive electrode active material in the form of secondary particles, and as a result, the resistance may increase. This increase in resistance is exacerbated as the particle size increases, and when the resistance increases, the capacity and output characteristics are adversely affected. Therefore, in the present invention, since a single particle having an average particle size D of 5 μm or less is used, the average particle size D of 5 μm or less is increased. 50 The positive electrode active material in the form of a single particle and / or a pseudo single particle minimizes the diffusion distance of lithium ions in the particle, and thus an increase in resistance can be suppressed.
[0164] The positive electrode active material in the form of a single particle and / or a pseudo single particle may have an average particle size D of primary particles. 505 μm or less, 4 μm or less, 3 μm or less, or 2 μm or less (e.g., 0.5 μm to 5 μm, preferably 1 μm to 5 μm and more preferably 2 μm to 5 μm). When the average particle size of the primary particles meets the above range, a single particle and / or pseudo single particle form of a positive electrode active material with excellent electrochemical properties can be formed. If the average particle size of the primary particles is too small, the number of aggregates of the primary particles constituting the positive electrode active material increases and reduces the effect of suppressing particle breakage during the rolling process, and if the average particle size of the primary particles is too large, the lithium diffusion path in the primary particles may increase and increase resistance and deteriorate the output characteristics.
[0165] In the present invention, it is desirable that the positive electrode active material in the form of a single particle and / or a pseudo-single particle has a unimodal particle size distribution. Conventionally, in order to increase the electrode density of the positive electrode active material layer, a bimodal positive electrode active material in which a large-particle positive electrode active material having a large average particle size and a small-particle positive electrode active material having a small average particle size are mixed has been widely used. However, for the positive electrode active material in the form of a single particle and / or a pseudo-single particle, if the particle size increases, the resistance is significantly increased due to the increase in the lithium movement path, so when large-diameter particles are mixed and used, problems of capacity and output characteristics degradation may occur. Therefore, in the present invention, the increase in resistance can be minimized by using a positive electrode active material with a unimodal distribution.
[0166] Next, the conductive agent is used to provide conductivity to the electrode, wherein any conductive agent can be used without particular limitation as long as it has suitable electronic conductivity without causing adverse chemical changes in the battery. Specific examples of the conductive agent can be graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; powders or fibers of metals such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and any one of them or a mixture of two or more thereof can be used. Based on the total weight of the positive electrode active material layer, the conductive agent can be generally included in an amount of 1wt% to 30wt%, preferably 1wt% to 20wt%, and more preferably 1wt% to 10wt%.
[0167] The binder improves the adhesion between the positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector, wherein specific examples of the binder can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber or its various copolymers, and any one of them or a mixture of two or more thereof can be used. Based on the total weight of the positive electrode active material layer, the binder can be included in an amount of 1wt% to 30wt%, preferably 1wt% to 20wt% and more preferably 1wt% to 10wt%.
[0168] If necessary, an insulating layer covering a portion of the positive electrode active material layer and a portion of the uncoated portion may be further formed on the positive electrode plate according to the present invention. The insulating layer may be formed in a direction parallel to the winding direction of the electrode assembly.
[0169] (2) Negative plate
[0170] The negative electrode plate may be formed in a structure in which a negative electrode active material layer is formed on one side or both sides of a long sheet-shaped negative electrode collector, and the negative electrode active material layer includes a negative electrode active material, a conductive agent, and a binder.
[0171] Specifically, the negative electrode plate may be prepared by a method in which a negative electrode slurry prepared by dispersing a negative electrode active material, a conductive agent, and a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, and water is applied to one or both sides of a long sheet of a negative electrode collector, the solvent of the negative electrode slurry is removed by a drying process, and rolling is performed. The negative electrode plate including the uncoated portion may be prepared by a method in which, when applying the negative electrode slurry, the negative electrode slurry is not applied to a partial region of the negative electrode collector (e.g., one end of the negative electrode collector).
[0172] A compound capable of reversibly inserting and extracting lithium can be used as the negative electrode active material. Specific examples of the negative electrode active material may be carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; such as silicon (Si), Si-Me alloy (wherein Me is at least one selected from the group consisting of Al, tin (Sn), Mg, Cu, Fe, lead (Pb), Zn, Mn, Cr, Ti, and Ni), SiO y(where, 0 < y < 2) and silicon-based materials such as Si-C composites; lithium metal thin films; metal materials such as Sn and Al that can alloy with lithium, and any one of them or a mixture of two or more of them can be used.
[0173] Preferably, the negative electrode plate according to the present invention may include a silicon-based negative electrode active material. The silicon-based negative electrode active material may be Si, Si-Me alloy (where, Me is at least one selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, and Ni), SiO y (where, 0 < y < 2), Si-C composite or a combination thereof, and may preferably be SiO y (where, 0 < y < 2). Since the silicon-based negative electrode active material has a high theoretical capacity, the capacity characteristics can be improved when the silicon-based negative electrode active material is included.
[0174] The silicon-based negative electrode active material may be doped with M b metal, and in this case, M b metal may be a Group I metal element or a Group II metal element, and specifically, may be lithium (Li), Mg, etc. Specifically, the silicon-based negative electrode active material may be Si, SiO b doped with M y (where, 0 < y < 2) or Si-C composite. For the metal-doped silicon-based negative electrode active material, the capacity of the active material is slightly reduced due to the doping element, but high energy density can be achieved due to its high efficiency.
[0175] In addition, the silicon-based negative electrode active material may further include a carbon coating layer on the particle surface. In this case, based on the total weight of the silicon-based negative electrode active material, the carbon coating amount may be 20 wt% or less, preferably 1 wt% to 20 wt%.
[0176] In addition, if necessary, the negative electrode plate may further include a carbon-based negative electrode active material as the negative electrode active material. The carbon-based negative electrode active material may be, for example, artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, or hard carbon, but is not limited thereto.
[0177] When using a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material as the negative electrode active material, as a weight ratio, the mixing ratio of the silicon-based negative electrode active material to the carbon-based negative electrode active material may be in the range of 1:99 to 20:80, preferably in the range of 1:99 to 15:85, and more preferably in the range of 1:99 to 10:90.
[0178] The negative electrode active material may be included in an amount of 80 wt % to 99 wt %, preferably 85 wt % to 99 wt %, and more preferably 90 wt % to 99 wt %, based on the total weight of the negative electrode active material layer.
[0179] As the negative electrode current collector, a negative electrode current collector commonly used in the art can be used, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or copper or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy can be used. The negative electrode current collector may generally have a thickness of 3 μm to 500 μm, and similar to the positive electrode current collector, microscopic irregularities may be formed on the surface of the current collector to improve the adhesion of the negative electrode active material. The negative electrode current collector may be used in various shapes such as a film, a sheet, a foil, a mesh, a porous body, a foam body, a non-woven fabric body, etc.
[0180] The conductive agent is used to provide conductivity to the negative electrode, wherein any conductive agent can be used without particular limitation as long as it has suitable electronic conductivity without causing adverse chemical changes in the battery. Specific examples of the conductive agent can be graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; powders or fibers of metals such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and any one of them or a mixture of two or more thereof can be used. Based on the total weight of the negative electrode active material layer, the conductive agent can be generally included in an amount of 1wt% to 30wt%, preferably 1wt% to 20wt%, and more preferably 1wt% to 10wt%.
[0181] The binder improves the binding property between the negative electrode active material particles and the binding property between the negative electrode active material and the negative electrode current collector, wherein specific examples of the binder may be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber or various copolymers thereof, and any one of them or a mixture of two or more thereof may be used. Based on the total weight of the negative electrode active material layer, the binder may be included in an amount of 1wt% to 30wt%, preferably 1wt% to 20wt% and more preferably 1wt% to 10wt%.
[0182] (3) Diaphragm
[0183] The separator separates the negative electrode and the positive electrode and provides a mobile path for lithium ions, wherein any separator can be used as a separator without particular limitation, as long as it is generally used in a lithium secondary battery. Specifically, a porous polymer film (for example, a porous polymer film prepared from a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure having two or more layers thereof) can be used as a separator. In addition, a typical porous nonwoven fabric can be used, for example, a nonwoven fabric formed by a high melting point glass fiber or a polyethylene terephthalate fiber. In addition, a coated separator including a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength.
[0184] Hereinafter, the present invention will be described in more detail according to specific examples.
[0185] Example
[0186] Example 1
[0187] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 3 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.25 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0188] By Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ] O2 positive electrode active material (which is in the form of a single particle and has an average particle size D 50 The positive electrode slurry was prepared by mixing the carbon nanotubes and the PVDF binder in a weight ratio of 97.8:0.6:1.6 in N-methylpyrrolidone. The positive electrode slurry was coated on one surface of the aluminum current collector, dried at 120°C, and then rolled to prepare a positive electrode plate.
[0189] The negative electrode active material (a mixture of graphite: SiO=95:5 weight ratio), a conductive agent (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) were mixed in water at a weight ratio of 96:2:1.5:0.5 to prepare a negative electrode slurry. The negative electrode slurry was coated on one surface of a copper current collector, dried at 150°C, and then rolled to prepare a negative electrode plate.
[0190] The separator was disposed between the positive electrode plate and the negative electrode plate prepared above so that they were stacked in the order of separator / positive electrode plate / separator / negative electrode plate, and then wound to prepare a jellyroll-type electrode assembly. After the electrode assembly prepared as described above was inserted into a cylindrical battery can having a diameter of 46 mm and a height of 80 mm, an electrolyte was injected to prepare a cylindrical lithium secondary battery.
[0191] Example 2
[0192] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 4 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.5 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0193] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0194] Example 3
[0195] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 4 wt% of vinylene carbonate (VC), 0.5 wt% of 1,3-propane sultone (PS), 1 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0196] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0197] Example 4
[0198] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 2 wt% of vinylene carbonate (VC), 0.5 wt% of 1,3-propane sultone (PS), 0.25 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0199] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0200] Comparative Example 1
[0201] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 2 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0202] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0203] Comparative Example 2
[0204] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 5 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.25 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0205] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0206] Comparative Example 3
[0207] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 3.5 wt% of vinylene carbonate (VC), 0.5 wt% of 1,3-propane sultone (PS), 1.5 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0208] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0209] Comparative Example 4
[0210] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 3 wt% of vinylene carbonate (VC), 0.5 wt% of 1,3-propane sultone (PS), 0.1 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0211] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0212] Comparative Example 5
[0213] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 2 wt% of vinylene carbonate (VC), 0.5 wt% of 1,3-propane sultone (PS), 1 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0214] A cylindrical type lithium secondary battery was prepared in the same manner as in Example 1 except that the above electrolyte was used.
[0215] Comparative Example 6
[0216] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 3 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.25 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0217] By Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ] O2 positive electrode active material (which is in the form of a single particle and has an average particle size D 50The positive electrode slurry was prepared by mixing the carbon nanotubes and the PVDF binder in a weight ratio of 97.8:0.6:1.6 in N-methylpyrrolidone. The positive electrode slurry was coated on one surface of the aluminum current collector, dried at 120°C, and then rolled to prepare a positive electrode plate.
[0218] The negative electrode active material (a mixture of graphite: SiO=95:5 weight ratio), a conductive agent (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) were mixed in water at a weight ratio of 96:2:1.5:0.5 to prepare a negative electrode slurry. The negative electrode slurry was coated on one surface of a copper current collector, dried at 150°C, and then rolled to prepare a negative electrode plate.
[0219] The separator was disposed between the positive electrode plate and the negative electrode plate prepared above so that they were stacked in the order of separator / positive electrode plate / separator / negative electrode plate, and then wound to prepare a jellyroll-type electrode assembly. After the electrode assembly prepared as described above was inserted into a cylindrical battery can having a diameter of 21 mm and a height of 70 mm, an electrolyte was injected to prepare a cylindrical lithium secondary battery.
[0220] Comparative Example 7
[0221] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 4 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.5 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0222] By Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ] O2 positive electrode active material (which is in the form of a single particle and has an average particle size D 50 The positive electrode slurry was prepared by mixing the carbon nanotubes and the PVDF binder in a weight ratio of 97.8:0.6:1.6 in N-methylpyrrolidone. The positive electrode slurry was coated on one surface of the aluminum current collector, dried at 120°C, and then rolled to prepare a positive electrode plate.
[0223] The negative electrode active material (a mixture of graphite: SiO=95:5 weight ratio), a conductive agent (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) were mixed in water at a weight ratio of 96:2:1.5:0.5 to prepare a negative electrode slurry. The negative electrode slurry was coated on one surface of a copper current collector, dried at 150°C, and then rolled to prepare a negative electrode plate.
[0224] The separator was disposed between the positive electrode plate and the negative electrode plate prepared above so that they were stacked in the order of separator / positive electrode plate / separator / negative electrode plate, and then wound to prepare a jellyroll-type electrode assembly. After the electrode assembly prepared as described above was inserted into a cylindrical battery can having a diameter of 21 mm and a height of 70 mm, an electrolyte was injected to prepare a cylindrical lithium secondary battery.
[0225] Comparative Example 8
[0226] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 3 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.25 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0227] By Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ] O2 positive electrode active material (which is in the form of a single particle and has an average particle size D 50 The positive electrode slurry was prepared by mixing the carbon nanotubes and the PVDF binder in a weight ratio of 97.8:0.6:1.6 in N-methylpyrrolidone. The positive electrode slurry was coated on one surface of the aluminum current collector, dried at 120°C, and then rolled to prepare a positive electrode plate.
[0228] The negative electrode active material (a mixture of graphite: SiO=95:5 weight ratio), a conductive agent (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) were mixed in water at a weight ratio of 96:2:1.5:0.5 to prepare a negative electrode slurry. The negative electrode slurry was coated on one surface of a copper current collector, dried at 150°C, and then rolled to prepare a negative electrode plate.
[0229] The separator was disposed between the positive electrode plate and the negative electrode plate prepared above so that they were stacked in the order of separator / positive electrode plate / separator / negative electrode plate, and then wound to prepare a jellyroll-type electrode assembly. After the electrode assembly prepared as described above was inserted into a cylindrical battery can having a diameter of 18 mm and a height of 65 mm, an electrolyte was injected to prepare a cylindrical lithium secondary battery.
[0230] Comparative Example 9
[0231] The non-aqueous solvent was prepared by dissolving LiPF6 in an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:5:75 volume ratio) so that the concentration of LiPF6 was 1.3 M, and the electrolyte was prepared by adding 4 wt% of vinylene carbonate (VC), 1 wt% of 1,3-propane sultone (PS), 0.5 wt% of LiPO2F2, 0.2 wt% of succinonitrile and 0.3 wt% of 1H-imidazole-1-carboxylic acid propargyl ester based on the total weight of the electrolyte.
[0232] By Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ] O2 positive electrode active material (which is in the form of a single particle and has an average particle size D 50 The positive electrode slurry was prepared by mixing the carbon nanotubes and the PVDF binder in a weight ratio of 97.8:0.6:1.6 in N-methylpyrrolidone. The positive electrode slurry was coated on one surface of the aluminum current collector, dried at 120°C, and then rolled to prepare a positive electrode plate.
[0233] The negative electrode active material (a mixture of graphite: SiO=95:5 weight ratio), a conductive agent (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) were mixed in water at a weight ratio of 96:2:1.5:0.5 to prepare a negative electrode slurry. The negative electrode slurry was coated on one surface of a copper current collector, dried at 150°C, and then rolled to prepare a negative electrode plate.
[0234] The separator was disposed between the positive electrode plate and the negative electrode plate prepared above so that they were stacked in the order of separator / positive electrode plate / separator / negative electrode plate, and then wound to prepare a jellyroll-type electrode assembly. After the electrode assembly prepared as described above was inserted into a cylindrical battery can having a diameter of 18 mm and a height of 65 mm, an electrolyte was injected to prepare a cylindrical lithium secondary battery.
[0235] Experimental Example 1 - High Temperature Life Characteristics Evaluation
[0236] High temperature life characteristics were evaluated for the cylindrical lithium secondary batteries prepared from Examples 1 to 4 and Comparative Examples 1 to 9.
[0237] Specifically, each of the cylindrical lithium secondary batteries prepared by Examples 1 to 4 and Comparative Examples 1 to 9 was charged to 4.2V at a rate of 0.33C under constant current-constant voltage (CC-CV) conditions at 45°C, and discharged to 2.5V at a rate of 0.33C under CC conditions. After the above-mentioned charging and discharging was set as one cycle and 200 cycles were performed, the capacity retention rate relative to the initial capacity after 200 cycles was measured. The value of the relative capacity retention rate of the capacity retention rate (indicated as 100) of the cylindrical lithium secondary battery of Comparative Example 1 after 200 cycles relative to the initial capacity is shown in Table 1 below.
[0238] [Table 1]
[0239] <![CDATA[W LiDFP / (IN VC +W PS )×F / H×100]]> Relative capacity retention rate (%) Example 1 3.59 106 Example 2 5.75 110 Example 3 12.78 112 Example 4 5.75 102 Comparative Example 1 0.00 100 Comparative Example 2 2.40 98 Comparative Example 3 21.56 95 Comparative Example 4 1.64 99 Comparative Example 5 23.00 94 Comparative Example 6 1.88 99 Comparative Example 7 3.00 98 Comparative Example 8 1.73 98 Comparative Example 9 2.77 97
[0240] As shown in Table 1, it was confirmed that the cylindrical type lithium secondary batteries of Examples 1 to 4 had better lifespan characteristics at high temperatures than the cylindrical type lithium secondary batteries of Comparative Examples 1 to 9.
[0241] Experimental Example 2 - Rapid Charging Characteristics Evaluation
[0242] The rapid charging characteristics were evaluated for the cylindrical lithium secondary batteries prepared by Examples 1 to 4 and Comparative Examples 1 to 9.
[0243] Specifically, each of the cylindrical lithium secondary batteries prepared by Examples 1 to 4 and Comparative Examples 1 to 9 was charged to 4.2V at a 2C rate under CC-CV conditions at 25°C, and discharged to 2.5V at a 0.33C rate under CC conditions. After the above-mentioned charging and discharging was set as one cycle and 100 cycles were performed, the capacity retention rate relative to the initial capacity after 100 cycles was measured. The value of the relative capacity retention rate of the capacity retention rate (indicated as 100) of the cylindrical lithium secondary battery of Comparative Example 1 after 100 cycles relative to the initial capacity is shown in Table 2 below.
[0244] [Table 2]
[0245] Relative capacity retention rate (%) Example 1 102 Example 2 103 Example 3 105 Example 4 101 Comparative Example 1 100 Comparative Example 2 94 Comparative Example 3 95 Comparative Example 4 92 Comparative Example 5 90 Comparative Example 6 94 Comparative Example 7 95 Comparative Example 8 92 Comparative Example 9 94
[0246] As shown in Table 2, it was confirmed that the cylindrical type lithium secondary batteries of Examples 1 to 4 had better rapid charging characteristics than the cylindrical type lithium secondary batteries of Comparative Examples 1 to 9.
Claims
1. A cylindrical lithium secondary battery, the cylindrical lithium secondary battery include: A core-wound electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator disposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is housed; an electrolyte injected into the battery can; and a sealing body that seals an open end of the battery can, The electrolyte includes a lithium salt, an organic solvent, and lithium difluorophosphate, vinylene carbonate, and 1,3-propane sultone as additives, and Satisfying formula 1 Formula 1: 3.5 ≤ W LiDFP / (W VC +W PS )×Ф / H×100≤20 Where, in Formula 1, W LiDFP is the weight percentage of the lithium difluorophosphate to the total electrolyte, W VC is the weight percentage of the vinylene carbonate to the total electrolyte, and W PS is the weight percentage of the 1,3-propane sultone to the total electrolyte, and Φ is the diameter of the battery can, which is measured in mm, and H is the height of the battery can, which is measured in mm.
2. The cylindrical lithium secondary battery according to claim 1, in, The positive electrode plate and the negative electrode plate each include an uncoated portion where an active material layer is not formed, and each have a structure in which at least a portion of the uncoated portion of the positive electrode plate or the negative electrode plate defines an electrode tab.
3. The cylindrical lithium secondary battery according to claim 1, in, The cylindrical type lithium secondary battery has a shape factor ratio of 0.4 or more.
4. The cylindrical lithium secondary battery according to claim 1, in, The electrolyte includes the lithium difluorophosphate in an amount of 0.01 wt % to 3 wt % based on the total weight of the electrolyte.
5. The cylindrical lithium secondary battery according to claim 1, in, The electrolyte includes the vinylene carbonate in an amount of 0.1 wt % to 10 wt % based on the total weight of the electrolyte.
6. The cylindrical lithium secondary battery according to claim 1, in, The electrolyte includes the 1,3-propane sultone in an amount of 0.1 wt % to 2 wt % based on the total weight of the electrolyte.
7. The cylindrical lithium secondary battery according to claim 1, in, The organic solvent includes ethylene carbonate.
8. The cylindrical lithium secondary battery according to claim 7, in, The ethylene carbonate is included in an amount of about 15 vol % to about 30 vol % based on the total organic solvent.
9. The cylindrical lithium secondary battery according to claim 1, in, The total concentration of the lithium salt included in the electrolyte is in the range of 0.8M to 2M.
10. The cylindrical lithium secondary battery according to claim 1, in, The electrolyte additionally includes a compound selected from the group consisting of succinonitrile, 1H-imidazole-1-carboxylic acid propargyl ester, and methyl-prop-2-ynyl carbonate.
11. The cylindrical lithium secondary battery according to claim 1, in, The positive electrode plate includes a positive electrode active material having an amount of nickel (Ni) of 85 atm % or more among transition metals other than lithium.
12. The cylindrical lithium secondary battery according to claim 11, in, The positive electrode active material is a lithium nickel-based oxide represented by Formula 1, Formula 1 Li a Ni b Co c M 1 d M 2 e O 2 Among them, in Formula 1, M 1 is manganese Mn, aluminum Al or a combination thereof, and M 2 is at least one selected from the group consisting of zirconium Zr, tungsten W, yttrium Y, barium Ba, calcium Ca, titanium Ti, magnesium Mg, tantalum Ta, and niobium Nb, and 0.8 ≤ a ≤ 1.2, 0.85 ≤ b < 1, 0 < c < 0.15, 0 < d < 0.15, and 0 ≤ e ≤ 0.
1.
13. The cylindrical lithium secondary battery according to claim 12, in, The positive active material includes a coating layer formed on a surface of the lithium nickel-based oxide and including boron B.
14. The cylindrical lithium secondary battery according to claim 1, in, The positive electrode plate includes a positive electrode active material composed of single particles, pseudo single particles or a combination thereof.
15. The cylindrical lithium secondary battery according to claim 1, in, The negative electrode plate includes a silicon-based negative electrode active material and a carbon-based negative electrode active material.
16. The cylindrical lithium secondary battery according to claim 15, in, The silicon-based negative electrode active material and the carbon-based negative electrode active material are included in a weight ratio of 1:99 to 20:
80.
17. The cylindrical lithium secondary battery according to claim 1, in, The cylindrical lithium secondary battery is a 46110 battery cell, a 4875 battery cell, a 48110 battery cell, a 4880 battery cell, a 4680 battery cell or a 4695 battery cell.