Nano composite material with tail loaded with metal oxide as well as preparation method and application of nano composite material

By preparing bullet-like AuNBPs@Ag nanomaterials with Janus structure and loading metal oxides at their tails, the problems of uncontrollable morphology and low modification success rate in the prior art are solved, and the morphology innovation and catalytic of nanomaterials are achieved Performance improvement.

CN119075984APending Publication Date: 2024-12-06WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207004.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

It is difficult to prepare nanomaterials with Janus structures, especially AuNBPs@Ag nanomaterials with non-spherical structures, and traditional preparation methods have problems such as uncontrollable morphology and low modification success rate.

Method used

By preparing bullet-like AuNBPs@Ag nanomaterials with Janus structure and loading different metal oxides at the tail, a structure composed of gold nanobicones and Ag nanorods was used, combined with asymmetric etching and hydrothermal method, nanometers were achieved Material morphology control and metal oxide loading.

Benefits of technology

It breaks through the morphological limitations of traditional Janus structures, achieves precise control of the morphology of nanomaterials, expands the functional and application fields of materials, and demonstrates excellent catalytic performance, especially in the efficiency of catalytic degradation of hydrogen peroxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075984A_ABST
    Figure CN119075984A_ABST
Patent Text Reader

Abstract

The invention discloses a nano composite material with the tail loaded with a metal oxide as well as a preparation method and application of the nano composite material. The nano material comprises bullet-shaped AuNBPs (at) Ag nano particles with a Janus structure and the metal oxide loaded at the tail of the bullet-shaped AuNBPs (at) Ag nano particles. The preparation method comprises the following steps: preparing Au seeds; au seeds are used for inducing and growing to form gold nano bipyramid AuNBPs with a controllable length-diameter ratio; a layer of silver nano material is grown on the surface of the gold nano bipyramid AuNBPs in a wrapping mode, and an AuNBPs (at) Ag nanorod is formed; the AuNBPs (at) Ag nanorod is subjected to asymmetric etching, so that a bullet-shaped AuNBPs (at) Ag nanomaterial with a Janus structure is obtained; and loading a metal oxide at the tail part of the bullet-shaped AuNBPs (at) Ag nano material to obtain the nano composite material. According to the preparation method, not only is the shackle of the spherical morphology of the traditional Janus structure broken through, but also the limitation that part of ligands protect the traditional preparation method is broken through, the bullet-shaped AuNBPs (at) Ag nano material with the brand-new morphology and the Janus structure is prepared, and an infinite idea is provided for subsequent preparation of the nano material with the Janus structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano materials, and in particular relates to a nano composite material with a tail loaded with metal oxides, a preparation method and an application thereof. Background Art

[0002] For a long time, it has been very challenging to controllably prepare nanomaterials with Janus structures. Most existing preparation methods focus on the preparation of spherical Janus structures, mainly by partially modifying spherical SiO2 and then growing another material. However, this method has certain limitations, namely, the spherical structure is too symmetrical, resulting in a low success rate of partial modification, the preparation process is uncontrollable, and the morphology of the spherical structure is relatively simple, which cannot further enrich the structure of the material.

[0003] At present, based on the unique optical properties of precious metal nanoparticles, especially Au and Ag nanomaterials with various morphologies, they are ideal choices for preparing various heterostructures. The energy gaps of Au and Ag are similar, and they are easy to form heterojunctions, core-shell structures, etc. However, there are few reports on the research of AuNBPs@Ag nanomaterials with Janus structure. On the one hand, this may be because most of the research on Janus structure uses spherical nanoparticles, and the particle size is mostly in the micrometer level; the size of Au nanoparticles is small, which is not easy to partially modify the ligand. On the other hand, it may be due to the wide application of SiO2 microspheres in Janus structure, which has led to the neglect of other materials by researchers. In addition, in the research of Janus structure, most of the focus is on spherical structure. The commonly used method is to use surfactants or organic capping agents to partially modify the surface of SiO2 microspheres, so that another part of the surface of SiO2 microspheres is exposed, and then the second active material is grown in situ to form a Janus structure. However, this has resulted in a relatively narrow research on Janus structure, and it has not been able to break through the shackles of spherical structure for a long time. The preparation methods have long focused on partial ligand protection and have failed to break through the limitations of this method. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a nanocomposite material with a metal oxide loaded at the tail, and a preparation method and application thereof. The present invention not only breaks through the shackles of the spherical morphology of the traditional Janus structure, but also breaks through the limitations of the traditional preparation method of partial ligand protection, and prepares a bullet-shaped AuNBPs@Ag nanomaterial with a Janus structure with a new morphology, which provides unlimited imagination for the subsequent preparation of nanomaterials with a Janus structure. In addition, the present invention also expands the application potential of AuNBPs@Ag nanomaterials as nanomotors after loading different metal oxides on the tail of the AuNBPs@Ag nanomaterial.

[0005] To achieve the above object, the present invention is implemented by the following technical solutions:

[0006] The invention provides a nanocomposite material with a metal oxide loaded on the tail. The nanocomposite material comprises bullet-shaped AuNBPs@Ag nanoparticles with a Janus structure and a metal oxide loaded on the tail of the bullet-shaped AuNBPs@Ag nanoparticles.

[0007] As a further optimization scheme of the present invention, the bullet-shaped AuNBPs@Ag nanoparticles are composed of gold nanobipyramids AuNBPs and Ag nanorods, one end of the gold nanobipyramids AuNBPs is exposed to form a tip structure, and the other end is wrapped by the Ag nanorods to form a rod-like structure; the metal oxide is loaded on the tail of the Ag nanorods.

[0008] As a further optimization scheme of the present invention, the aspect ratio of the bullet-shaped AuNBPs@Ag nanoparticles can be adjusted in the range of 4-6.

[0009] As a further optimization scheme of the present invention, the metal oxide includes any one of manganese dioxide, titanium dioxide, cerium dioxide and cuprous oxide.

[0010] The present invention also provides a method for preparing a nanocomposite material having a tail loaded with metal oxides, the method comprising:

[0011] preparing Au seeds;

[0012] Using the Au seeds to induce the growth of gold nanobipyramids AuNBPs with controllable aspect ratio;

[0013] A layer of silver nanomaterial is coated and grown on the surface of the gold nanobipyramid AuNBPs to form AuNBPs@Ag nanorods;

[0014] Asymmetric etching is performed on the AuNBPs@Ag nanorods to obtain bullet-shaped AuNBPs@Ag nanomaterials having a Janus structure;

[0015] A metal oxide is loaded on the tail of the bullet-shaped AuNBPs@Ag nanomaterial to obtain a nanocomposite material.

[0016] As a further optimization scheme of the present invention, the preparation of the gold nanobipyramid AuNBPs includes:

[0017] In a solution containing hexadecyltrimethylammonium bromide, chloroauric acid, silver nitrate, hydrochloric acid and ascorbic acid, different amounts of Au seeds were added to form gold nanobipyramids AuNBPs with controllable aspect ratio through self-assembly and growth processes.

[0018] As a further optimization scheme of the present invention, the preparation of the AuNBPs@Ag nanorods includes:

[0019] Gold nanobipyramids AuNBPs were mixed with hexadecyltrimethylammonium chloride, silver nitrate and ascorbic acid, and a silver nanolayer was grown on the surface of the gold nanobipyramids AuNBPs through a reduction reaction of silver ions.

[0020] As a further optimization scheme of the present invention, the asymmetric etching step includes:

[0021] A mixed solution containing chloroauric acid, ascorbic acid, sodium hydroxide and hexadecyltrimethylammonium bromide is prepared and stirred evenly at room temperature; the AuNBPs@Ag nanorods are added to the mixed solution and reacted in a water bath at 25-35° C. for a period of time, and purified after the reaction is completed;

[0022] The purified nanorods were redispersed in a solution containing hexadecyltrimethylammonium bromide, and sodium bicarbonate, hydrogen peroxide, potassium thiocyanate and cobalt nitrate were added in sequence. The reaction was carried out in a water bath at 60-80°C for a period of time. After the reaction was completed, the nanorods were purified to obtain bullet-shaped AuNBPs@Ag nanomaterials with a Janus structure.

[0023] As a further optimization scheme of the present invention, the step of loading the metal oxide on the tail portion comprises:

[0024] The bullet-shaped AuNBPs@Ag nanomaterials were dispersed in a solution containing hexadecyltrimethylammonium bromide, and then a solution containing a metal oxide precursor was added and reacted at 50-70°C for a period of time to load the metal oxide on the tail of the bullet-shaped AuNBPs@Ag nanomaterials.

[0025] The invention also provides a nano-composite material with a metal oxide loaded at the tail for use as a nano-motor in catalytic degradation of hydrogen peroxide.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention uses an innovative method to prepare a Janus structure with a bullet-shaped morphology instead of a traditional spherical structure, breaking through the limitation that most traditional Janus structures are spherical in morphology. This provides a new way to prepare a Janus structure with a unique morphology.

[0028] (2) The present invention adopts asymmetric etching technology to achieve precise control of the morphology of nanomaterials and successfully prepares bullet-shaped AuNBPs@Ag nanomaterials with Janus structure. This method breaks through the limitations of traditional preparation methods with partial ligand protection, realizes continuous growth and modification of nanomaterials through hydrothermal method, improves preparation efficiency, and provides a more flexible method for preparing Janus structure.

[0029] (3) By adjusting the amount of Au seeds, the present invention can adjust the aspect ratio of the bullet-shaped AuNBPs@Ag nanomaterial from 4.0 to 6.0, which provides more possibilities for meeting different application requirements.

[0030] (4) The present invention realizes the loading of different types of metal oxides (such as Cu2O, TiO2, MnO2, CeO2) at one end of the tail of the nanomaterial by utilizing the difference in surface tip curvature of the bullet-shaped AuNBPs@Ag nanomaterial, further broadening the functionality and application field of the nanomaterial.

[0031] (5) The nanocomposites loaded with metal oxides exhibited excellent catalytic performance. Taking MnO2 as an example, the loaded nanocomposites performed well in the catalytic degradation of H2O2, and the degradation efficiency was much higher than that of the bullet-shaped AuNBPs@Ag nanomaterials or MnO2 alone, as well as their physical mixtures. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a transmission electron micrograph of the bullet-shaped AuNBPs@Ag nanomaterial without MnO2 loaded prepared in Example 1.

[0033] Figure 2 This is a transmission electron microscopy image of the MnO2-loaded nanocomposite material prepared in Example 1.

[0034] Figure 3 This is a transmission electron micrograph of the bullet-shaped AuNBPs@Ag nanomaterial without MnO2 loaded prepared in Example 2.

[0035] Figure 4 This is a transmission electron microscopy image of the MnO2-loaded nanocomposite material prepared in Example 2.

[0036] Figure 5 This is a transmission electron micrograph of the bullet-shaped AuNBPs@Ag nanomaterial without MnO2 loaded prepared in Example 3.

[0037] Figure 6 This is a transmission electron microscopy image of the MnO2-loaded nanocomposite material prepared in Example 3.

[0038] Figure 7 Statistical chart of the longitudinal length and transverse diameter of the bullet-shaped AuNBPs@Ag nanomaterials prepared in Example 1, Example 2, and Example 3.

[0039] Figure 8 Statistical chart of the aspect ratio of the bullet-shaped AuNBPs@Ag nanomaterials prepared in Example 1, Example 2, and Example 3.

[0040] Fig. 9 It is a line graph showing the catalytic degradation of H2O2 by different materials. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as limiting the present invention and is only used as an example.

[0042] On the one hand, the present invention provides a nanocomposite material with a metal oxide loaded on the tail, the nanocomposite material comprising bullet-shaped AuNBPs@Ag nanoparticles having a Janus structure and a metal oxide loaded on the tail of the bullet-shaped AuNBPs@Ag nanoparticles.

[0043] In some embodiments, the bullet-shaped AuNBPs@Ag nanoparticles are composed of gold nanobipyramid AuNBPs and Ag nanorods, one end of the gold nanobipyramid AuNBPs is exposed to form a pointed structure, and the other end is wrapped by the Ag nanorod to form a rod-like structure; the metal oxide is loaded on the tail of the Ag nanorod.

[0044] In some embodiments, the aspect ratio of the bullet-shaped AuNBPs@Ag nanoparticles can be adjusted in the range of 4-6.

[0045] In some embodiments, the metal oxide includes any one of manganese dioxide, titanium dioxide, cerium dioxide and cuprous oxide.

[0046] On the other hand, the present invention also provides a method for preparing a nanocomposite material having a tail loaded with a metal oxide, the preparation method comprising:

[0047] Synthesis of Au seeds:

[0048] Weigh 150-180 mg of hexadecyltrimethylammonium chloride (CTAC) and dissolve it in 10 ml of ultrapure water. After it is completely dissolved, add 50 ml of 50-80 mM HAuCl4 solution, followed by 9-12 mg of citric acid. Stir for 3-5 minutes, quickly add 250 ml of 30-60 mM NaBH4, stir for 3-5 minutes, and stir in an 80-90°C oil bath for 90-120 minutes.

[0049] Synthesis of gold nanobipyramids AuNBPs:

[0050] Add 200 ml of 80-150 mM hexadecyltrimethylammonium bromide (CTAB), 3 ml of 20-50 mM HAuCl4 solution, 2 ml of 10-20 mM AgNO3 solution, 4 ml of 1-3 M HCl solution, and 2 ml of 80-120 mM ascorbic acid (AA) solution to a round-bottom flask, and stir at room temperature for 3-5 min. Then add 3-5 ml of the Au seeds prepared above. Incubate in a water bath at 25-35 °C for 3-5 h.

[0051] Among them, hexadecyl trimethylammonium bromide is used as a ligand, HAuCl4 is used as a gold source, AgNO3 is used to regulate the crystal growth, HCl is used to regulate the pH, and ascorbic acid is used as a reducing agent. The aspect ratio of the bullet-shaped AuNBPs@Ag nanoparticles can be adjusted by adjusting the amount of Au seeds added, and the molar ratio of Au seeds to HAuCl4 gold source ranges from 1:70 to 130.

[0052] Synthesis of AuNBPs@Ag nanorods:

[0053] The prepared gold nanobipyramid AuNBPs were centrifuged and purified at 9500rpm for 8-12min, and centrifuged and purified twice. The purified gold nanobipyramid AuNBPs were then redispersed in ultrapure water until the absorbance was 0.5-1. 10-30ml of the redispersed gold nanobipyramid AuNBPs were added to 30ml, 30-50mM CTAC solution. Stir and disperse for 3-5min, then add 300-400ml of AgNO3 solution, stir and disperse for 3-5min, and then add 0.1-0.5M ascorbic acid, which is half the volume of the AgNO3 solution. Water bath at 50-70℃ for 3-6h. After the reaction is complete, centrifuge and purify at 9500rpm for 8-12min, and redisperse in 10-20ml ultrapure water.

[0054] Asymmetric etching of AuNBPs@Ag nanorods:

[0055] Add 750ml of 0.01-0.03M HAuCl4 solution, 500ml of 0.1-0.3M AA solution, 500ml of 0.05-0.15M NaOH solution, and 50ml of 0.1-0.3M CTAB solution to a round-bottom flask. After adding all the solutions, stir at room temperature for 3-5min. Then add 10-15ml of the above-dispersed AuNBPs@Ag nanorods and place in a water bath at 25-35℃ for 5-8h. After the reaction is complete, centrifuge at 9500rpm for purification.

[0056] The AuNBPs@Ag nanorods purified by centrifugation were redispersed in 200ml of 1-5mM CTAB solution. Subsequently, 2ml of 0.1-0.5M NaHCO3 solution, 2ml of 0.1-0.5M H2O2 solution, 1ml of 0.05-0.15M KSCN solution, and 2ml of 10-30mM Co(NO3)2 solution were gradually added. Water bath was performed at 60-80℃ for 15-25min. Purification by centrifugation at 9500rpm can obtain bullet-shaped AuNBPs@Ag nanomaterials with Janus structure.

[0057] Mechanism analysis of asymmetric etching: In the asymmetric etching process, HAuCl4 is used to break the balance and perform asymmetric etching. - The standard electrode potential of Au / Au is 1.002, and the standard electrode potential of Ag / AgCl is -0.222. - The standard electrode potentials of Au / Au and Ag / AgCl indicate that the redox reaction between the two can proceed spontaneously. Therefore, during the etching process, HAuCl4 can replace the Ag in the AuNBPs@Ag rods with free Ag. + , thus achieving the purpose of etching. However, due to the high symmetry of the two ends of the AuNBPs@Ag rod, the HAuCl4 etching process initially proceeds from both ends simultaneously, but as the etching reaction occurs, the etching reaction at one end must first break the balance, and under the action of reaction kinetics, the subsequent HAuCl4 etching process will be concentrated on the end that breaks the balance, thus leading to the occurrence of asymmetric etching.

[0058] Tail loading metal oxide:

[0059] The purified bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was redispersed in 2 ml of 0.1-0.3 M hexadecyltrimethylammonium bromide solution, and after sufficient stirring, 200 ml of 1-2 mM KMnO4 / TiCl3 / Ce(CH3COO)3 / CuCl2 solution was added, and then water was added to make the volume 10 ml, and the reaction was carried out in an oven at 50-70°C for 90 min. After centrifugal purification, a nanocomposite material with tail-loaded MnO2 / TiO2 / CeO2 / Cu2O was obtained.

[0060] Mechanism of tail loading of metal oxides:

[0061] Because the surface curvature of the Ag rod tail and the Au tip is very different, the curvature of the Au tip is larger and the morphology is sharper, so it is not easy for metal oxides to deposit during the in-situ reduction process. The curvature of the Ag rod tail is smaller and the morphology is flatter, so it is easier for metal oxides to deposit during the in-situ reduction process. Therefore, during the in-situ reduction process, the metal oxide will gradually and selectively deposit on the side of the Ag rod tail with a smaller curvature.

[0062] In some embodiments, the present invention provides a nanocomposite material having a tail loaded with a metal oxide for use as a nanomotor in catalytic degradation of hydrogen peroxide.

[0063] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0064] Example 1

[0065] Weigh 150 mg of hexadecyltrimethylammonium chloride (CTAC) and dissolve it in 10 ml of ultrapure water. After it is completely dissolved, add 50 ml of 50 mM HAuCl4 solution, followed by 9 mg of citric acid. Stir for 3 min, quickly add 250 ml of 30 mM NaBH4, stir for 3 min, and stir in an 80°C oil bath for 90 min.

[0066] Add 200 ml of 80 mM hexadecyltrimethylammonium bromide (CTAB), 3 ml of 20 mM HAuCl4 solution, 2 ml of 10 mM AgNO3 solution, 4 ml of 1 M HCl solution, and 2 ml of 80 mM ascorbic acid (AA) solution to a round-bottom flask and stir for 3-5 min at room temperature. Then add 3 ml of the Au seeds prepared above. Incubate in a water bath at 25 °C for 3 h.

[0067] The prepared gold nanobipyramid AuNBPs were centrifuged and purified at 9500rpm for 8min, and centrifuged and purified twice. The purified gold nanobipyramid AuNBPs were then redispersed in ultrapure water until the absorbance was 0.5. 10ml of the redispersed gold nanobipyramid AuNBPs was added to 30ml, 30mM CTAC solution. Stir and disperse for 3min, then add 300ml of AgNO3 solution, stir and disperse for 3min, and then add 0.1M ascorbic acid with half the volume of the AgNO3 solution. Water bath at 50℃ for 3h. After the reaction is complete, centrifuge and purify at 9500rpm for 8min, and redisperse in 10ml ultrapure water.

[0068] Add 750 ml of 0.01M HAuCl4 solution, 500 ml of 0.1M AA solution, 500 ml of 0.05M NaOH solution, and 50 ml of 0.1M CTAB solution to a round-bottom flask. After adding all the solution, stir at room temperature for 3 minutes. Then add 10 ml of the above-dispersed AuNBPs@Ag nanorods and place in a water bath at 25°C for 5 hours. After the reaction is complete, centrifuge at 9500 rpm for purification.

[0069] The AuNBPs@Ag nanorods purified by centrifugation were redispersed in 200ml of 1mM CTAB solution. Then, 2ml of 0.1M NaHCO3 solution, 2ml of 0.1M H2O2 solution, 1ml of 0.05M KSCN solution, and 2ml of 10mM Co(NO3)2 solution were gradually added. The mixture was placed in a water bath at 60℃ for 15min. After centrifugation at 9500rpm, the bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was obtained.

[0070] The purified bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was redispersed in 2 ml of 0.1 M hexadecyltrimethylammonium bromide solution, and after sufficient stirring, 200 ml of 1 mM KMnO4 solution was added, followed by water addition to make the volume to 10 ml, and reacted in an oven at 50°C for 90 min. After centrifugal purification, a nanocomposite material with MnO2 loaded on the tail was obtained.

[0071] Example 2

[0072] Weigh 160 mg of hexadecyltrimethylammonium chloride (CTAC) and dissolve it in 10 ml of ultrapure water. After it is completely dissolved, add 50 ml of 70 mM HAuCl4 solution, followed by 10 mg of citric acid. Stir for 5 min, quickly add 250 ml of 50 mM NaBH4, stir for 5 min, and stir in a 90°C oil bath for 120 min.

[0073] Add 200 ml of 120 mM hexadecyltrimethylammonium bromide (CTAB), 3 ml of 40 mM HAuCl4 solution, 2 ml of 20 mM AgNO3 solution, 4 ml of 2 M HCl solution, and 2 ml of 100 mM ascorbic acid (AA) solution to a round-bottom flask and stir for 5 min at room temperature. Then add 4 ml of the Au seeds prepared above. Incubate in a water bath at 30°C for 3-5 h.

[0074] The prepared gold nanobipyramid AuNBPs were centrifuged and purified at 9500rpm for 10min, and centrifuged and purified twice. The purified gold nanobipyramid AuNBPs were then redispersed in ultrapure water until the absorbance was 0.8. Take 20ml of the redispersed gold nanobipyramid AuNBPs to 30ml, 40mM CTAC solution. Stir and disperse for 5min, then add 300ml of AgNO3 solution, stir and disperse for 5min, and then add 0.3M ascorbic acid with half the volume of AgNO3 solution. Water bath at 60℃ for 5h. After the reaction is complete, centrifuge and purify at 9500rpm for 10min, and redisperse in 15ml ultrapure water.

[0075] Add 750 ml of 0.02M HAuCl4 solution, 500 ml of 0.2M AA solution, 500 ml of 0.1M NaOH solution, and 50 ml of 0.2M CTAB solution to a round-bottom flask. After adding all the solution, stir at room temperature for 5 minutes. Then add 10 ml of the above-dispersed AuNBPs@Ag nanorods and place in a water bath at 30°C for 6 hours. After the reaction is complete, centrifuge at 9500 rpm for purification.

[0076] The AuNBPs@Ag nanorods purified by centrifugation were redispersed in 200ml of 3mM CTAB solution. Then, 2ml of 0.3M NaHCO3 solution, 2ml of 0.3M H2O2 solution, 1ml of 0.10M KSCN solution, and 2ml of 20mM Co(NO3)2 solution were gradually added. The mixture was placed in a water bath at 70℃ for 20min. After centrifugation at 9500rpm, the bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was obtained.

[0077] The purified bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was redispersed in 2 ml of 0.2 M hexadecyltrimethylammonium bromide solution, and after sufficient stirring, 200 ml of 1.5 mM TiCl3 solution was added, followed by water addition to make the volume to 10 ml, and reacted in an oven at 60°C for 90 min. After centrifugal purification, a nanocomposite material with TiO2 loaded at the tail was obtained.

[0078] Example 3

[0079] Weigh 180 mg of hexadecyltrimethylammonium chloride (CTAC) and dissolve it in 10 ml of ultrapure water. After it is completely dissolved, add 50 ml of 80 mM HAuCl4 solution, followed by 12 mg of citric acid. Stir for 5 min, quickly add 250 ml of 60 mM NaBH4, stir for 5 min, and stir in a 90°C oil bath for 120 min.

[0080] Add 200 ml of 150 mM hexadecyltrimethylammonium bromide (CTAB), 3 ml of 50 mM HAuCl4 solution, 2 ml of 20 mM AgNO3 solution, 4 ml of 3 M HCl solution, and 2 ml of 120 mM ascorbic acid (AA) solution to a round-bottom flask and stir for 5 min at room temperature. Then add 5 ml of the Au seeds prepared above. Incubate in a water bath at 35 °C for 5 h.

[0081] The prepared gold nanobipyramid AuNBPs were centrifuged and purified at 9500rpm for 12min, and centrifuged and purified twice. The purified gold nanobipyramid AuNBPs were then redispersed in ultrapure water until the absorbance was 1. 30ml of the redispersed gold nanobipyramid AuNBPs were added to 30ml, 50mM CTAC solution. Stir and disperse for 5min, then add 400ml of AgNO3 solution, stir and disperse for 5min, and then add 0.5M ascorbic acid with half the volume of the AgNO3 solution. Water bath at 70℃ for 6h. After the reaction is complete, centrifuge and purify at 9500rpm for 12min, and redisperse in 20ml ultrapure water.

[0082] Add 750 ml of 0.03M HAuCl4 solution, 500 ml of 0.3M AA solution, 500 ml of 0.15M NaOH solution, and 50 ml of 0.3M CTAB solution to a round-bottom flask. After adding all the solution, stir at room temperature for 5 min. Then add 15 ml of the above-dispersed AuNBPs@Ag nanorods and place in a water bath at 35°C for 8 h. After the reaction is complete, centrifuge at 9500 rpm for purification.

[0083] The AuNBPs@Ag nanorods purified by centrifugation were redispersed in 200ml of 5mM CTAB solution. Then, 2ml of 0.5M NaHCO3 solution, 2ml of 0.5M H2O2 solution, 1ml of 0.15M KSCN solution, and 2ml of 30mM Co(NO3)2 solution were gradually added. The mixture was placed in a water bath at 80℃ for 25min. After centrifugation at 9500rpm, the bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was obtained.

[0084] The purified bullet-shaped AuNBPs@Ag nanomaterial with Janus structure was redispersed in 2 ml of 0.3 M hexadecyltrimethylammonium bromide solution. After sufficient stirring, 200 ml of 2 mM Ce(CH3COO)3 solution was added, followed by water addition to make the volume to 10 ml. The mixture was reacted in an oven at 70°C for 90 min. After centrifugal purification, a nanocomposite material with CeO2 loaded at the tail was obtained.

[0085] Figure 1 This is a transmission electron microscopy image of the bullet-shaped AuNBPs@Ag nanomaterial without MnO2 prepared in Example 1. Figure 1 It can be clearly seen that the morphology of the Janus structure prepared by this method is significantly different from the traditional spherical structure, and it presents a bullet-like morphology. From the TEM image, it can be seen that this Janus structure consists of two parts with obvious differences in contrast, one of which is the gold nanobipyramid AuNBPs with high contrast, and the other part with low contrast is the rod-like Ag nanorods, which together form a new type of Janus structure. Figure 2 This is a transmission electron microscope image of the MnO2-loaded nanocomposite prepared in Example 1. Figure 2 The neutron bullet-shaped AuNBPs@Ag nanomaterial has a longitudinal length of 131.8 nm, a lateral diameter of 30.1 nm, and an aspect ratio of 4.4.

[0086] Figure 3 This is a transmission electron micrograph of the bullet-shaped AuNBPs@Ag nanomaterial without MnO2 loaded prepared in Example 2. Similarly, it is composed of a gold nanobipyramid AuNBPs structure with a higher contrast and an Ag nanorod structure with a lower contrast. Figure 4 This is a transmission electron microscopy image of the MnO2-loaded nanocomposite prepared in Example 2. Since the TiO2 particles loaded at the tail are relatively large, they partially cover the bullet-shaped AuNBPs@Ag nanomaterial. Figure 4 The neutron bullet-shaped AuNBPs@Ag nanomaterial has a longitudinal length of 136.8 nm, a lateral diameter of 27.0 nm, and an aspect ratio of 5.1.

[0087] Figure 5 This is a transmission electron micrograph of the bullet-shaped AuNBPs@Ag nanomaterial without MnO2 loaded prepared in Example 3. Similarly, it is composed of a gold nanobipyramid AuNBPs structure with a higher contrast and an Ag nanorod structure with a lower contrast. Figure 6 This is a transmission electron microscopy image of the MnO2-loaded nanocomposite prepared in Example 3. Figure 6The neutron bullet-shaped AuNBPs@Ag nanomaterial has a longitudinal length of 145.2 nm, a transverse diameter of 24.8 nm, and an aspect ratio of 5.9. The Janus structure prepared by the present invention not only has a novel bullet-like structure morphology, but also can adjust its aspect ratio as needed.

[0088] Figure 7 The longitudinal length and transverse diameter of the bullet-shaped AuNBPs@Ag nanomaterials prepared in Example 1, Example 2, and Example 3 are statistical diagrams. It can be seen from the figure that the longitudinal lengths are 131.8 nm, 136.8 nm, and 145.2 nm, respectively, increasing in sequence, and the transverse diameters are 30.1 nm, 27.0 nm, and 24.8 nm, respectively, decreasing in sequence. The longitudinal lengths and transverse diameters can be adjusted as needed.

[0089] Figure 8 The aspect ratio statistics of the bullet-shaped AuNBPs@Ag nanomaterials prepared in Example 1, Example 2, and Example 3. It can be seen from the figure that the aspect ratios are 4.4, 5.1, and 5.9, respectively, increasing in sequence. Similarly, the longitudinal length and transverse diameter can be adjusted as needed, thereby adjusting the aspect ratios.

[0090] Fig. 9 It is a line graph of the catalytic degradation of H2O2 by different materials. Fig. 9 It can be seen that when only H2O is added, the concentration of H2O2 hardly changes within 60 minutes; when only bullet-shaped AuNBPs@Ag nanomaterials are added, the concentration of H2O2 only drops to 73% within 60 minutes; when only MnO2 is added, the concentration of H2O2 only drops to 65% within 60 minutes; after simple physical mixing of bullet-shaped AuNBPs@Ag nanomaterials and MnO2, the degradation rate of H2O2 within 60 minutes is improved, dropping to 38%; and after adding the nanocomposite material loaded with MnO2, the concentration of H2O2 only drops to 17% within 60 minutes. The nanocomposite material loaded with MnO2 exhibits excellent catalytic ability for H2O2, thus expanding the application potential of nanocomposites as nanomotors after loading different metal oxides.

[0091] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A nanocomposite material with a tail loaded with metal oxide, characterized in that: The nanocomposite material comprises bullet-shaped AuNBPs@Ag nanoparticles with a Janus structure and metal oxides loaded on the tails of the bullet-shaped AuNBPs@Ag nanoparticles.

2. The nanocomposite material of claim 1, characterized in that: The bullet-shaped AuNBPs@Ag nanoparticles are composed of gold nanobipyramid AuNBPs and Ag nanorods. One end of the gold nanobipyramid AuNBPs is exposed to form a tip structure, and the other end is wrapped by the Ag nanorod to form a rod-like structure. The metal oxide is loaded on the tail of the Ag nanorod.

3. The nanocomposite material of claim 1, wherein: The aspect ratio of the bullet-shaped AuNBPs@Ag nanoparticles can be adjusted in the range of 4-6.

4. The nanocomposite material of claim 1, characterized in that: The metal oxide includes any one of manganese dioxide, titanium dioxide, cerium dioxide and cuprous oxide.

5. A method for preparing a nanocomposite material having a tail loaded with a metal oxide, characterized in that: The preparation method comprises: preparing Au seeds; Using the Au seeds to induce the growth of gold nanobipyramids AuNBPs with controllable aspect ratio; A layer of silver nanomaterial is coated and grown on the surface of the gold nanobipyramid AuNBPs to form AuNBPs@Ag nanorods; Asymmetric etching is performed on the AuNBPs@Ag nanorods to obtain bullet-shaped AuNBPs@Ag nanomaterials having a Janus structure; A metal oxide is loaded on the tail of the bullet-shaped AuNBPs@Ag nanomaterial to obtain a nanocomposite material.

6. The method for preparing a nanocomposite material having a tail loaded with metal oxide according to claim 5, characterized in that: The preparation of the gold nanobipyramid AuNBPs includes: In a solution containing hexadecyltrimethylammonium bromide, chloroauric acid, silver nitrate, hydrochloric acid and ascorbic acid, different amounts of Au seeds were added to form gold nanobipyramids AuNBPs with controllable aspect ratio through self-assembly and growth processes.

7. The method for preparing a nanocomposite material having a tail loaded with metal oxide according to claim 5, characterized in that: The preparation of the AuNBPs@Ag nanorods comprises: Gold nanobipyramids AuNBPs were mixed with hexadecyltrimethylammonium chloride, silver nitrate and ascorbic acid, and a silver nanolayer was grown on the surface of the gold nanobipyramids AuNBPs through a reduction reaction of silver ions.

8. The method for preparing a nanocomposite material having a tail loaded with metal oxide according to claim 5, characterized in that: The asymmetric etching step comprises: A mixed solution containing chloroauric acid, ascorbic acid, sodium hydroxide and hexadecyltrimethylammonium bromide is prepared and stirred evenly at room temperature; the AuNBPs@Ag nanorods are added to the mixed solution and reacted in a water bath at 25-35° C. for a period of time, and purified after the reaction is completed; The purified nanorods were redispersed in a solution containing hexadecyltrimethylammonium bromide, and sodium bicarbonate, hydrogen peroxide, potassium thiocyanate and cobalt nitrate were added in sequence. The reaction was carried out in a water bath at 60-80°C for a period of time. After the reaction was completed, the nanorods were purified to obtain bullet-shaped AuNBPs@Ag nanomaterials with a Janus structure.

9. The method for preparing a nanocomposite material having a tail loaded with metal oxide according to claim 5, characterized in that: The step of loading the metal oxide at the tail portion comprises: The bullet-shaped AuNBPs@Ag nanomaterials were dispersed in a solution containing hexadecyltrimethylammonium bromide, and then a solution containing a metal oxide precursor was added and reacted at 50-70°C for a period of time to load the metal oxide on the tail of the bullet-shaped AuNBPs@Ag nanomaterials.

10. Use of the nanocomposite material with a metal oxide loaded on the tail as claimed in any one of claims 1 to 4 as a nanomotor in catalytic degradation of hydrogen peroxide.