Glass article manufacturing method and glass article

By grinding the glass material in one-stage by using grinding wheels of specific particle sizes, the chip problem in chamfering processing is solved, the shape accuracy and quality improvement is achieved, and the process time is simplified.

CN119077443APending Publication Date: 2024-12-06AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410706041.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2024-06-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing glass article manufacturing methods, it is difficult to sufficiently reduce the generation of chips during chamfering processing, which affects shape accuracy and quality.

Method used

The end surface of the glass material with an arithmetic average height Sa of 0.1 μm or more and less than 1.0 μm is grounded in one stage to form a chamfered part to ensure that the arithmetic average height Sa of the chamfered part is at The maximum value of chips is controlled to be less than 35 μm.

Benefits of technology

While maintaining the desired shape, significantly reduce chips, improve the surface quality and shape accuracy of glass items, and simplify process time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077443A_ABST
    Figure CN119077443A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to reduce cuttings while obtaining a desired shape by chamfering. A method for manufacturing a glass article (10T) includes: cutting a glass base material (10) to obtain a glass material (10S) having a first main surface (10A), a second main surface (10B), and an end surface (10C) connecting the first main surface (10A) and the second main surface (10B), the arithmetic mean height (Sa) of the end surface (10C) being 0.1 [mu] m or more and less than 1.0 [mu] m; and grinding the end surface (10C) in a state in which the arithmetic mean height (Sa) is at least 0.1 [mu] m and less than 1.0 [mu] m by using a grinding wheel (W) having abrasive grains having a median diameter (D50) of 8 [mu] m to 24 [mu] m, thereby forming a chamfered portion (10D2).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a glass article and a glass article. Background Art

[0002] It is known to manufacture glass articles of a desired shape by chamfering the end face of glass. When manufacturing glass articles in this way, the glass is usually cut with a cutter, a scriber, etc., and the cut surface is subjected to a two-stage chamfering process. For example, Patent Document 1 describes that the end face of glass is further ground after being chamfered.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2022 / 149512 Summary of the invention

[0006] However, in the above method, there is a risk that the chips of the chamfered portion cannot be sufficiently reduced. Therefore, it is required to obtain a desired shape by chamfering while reducing the chips.

[0007] An object of the present invention is to provide a method for producing a glass article and a glass article which can obtain a desired shape by chamfering while reducing cutting chips.

[0008] The manufacturing method of the glass article disclosed in the present invention includes: cutting a glass mother material to obtain a glass material having a first main surface, a second main surface, and an end surface connecting the first main surface and the second main surface, and the arithmetic mean height Sa of the above-mentioned end surfaces is greater than 0.1μm and less than 1.0μm; and using a grinding wheel with abrasive grains with a median diameter D50 of 8μm to 24μm to grind the above-mentioned end surfaces in a state where the arithmetic mean height Sa is greater than 0.1μm and less than 1.0μm to form a chamfered portion.

[0009] The glass article disclosed in the present invention is a glass article having a first main surface, a second main surface, and an end surface connecting the first main surface and the second main surface, the end surface having a side surface portion and a chamfered portion connecting the side surface portion and the first main surface, the arithmetic mean height Sa of the chamfered portion being 0.1 μm to 0.8 μm, and the maximum value of the size of chips existing in an interval of 100 mm in length in the circumferential direction of the chamfered portion when observed from the first main surface side is less than 35 μm.

[0010] According to the present invention, it is possible to obtain a desired shape by chamfering and reduce chips. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a schematic cross-sectional view of a glass base material.

[0012] Figure 2 It is a schematic top view of a glass base material.

[0013] Figure 3 is a schematic top view of a glass material.

[0014] Figure 4 This is a schematic diagram for explaining a method for producing a glass article.

[0015] Figure 5 is a schematic cross-sectional view of a glass object.

[0016] Figure 6 is a schematic top view of a glass object.

[0017] Figure 7 This is a flowchart that explains the manufacturing process of glass products.

[0018] Explanation of symbols

[0019] 10Glass base material

[0020] 10A 1st main surface

[0021] 10B 2nd main side

[0022] 10C, 10D end face

[0023] 10D1 Side face

[0024] 10D2 chamfering part

[0025] 10S glass material

[0026] 10T glass items

[0027] W Grinding Wheel DETAILED DESCRIPTION

[0028] The preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. It should be noted that the present invention is not limited to the embodiments, and when there are multiple embodiments, embodiments formed by combining the embodiments are also included. In addition, numerical values ​​include rounded ranges.

[0029] In this embodiment, the glass base material 10 is cut to obtain a glass material 10S, and the glass material 10S is ground to produce a glass article 10T. Hereinafter, the glass base material 10, a method for producing the glass material 10S from the glass base material 10, and a method for producing the glass article 10T from the glass material 10S are described.

[0030] It should be noted that the glass article 10T in this embodiment is provided in a vehicle-mounted display device and is used as a covering material on the surface of the vehicle-mounted display device. That is, the glass article 10T is provided on the surface (display surface) of a display panel of the vehicle-mounted display device to protect the display surface of the display panel. However, the use of the glass article 10T is arbitrary, and it can be used as a covering material for a display device for purposes other than vehicle-mounted use, as a covering material for a device other than a display device, and can also be used for purposes other than a covering material.

[0031] (Glass base material)

[0032] Figure 1 is a schematic cross-sectional view of a glass mother material. Figure 2 is a schematic top view of the glass matrix. Figure 1 As shown, the glass base material 10 is a transparent glass plate-shaped member. It should be noted that the plate-shaped here is not limited to a flat plate, and may refer to a plate-shaped main surface having a width greater than a thickness, and the transparent here may refer to the transmission of visible light.

[0033] Hereinafter, one principal surface of the glass mother material 10 is referred to as the first principal surface 10A, the principal surface on the opposite side of the first principal surface 10A is referred to as the second principal surface 10B, and the end surface (side surface) connecting the first principal surface 10A and the second principal surface 10B is referred to as the end surface 10X. In addition, the thickness direction of the glass mother material 10, i.e., the direction connecting the second principal surface 10B and the first principal surface 10A, is referred to as the Z direction. In addition, a direction perpendicular to the Z direction (in the direction between Figure 1 In the example, the left-right direction) is set as the X direction, and the direction perpendicular to the Z direction and the X direction (in Figure 1 In the example, the direction perpendicular to the paper surface) is set as the Y direction. In addition, a direction along the X direction (in Figure 1 In the example, the right direction) is set as direction X1, and the other direction along the X direction (in Figure 1 In the example, the left direction) is set as direction X2, and a direction along the Y direction (in Figure 1 In the example, the direction toward the back of the paper) is set as direction Y1, and the other direction along the Y direction (in Figure 1 In the example, the direction toward the near front side of the paper surface) is set as direction Y2, one direction along the Z direction (the direction from the second main surface 10B toward the first main surface 10A) is set as direction Z1, and the other direction along the Z direction (the direction from the first main surface 10A toward the second main surface 10B) is set as direction Z2.

[0034] It should be noted that the Z direction here may be a direction perpendicular to the first main surface 10A at the center position of the glass base material 10 .

[0035] exist Figure 2In the example, the glass base material 10 is a rectangular flat plate when viewed from the Z direction, but the shape of the glass base material 10 can be arbitrary. For example, the glass base material 10 is not limited to a rectangle when viewed from the Z direction, and can also be a polygon, a circle, an ellipse, etc.

[0036] exist Figure 1 In the example of , the glass matrix 10 is a flat plate with the first principal surface 10A and the second principal surface 10B being flat, but it is not limited thereto and may also be a flat plate with a curved shape. That is, the glass matrix 10 may also be a curved surface with the first principal surface 10A and / or the second principal surface 10B convex in the Z direction.

[0037] When the first principal surface 10A and / or the second principal surface 10B of the glass mother material 10 are curved surfaces convex in the Z direction, the radius of curvature of the first principal surface 10A and / or the second principal surface 10B of the glass mother material 10 is preferably 10000 mm or less, more preferably 5000 mm or less, and further preferably 3000 mm or less. When the first principal surface 10A and / or the second principal surface 10B of the glass mother material 10 are curved surfaces convex in the Z direction, the radius of curvature of the first principal surface 10A and / or the second principal surface 10B of the glass mother material 10 is preferably 10 mm or more, more preferably 50 mm or more, further preferably 100 mm or more, and further preferably 200 mm or more. In other words, when the first principal surface 10A and / or the second principal surface 10B of the glass mother material 10 are curved surfaces convex in the Z direction, the curvature radius of the first principal surface 10A and / or the second principal surface 10B of the glass mother material 10 is preferably 10 mm to 10000 mm, more preferably 50 mm to 5000 mm, further preferably 100 mm to 3000 mm, and further preferably 200 mm to 3000 mm.

[0038] The thickness D of the glass mother material 10 is preferably 0.1 mm or more, more preferably 0.7 mm or more, further preferably 1.0 mm or more, and particularly preferably 1.1 mm or more. In addition, the thickness D of the glass mother material 10 is preferably 5 mm or less, more preferably 3 mm or less, and further preferably 1.3 mm or less. In other words, the thickness D of the glass mother material 10 is preferably 0.1 mm to 5 mm, more preferably 0.7 mm to 5 mm, further preferably 1.0 mm to 3 mm, and particularly preferably 1.1 mm to 1.3 mm. It should be noted that the thickness D of the glass mother material 10 refers to the length in the Z direction from the first principal surface 10A to the second principal surface 10B.

[0039] Fracture toughness value K of glass matrix 10 IC Preferably 0.6 (MPa·m 0.5 ) or more, more preferably 0.6 (MPa·m 0.5 )~1.00(MPa·m 0.5), more preferably 0.65 (MPa·m 0.5 )~0.70(MPa·m 0.5 ). Fracture toughness value K IC For example, it can be measured according to the Double Cleavage Drilled Compression (DCDC) method described in Non-Patent Document (NEW GASS Vol. 15 No. 2 2000 p18).

[0040] The glass matrix 10 may be an amorphous glass or a crystallized glass containing crystals on the surface or inside. As the glass matrix 10, for example, alkali-free glass, soda-lime glass, soda-lime silicate glass, aluminosilicate glass, borosilicate glass, lithium aluminosilicate glass, etc. may be used. In order to properly perform chemical strengthening, the material of the glass matrix 10 is preferably alkali glass. Further, as the glass matrix 10, aluminosilicate glass and lithium aluminosilicate glass are preferred, which can easily introduce large stress through strengthening treatment to obtain thin but high-strength glass even if the thickness is thin. Chemically strengthened glass based on aluminosilicate glass (for example, "Dragontrail (registered trademark)" manufactured by AGC Corporation) can also be appropriately used.

[0041] The glass base material 10 may contain 50% to 80% of SiO in terms of mol% based on oxides. 2 , 1% to 20% Al 2 O 3 and 6% to 20% Na 2 O. In addition, the glass base material 10 may contain 50 to 80% of SiO in terms of mol% based on oxides. 2 , 0.1~25%Al 2 O 3 3~30%Li 2 O+Na 2 O+K 2 O, 0-25% MgO, 0-25% CaO and 0-5% ZrO 2 In addition, the glass base material 10 may contain 50% to 80% of SiO in terms of mol% based on oxides. 2 , 1% to 20% Al 2 O 3 , 6% ~ 20% Na 2 O, 0% to 11% K 2 O, 0% to 15% MgO, 0% to 6% CaO and 0% to 5% ZrO 2It should be noted that the numerical range indicated by "~" indicates a range including the numerical values ​​recorded before and after "~" as the lower limit and the upper limit. In addition, for example, 50% to 80% here means 50% to 80% when the molar percentage of the total amount of the glass matrix 10 is set to 100%, and the same applies to other numerical ranges. In addition, for example, Li 2 O+Na 2 O+K 2 O refers to Li 2 O、Na 2 O and K 2 The total content of O is the same as the case where "+" is used for other symbols.

[0042] More specifically, as a more preferable composition of the glass matrix 10, the following glass compositions can be cited. It should be noted that, for example, "containing 0% to 25% of MgO" means that MgO is not essential but can be contained at 25%. Glass (i) is included in soda-lime silicate glass, glasses (ii) and (iii) are included in aluminosilicate glass, and glasses (iv) to (vi) are included in lithium aluminosilicate glass.

[0043] (i) The composition expressed in mol% contains 63% to 73% SiO 2 , 0.1%~5.2%Al 2 O 3 , 10% ~ 16% Na 2 O, 0% to 1.5% K 2 O, 0% to 5% Li 2 Glass containing 0, 5% to 13% MgO and 4% to 10% CaO.

[0044] (ii) The composition expressed in mol% contains 50% to 74% SiO 2 1% to 10% Al 2 O 3 , 6% ~ 14% Na 2 O, 3% to 11% K 2 O, 0% to 5% Li 2 O, 2% to 15% MgO, 0% to 6% CaO and 0% to 5% ZrO 2 、SiO 2 and Al 2 O 3 The total content of Na is less than 75%. 2 O and K 2 Glass containing 12% to 25% in total O and 7% to 15% in total MgO and CaO.

[0045] (iii) The composition expressed in mol% contains 68% to 80% SiO 2 4% to 10% Al 2 O 3 , 5% ~ 15% Na 2 O, 0% to 1% K 2 O, 0% to 5% Li 2 O, 4% to 15% MgO and 0% to 1% ZrO 2 of glass.

[0046] (iv) The composition expressed in mol% contains 67% to 75% SiO 2 , 0%~4%Al 2 O 3 , 7% ~ 15% Na 2 O, 1% to 9% K 2 O, 0% to 5% Li 2 O, 6% to 14% MgO and 0% to 1.5% ZrO 2 、SiO 2 and Al 2 O 3 The total content of Na is 71% to 75%. 2 O and K 2 Glass having a total O content of 12% to 20% and a CaO content of less than 1% when CaO is contained.

[0047] (v) The composition expressed in mol% contains 56% to 73% SiO 2 , 10% to 24% Al 2 O 3 , 0% to 6% B 2 O 3 , 0%~6%P 2 O 5 2%~7%Li 2 O, 3% ~ 11% Na 2 O, 0% to 5% K 2 O, 0% to 8% MgO, 0% to 2% CaO, 0% to 5% SrO, 0% to 5% BaO, 0% to 5% ZnO, 0% to 2% TiO 2 , 0% to 4% ZrO 2 of glass.

[0048] (vi) The composition expressed in mol% contains 58% to 80% SiO 2 , 13% to 18% Al 2 O 3 , 0% to 5% B 2 O 3, 0.5%~4%P 2 O 5 3% to 10% Li 2 O, 5% ~ 20% Na 2 O, 0% to 2% K 2 O, 0% to 11% MgO, 0% to 20% CaO, 0% to 20% SrO, 0% to 15% BaO, 0% to 10% ZnO, 0% to 1% TiO 2 , 0% to 2% ZrO 2 of glass.

[0049] The glass matrix 10 is preferably not chemically strengthened. Further, the glass material 10S obtained by cutting the glass matrix 10 and the glass article 10T obtained by grinding the glass material 10S are preferably not chemically strengthened. Since the glass matrix 10 is not chemically strengthened, the occurrence of defects during cutting and chamfering can be suppressed. Therefore, the material (composition) of the glass material 10S and the glass article 10T is preferably the same as the material (composition) of the glass matrix 10.

[0050] However, the glass article 10T after grinding can be chemically strengthened. The chemically strengthened glass article 10T is suitable for use as a protective glass for a display device. When the glass article 10T after grinding is chemically strengthened, the composition of the glass base material 10 is equivalent to the composition of the central part of the glass article 10T in the plate thickness direction. Specifically, if the element released by substitution during chemical strengthening is regarded as the element before substitution, and the element incorporated by substitution through chemical strengthening is regarded as the substitution element, it can be said that the glass base material 10 has a composition in which the surface layer of the glass article 10T after chemical strengthening contains the element before substitution instead of the substitution element.

[0051] (Manufacture of glass materials)

[0052] Figure 3 1 is a schematic top view of a glass material. In the present manufacturing method, a glass material 10S is obtained by cutting a glass matrix 10. Figure 3 As shown in FIG. 1 , the glass material 10S has a first main surface 10A, a second main surface 10B, and an end surface 10C connecting the first main surface 10A and the second main surface 10B. The first main surface 10A of the glass material 10S corresponds to the first main surface 10A of the glass mother material 10, and the second main surface 10B of the glass material 10S corresponds to the second main surface 10B of the glass mother material 10. Therefore, the thickness of the glass material 10S is the same as the thickness D of the glass mother material 10.

[0053] At least a portion of the end face 10C of the glass material 10S is a cut surface formed by cutting the glass base material 10. In the present manufacturing method, the glass base material 10 is cut in such a manner that the arithmetic mean height Sa of the end face 10C of the glass material 10S is greater than or equal to 0.1 μm and less than 1.0 μm. The arithmetic mean height Sa of the end face 10C of the glass material 10S is preferably 0.2 μm to 0.7 μm, and more preferably 0.3 μm to 0.7 μm. By setting the lower limit of the arithmetic mean height Sa of the end face 10C to such a range, it is possible to suppress the grinding wheel W from sliding on the end face 10C due to the end face 10C being too smooth and failing to perform grinding properly, and a desired shape can be obtained by chamfering the grinding wheel W. In addition, by setting the upper limit of the arithmetic mean height Sa of the end face 10C to such a range and combining it with the chamfering method described below, it is possible to reduce chips.

[0054] It should be noted that the arithmetic mean height Sa of the end surface 10C may be the arithmetic mean height Sa of a 90 μm×60 μm region in contact with the main surface (the first main surface 10A or the second main surface 10B) in the entire region of the end surface 10C when viewed from a direction perpendicular to the Z direction. The arithmetic mean height Sa can be measured by a method based on ISO 25178.

[0055] It should be noted that for the arithmetic mean height Sa, three random locations are selected from the end surface 10C, and the arithmetic mean height Sa in the area of ​​90 μm×60 μm is measured at each location, and the average value is used. Three random points are selected from the entire area without deviation, and outlier points are avoided. The same is true for the arithmetic mean height Sa and the maximum height Sz at other locations.

[0056] In the present manufacturing method, the glass base material 10 is preferably cut so that the maximum height Sz of the end surface 10C of the glass material 10S is 1 μm to 10 μm. By setting the lower limit of the maximum height Sz of the end surface 10C to such a range, it is possible to prevent the end surface 10C from being too smooth to be properly ground by the grinding wheel W, and a desired shape can be obtained by chamfering using the grinding wheel W. By setting the upper limit of the maximum height Sz of the end surface 10C to such a range, it is possible to reduce chips.

[0057] It should be noted that the maximum height Sz of the end surface 10C may be the maximum height Sz of a 90 μm×60 μm region in contact with the main surface (the first main surface 10A or the second main surface 10B) in the entire region of the end surface 10C when viewed from a direction perpendicular to the Z direction. The maximum height Sz can be measured by a method based on ISO 25178.

[0058] like Figure 2As shown, in the example of this embodiment, an imaginary line T described later is set on the glass base material 10, the glass base material 10 is cut along the imaginary line T, and the portion surrounded by the imaginary line T is cut out from the glass base material 10 to obtain a glass material 10S. Hereinafter, the center of the glass material 10S is taken as the center O. That is, Figure 2 In the example of , the entire region of the end surface 10C of the glass material 10S becomes a cut surface along the imaginary line T. It should be noted that the center O of the glass material 10S refers to the center position of the glass material 10S when viewed from the Z direction, and the radial direction and the circumferential direction refer to the radial direction and the circumferential direction when the axis passing through the center O of the glass material 10S along the Z direction is the axial direction. The same shall apply unless otherwise specified below.

[0059] However, the glass base material 10 is not limited to being cut over the entire circumferential section. In this case, a portion of the end face 10C of the glass material 10S becomes the cut surface, and the remaining portion of the end face 10C of the glass material 10S becomes the portion corresponding to the end face 10X of the glass base material 10 (i.e., the end face 10X of the glass base material 10 that has not been cut). Thus, when only a portion of the end face 10C becomes the cut surface, it is preferred that the end face 10C is cut over the entire region, i.e., including the end face 10X, and the arithmetic mean height Sa and the maximum height Sz are within the above ranges.

[0060] exist Figure 3 In the example of FIG. 1 , when the glass base material 10 is viewed from the Z direction, the four vertices of the rectangle are R-shaped (curved). However, the shape of the glass base material 10 viewed from the Z direction may be arbitrary.

[0061] In addition, the end surface 10C of the glass material 10S obtained by cutting is preferably flat in the Z direction, for example, preferably has no chamfered portion. The end surface 10C of the glass material 10S is more preferably perpendicular to the first main surface 10A. The perpendicularity here is not limited to strictly 90 degrees, and may also include about 85 degrees to 95 degrees.

[0062] (Cutting by laser)

[0063] The method of cutting the glass base material 10 to obtain the glass material 10S may be arbitrary, but in this embodiment, the laser light L is irradiated onto the main surface of the glass base material 10 to cut the glass base material 10. More specifically, in this embodiment, Figure 1 As shown, the first main surface 10A of the glass base material 10 is irradiated with laser light L to form a modified portion H in the glass base material 10, and the glass base material 10 is fractured (cut) starting from the modified portion H, thereby obtaining a glass material 10S. It should be noted that the laser light L may be irradiated not on the first main surface 10A but on the second main surface 10B.

[0064] like Figure 1As shown, in the present manufacturing method, laser L is irradiated from an irradiation device M onto the first main surface 10A of the glass mother material 10 to form a modified portion H in the glass mother material 10. The modified portion H is a layer whose density and / or refractive index changes through structural changes of the glass or through melting and resolidification of the glass. The modified portion H may contain voids. It should be noted that the laser L forms the modified portion H, for example, through nonlinear absorption. Nonlinear absorption is also called multiphoton absorption. The probability of multiphoton absorption is nonlinear with respect to the photon density (power density of the laser L), and the probability increases sharply as the photon density increases. For example, the probability of two-photon absorption is proportional to the square of the photon density.

[0065] It should be noted that, for the portion of the glass base material 10 where the modified portion H is not formed (the portion not irradiated with the laser light L), a portion where at least one of the density, the refractive index, the unpaired electron density, and the fictive temperature is different can be the modified portion H. It should be noted that the portion where the modified portion H is not formed can refer to, for example, a position that is more than 10 mm away from the virtual line T described later when viewed from the Z direction.

[0066] like Figure 1 As shown, the irradiation device M for irradiating the laser light L includes a light source unit M1, an optical system M2, and a scanning mechanism M3. The light source unit M1 is a light source for generating the laser light L. The light source unit M1 may be any device, but for example, a Nd-doped YAG crystal (Nd:YAG) or the like may be used. The optical system M2 is provided on the traveling direction side of the laser light L relative to the light source unit M1, and the laser light L from the light source unit M1 is incident. The optical system M2 emits the incident laser light L toward the first principal surface 10A. The scanning mechanism M3 is a mechanism for scanning (scanning) the laser light L. That is, the scanning mechanism M3 causes the position where the laser light L is irradiated to the first principal surface 10A, i.e., the irradiation position, to scan (move) in a direction parallel to the first principal surface 10A. The scanning mechanism M3 may be any mechanism as long as it is capable of scanning the laser light L, and may be, for example, a galvano mirror or the like. It should be noted that the configuration of the irradiation device M is not limited to the above description, and may be any configuration that is capable of irradiating the laser light L while scanning the irradiation position in a direction parallel to the first principal surface 10A. For example, the irradiation position may be scanned by fixing the position of the laser head irradiating the laser light L such as the light source unit M1 and the optical system M2 and moving the glass base material 10 irradiated with the laser light L. In other words, the irradiation position may be scanned by moving the relative position of the spot position of the laser light L and the glass base material 10.

[0067] The scanning of the laser light L is not limited to the direction parallel to the first main surface 10A, but may also be performed in the direction perpendicular to the first main surface 10A, that is, in the thickness direction of the glass article 10a. For example, when the thickness of the glass article 10a is 3 mm or more, the stress required for fracture can be easily reduced by scanning in the thickness direction.

[0068] In addition, it is preferable that the laser light L has a linear power distribution in the optical axis direction. In addition, a laser light having a power distribution with at least one peak in the optical axis direction can be used as the laser light L. Thus, the modified portion H can be formed in the thickness direction with high precision.

[0069] It should be noted that the laser light L can be linearly focused by self-focusing due to the nonlinear Kerr effect, or can be linearly focused by the optical system M2. As a specific optical system M2 in this case, for example, an optical system using an axicon lens, an optical system using a birefringent material, an optical system using a diffractive optical element, or an optical system using optical aberrations can be used.

[0070] The wavelength range of the laser light L is preferably 250 nm to 3000 nm. The laser light with a wavelength range of 250 nm to 3000 nm can transmit the glass matrix 10 to a certain extent, so that nonlinear absorption can be generated inside the glass matrix 10 to appropriately form the modified portion H. The wavelength range is more preferably 260 nm to 2500 nm.

[0071] In addition, the laser L is preferably a pulsed light (pulsed oscillating laser). The pulse width of the laser L is preferably 10fs to 1000ns. In addition, if it is a pulsed laser with a pulse width of less than 1000ns, it is easy to increase the photon density, and nonlinear absorption can be generated inside the glass mother material 10 to form a modified portion H. The pulse width is preferably 100fs to 100ns. The laser L can output a pulse group called a burst. A pulse group has, for example, 3 to 50 pulses of light, each of which has a pulse width of less than 10ns. In a pulse group, the energy of the pulse light can be gradually reduced. The energy of a pulse or a pulse group is appropriately set to be able to form a point-shaped or line-shaped modified portion or crack that is continuously formed in the thickness direction of the glass mother material 10. For example, it is 10μJ to 5000μJ, preferably 20μJ to 3000μJ, and more preferably 30μJ to 2000μJ.

[0072] In this manufacturing method, by irradiating the laser light L while scanning the irradiation position, a plurality of modified portions H are formed at predetermined intervals along the scanning direction (movement direction) of the irradiation position. Figure 2As shown, a scanning trajectory of the irradiation position of the laser L, i.e., an imaginary line T, is set on the first principal surface 10A of the glass mother material 10. Then, in the present manufacturing method, by irradiating the laser L along the imaginary line T while scanning (moving) the irradiation position on the first principal surface 10A of the glass mother material 10, a plurality of modified portions H arranged at prescribed intervals along the imaginary line T are formed. The interval between each modified portion H is, for example, 2μm to 25μm, preferably 3μm to 20μm. If it is within this range, it is easy to improve the quality of the cut surface after cutting in the subsequent process. It should be noted that in Figure 2 In the example, the imaginary line T is a shape that surrounds the center O of the glass base material 10 throughout the entire circumferential range, but the shape of the imaginary line T can be set arbitrarily. The length of the imaginary line T can also be arbitrary, for example, preferably 10 mm or more, more preferably 100 mm to 5000 mm, and further preferably 800 mm to 2000 mm.

[0073] It should be noted that the method of cutting the glass base material 10 to obtain the glass material 10S is not limited to the irradiation of the laser light L. For example, the glass base material 10 may be cut using a cutter scriber or a grinding wheel to obtain the glass material 10S.

[0074] (Manufacture of glass products)

[0075] Figure 4 Schematic diagram for explaining a method for manufacturing a glass article. In this manufacturing method, the end face 10C of a glass material 10S in a state where the arithmetic mean height Sa is in the above range (0.1 μm or more and less than 1.0 μm) is ground by a grinding wheel W having a median diameter D50 of 8 μm to 24 μm, and a chamfered portion 10D2 is formed on the end face 10C, thereby manufacturing a glass article 10T having a chamfered portion 10D2. That is, in this embodiment, other processing steps are not performed on the end face 10C of the glass material 10S in the state described above, and the end face 10C of the glass material 10S in a state where other processing steps are not performed is ground by a grinding wheel W having a median diameter D50 of 8 μm to 24 μm, thereby obtaining a glass article 10T. The grinding wheel W will be described later.

[0076] In the present manufacturing method, the end surface 10C of the glass material 10S is ground with a grinding wheel W to remove at least a portion of the end surface 10C of the glass material 10S to form the end surface 10D, thereby obtaining the glass material 10S having the end surface 10D as a glass article 10T.

[0077] The glass article 10T has a first main surface 10A, a second main surface 10B, and an end surface 10D connecting the first main surface 10A and the second main surface 10B. The first main surface 10A of the glass article 10T corresponds to the first main surface 10A of the glass material 10S, and the second main surface 10B of the glass article 10T corresponds to the second main surface 10B of the glass material 10S. Therefore, the thickness of the glass article 10T is the same as the thickness of the glass material 10S (the thickness D of the glass base material 10).

[0078] (End face)

[0079] The end surface 10D of the glass article 10T is an end surface (side surface) connecting the first main surface 10A and the second main surface 10B. The end surface 10D includes a side surface portion 10D1 and a chamfered portion 10D2. The side surface portion 10D1 of the glass article 10T is the radially outermost surface (side surface) of the glass material 10S. The side surface portion 10D1 may be flat or curved.

[0080] The chamfered portion 10D2 is a chamfered surface connecting the side surface portion 10D1 and the main surface (the first main surface 10A or the second main surface 10B). Figure 4 When viewed in the Y direction (in the example of FIG. 1 ), the chamfered portion 10D2 is inclined relative to both the side portion 10D1 and the main surface (the first main surface 10A or the second main surface 10B). The chamfered portion 10D2 may be flat (ie, C-chamfered) or curved (R-chamfered).

[0081] In the present embodiment, the end surface 10D includes the chamfered portion 10D2 connecting the side surface portion 10D1 and the first main surface 10A and the chamfered portion 10D2 connecting the side surface portion 10D1 and the second main surface 10B as the chamfered portion 10D2. However, the end surface 10D may include only one of the chamfered portion 10D2 connecting the side surface portion 10D1 and the first main surface 10A and the chamfered portion 10D2 connecting the side surface portion 10D1 and the second main surface 10B.

[0082] (grinding wheel)

[0083] The grinding wheel W is a grinding wheel having abrasive grains with a median diameter D50 of 8 μm to 24 μm. That is, the grinding wheel W is a component for grinding with a plurality of abrasive grains with a median diameter D50 of 8 μm to 24 μm provided on the surface. The median diameter D50 of the abrasive grains of the grinding wheel W is preferably 9.4 μm to 20.5 μm, and more preferably 9.4 μm to 16.2 μm. By setting the upper limit of the median diameter D50 of the abrasive grains within this range, the chips can be reduced, and by setting the lower limit of the median diameter D50 of the abrasive grains within this range, the chips can be appropriately reduced using the abrasive grains that are generally circulated.

[0084] In addition, the median diameter D50 of the abrasive grains can be measured using a particle size distribution meter.

[0085] The material of the abrasive grains provided on the grinding wheel W may be any material, and examples thereof include single crystal diamond, cubic boron nitride, silicon carbide, aluminum oxide, etc., and single crystal diamond is preferred.

[0086] The shape of the grinding wheel W is not particularly limited, and may be cylindrical, spherical, etc., but is preferably a molded grinding wheel (round grindstone) having a first part W1 and a second part W2. The molded grinding wheel is a grinding wheel having a grinding surface that matches the shape of the target workpiece. The first part W1 is a part having a grinding surface corresponding to the side portion 10D1, in other words, having a grinding surface for forming the side portion 10D1. The first part W1 is cylindrical, and the outer peripheral surface is a grinding surface. The second part W2 is a part having a grinding surface corresponding to the chamfered portion 10D2, in other words, having a grinding surface for forming the chamfered portion 10D2. The second part W2 is connected to the first part W1 on the axial side, and is a conical shape whose diameter increases as it moves away from the first part W1, and the outer peripheral surface is a grinding surface. In the present embodiment, the grinding wheel W has a second part W2 disposed on one side of the axial direction of the first part W1 and a second part W2 disposed on the other side of the axial direction of the first part W1 as the second part W2.

[0087] The abrasive grains described above are provided on the grinding surface of the first portion W1 and the grinding surface of the second portion W2.

[0088] The boundary portion between the grinding surface (peripheral surface) of the first part W1 and the grinding surface (peripheral surface) of the second part W2 is preferably R-shaped (curved). The radius of curvature of the boundary portion is preferably 0.05 mm or more, more preferably 0.1 mm to 0.5 mm, and further preferably 0.2 mm to 0.3 mm. When the radius of curvature of the boundary portion is within this range, the radius of curvature of the boundary portion between the side surface portion 10D1 obtained by grinding and the chamfered portion 10D2 may also be within this range, and chips can be more appropriately reduced.

[0089] (Grinding with a grinding wheel)

[0090] In the present manufacturing method, Figure 4 As shown in the figure, the grinding wheel W is rotated with the central axis along the axial direction of the grinding wheel W as the rotation axis, and the grinding wheel W is pressed against the end face 10C of the glass material 10S. As a result, the end face 10C is ground to form the end face 10D. In this embodiment, the portion of the end face 10C of the glass material 10S pressed by the first part W1 is ground (removed) by the first part W1 to form the side face 10D1. Then, the portion of the end face 10C of the glass material 10S pressed by the second part W2 is ground (removed) by the second part W2 to form the chamfered portion 10D2.

[0091] Here, the machining allowance of the end surface 10C produced by grinding with the grinding wheel W is referred to as the machining allowance A1. The machining allowance A1 refers to the machining allowance in the direction perpendicular to the end surface 10C (side surface 10D1) of the side surface 10D1 (in Figure 4 In the example, the machining allowance A1 is the machining allowance in the direction X). In other words, the machining allowance A1 refers to the distance from the end face 10C to the side face 10D1 in the direction perpendicular to the end face 10C (side face 10D1) when the center of the glass material 10S before grinding and the center of the glass article 10T after grinding are placed in the same position. In this case, the machining allowance A1 is preferably 0.05mm to 0.3mm, more preferably 0.05mm to 0.15mm, and further preferably 0.1mm to 0.15mm. By setting the lower limit of the machining allowance A1 to this range, chips can be fully removed, and by setting the upper limit of the machining allowance A1 to this range, the grinding time can be suppressed from becoming longer.

[0092] Thus, in the present embodiment, the end surface 10C of the glass material 10S having an arithmetic mean height Sa of 0.1 μm or more and less than 1.0 μm is ground using a grinding wheel W having abrasive grains having a median diameter D50 of 8 μm to 24 μm, and the chamfered portion 10D2 is formed on the end surface 10C, thereby manufacturing a glass article 10T having the chamfered portion 10D2 formed thereon.

[0093] In addition, as described above, in the present embodiment, a molded grinding wheel is used as the grinding wheel W, and the end face 10C is ground by the first part W1 and the second part W2, thereby forming the side face 10D1 and the chamfered portion 10D2 at the same time. However, the present invention is not limited thereto, and the side face 10D1 and the chamfered portion 10D2 may be formed separately. In this case, for example, the end face 10C is ground by the grinding wheel W having the first part W1 to form the side face 10D1. Then, the boundary portion between the side face 10D1 and the main face (the first main face 10A or the second main face 10B) is ground by the grinding wheel W having the second part W2 to form the chamfered portion 10D2. In this case, it can also be said that the side face 10D1 is formed by one-stage grinding only by the grinding wheel W having the first part W1, and the chamfered portion 10D2 is formed by one-stage grinding only by the grinding wheel W having the second part W2.

[0094] In addition, in the present embodiment, the side surface 10D1 is a ground surface formed by grinding the end surface 10C, but the present invention is not limited thereto, and the portion of the end surface 10C that is not ground and remains may be used as the side surface 10D1. In this case, for example, the boundary portion between the end surface 10C and the main surface (the first main surface 10A or the second main surface 10B) is ground using a grinding wheel W having a second portion W2 to form a chamfered portion 10D2. That is, in this case, only the chamfered portion 10D2 of the end surface 10D becomes a ground surface.

[0095] (Characteristics of the end face)

[0096] Next, the characteristics of the end surface 10D of the glass article 10T formed by grinding will be described. Figure 5 is a schematic cross-sectional view of a glass object, Figure 6 is a schematic top view of a glass object.

[0097] The arithmetic mean height Sa of the chamfered portion 10D2 of the glass article 10T is preferably 0.1 μm to 0.8 μm, more preferably 0.1 μm to 0.5 μm. The maximum height Sz of the chamfered portion 10D2 of the glass article 10T is preferably 1.0 μm to 20 μm, more preferably 1.0 μm to 10 μm, and further preferably 1.0 μm to 5 μm. By setting the arithmetic mean height Sa and the maximum height Sz of the chamfered portion 10D2 to this range, the chamfered portion 10D2 can be smoothed and damage starting from the chamfered portion 10D2 can be suppressed. There is no particular limitation on the method for setting the arithmetic mean height Sa to the above range, but as in the present embodiment, in the grinding process for forming the end face 10D, it is preferred that the end face 10D is formed by only performing one-stage grinding using the grinding wheel W instead of performing multi-stage grinding using a plurality of grinding wheels W having different abrasive grain sizes. Here, the one-stage grinding refers to grinding the same area with only one type of grinding wheel W, and the multi-stage grinding refers to grinding the same area sequentially with multiple types of grinding wheels.

[0098] It should be noted that the arithmetic mean height Sa and the maximum height Sz of the chamfered portion 10D2 may be the arithmetic mean height Sa and the maximum height Sz in a region of 90 μm×60 μm in the entire region of the chamfered portion 10D2 .

[0099] The angle θ of the chamfered portion 10D2 of the glass article 10T is preferably 30° to 60°, more preferably 40° to 60°, and further preferably 45° to 60°. Figure 5 As shown in FIG. 1 , the angle θ is the angle between the side surface 10D1 and the chamfered portion 10D2. By making the angle θ within this range, the boundary between the main surface and the chamfered portion 10D2 can be suppressed from being too sharp, and the chips can be appropriately reduced. It should be noted that, in the case where the chamfered portion 10D2 is a curved surface, the angle formed by the tangent line of the most protruding part of the chamfered portion 10D2 and the side surface 10D1 can be taken as the angle θ. It should be noted that, in the case where the side surface 10D1 is a curved surface, the angle formed by the tangent line of the chamfered portion 10D2 and the most protruding part of the side surface 10D1 can be taken as the angle θ.

[0100] Here, if Figure 6 As shown in FIG. 1 , a section (region) having a length of 100 mm in the circumferential direction of the chamfered portion 10D2 of the glass article 10T when viewed from the first main surface 10A side is defined as region AR. Figure 6As shown, the area AR refers to the area from any position AR1 on the chamfered portion 10D2 to a position AR2 on the chamfered portion 10D2 that is 100 mm away in the circumferential direction relative to the position AR1 in the entire area of ​​the chamfered portion 10D2. In this case, the maximum value of the chip size in the area AR is preferably 35 μm or less, and more preferably 30 μm or less. The chip size here refers to the depth of the chip depression when the chip is a depression (concave) from the chamfered portion 10D2, and refers to the protruding length of the chip from the chamfered portion 10D2 when the chip protrudes from the chamfered portion 10D2. The maximum value of the chip size refers to the size of the largest chip among the chips in the area AR. By setting the maximum value of the chip size to this range, the chip can be kept small and cracks starting from the chamfered portion 10D2 can be suppressed.

[0101] The arithmetic mean height Sa of the side surface 10D1 of the glass article 10T is preferably 0.1 μm to 0.8 μm, more preferably 0.1 μm to 0.5 μm, and further preferably 0.1 μm to 0.3 μm. The maximum height Sz of the side surface 10D1 of the glass article 10T is preferably 1.0 μm to 20 μm, more preferably 1.0 μm to 10 μm, and further preferably 1.0 μm to 5 μm. By setting the arithmetic mean height Sa and the maximum height Sz of the side surface 10D1 to be within this range, the end surface 10D can be made smooth and damage starting from the end surface 10D can be suppressed.

[0102] It should be noted that the arithmetic mean height Sa and the maximum height Sz of the side surface portion 10D1 may be the arithmetic mean height Sa and the maximum height Sz in a region of 90 μm×60 μm in the entire region of the side surface portion 10D1 .

[0103] The boundary between the side surface 10D1 and the chamfered portion 10D2 of the glass article 10T is preferably R-shaped (curved). The radius of curvature of the boundary is preferably 0.05 mm or more, more preferably 0.1 mm to 0.5 mm, and further preferably 0.2 mm to 0.3 mm. When the radius of curvature of the boundary is within this range, cracks starting from the chamfered portion 10D2 can be suppressed.

[0104] The chamfered portion 10D2 of the glass article 10T may also be formed with grinding lines extending in the circumferential direction over the entire area. Although the glass article 10T is chamfered by grinding, the chips can be kept small. The grinding lines are grinding marks left by the grinding wheel W. It is preferred that a plurality of grinding lines are formed in the chamfered portion 10D2 in an array along the Z direction.

[0105] In addition, when the side surface portion 10D1 is also formed by grinding, it is preferred that grinding lines extending in the circumferential direction are also formed over the entire area of ​​the side surface portion 10D1. It is preferred that a plurality of grinding lines are formed in the side surface portion 10D1 in an array along the Z direction. That is, in this case, it is preferred that grinding lines extending in the circumferential direction are formed over the entire area of ​​the end surface 10D.

[0106] Grinding lines can be confirmed using a microscope.

[0107] In the present embodiment, the glass article 10T manufactured by grinding using a grinding wheel W, that is, the glass article 10T in a state where the above-mentioned properties are obtained by grinding, is not subjected to further mechanical processing (grinding / grinding) on ​​the end surface 10D. However, for example, the glass article 10T in a state where the above-mentioned properties are obtained by grinding may be subjected to processing other than mechanical processing (e.g., chemical strengthening, bending formation, formation of layers such as an anti-glare layer, an anti-reflection layer, and an anti-fouling layer).

[0108] (Manufacturing Process)

[0109] The process flow of the method for producing the glass article 10T described above will be described. Figure 7 This is a flow chart that explains the manufacturing process of glass products. Figure 7 As shown, in the present manufacturing method, a glass matrix 10 is prepared, and the glass matrix 10 is cut to obtain a glass material 10S (step S10). Then, the end face 10C of the glass material 10S obtained by cutting is ground using a grinding wheel W to obtain a glass article 10T having an end face 10D including a chamfered portion 10D2 (step S12).

[0110] (Effect)

[0111] As described above, the manufacturing method of the first aspect of the present disclosure includes: cutting the glass mother material 10 to obtain a glass material 10S having a first main surface 10A, a second main surface 10B and an end surface 10C, and the arithmetic mean height Sa of the end surface 10C is greater than 0.1 μm and less than 1.0 μm; and using a grinding wheel W with abrasive grains having a median diameter D50 of 8 μm to 24 μm to grind the end surface 10C in a state where the arithmetic mean height Sa is greater than 0.1 μm and less than 1.0 μm to form a chamfered portion 10D2.

[0112] When grinding the end face 10C of a glass material 10S to manufacture a glass article 10T having a chamfered portion, a plurality of grinding wheels with different abrasive grain sizes are generally used to perform multi-stage grinding on the end face 10C. However, after in-depth research, the inventors found that when multi-stage grinding is performed, the chips of the chamfered portion become larger. Then, the inventors found a manufacturing condition that can reduce the chips while forming the chamfered portion to obtain a desired shape. That is, in the present manufacturing method, the glass mother material 10 is cut to manufacture a glass material 10S whose arithmetic mean height Sa of the end face 10C is within the above range, and the end face 10C in a state where the arithmetic mean height Sa is within the above range is ground in one stage using a grinding wheel W with an abrasive grain size within the above range, thereby reducing the chips while obtaining the desired shape.

[0113] The manufacturing method according to the second aspect of the present disclosure is preferably: in the manufacturing method according to the first aspect, the glass article 10T has a side surface 10D1 and a chamfered portion 10D2 connecting the first main surface 10A or the second main surface 10B and the side surface 10D1, and the chamfered portion 10D2 and the side surface 10D1 are formed by grinding the end surface 10C in a state where the arithmetic mean height Sa is 0.1 μm or more and less than 1.0 μm with a grinding wheel W having abrasive grains with a median diameter D50 of 8 μm to 24 μm. According to the present disclosure, by forming the side surface 10D1 by one-stage grinding and forming the chamfered portion 10D2 by one-stage grinding, it is possible to obtain a desired shape while reducing chips.

[0114] The manufacturing method according to the third aspect of the present disclosure is preferably: in the manufacturing method according to the second aspect, the end face 10C is removed by 0.05 mm to 0.3 mm in a direction perpendicular to the end face 10C by grinding with a grinding wheel W to form the side face 10D1. According to the present disclosure, by setting the machining allowance A1 to be within this range, the end face 10C can be appropriately ground while suppressing the grinding time from being prolonged.

[0115] The manufacturing method of the fourth aspect of the present disclosure is preferably: in the manufacturing method of the second aspect or the third aspect, a molded grinding wheel having a grinding surface corresponding to the chamfered portion 10D2 and the side portion 10D1 is used as the grinding wheel W, and the end face 10C is ground, and the chamfered portion 10D2 and the side portion 10D1 are formed at the same time. According to the present disclosure, by using a molded grinding wheel, the end face 10C can be appropriately ground.

[0116] The manufacturing method of the fifth aspect of the present disclosure is preferably that in any one of the manufacturing methods of the first to fourth aspects, the angle θ of the chamfered portion 10D2 is 45° to 60°. By manufacturing the chamfered portion 10D2 so that the angle θ is within this range, cracks starting from the chamfered portion 10D2 can be suppressed.

[0117] The manufacturing method of the sixth aspect of the present disclosure is preferably: in the manufacturing method of any one of the first to fifth aspects, laser light L is irradiated along an imaginary line T set on the main surface (the first main surface 10A or the second main surface 10B) of the glass mother material 10, a modified portion H along the imaginary line T is formed on the glass mother material 10, and the glass mother material 10 is fractured with the modified portion H along the imaginary line T as a starting point to obtain a glass material 10S having an arithmetic mean height Sa of the end surface 10C of 0.1 μm or more and less than 1.0 μm. According to the present disclosure, by cutting the glass mother material 10 using the laser light L, a glass material 10S having an arithmetic mean height Sa of the end surface 10C within the above range can be appropriately manufactured.

[0118] The manufacturing method according to claim 7 of the present disclosure is preferably that in the manufacturing method according to claim 6, the laser light L is a pulsed laser light. According to the present disclosure, the glass material 10S having the arithmetic mean height Sa of the end faces 10C within the above range can be appropriately manufactured by using pulsed laser light.

[0119] The manufacturing method according to the eighth aspect of the present disclosure is preferably that in the manufacturing method according to the sixth or seventh aspect, the wavelength range of the laser light L is 250 nm to 3000 nm. According to the present disclosure, by using infrared laser light in such a wavelength range, the glass material 10S having the arithmetic mean height Sa of the end surface 10C in the above range can be appropriately manufactured.

[0120] The glass article 10T of the ninth aspect of the present disclosure comprises a first main surface 10A, a second main surface 10B and an end surface 10D, the end surface 10D comprises a side surface portion 10D1 and a chamfered portion 10D2 connecting the side surface portion 10D1 and the first main surface 10A, the arithmetic mean height Sa of the chamfered portion 10D2 is 0.1 μm to 0.8 μm, and the maximum value of the size of the chips existing in the interval (area AR) of 100 mm in the circumferential direction of the chamfered portion 10D2 when viewed from the first main surface 10A side is 35 μm or less. According to the present disclosure, a glass article 10T having a desired shape and reduced chips can be obtained.

[0121] The glass article 10T of the tenth aspect of the present disclosure is preferably the glass article of the ninth aspect, wherein the chamfered portion 10D2 has a grinding line extending in the circumferential direction when viewed from the first main surface 10A. According to the present disclosure, a glass article 10T having a desired shape and reduced chips can be obtained.

[0122] The glass article 10T of the 11th aspect of the present disclosure is preferably the glass article of the 9th or 10th aspect, wherein the radius of curvature of the boundary between the chamfered portion 10D2 and the side portion 10D1 is 0.05 mm or more. By setting the radius of curvature of the boundary to be within this range, cracks starting from the chamfered portion 10D2 can be suppressed.

[0123] The glass article 10T of the twelfth aspect of the present disclosure is preferably the glass article of any one of the ninth to eleventh aspects, wherein the arithmetic mean height Sa of the chamfered portion 10D2 is 0.1 μm to 0.5 μm. By setting the arithmetic mean height Sa of the chamfered portion 10D2 within this range, cracks from the chamfered portion 10D2 can be suppressed.

[0124] The glass article 10T of the 13th aspect of the present disclosure is preferably the glass article of any one of the 9th to 12th aspects, wherein the angle θ of the chamfered portion 10D2 is 45° to 60°. By manufacturing the chamfered portion 10D2 so that the angle θ is within this range, the chips can be appropriately reduced.

[0125] (Example)

[0126] Next, examples will be described. Table 1 is a table showing production conditions and evaluation results of each example.

[0127]

[0128] (Example 1)

[0129] In Example 1, a glass matrix having a thickness of 1.3 mm was prepared. As the glass matrix, Dragontrail (registered trademark) manufactured by AGC Corporation was used. For the glass matrix, an imaginary line was set to surround the center of the glass matrix over the entire interval in the circumferential direction, and StarPico3 manufactured by Rofin Corporation was used to irradiate a laser (pulsed laser) along the imaginary line under the following conditions to form a modified portion.

[0130] Wavelength: 1064nm

[0131] Optical system: Coherent Smart Cleave

[0132] Pulse width: 10ps

[0133] Burst pulse number: 4 burst pulses

[0134] Irradiation spacing: 5μm

[0135] Pulse energy: 523μJ

[0136] Feed speed (scanning speed): 11250mm / min

[0137] Output: 39.2W

[0138] In Example 1, the glass mother material having the modified portion formed thereon was cut along the modified portion to obtain a glass material. Then, the arithmetic mean height Sa and the maximum height Sz of the end face (cut face) of the glass material were measured. The arithmetic mean height Sa and the maximum height Sz of the end face 10C are measured values ​​in a 90 μm×60 μm region in contact with the main surface when viewed from a direction perpendicular to the Z direction in the entire region of the end face.

[0139] In Example 1, the glass material obtained by cutting without grinding was treated as a glass article.

[0140] (Example 2)

[0141] In Example 2, a glass material was obtained by the same method as in Example 1. In Example 2, the end surface of the obtained glass material was ground using a molding grinding wheel having abrasive grains of a particle size of #800 and a median diameter D50 of 16.2 μm to obtain a glass article having a chamfered portion with an angle of 45°. The machining allowance during grinding (machining allowance A1 in the above embodiment) was 0.1 mm.

[0142] The arithmetic mean height Sa and the maximum height Sz of the side surface portion (the side surface portion 10D1 in the above-mentioned embodiment) of the glass article obtained by grinding are measured.

[0143] In Table 1, both the example in which "none" was given for the first time and the condition was given for the second time and the example in which "none" was given for the second time and the condition was given for the first time mean that grinding was performed only once.

[0144] (Example 3~Example 4)

[0145] In Examples 3 and 4, except that the grinding conditions of the end surface of the glass material were changed as shown in Table 1, the same method as in Example 2 was used to obtain glass articles.

[0146] (Example 5~Example 6)

[0147] In Examples 5 and 6, the same glass matrix as in Example 1 was cut using a grinding wheel with a grit size of #800 (manufactured by Tokyo Diamond Tool Manufacturing Co., Ltd.) to obtain glass materials. The feed rate during cutting was 100 mm / min to 200 mm / min. The end faces of the obtained glass materials were ground under the grinding conditions shown in Table 1 to obtain glass articles.

[0148] (Example 7)

[0149] In Example 7, a superhard tool (made by Samsung Diamond Industries, Ltd.) was used to cut the glass matrix material identical to Example 1 to obtain a glass material. The feed rate during cutting was 6000 mm / min. After the surface of the obtained glass material was ground in the first stage using a molding grinding wheel (made by Tokyo Diamond Industries, Ltd.) having a particle size of #400, the molding grinding wheel identical to Example 2 was used to grind in the second stage to obtain a glass article.

[0150] (Example 8)

[0151] In Example 8, except that the grinding conditions were as shown in Table 1, a glass article was obtained by the same method as in Example 7.

[0152] (Example 9)

[0153] In Example 9, except that the grinding conditions were as shown in Table 1, a glass article was obtained by the same method as in Example 5.

[0154] (Example 10)

[0155] In Example 10, except that the grinding conditions were as shown in Table 1, a glass article was obtained by the same method as in Example 2.

[0156] (Example 11)

[0157] In Example 11, the same glass base material as in Example 1 was cut using a grinding wheel with a grain size of #200 (manufactured by Noritake Co., Ltd.) to obtain a glass material. The feed rate during cutting was 100 mm / min. The end surface of the obtained glass material was ground under the grinding conditions shown in Table 1 to obtain a glass article.

[0158] (Example 12~Example 13)

[0159] In Examples 12 and 13, CO 2 The same glass base material as in Example 1 was cut by laser to obtain a glass material. 2 The laser irradiation device was SR15i manufactured by Rofin, and the irradiation conditions were as follows.

[0160] Wavelength: 10600nm

[0161] ·Spot diameter: 6.58mm

[0162] Output: 47.3W

[0163] Feed speed (scanning speed): 1800mm / min

[0164] In Examples 12 and 13, the end faces of the obtained glass materials were ground under the grinding conditions shown in Table 1 to obtain glass articles.

[0165] (evaluate)

[0166] In the evaluation, the maximum value of the size of the chips of the glass article of each example was measured. The maximum value of the size of the chips was measured using a microscope. The maximum value of the size of the chips was evaluated as acceptable if it was less than 40 μm, and as unacceptable if it was greater than 40 μm.

[0167] In the evaluation, the chamfered shape was evaluated, and the case where the chamfered shape was obtained was rated as A (acceptable), and the case where the chamfered shape was not obtained was rated as B (unacceptable).

[0168] As shown in Table 1, in Examples 2 to 6 (Examples) in which a glass material having an arithmetic mean height Sa of the end face of 0.1 μm or more and less than 1.0 μm was ground in one stage using a grinding wheel having a median diameter D50 of 8 μm to 24 μm, both the chip size and chamfer shape were qualified, and it can be seen that the desired shape can be obtained by chamfering while reducing the chips.

[0169] On the other hand, in Example 1 and Examples 7 to 13 (Comparative Examples), at least one of the chip size and the chamfer shape was unacceptable, and it was found that both obtaining a desired shape by chamfering and reducing the size of the chips could not be achieved.

[0170] For example, in Example 1, grinding was not performed, so the chamfer shape and the size of the chips were unqualified. In Example 7, the end face of the glass material was rough, and two-stage grinding was performed, so the chips became larger. In Example 8, although it was one-stage grinding, the end face of the glass material was rough, so the chips became larger. In Example 9, although it was one-stage grinding, the particle size of the grinding wheel used for grinding was large, so the chips became larger. In Example 10, the particle size of the grinding wheel used for grinding (here is the first grinding) was too large relative to the end face in a state of being greater than 0.1μm and less than 1.0μm, so the chips became larger. In Example 11, although it was one-stage grinding, the end face of the glass material was rough, so the chips became larger. In Example 12, the end face of the glass material was too smooth, and two-stage grinding was performed, so the chips became larger. In Example 13, although it was one-stage grinding, the end face of the glass material was too smooth, so it could not be ground, and the desired chamfer shape could not be obtained.

[0171] Alternatively, a process evaluation was performed. In the process evaluation, when the process time required for cutting the glass matrix to obtain the glass material and grinding the glass material to obtain the glass article in Examples 5 and 6 (grinding wheel cutting) was set to 100%, it was evaluated whether the process time could be reduced to less than 20%. In this evaluation, in Examples 2 to 4, the process time could be reduced to less than 20%. That is, as shown in Examples 2 to 4, it can be seen that the process time is shortened by using a pulsed laser, which is more preferable.

[0172] Above, the embodiments of the present invention have been described, but the embodiments are not limited by the contents of the embodiments. In addition, the above-mentioned constituent elements include elements that can be easily thought of by those skilled in the art, substantially the same elements, and elements of so-called equivalent scopes. Moreover, the above-mentioned constituent elements can be appropriately combined. Moreover, various omissions, substitutions or changes of constituent elements can be performed without departing from the scope of the gist of the above-mentioned embodiments.

[0173] This application is based on Japanese patent application No. 2023-093319 filed on June 6, 2023, the contents of which are incorporated herein by reference.

Claims

1. A method for manufacturing a glass article, comprising the following steps: Cutting the glass base material to obtain a glass material having a first main surface, a second main surface, and an end surface connecting the first main surface and the second main surface, wherein the arithmetic mean height Sa of the end surface is greater than or equal to 0.1 μm and less than 1.0 μm; and The end surface in a state where the arithmetic mean height Sa is 0.1 μm or more and less than 1.0 μm is ground using a grinding wheel having abrasive grains having a median diameter D50 of 8 μm to 24 μm to form a chamfered portion.

2. The method for manufacturing a glass article according to claim 1, wherein: The glass article has a side surface portion, and the chamfered portion connecting the first main surface or the second main surface and the side surface portion. The chamfered portion and the side surface portion are formed by grinding the end surface having an arithmetic mean height Sa of 0.1 μm or more and less than 1.0 μm using a grinding wheel having abrasive grains having a median diameter D50 of 8 μm to 24 μm.

3. The method for manufacturing a glass article according to claim 2, wherein: The side surface portion is formed by grinding with the grinding wheel to remove 0.05 mm to 0.3 mm of the end surface in a direction perpendicular to the end surface.

4. The method for manufacturing a glass article according to claim 2 or 3, wherein: The chamfered portion and the side surface are formed while grinding the end surface using a molded grinding wheel having grinding surfaces corresponding to the chamfered portion and the side surface as the grinding wheel.

5. The method for producing a glass article according to any one of claims 1 to 3, wherein: The angle of the chamfered portion is 45° to 60°.

6. The method for producing a glass article according to any one of claims 1 to 3, wherein: Laser is irradiated along an imaginary line set on the main surface of the glass mother material to form a modified portion along the imaginary line on the glass mother material, and the glass mother material is fractured with the modified portion along the imaginary line as a starting point to obtain the glass material having an arithmetic mean height Sa of the end face greater than 0.1 μm and less than 1.0 μm.

7. The method for manufacturing a glass article according to claim 6, wherein: The laser light is a pulsed laser light.

8. The method for manufacturing a glass article according to claim 6, wherein: The wavelength range of the laser is 250nm to 3000nm.

9. A glass article comprising a first main surface, a second main surface, and an end surface connecting the first main surface and the second main surface, The end surface has a side surface portion and a chamfered portion connecting the side surface portion and the first main surface, The arithmetic mean height Sa of the chamfered portion is 0.1 μm to 0.8 μm, The maximum value of the size of the chips existing in a section having a length of 100 mm in the circumferential direction of the chamfered portion when viewed from the first main surface side is 35 μm or less.

10. The glass article according to claim 9, wherein: The chamfered portion has a grinding line extending in the circumferential direction when viewed from the first main surface side.

11. The glass article according to claim 9 or 10, wherein: The radius of curvature of the boundary portion between the chamfered portion and the side surface portion is greater than or equal to 0.05 mm.

12. The glass article according to claim 9 or 10, wherein: The arithmetic mean height Sa of the chamfered portion is 0.1 μm to 0.5 μm.

13. The glass article according to claim 9 or 10, wherein: The angle of the chamfered portion is 45° to 60°.