Method for co-producing iron phosphate, sulfuric acid, hydrogen and carbon dioxide by utilizing industrial solid waste
Through iodine circulation coupling technology, industrial solid waste is used to prepare chemical products such as iron phosphate and sulfuric acid, which solves the problems of industrial solid waste resource utilization and carbon emission reduction, and achieves efficient energy utilization and environmental protection.
Patent Information
- Application Number
- CN202310657251.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-05
AI Technical Summary
The existing technology is difficult to effectively utilize industrial solid waste, resulting in environmental pollution and waste of resources, and the carbon emission problem of fossil energy has not been effectively solved.
Through iodine circulation coupling of iron cycles mainly composed of iron-containing solid waste and sulfur cycles mainly composed of sulfur-containing solid waste, carbon energy is used to prepare iron phosphate, sulfuric acid, hydrogen and carbon dioxide, so as to achieve coordinated coupling of substances and energy cascade utilization, solving the problem of Pollution and solid waste resource utilization problems in the production process of fossil energy hydrogen production and various high-value chemical products.
It has achieved low energy consumption, high concentration capture and acquisition of carbon dioxide, promoted carbon emission reduction, improved energy utilization efficiency, and achieved high-value utilization of solid waste resources and protection of the ecological environment.
Abstract
Description
Technical Field
[0001] The invention relates to the fields of new energy, solid waste environmental protection and chemical technology, and in particular to a method for co-producing ferric phosphate, sulfuric acid, hydrogen and carbon dioxide by utilizing industrial solid waste. Background Art
[0002] Carbon emissions from the use of fossil energy have caused global climate change. The development of renewable energy with the purpose of carbon emission reduction will reshape the new pattern of world energy production and supply. As important components of renewable energy, wind energy, solar energy, ocean energy, etc. are volatile, intermittent and unstable, forming an urgent need for energy storage technology. Among them, energy storage includes advanced battery technology based on the utilization of lithium elements, and radiates downward to involve key technical elements such as phosphorus, manganese, iron, and cobalt, which has reshaped the new pattern of world mineral resource demand. Taking the development of lithium batteries in my country as an example, the shipment volume in 2022 increased rapidly by 100% compared with 2021, which involved lithium-ion lithium iron phosphate positive electrode materials, and its shipment volume increased by 151% year-on-year. The upstream raw material of lithium iron phosphate is iron phosphate. Iron phosphate will form a huge demand situation due to the development of lithium batteries, involving issues such as phosphoric acid production and iron sources, and also involving a large amount of industrial solid waste phosphogypsum produced by the phosphorus industry. Its consumption has seriously affected the efficient development of phosphoric acid and its downstream lithium battery industry. Similar changes in demand also involve light metals such as aluminum, magnesium and their alloys, which are mainly used in important components of today's carbon emissions, such as transportation. The lightweight and high-strength requirements of various transportation vehicles are imperative. Therefore, global carbon emission reduction has spawned the rapid growth of lightweight new energy transportation vehicles, which has brought new attention to the mineral resources of light metals such as aluminum, magnesium and their alloys. The development of the aluminum-magnesium light metal industry will inevitably involve the output of related mineral solid wastes, such as the huge amount of red mud solid waste output from the aluminum industry. It is noted that there is a high proportion of non-mineral iron sources in the red mud.
[0003] Changes in the utilization of mineral resources and their production capacity will inevitably involve an increase in mineral solid waste. The long-term accumulation of mineral solid waste has made it unbearable to dispose of it, which has a huge impact on the environment and poses a challenge to further improving mineral production capacity and the coordinated development of the ecological environment. Considering the energy storage and lightweight metal mineral industries at a macro level can find a new way to utilize solid waste, and it can also profoundly affect the upstream production process, and have the opportunity to change the existing industrial structure, solve key core technical problems such as the singleness of the industrial chain, energy utilization, and energy consumption rate, thereby actively contributing to the cause of carbon emission reduction as a whole. Summary of the invention
[0004] The purpose of the present invention is to provide a method for co-producing ferric phosphate, sulfuric acid, hydrogen and carbon dioxide using industrial solid waste. The present invention uses an iodine cycle to couple an iron cycle mainly based on iron-containing solid waste and a sulfur cycle mainly based on sulfur-containing solid waste, and simultaneously obtains ferric phosphate, sulfuric acid, ferrous sulfate, or further involves a variety of chemical and resource products such as ammonium sulfate and rare metals, and solves many problems such as hydrogen production and carbon concentration from fossil energy, pollution in the production process of various high-value chemical products, resource utilization of solid waste, ecological environmental protection, and process economy through material synergistic coupling and energy cascade utilization.
[0005] The present invention is achieved through the following technical solutions:
[0006] The method of utilizing industrial solid waste to co-produce ferric phosphate, sulfuric acid, hydrogen and carbon dioxide comprises the following steps: using sulfur-containing solid waste containing calcium as a sulfur source, using iron-containing solid waste as an iron source, using iodine as a reaction circulation medium, and using carbon-containing energy as energy input; firstly converting sulfur oxides generated in the thermal reduction cycle of the sulfur-containing solid waste into sulfuric acid through iodine, and then reacting with low-valent iron generated in the thermal reduction cycle of the iron-containing solid waste to prepare ferrous sulfate, further reacting with concentrated sulfuric acid to prepare ferric sulfate, and finally reacting with phosphoric acid or monoammonium phosphate to obtain ferric phosphate; and the carbon-containing energy produces hydrogen and carbon dioxide in addition to the energy supply.
[0007] The present invention solves the key core technical problems such as the singleness of the industrial chain, energy utilization, and energy consumption rate through material synergistic coupling and energy cascade utilization, thereby actively contributing to the cause of carbon emission reduction as a whole. Coupling the utilization of carbon-containing energy with the disposal of mining and metallurgical solid waste is an effective way to actively realize material synergistic coupling and energy cascade utilization, and can also capture and obtain carbon dioxide with low energy consumption and high concentration. Therefore, it is an important measure for the clean and efficient use of carbon-containing energy, the high value of solid waste resource recycling, and the rationalization of ecological environmental protection.
[0008] Preferably, the method comprises the following steps:
[0009] (1) Thermal reduction conversion of sulfur-containing solid waste: The sulfur-containing solid waste containing calcium elements is thermally reduced with the first carbon-containing energy source to obtain a solid phase product containing CaO and a solid phase product containing CO. 2 、SO 2 and H 2 The gas phase product of O is separated from the gas and condensed, and the solid phase product CaO is used for building materials or harmless treatment of phosphogypsum;
[0010] (2) Preparation of sulfuric acid with iodine circulation: The gaseous product obtained in step (1) is combined with elemental iodine and water and introduced into a sulfuric acid preparation reactor. The temperature and reaction atmosphere are adjusted to generate a mixture of sulfuric acid and hydroiodic acid. The mixture is further separated by density difference to obtain sulfuric acid and hydroiodic acid. Pure carbon dioxide is also generated. The hydroiodic acid is concentrated by distillation and then decomposed by heating to obtain pure hydrogen and recyclable elemental iodine.
[0011] (3) Thermal reduction conversion of iron-containing solid waste: Through the thermal reduction reaction of iron-containing solid waste and the second carbon-containing energy source, a solid phase product containing FeO and Fe and a solid phase product containing CO are obtained. 2 and H 2 O gas phase product, after gas-solid separation and condensation, obtain pure carbon dioxide and solid phase product, the solid phase product can be used for step (4) or water decomposition to produce hydrogen and extract rare precious metals, the water vapor condensed in the thermal reduction conversion process of iron-containing solid waste is used as the raw material of iodine circulation reaction in step (2);
[0012] (4) Preparation of ferric phosphate: The solid phase product obtained in step (3) is mixed with sulfuric acid obtained in step (2) through iodine recycling, and ferrous sulfate is obtained after filtration. The ferrous sulfate is reacted with concentrated sulfuric acid (further sulfated) to obtain ferric sulfate. The ferric sulfate is then reacted with phosphoric acid. After precipitation and filtration, the excess acid is neutralized with ammonia water to obtain ferric phosphate. The by-product ammonium sulfate solution produced in the above process can be dehydrated by utilizing the waste heat of step (1) or step (3) to obtain ammonium sulfate.
[0013] The present invention uses thermal reduction to convert sulfur-containing solid waste to obtain sulfur dioxide, iodine is circulated to convert sulfur dioxide to prepare sulfuric acid, and iron-containing solid waste is thermally reduced to obtain solid phase products FeO and Fe. The solid phase products FeO and Fe are combined with sulfuric acid to produce ferrous sulfate. The ferrous sulfate is further sulfated to obtain ferric sulfate. The ferric sulfate is combined with phosphoric acid to prepare ferric phosphate, and hydrogen and carbon dioxide are co-produced at the same time.
[0014] In the present invention, for the component differences of different industrial solid wastes, a strategy of material energy coupling utilization guided by carbon-containing energy thermal reduction conversion and product demand is adopted, with carbon-containing fuel as energy input source, iodine as circulating medium, and iodine is used to convert sulfur oxides produced in the sulfur-containing solid waste thermal reduction cycle into sulfuric acid, react with iron to obtain ferrous sulfate, and then react with phosphoric acid, etc., to finally obtain ferric phosphate. This process can achieve effective emission reduction of carbon dioxide, and the iodine and phosphoric acid used are products of phosphorus chemical enterprises, that is, the solid waste treatment of phosphorus chemical enterprises can be achieved through resource self-sufficiency. At the same time, the quicklime (CaO) produced in the process can also be used for the harmless treatment of phosphogypsum, achieving the effect of "treating waste with waste".
[0015] The present invention couples the utilization of carbon-containing energy with the disposal of mining and metallurgical solid waste, which is an effective way to actively realize the synergistic coupling of materials and the cascade utilization of energy. It can also capture and obtain carbon dioxide with low energy consumption and high concentration. Therefore, it is an important measure for the cleanliness and efficiency of carbon-containing energy, the high value of the recycling of solid waste resources, and the rationalization of ecological environmental protection.
[0016] Preferably, the sulfur-containing solid waste containing calcium elements includes phosphogypsum and desulfurized gypsum, and the iron-containing solid waste includes aluminum solid waste red mud, steel solid waste slag, blast furnace slag, iron-containing dust mud and low-grade iron ore. The sulfur-containing solid waste raw materials need to contain sulfur and calcium elements, and the iron-containing solid waste raw materials need to contain iron elements.
[0017] Preferably, the first carbon-containing energy source described in step (1) is selected from carbon-containing primary fossil energy, carbon-containing renewable biomass, carbon-containing solid waste and the post-processed products of the foregoing three, and the second carbon-containing energy source described in step (3) is selected from carbon-containing primary fossil energy, carbon-containing renewable biomass, carbon-containing solid waste and the post-processed products of the foregoing three.
[0018] Preferably, the temperature of the thermal reduction reaction of the sulfur-containing solid waste containing calcium elements and the first carbon-containing energy source in step (1) is 600°C-1300°C, the atmosphere of the thermal reduction reaction is water vapor or a mixture of carbon dioxide and water vapor, the molar ratio of carbon dioxide and water vapor in the mixture of carbon dioxide and water vapor is 1:0.25-1:5, and the molar ratio of the sulfur-containing solid waste containing calcium elements to the first carbon-containing energy source is 1:1.25-1:1.75. More preferably, the molar ratio of carbon dioxide and water vapor in the mixture of carbon dioxide and water vapor is 1:0.5-1:1.
[0019] In the thermal reduction reaction, carbon-containing energy uses carbon dioxide or water as an auxiliary to accelerate the reaction, but is not actually consumed, i.e., C+H 2 O=CO+H 2 , C+CO 2 =2CO, CO and H 2 Finally, it is oxidized to CO 2 and H 2 O, using CaSO 4 And subsequent Fe 2 O 3 The oxygen in the oxygen-containing compound provides the oxygen element.
[0020] Preferably, in the iodine cycle described in step (2), relative to SO 2 The excess coefficient of elemental iodine is 1-10, the excess coefficient of water is 1-8, the temperature for preparing sulfuric acid is 20°C-200°C, and the heat required for the iodine cycle in step (2) comes from the waste heat of step (1) or step (3).
[0021] More preferably, the heating decomposition temperature of the hydroiodic acid in step (2) is 300°C-600°C.
[0022] Preferably, the temperature of the thermal reduction reaction of the iron-containing solid waste and the second carbon-containing energy in step (3) is 600°C-1300°C, the atmosphere of the thermal reduction reaction is water vapor or a mixture of carbon dioxide and water vapor, the molar ratio of carbon dioxide and water vapor in the mixture of carbon dioxide and water vapor is 1:0.25-1:2.5, and the mass ratio of the iron-containing solid waste to the second carbon-containing energy is 1:0.1-1:0.75. More preferably, the molar ratio of carbon dioxide and water vapor in the mixture of carbon dioxide and water vapor is 1:1-1:2.
[0023] Preferably, the water vapor obtained after condensing the gaseous product in step (1) is used as the raw material for the iodine circulation reaction in step (2).
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention couples an iodine cycle with an iron cycle mainly composed of iron-containing solid waste and a sulfur cycle mainly composed of sulfur-containing solid waste, thereby obtaining ferric phosphate, sulfuric acid, ferrous sulfate, or further a variety of chemical and resource products such as ammonium sulfate and rare metals. Through material synergistic coupling and energy cascade utilization, the present invention solves many problems such as hydrogen production and carbon concentration from fossil energy, pollution in the production process of various high-value chemical products, resource utilization of solid waste, ecological environmental protection, and process economy.
[0026] (2) The present invention solves key core technical problems such as the singleness of the industrial chain, energy utilization, and energy consumption rate through material synergistic coupling and energy cascade utilization, thereby actively contributing to the cause of carbon emission reduction as a whole. Coupling the utilization of carbon-containing energy with the disposal of mining and metallurgical solid waste is an effective way to actively achieve material synergistic coupling and energy cascade utilization, and can also capture and obtain carbon dioxide with low energy consumption and high concentration. Therefore, it is an important measure to clean and efficiently carbon-containing energy, recycle solid waste resources and rationalize ecological environmental protection. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below with reference to the examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples where specific conditions are not specified are generally based on conventional conditions in the art or conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are considered to be raw materials and reagents that can be obtained through commercial channels such as conventional markets.
[0028] A method for co-producing iron phosphate, sulfuric acid, hydrogen and carbon dioxide using industrial solid waste, specifically comprising the following steps:
[0029] (1) Thermal reduction conversion of sulfur-containing solid waste: The calcium-containing sulfur-containing solid waste is reacted with the first carbon-containing energy source, and the CaSO in the sulfur-containing solid waste is reduced by adjusting the temperature and reaction atmosphere. 4 Convert to SO 2 The solid phase products (CaO) and gas phase products (CO 2 、SO 2 , H 2 After gas-solid separation and condensation, the chemical product quicklime (CaO) can be used for building materials or harmless treatment of phosphogypsum. 2 and SO 2 The tail gas will be used in step (2), and the water vapor condensed during the thermal reduction conversion process of the sulfur-containing solid waste can be used as a recycled reaction raw material.
[0030] (2) Preparation of sulfuric acid by iodine cycle: The CO-containing 2 and SO 2 tail gas, combined with elemental iodine (I 2 ) and water are introduced into a sulfuric acid preparation reactor. By adjusting the temperature and reaction atmosphere, a gas-liquid-solid three-phase combined reaction is performed at a relatively low temperature to generate mixed sulfuric acid (H 2 SO 4 ) and hydroiodic acid (HI). The upper layer of sulfuric acid (H 2 SO 4 ) products, while producing pure carbon dioxide; the hydroiodic acid (HI) in the lower layer is concentrated by distillation and decomposed by heating to obtain pure hydrogen (H 2 ) and recyclable elemental iodine (I 2 ) is returned to the raw material side. The reaction energy supply of this step can come from the waste heat of step (1) and step (3).
[0031] (3) Thermal reduction conversion of iron-containing solid waste: The iron-containing solid waste is reacted with the second carbon-containing energy source to reduce the Fe 2 O 3 Converted into FeO and Fe, and then reacted with the gaseous products (CO 2 , H 2 O) After gas-solid separation and condensation, a pure carbon dioxide product is obtained. The solid phase products (FeO, Fe) can be used in step (4) or water decomposition to produce hydrogen and extract rare and precious metals. The water vapor condensed during the thermal reduction conversion of the iron-containing solid waste can be used as a recycled reaction raw material.
[0032] (4) Sulfation to ferrous sulfate and phosphoric acid to prepare ferric phosphate: FeO and Fe obtained in the thermal reduction conversion process of iron-containing solid waste in step (3) are mixed with sulfuric acid obtained in the iodine cycle in step (2), and filtered to obtain a ferrous sulfate product; the ferrous sulfate solution is then reacted with phosphoric acid, and after precipitation and filtration, the excess acid is neutralized with ammonia water to obtain an ferric phosphate product. The ammonium sulfate solution produced as a byproduct in the process can be dehydrated using the waste heat of step (1) or step (3) to obtain an ammonium sulfate product.
[0033] In the following embodiments, the preferred sulfur-containing solid waste includes industrial solid waste gypsum such as phosphogypsum and desulfurized gypsum, and the iron-containing solid waste includes one of aluminum solid waste red mud, steel solid waste steel slag, blast furnace slag, iron-containing dust mud, low-grade iron ore or a mixture thereof. The sulfur-containing solid waste raw material needs to contain sulfur and calcium elements, and the iron-containing solid waste raw material needs to contain iron elements.
[0034] The first carbon-containing energy in step (1) and the second carbon-containing energy in step (3) are carbon-containing primary fossil energy, renewable biomass, carbon-containing solid waste, and all possible post-processing products of the foregoing three.
[0035] The solid phase products (CaO) and gas phase products (CO 2 、SO 2 , H 2 O) After gas-solid separation and condensation, the obtained chemical product quicklime (CaO) can be used for building materials or harmless treatment of phosphogypsum. The solid phase products (FeO, Fe) and gas phase products (CO 2 , H 2 O) After gas-solid separation and condensation, a pure carbon dioxide product is obtained.
[0036] In the following embodiments, preferably, the temperature for thermal reduction conversion of the sulfur-containing solid waste containing calcium elements with the first carbon-containing energy source in step (1) is 600°C-1300°C, the atmosphere for thermal reduction reaction of the sulfur-containing solid waste with the first carbon-containing energy source is water vapor or a mixture of carbon dioxide and water vapor, the molar ratio of carbon dioxide and water vapor in the mixture of carbon dioxide and water vapor is 1:0.25-1:5, and the molar ratio of the sulfur-containing solid waste to the first carbon-containing energy source is 1:1.25-1:1.75. Further preferably, the molar ratio of carbon dioxide and water vapor is 1:0.5-1:1, and the temperature for thermal reduction conversion of the sulfur-containing solid waste with the first carbon-containing energy source is 1100°C-1250°C.
[0037] In the following embodiments, preferably, the temperature of the thermal reduction conversion of the iron-containing solid waste and the second carbon-containing energy in step (3) is 600°C-1100°C, the molar ratio of carbon dioxide to water vapor is 1:0.25-1:2.5, the atmosphere of the thermal reduction reaction of the iron-containing solid waste and the second carbon-containing energy is water vapor or a mixed gas of carbon dioxide and water vapor, the molar ratio of carbon dioxide and water vapor in the mixed gas of carbon dioxide and water vapor is 1:0.25-1:2.5, and the molar ratio of the iron-containing solid waste to the second carbon-containing energy is 1:0.1-1:0.75. Further preferably, the molar ratio of carbon dioxide and water vapor in the mixed gas of carbon dioxide and water vapor is 1:1-1:2, and the temperature of the thermal reduction conversion of the iron-containing solid waste and the second carbon-containing energy is 950°C-1000°C.
[0038] The following preferred embodiment is that in step (2) of the iodine cycle, relative to SO 2 , the excess coefficient of elemental iodine is 1-10, the excess coefficient of water is 1-8, the temperature for preparing sulfuric acid in gas-liquid-solid three-phase is 20℃-180℃, the heating decomposition temperature of hydroiodic acid (HI) is 200℃-1000℃, and the process heat of step (2) can be derived from the waste heat of step (1). Further preferably, in the iodine cycle, relative to SO 2 , the excess coefficient of elemental iodine is 2-5, and the temperature for preparing sulfuric acid by gas-liquid-solid three-phase method is 60℃-90℃.
[0039] Example 1
[0040] A technical approach for co-producing iron phosphate, sulfuric acid, hydrogen and carbon dioxide using industrial solid waste comprises the following steps:
[0041] (1) Thermal reduction conversion of sulfur-containing solid waste and iron-containing solid waste: Using phosphogypsum as the sulfur-containing solid waste and coal as the fuel, the reaction product was separated and condensed to obtain CO 2 and SO 2 The mixed tail gas and the chemical product quicklime (CaO) are produced. Red mud is used as the iron-containing solid waste and coal is used as the fuel. At 1000°C, the molar ratio of carbon dioxide and water vapor is 1:2. After separation and condensation of the reaction products, pure carbon dioxide and solid products (FeO and Fe mixture) are obtained.
[0042] (2) Preparation of sulfuric acid by iodine cycle: CO obtained in step (1) 2 and SO 2 The mixed tail gas is introduced into a multi-stage sulfuric acid reactor, the excess coefficient of elemental iodine is 4, the excess coefficient of water is 8, and the temperature is 70°C to generate mixed sulfuric acid (H 2 SO 4 ) and hydroiodic acid (HI), and the upper layer of sulfuric acid (H 2 SO4 ) products and pure carbon dioxide products, the lower layer of hydroiodic acid (HI) is heated and decomposed at 500 ° C to obtain pure hydrogen (H 2 ) and recyclable elemental iodine (I 2 ).
[0043] (3) Preparation of ferric phosphate by sulfuric acid-ferrous iron-phosphoric acid: The solid phase product (FeO and Fe mixture) obtained from the thermal reduction conversion process of iron-containing solid waste is mixed with sulfuric acid obtained from iodine circulation, filtered to obtain ferrous sulfate product, and the ferrous sulfate solution is then reacted with phosphoric acid, filtered and precipitated, and then the excess acid is neutralized with ammonia water to obtain ferric phosphate product. The ammonium sulfate solution produced as a byproduct in the process is dehydrated to obtain the ammonium sulfate product.
[0044] (4) The chemical product quicklime (CaO) obtained in step (1) can be used for harmless treatment of building materials or phosphogypsum, and the water vapor condensed during the thermal reduction conversion process of sulfur-containing solid waste and iron-containing solid waste can be recycled to participate in the reaction of step (1). The elemental iodine (I 2 ) can be recycled and the above steps (1)-(3) are repeated to obtain the same product as above.
[0045] In this embodiment, the carbon capture rate of thermal reduction conversion of phosphogypsum was measured to be 97%, SO 2 The release rate is 99%, the carbon capture rate of red mud thermal reduction conversion is 99%, and the CO 2 95% pure, single pass SO2 with iodine cycle 2 The conversion rate was 45%.
[0046] Example 2
[0047] Same as Example 1, except that:
[0048] In step (1), the thermal reduction conversion temperature of sulfur-containing solid waste phosphogypsum and coal is 1250°C, the molar ratio of carbon dioxide and water vapor in the thermal reduction reaction atmosphere of sulfur-containing solid waste phosphogypsum and coal is 1:1, the thermal reduction conversion temperature of iron-containing solid waste red mud and coal is 950°C, and the excess coefficient of elemental iodine in step (2) is 2, and the temperature is 90°C.
[0049] In this embodiment, the carbon capture rate of thermal reduction conversion of phosphogypsum was measured to be 99%, SO 2 The release rate is 99%, and the single-pass SO 2 The conversion rate was 33%.
[0050] Example 3
[0051] Same as Example 1, except that:
[0052] The carbon-containing fuel is biomass, and the biomass is sawdust. The thermal reduction conversion temperature of the sulfur-containing solid waste phosphogypsum and the sawdust in step (1) is 1200° C., and the molar ratio of carbon dioxide to water vapor in the thermal reduction reaction atmosphere of the sulfur-containing solid waste phosphogypsum and coal is 1:1. The thermal reduction conversion temperature of the iron-containing solid waste red mud and the sawdust is 950° C., and the molar ratio of carbon dioxide to water vapor in the thermal reduction reaction atmosphere of the iron-containing solid waste red mud and the sawdust is 1:1. In step (2), the excess coefficient of elemental iodine is 5, the excess coefficient of water is 8, and the temperature is 60° C.
[0053] In this embodiment, the carbon capture rate of thermal reduction conversion of phosphogypsum was measured to be 98%, SO 2 The release rate is 98%, the carbon capture rate of red mud thermal reduction conversion is 98%, and the CO 2 99% purity, 99% purity hydrogen, single pass SO for iodine cycle 2 The conversion rate was 42%.
[0054] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for co-producing iron phosphate, sulfuric acid, hydrogen and carbon dioxide using industrial solid waste, characterized in that: The method comprises the following steps: using sulfur-containing solid waste containing calcium as a sulfur source, using iron-containing solid waste as an iron source, using iodine as a reaction circulation medium, and using carbon-containing energy as an energy input; firstly converting sulfur oxides produced in the thermal reduction cycle of the sulfur-containing solid waste into sulfuric acid through iodine, and then reacting with low-valent iron produced in the thermal reduction cycle of the iron-containing solid waste to prepare ferrous sulfate, further reacting with concentrated sulfuric acid to prepare ferric sulfate, and finally reacting with phosphoric acid or monoammonium phosphate to prepare ferric phosphate; and the carbon-containing energy produces hydrogen and carbon dioxide in addition to the energy supply.
2. The method according to claim 1, characterized in that The specific steps include: (1) Thermal reduction conversion of sulfur-containing solid waste: The sulfur-containing solid waste containing calcium elements is thermally reduced with the first carbon-containing energy source to obtain a solid phase product containing CaO and a gas phase product containing CO2, SO2 and H2O. After gas-solid separation and condensation, the solid phase product CaO is used for building materials or harmless treatment of phosphogypsum; (2) Preparation of sulfuric acid with iodine circulation: The gaseous product obtained in step (1) is combined with elemental iodine and water and introduced into a sulfuric acid preparation reactor. The temperature and reaction atmosphere are adjusted to generate a mixture of sulfuric acid and hydroiodic acid. The mixture is further separated by density difference to obtain sulfuric acid and hydroiodic acid. Pure carbon dioxide is also generated. The hydroiodic acid is concentrated by distillation and then decomposed by heating to obtain pure hydrogen and recyclable elemental iodine. (3) Thermal reduction conversion of iron-containing solid waste: A solid phase product containing FeO and Fe and a gas phase product containing CO2 and H2O are obtained by thermal reduction reaction of the iron-containing solid waste with a second carbon-containing energy source. After gas-solid separation and condensation, pure carbon dioxide and solid phase products are obtained. The solid phase product is used in step (4) or water decomposition to produce hydrogen and extract rare and precious metals. The water vapor condensed in the thermal reduction conversion process of the iron-containing solid waste is used as the raw material for the iodine circulation reaction in step (2); (4) preparing ferric phosphate: the solid phase product obtained in step (3) is mixed with the sulfuric acid obtained in step (2) through iodine recycling, and ferrous sulfate is obtained after filtering. The ferrous sulfate reacts with concentrated sulfuric acid to obtain ferric sulfate. The ferric sulfate reacts with phosphoric acid, and after precipitation and filtration, the excess acid is neutralized with ammonia water to obtain ferric phosphate. The by-product ammonium sulfate solution produced in the above process is dehydrated using the waste heat of step (1) or step (3) to obtain ammonium sulfate.
3. The method according to claim 1 or 2, characterized in that: The sulfur-containing solid waste containing calcium elements includes phosphogypsum and desulfurized gypsum, and the iron-containing solid waste includes aluminum solid waste red mud, steel solid waste slag, blast furnace slag, iron-containing dust mud and low-grade iron ore.
4. The method according to claim 2, characterized in that: The first carbon-containing energy source described in step (1) is selected from carbon-containing primary fossil energy, carbon-containing renewable biomass, carbon-containing solid waste and the post-processed products of the foregoing three. The second carbon-containing energy source described in step (3) is selected from carbon-containing primary fossil energy, carbon-containing renewable biomass, carbon-containing solid waste and the post-processed products of the foregoing three.
5. The method according to claim 2, characterized in that: The temperature of the thermal reduction reaction of the sulfur-containing solid waste containing calcium elements and the first carbon-containing energy source in step (1) is 600°C-1300°C, the atmosphere of the thermal reduction reaction is water vapor or a mixed gas of carbon dioxide and water vapor, the molar ratio of carbon dioxide to water vapor in the mixed gas of carbon dioxide and water vapor is 1:0.25-1:5, and the molar ratio of the sulfur-containing solid waste containing calcium elements to the first carbon-containing energy source is 1:1.25-1:1.
75.
6. The method according to claim 2, characterized in that In the iodine cycle described in step (2), the excess coefficient of elemental iodine relative to SO2 is 1-10, the excess coefficient of water is 1-8, the temperature for preparing sulfuric acid is 20°C-200°C, and the heat required for the iodine cycle in step (2) comes from the waste heat of step (1) or step (3).
7. The method according to claim 2 or 6, characterized in that: The heating decomposition temperature of the hydroiodic acid described in step (2) is 300°C-600°C.
8. The method according to claim 2, characterized in that: The temperature of the thermal reduction reaction of the iron-containing solid waste and the second carbon-containing energy in step (3) is 600°C-1300°C, the atmosphere of the thermal reduction reaction is water vapor or a mixed gas of carbon dioxide and water vapor, the molar ratio of carbon dioxide to water vapor in the mixed gas of carbon dioxide and water vapor is 1:0.25-1:2.5, and the molar ratio of the iron-containing solid waste to the second carbon-containing energy is 1:0.1-1:0.
75.
9. The method according to claim 2, characterized in that: The water vapor obtained after condensing the gaseous product in step (1) is used as the raw material for the iodine circulation reaction in step (2).
Citation Information
Patent Citations
Graphene / phosphoric acid iron-lithium composite material with sandwich structure and preparation method thereof
CN102148371A
Method for synthesizing metal compound by using carbon thermal reduction method
CN102376951A