Preparation method of anion-doped high-performance sodium battery positive electrode material
Through the preparation of anion-doped high-entropy layered oxide materials, the problem of insufficient energy density of the positive electrode material of sodium ion battery is solved, high specific capacity and long cycle stability are achieved, and the industrial application of sodium ion batteries is promoted.
Patent Information
- Application Number
- CN202410961038.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-12-06
AI Technical Summary
The energy density of existing sodium ion battery cathode materials is low, limiting their large-scale production and application.
The preparation method of anion-doped high-entropy layered oxide sodium electropositive electrode material is adopted. By mixing elements such as sodium, lithium, manganese, copper, zinc, nickel in a specific proportion, adding citric acid, titanium dioxide, sodium fluoride to high temperatures Sintering, combining conductive additives and polyvinylidene fluoride to prepare a sodium-electrode material with high specific capacity.
It significantly improves the specific capacity of sodium ion batteries and the performance of the battery under large currents, achieves high energy density, and promotes the industrial development of sodium ion batteries.
Smart Images

Figure CN119080077A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a sodium ion battery, and in particular to a method for preparing an anion-doped high-performance sodium battery positive electrode material, belonging to the field of battery preparation. Background Art
[0002] In recent years, the development of renewable, sustainable and environmentally friendly new energy has become a consensus of mankind, and renewable energy such as solar energy and wind energy has been vigorously developed. However, such new energy sources often have intermittent problems in time and space, so large-scale energy storage equipment is needed for regulation. Compared with the widely used lithium-ion batteries (LIBs), sodium-ion batteries (SIBs) are lower in cost and are expected to be used in the field of large-scale energy storage in the future.
[0003] In sodium-ion batteries, the cathode material provides active sodium ions and high redox potential, which plays a vital role in determining the battery operating voltage and reversible capacity. Therefore, the development of high-capacity and high-potential cathode materials is crucial for their practical application. x MO2 (M=Co, Mn, Fe, Cu, Zn, Cr, Ni, Ti, etc.) is a research hotspot. When it is composed of 5 or more transition metal elements in an equiatomic ratio or a nearly equiatomic ratio, it usually has a higher entropy value and is called a high entropy oxide. High entropy oxides have similar thermodynamic high entropy effects, kinetic hysteresis diffusion effects, structural lattice distortion effects, and performance "cocktail" effects as high entropy alloys, and can exhibit some properties far superior to traditional oxides, such as high fracture toughness, high strength, good high temperature / low temperature performance, good energy storage performance, etc. Therefore, energy storage researchers have been interested in the study of high entropy oxides. However, in the prior art, the energy density of the prepared high entropy oxide cathode material is still not high enough, which hinders its large-scale production. It is necessary to develop a sodium battery cathode material with a higher energy density. Summary of the invention
[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing an anion-doped high-performance sodium battery positive electrode material, so as to further improve the energy density of sodium ion batteries and promote the industrial development of sodium ion batteries.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing an anion-doped high-performance sodium cathode material comprises the following steps:
[0007] S1: Mix the sodium source, lithium source, manganese source, copper source, zinc source and nickel source in powder form according to the element ratio of Na0.8Mn0.63Cu0.15Zn0.02Ni0.1Li0.08, dissolve them in deionized water or ethanol solvent, and then add citric acid at 1-3.5 times the molar amount of metal atoms;
[0008] S2: Stirring in a water bath at 60-95°C for 2-8h until the solution evaporates to dryness, then drying at 100-200°C for 6-24h, and then sintering at high temperature in air or oxygen atmosphere at a temperature of 400-600°C for 3-12h, with a heating rate of 1-10°C / min from room temperature to the sintering temperature, and continuing to cool to room temperature to obtain a precursor material;
[0009] S3: adding titanium dioxide and sodium fluoride according to the element composition Na0.8Mn0.63Cu0.15Zn0.02Ni0.1Li0.08Ti0.01O2-xFx after anion doping, where 0<x≤0.3, and grinding thoroughly to obtain a mixed powder sample with a particle size in the range of 10-500nm;
[0010] S4: The raw material mixture sample is pressed into tablets under 10-30MPa conditions, and then subjected to high-temperature sintering treatment at a temperature of 600-1200°C for 8-24h with air or oxygen as a protective gas, wherein the heating rate from room temperature to the sintering temperature is 3-10°C / min, and then cooled to room temperature to prepare an anion-doped high-entropy layered oxide sodium positive electrode material Na0.8Mn0.63Cu0.15Zn0.02Ni0.1Li0.08Ti0.01O2-xFx, wherein 0<x≤0.3;
[0011] S5: The positive electrode material obtained in S4 is mixed with a conductive additive and polyvinylidene fluoride in a mass ratio of 7:2:1, and then 5-20 liters of N-methylpyrrolidone solvent is added per kilogram of electrode material to mix evenly, and a positive electrode sheet is prepared through a slurry mixing, coating and drying process, and the active material loading amount is 2-3.5 mg cm-2;
[0012] S6: The positive electrode prepared in S5 and the negative electrode of the metal sodium sheet are assembled into a sodium ion battery. The electrolyte consists of 1 mol / L NaPFO6, a mixed solvent of propylene carbonate / ethyl methyl carbonate with a volume ratio of 1:1, and 4% fluoroethylene carbonate. The diaphragm uses a porous glass carbon fiber membrane. The button battery is assembled in a glove box filled with argon with a water oxygen value below 0.1 ppm.
[0013] Preferably, the method of mixing the raw materials in step S1 includes any one of sol-gel mixing, ball milling mixing, and co-precipitation mixing.
[0014] Preferably, the sodium source includes any one of sodium carbonate, sodium citrate, sodium acetate, and sodium nitrate, or a combination of at least two of them.
[0015] Preferably, the lithium source includes any one of lithium carbonate, lithium citrate, lithium acetate, and lithium nitrate, or a combination of at least two of them.
[0016] Preferably, the manganese source includes any one or a combination of at least two of manganese trioxide, manganese oxide, manganese acetate, manganese nitrate, and manganese hydroxide.
[0017] Preferably, the copper source includes any one of copper oxide, copper citrate, copper acetate, and copper nitrate, or a combination of at least two of them.
[0018] Preferably, the zinc source includes any one of zinc oxide, zinc nitrate, and zinc acetate, or a combination of at least two of them.
[0019] Preferably, the nickel source includes any one of nickel oxide, nickel hydroxide, nickel acetate, and nickel nitrate, or a combination of at least two of them.
[0020] The beneficial effects of the present invention are as follows: the high entropy oxide positive electrode material is regulated by anion doping, and the advantages of multiple elements in the high entropy oxide material are combined to improve the specific capacity of the high entropy positive electrode material, and the specific capacity is high under large current, which is easy to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The sodium positive electrode material Na obtained in Example 1 of the present invention 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 1. 9F 0.1 XRD pattern of high entropy oxide;
[0022] Figure 2 The sodium positive electrode material Na obtained in Example 1 of the present invention 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 1. 9F 0.1 SEM image of high entropy oxide;
[0023] Figure 3 The sodium positive electrode material Na obtained in Example 1 of the present invention 0.8 Mn 0.63 Cu0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 1. 9F 0.1 The charge and discharge rate performance curve of sodium-ion batteries assembled with high entropy oxides; DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings. The technical solution of the present invention is further explained below in conjunction with the specific implementation method, but it should be noted that the specific implementation method is only a specific implementation and explanation of the essence of the technical solution of the present invention, and should not be understood as a limitation on the protection scope of the present invention.
[0025] (1) Sodium acetate, lithium acetate, manganese acetate, copper acetate, zinc acetate, and nickel acetate are prepared according to the element composition of the positive electrode material of the sodium ion battery. 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 1.9 F 0.1 , dissolved in deionized water, citric acid was added at 1.2 times the molar amount of metal atoms, stirred for 2 hours, stirred in a water bath at 80°C until the solution evaporated, dried at 150°C for 6 hours, and then sintered at 450°C for 5 hours in an air atmosphere, wherein the heating rate from room temperature to the sintering temperature was 2°C / min, and then cooled to room temperature to obtain a precursor material free of titanium source and fluorine source; then titanium dioxide and sodium fluoride were added according to the elemental composition after anion doping, and ground for 1 hour to obtain a mixed powder sample with a particle size of 10-500nm. ;
[0026] (2) The mixed powder sample obtained in S1 was pressed into a disc with a diameter of 14 cm by a tablet press at 20 MPa, and then the disc was sintered at 8500° C. at a heating rate of 5° C. / min in an air atmosphere for 12 h, and then cooled to room temperature in the furnace to obtain a sodium ion battery positive electrode material.
[0027] Several mixing methods in S1, the sol-gel method is exemplified as follows: dissolving a sodium source, a lithium source, a manganese source, a copper source, a zinc source and a nickel source in deionized water in corresponding proportions, adding a certain amount of citric acid solution (the molar ratio of metal ions: citric acid can be 1 to 3.5) dropwise to the above solution, heating in a water bath (such as 60 to 95°C) until the solution is evaporated and a gel is formed, then heating the gel (such as heating at 110 to 150°C for more than 20 hours), sintering in air or oxygen atmosphere (such as temperature of 400-600°C, time of 3-12 hours, heating rate of 1-10°C / min), cooling to room temperature, adding a titanium source and a fluorine source, grinding, and obtaining a mixed powder.
[0028] The ball milling method is exemplified as follows: sodium source, lithium source, manganese source, copper source, zinc source, nickel source, titanium source and fluorine source are placed in an agate ball mill according to corresponding proportions, a certain amount of auxiliary agent is added after the ball mill is placed in the ball mill, and then ball milling is performed. The auxiliary agent is one of ethanol and methanol or a mixture of the two, and ball milling is performed (such as ball milling at a speed of 300 to 600 rpm for 6 to 24 hours). Drying after ball milling, the drying temperature is 40-90°C, and the time is 6-24 hours to obtain a mixed powder.
[0029] The co-precipitation method is exemplified as follows: dissolving a lithium source, a manganese source, a copper source, a zinc source and a nickel source in deionized water, adding ammonia water and sodium hydroxide, adjusting the pH to alkaline (such as 9.5-11) and aging (such as aging at 40-60°C for more than 24 hours) to obtain a hydroxide precursor, and then manually grinding the precursor powder with a sodium source, a titanium source and a fluorine source in a mortar in a certain proportion to obtain a mixed powder.
[0030] like Figure 1 As shown, the sodium positive electrode material Na obtained in this embodiment 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 1. 9F 0.1 The XRD diffraction pattern of the high entropy layered oxide conforms to the PDF card of the P2 phase structure. That is, a high entropy layered oxide sodium positive electrode material with a P2 phase structure is synthesized by anion doping.
[0031] like Figure 2 As shown, the sodium positive electrode material Na obtained in this embodiment 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 1. 9F0.1 High entropy oxides have a typical layered structure with a particle size of 0.5 to 3 μm.
[0032] Battery Assembly:
[0033] (1) Preparation of positive electrode sheet:
[0034] The positive electrode material was mixed with a conductive additive (SuperP) and a binder (polyvinylidene fluoride) in a mass ratio of 7:2:1, and an appropriate amount of solvent N-methylpyrrolidone (0.5 ml / 100 mg) was added. The positive electrode sheet (active material loading of 2-3.5 mg cm) was prepared through a process of slurry mixing, coating, and drying. -2 );
[0035] (2) Assembling sodium ion batteries:
[0036] The prepared positive electrode sheet and the metal sodium negative electrode sheet are assembled into a sodium ion battery; the electrolyte consists of 1 mol / LNaPFO6, a mixed solvent of propylene carbonate / ethyl methyl carbonate with a volume ratio of 1:1, and fluoroethylene carbonate (added in an amount of 4%); the diaphragm uses a porous glass carbon fiber membrane, and the button battery is assembled in a glove box filled with argon with a water oxygen value below 0.1 ppm.
[0037] like Figure 3 As shown, the sodium ion battery assembled with the positive electrode material has a discharge capacity of 122.4 mAh / g after 500 cycles in the voltage range of 1.8-4.3 V and a current density of 5C (0.6 A / g), and has good cycle stability.
[0038] As can be seen from the above, the sodium positive electrode material Na obtained in the embodiment of the present invention 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.0 1O 1.9 F 0.1 Sodium-ion batteries assembled from high-entropy layered oxides have high specific capacity and excellent long-cycle stability.
Claims
1. A method for preparing an anion-doped high-performance sodium cathode material, characterized in that: The steps include: S1: Sodium source, lithium source, manganese source, copper source, zinc source and nickel source are mixed according to Na 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 The powders are mixed with the element ratio composition, dissolved in deionized water or ethanol solvent, and then citric acid is added at 1-3.5 times the molar amount of metal atoms; S2: Stirring in a water bath at 60-95°C for 2-8h until the solution evaporates to dryness, then drying at 100-200°C for 6-24h, and then sintering at high temperature in air or oxygen atmosphere at a temperature of 400-600°C for 3-12h, with a heating rate of 1-10°C / min from room temperature to the sintering temperature, and continuing to cool to room temperature to obtain a precursor material; S3: Then according to the element composition of anion doping Na 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 2-x F x , wherein 0<x≤0.3, titanium dioxide and sodium fluoride are added, and after sufficient grinding, a mixed powder sample is obtained, and the particle size is in the range of 10-500nm; S4: The raw material mixture sample is pressed into a tablet under 10-30MPa conditions, and then subjected to high-temperature sintering treatment at a temperature of 600-1200°C for 8-24h with air or oxygen as a protective gas, wherein the heating rate from room temperature to the sintering temperature is 3-10°C / min, and then cooled to room temperature to prepare an anion-doped high-entropy layered oxide sodium positive electrode material Na 0.8 Mn 0.63 Cu 0.15 Zn 0.02 Ni 0.1 Li 0.08 Ti 0.01 O 2-x F x , where 0<x≤0.3; S5: The positive electrode material obtained in step 4 is mixed with the conductive additive and polyvinylidene fluoride in a mass ratio of 7:2:1, and then 5-20 liters of N-methylpyrrolidone solvent are added per kilogram of electrode material to mix evenly. The positive electrode sheet is prepared through a slurry mixing, coating and drying process, and the active material loading is 2-3.5 mg cm -2 ; S6: Assemble the positive electrode prepared in step 5 and the metal sodium negative electrode into a sodium ion battery. The electrolyte consists of 1 mol / L NaPFO6, a mixed solvent of propylene carbonate / ethyl methyl carbonate with a volume ratio of 1:1, and 4% fluoroethylene carbonate. The diaphragm uses a porous glass carbon fiber membrane. The button battery is assembled in a glove box filled with argon with a water oxygen value below 0.1 ppm.
2. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The method of mixing the raw materials in step S1 includes any one of sol-gel mixing, ball milling mixing, and coprecipitation mixing.
3. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The sodium source includes any one of sodium carbonate, sodium citrate, sodium acetate, and sodium nitrate, or a combination of at least two of them.
4. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The lithium source includes any one of lithium carbonate, lithium citrate, lithium acetate, and lithium nitrate, or a combination of at least two of them.
5. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The manganese source includes any one of manganese trioxide, manganese oxide, manganese acetate, manganese nitrate, and manganese hydroxide, or a combination of at least two of them.
6. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The copper source includes any one of copper oxide, copper citrate, copper acetate, and copper nitrate, or a combination of at least two of them.
7. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The zinc source includes any one of zinc oxide, zinc nitrate, and zinc acetate, or a combination of at least two of them.
8. The method for preparing an anion-doped high-performance sodium positive electrode material according to claim 1, characterized in that: The nickel source includes any one of nickel oxide, nickel hydroxide, nickel acetate, and nickel nitrate, or a combination of at least two of them.