Hydraulic composition, powdered additive, powdered tackifier, and method for producing same
By using polyethylene glycol (PEG) derivatives to impregnate the water-soluble porous powder and water-soluble cellulose ether, the problem of reducing compressive strength caused by the increase in the amount of air in the hydraulic composition is solved, and the fluidity and resistance are improved Frost damage, simplifies the processing process and reduces costs.
Patent Information
- Application Number
- CN202410719811.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-06
- Filing Date
- 2024-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
The existing hydraulic compositions have problems in use that increase the amount of air and lead to a decrease in compressive strength. The traditional defoaming agent is cumbersome and costly. Although sulfoethyl cellulose can improve the resistance to freezing damage, it may cause fluidity. deterioration.
Polyethylene glycol (PEG) derivatives impregnate water-soluble porous powder as powder additives or tackifiers, combined with water-soluble cellulose ethers, improve the fluidity of hydraulic compositions through specific chemical structures and processes. Exudation and frost damage resistance.
Improved fluidity, ooze and frost damage resistance of hydraulic compositions are achieved, while simplifying the processing process, reducing costs, and improving product performance.
Smart Images

Figure BDA0004876724700000281 
Figure BDA0004876724700000291 
Figure BDA0004876724700000292
Abstract
Description
Technical Field
[0001] The present invention relates to a hydraulic composition, a powdery additive, a powdery thickener, and a method for producing the hydraulic composition. Background Art
[0002] Water-soluble cellulose ethers represented by hydroxyalkyl alkyl cellulose are widely used as thickeners for reducing exudation without losing fluidity. However, water-soluble cellulose ethers have the ability to introduce air, and there is a risk that the amount of air in the hydraulic composition or concrete increases to exceed the standard (4.5±1.5%), thereby reducing the compressive strength of the concrete. Therefore, one way to avoid the risk is to add a defoaming agent to remove bubbles to reduce the amount of air.
[0003] Various compounds are known as defoamers. For example, Patent Document 1 discloses a surfactant in the form of a polyether compound as a nonionic defoamer.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: JP-A-2008-037663
[0007] Patent Document 2: JP-A-2011-184236
[0008] Patent Document 3: JP-A-2017-065995
[0009] Patent Document 4: JP-A H05-085791
[0010] Non-patent document 1: "Method of emulsion formulation design, pages 2-9", Nihon Emulsion Co., Ltd., "What is emulsion formulation design with organic concept diagram?" [January 10, 2023], URL <https: / / www.nihon-emulsion.co.jp / tech / organic.html>
[0011] Non-patent document 2: Durability of concrete structures: Frost damage (Hasegawa Hisao, Fujiwara Tadashi: Gihodo Publishing, page 63, February 1988) Summary of the invention
[0012] Since polyether compounds are liquid or waxy solid, they must be dissolved in AE water reducers etc. before use, which leads to the problem of complicated handling. This problem can be overcome by impregnating highly oil-absorbing inorganic powders such as silica with polyether compounds to convert the polyether compounds into powder form (see Patent Documents 1 and 2). Measurements of the bubble spacing coefficients of cement compositions and hydraulic compositions (described in Patent Documents 1 and 2) (described in Patent Document 3) show that defoamers impregnated with inorganic powders tend to selectively remove entrained air in the form of fine bubbles of 50 to 500 μm in diameter, which are believed to be useful for freezing resistance, compared with pure defoamers (defoamers alone). Defoamers impregnated with inorganic powders (as proposed in Patent Documents 1 and 2) can sometimes deteriorate freezing resistance. There is still room for improvement.
[0013] As a hydraulic composition having excellent frost resistance even when using a water-soluble cellulose ether, for example, Patent Document 4 discloses a concrete composition comprising a cement binder, aggregate, water, a water reducing agent, and an AE agent, wherein an alkali metal salt of sulfoethyl cellulose and a nonionic water-soluble cellulose ether are added in an amount of 0.02 to 0.5% by weight relative to the cement binder. Although the sulfoethyl cellulose used in Patent Document 4 does not increase the air introduction of the hydraulic composition, it may cause another problem, namely, deterioration of fluidity. In addition, sulfoethyl cellulose is expensive, so it is not preferred from an economic point of view. There is still room for improvement.
[0014] The present invention aims to provide a powdered additive or powdered thickener for hydraulic compositions, which is easy to handle and effective in formulating hydraulic compositions with improved fluidity, reduced oozing and improved frost resistance; a hydraulic composition and a method for producing the hydraulic composition.
[0015] The present inventors have found that the outstanding problems of hydraulic compositions including freezing resistance, fluidity and exudation can be overcome when a water-soluble cellulose ether is used in combination with a polyethylene glycol (PEG) derivative having a specific chemical structure. When a powdered additive in the form of a water-soluble porous powder impregnated with a polyethylene glycol (PEG) derivative having a specific chemical structure is used, the problem of complicated handling of the additive can be overcome while maintaining the improvement of freezing resistance, fluidity and exudation reduction of the hydraulic composition.
[0016] In one aspect, the present invention provides a powdered additive for a hydraulic composition, comprising a water-soluble porous powder impregnated with a polyethylene glycol derivative, wherein the polyethylene glycol derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw of 300 to 2500 relative to a polystyrene standard measured by gel permeation chromatography, and has at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
[0017] In a preferred embodiment, the polyethylene glycol derivative is at least one of the compounds represented by the general formulae (A1) and (A2):
[0018] RCOO-(C2H4O) n -H (A1)
[0019] (RCOO-(C2H4O) n1 ) t R 1 ((OC2H4) n2 -OH) u (A2)
[0020] Wherein, R and n are as defined above, R 1 A residue obtained by removing a hydroxyl group from a polyol having 2 to 5 hydroxyl groups, wherein the residue is a 2- to 5-valent C2-C5 straight-chain or branched hydrocarbon group, t and u are each integers of 1 to 4, the sum of t and u is an integer of 2 to 5, n1 and n2 are each an integer greater than 0, and n1×t+n2×u is an integer of 3 to 30.
[0021] In a preferred embodiment, the water-soluble porous powder is a water-soluble porous polysaccharide.
[0022] In a preferred embodiment, the volume density of the water-soluble porous powder is 0.10 to 0.25 g / cm 3 .
[0023] In a preferred embodiment, in the cumulative molecular weight distribution of the water-soluble porous powder measured by gel permeation chromatography, the cumulative value of the concentration fraction of a molecular weight of 10,000 is preferably 30 to 90%.
[0024] In a preferred embodiment, the dextrose equivalent (DE) of the water-soluble porous powder is 2-18.
[0025] In the particle size distribution of the water-soluble porous body measured by a dry laser method, the average particle size of the water-soluble porous powder is 10 to 230 μm and the volume ratio of particles with a particle size of 300 μm or more is 0 to 10%.
[0026] In the particle size distribution of the additive measured by a dry laser method, the average particle size of the additive is preferably 40 to 280 μm, and the volume ratio of particles having a particle size of 300 μm or more is 0 to 10%.
[0027] In another aspect, the present invention provides a powdered viscosity enhancing agent for a hydraulic composition, comprising a powdered additive as defined herein and a water-soluble cellulose ether.
[0028] In the thickener, the water-soluble cellulose ether is hydroxyalkyl alkyl cellulose.
[0029] In the thickener, the viscosity of a 2 wt % aqueous solution of the water-soluble cellulose ether at 20° C. is preferably 15 to 450,000 mPa·s.
[0030] The tackifier may further include a water repellent.
[0031] In a further aspect, the present invention provides a hydraulically settable composition comprising a powdered additive as defined herein, a hydraulic substance and water.
[0032] The hydraulic composition may further include a water-soluble cellulose ether and / or a water repellent.
[0033] In a preferred embodiment, the hydraulic composition is a concrete composition further comprising fine aggregate, coarse aggregate, and a water reducing agent, wherein the slump of the concrete composition measured by the method of JIS A1101 is 8 to 21 cm, and the compressive strength of the concrete composition measured by the method of JIS A 1108 at 28 days is 18 to 45 N / mm 2 .
[0034] In yet another aspect, the present invention provides a hydraulic composition comprising a powdered tackifier as defined herein, a hydraulic substance and water.
[0035] In a preferred embodiment, the hydraulic composition is a concrete composition further comprising fine aggregate, coarse aggregate, and a water reducing agent, wherein the slump of the concrete composition measured by the method of JIS A1101 is 8 to 21 cm, and the compressive strength of the concrete composition measured by the method of JIS A 1108 at 28 days is 18 to 45 N / mm 2 .
[0036] In yet another aspect, the present invention provides a method for producing a hydraulic composition comprising a hydraulic substance, water and a polyethylene glycol derivative, the method comprising the step of adding a powdered additive as defined herein to the step of mixing the components of the hydraulic composition.
[0037] Preferably, the hydraulic composition further comprises fine aggregate, coarse aggregate, and a water reducing agent to form a concrete composition, wherein the slump of the concrete composition measured by the method of JIS A 1101 is 8 to 21 cm, and the compressive strength of the concrete composition measured by the method of JIS A 1108 at 28 days is 18 to 45 N / mm 2 .
[0038] In yet another aspect, the present invention provides a method for producing a hydraulic composition comprising a hydraulic substance, water, a water-soluble cellulose ether and a polyethylene glycol derivative, the method comprising the step of adding a powdered additive as defined herein to the step of mixing the components of the hydraulic composition.
[0039] Preferably, the hydraulic composition further comprises fine aggregate, coarse aggregate, and a water reducing agent to form a concrete composition having a slump of 8 to 21 cm as measured by the method of JIS A 1101 and a compressive strength of 18 to 45 N / mm2 as measured by the method of JIS A 1108 at 28 days. 2 .
[0040] Advantageous Effects of the Invention
[0041] By using the powdery additive for hydraulic compositions and the powdery thickener, it is possible to easily produce a hydraulic composition having improved freezing resistance, fluidity, and reduced oozing out.
[0042] Preferred Embodiments
[0043] As used herein, Mw means weight average molecular weight, GPC means gel permeation chromatography, DS means “degree of substitution”, and MS means “molar substitution.” The notation (Cn-Cm) indicates a group containing n to m carbon atoms per group.
[0044] The inventors first attempted to solve the problem of complicated additive handling. Since the defoamer dissolves slowly from the inorganic powder during the manufacture of the hydraulic composition, the defoamer in the form of impregnated inorganic powder can selectively remove fine bubbles with a diameter of less than 200 μm, which are considered to be useful for freezing resistance. For the defoamer itself, it is necessary to select a material that does not remove fine bubbles called entrained air, which are considered to be useful for freezing resistance, but can remove coarse bubbles called entrapped air, which are considered to be detrimental to freezing resistance.
[0045] Then, the inventors speculate that the polyethylene glycol (PEG) derivatives with a specific structure have an impact on the easy removal of bubble diameter and defoaming when functioning as a defoaming agent (considering frost resistance). In addition, as an object to be impregnated, water-soluble porous powders are of interest. Although PEG derivatives tend to remove coarse bubbles without removing fine bubbles, they are effective for improving flow and reducing exudation. When using a water-soluble porous powder as an object to be impregnated, dissolution is improved so that coarse or large bubbles can be further selectively removed. That is, a powdered additive in the form of a PEG derivative impregnated in a water-soluble porous powder successfully and advantageously improves the frost resistance, fluidity and reduced exudation of a hydraulic composition.
[0046] <Powdered Additives>
[0047] One embodiment of the present invention is a powdered additive for a hydraulic composition, comprising a water-soluble porous powder impregnated with a polyethylene glycol (PEG) derivative. The PEG derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw of 300 to 2500 measured by gel permeation chromatography relative to a polystyrene standard, and has at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
[0048] (Polyethylene glycol derivatives)
[0049] The PEG derivatives should have an IOB value of 0.3 to 1.8 in the organic concept diagram, a weight average molecular weight Mw of 300 to 2500 measured by GPC relative to a polystyrene standard, and at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
[0050] [IOB value]
[0051] The IOB value of the PEG derivative in the organic concept diagram is 0.3 to 1.8, preferably 0.7 to 1.2. If the IOB value is less than 0.3, the water solubility of the PEG derivative is poor. If the IOB value exceeds 1.8, the PEG derivative has a stronger surfactant effect and a poor defoaming effect, and cannot impart frost damage resistance to the hydraulic composition.
[0052] As the fluidity of the hydraulic composition decreases, more air is easily introduced during the mixing step, and thus a stronger defoaming ability is required. In this sense, the fluidity of the hydraulic composition is related to the IOB value of the PEG derivative in the organic concept diagram.
[0053] Specifically, in the case of a hydraulic composition having a slump of 8 to 21 cm obtained by the method in JIS A 1101, the IOB value of the PEG derivative in the organic concept diagram should preferably be 0.3 to 1.4, more preferably 0.7 to 1.4, and further preferably 0.7 to 1.2. In the case of a medium-flow concrete composition having a slump flow of 35 to 50 cm as specified in the East / Central / West Japan Expressway Tunnel Construction Management Guidelines and a high-flow concrete composition having a slump flow of 55 to 75 cm as specified in the Construction Code of Concrete Standard Specification 2017, the IOB value of the PEG derivative in the organic concept diagram should preferably be 0.9 to 1.8, and more preferably 0.9 to 1.6.
[0054] It should be noted that the IOB (Inorganic Organic Balance) value in the organic concept diagram is the ratio of the inorganic value (IV) to the organic value (OV) determined based on the organic concept diagram. That is, IOB = IV / OV (the same below). The OV and IV of a compound are determined by adding the predetermined values of the groups or sites on the compound in the entire molecule. For IOB, reference should be made to "Methods for Emulsification Formula Design Pages 2-9", Japan Emulsion Co., Ltd., "What is the Emulsification Formula Design of the Organic Concept Diagram?" (Non-Patent Document 1).
[0055] Depending on the specific purpose, the PEG derivatives can be used alone or in combination of two or more. When two or more PEG derivatives are used, the IOB of each PEG derivative in the organic concept diagram is 0.3 to 1.8.
[0056] [Weight average molecular weight]
[0057] The Mw of the PEG derivative measured by GPC relative to a polystyrene standard is 300 to 2500, preferably 500 to 1300, and more preferably 500 to 1200. If the Mw is less than 300, the PEG derivative has poor dispersibility in water. If the Mw exceeds 2500, the PEG derivative cannot reduce the bleeding of the hydraulic composition.
[0058] The Mw of PEG derivatives can be measured by GPC using tetrahydrofuran (THF) as a developing solvent relative to a polystyrene standard. Specifically, the test solution is injected into a high performance liquid chromatography device using a size exclusion column, the dissolution time is measured, and the Mw (hereinafter the same) is determined by comparing the measured value with a calibration curve of a standard solution.
[0059] In PEG derivatives, the average number of added moles "n" of ethyleneoxy groups (-C2H4O-, EO) that affects the molecular weight is related to the IOB value. Therefore, like the IOB value, Mw is related to the fluidity of the hydraulic composition. Specifically, in the case of a hydraulic composition having a slump of 8 to 21 cm based on the method in JISA 1101, the Mw of the PEG derivative is preferably 300 to 1300, more preferably 500 to 1300, and further preferably 500 to 1200. In the case of a medium-flowing concrete composition with a slump flow of 35 to 50 cm specified in the East / Central / West Japan Expressway Tunnel Construction Management Guidelines and a high-flowing concrete composition with a slump flow of 55 to 75 cm specified in the Construction Code of Concrete Standard Specification 2017, the Mw of the PEG derivative is preferably 700 to 2500, and more preferably 700 to 1700.
[0060] [Structure of PEG derivatives]
[0061] PEG derivatives are asymmetric linear or branched structures with at least one RCOO (C2H4O) n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group (ie, has no functional group other than -OH group at the terminal).
[0062] In PEG derivatives, RCOO(C2H4O) in the molecule n The number of - is at least 1, preferably 1 to 4, and more preferably 1.
[0063] From the viewpoint of improving the fluidity and frost damage resistance of the hydraulic composition and the dispersibility of the PEG derivative in water, R is C 10 To C 24 , preferably C16 To C 22 A linear or branched monovalent hydrocarbon group. Examples of the monovalent hydrocarbon group R include linear alkyl groups such as lauryl, cetyl, stearyl, behenyl, undecyl, pentadecyl, heptadecyl, and heneicosyl; branched alkyl groups such as isostearyl, octyldodecyl, decyltetradecyl, isoheptadecyl, 16-methylhexadecyl, 2-octylundecyl, and 2-decyltridecyl; and linear alkenyl groups such as oleyl. From the perspective of the availability and handling of the compound, it is preferred that R is a linear or branched alkyl group such as heptadecyl or isoheptadecyl.
[0064] From the perspective of improving the resistance to freezing damage, the PEG derivative also has an ester bond (—COO—).
[0065] From the perspective of reducing the bleeding of the hydraulic composition, improving the frost resistance and preventing foaming, the average added molar number n of ethyleneoxy (-C2H4O-) is an integer of 3 to 40, preferably an integer of 5 to 30, and more preferably an integer of 5 to 20.
[0066] The PEG derivative is preferably at least one of the compounds having the general formula (A1) and the general formula (A2). The compound having the formula (A1) and the compound having the formula (A2) are referred to as compounds A1 and A2, respectively.
[0067] RCOO-(C2H4O) n -H (A1)
[0068] (RCOO-(C2H4O) n1 ) t R 1 ((OC2H4) n2 -OH) u (A2)
[0069] In formula (A1) and (A2), R is independently C 10 ~C 24 A linear or branched monovalent hydrocarbon group, R 1 The residue is a residue obtained by removing a hydroxyl group from a polyol having 2 to 5 hydroxyl groups, the residue being a C2 to C5 straight-chain or branched hydrocarbon group having a valence of 2 to 5, the average number of moles of ethyleneoxy (-C2H4O-) added n being an integer of 3 to 40, t and u being each an integer of 1 to 4, and the sum of t and u being an integer of 2 to 5 (equivalent to the number of moles of R obtained therefrom) 1 The number of hydroxyl groups in the polyol), n1 and n2 are each an integer greater than 0 (equivalent to the average number of added moles of ethylene oxide (-C2H4O-)), and n1×t+n2×u is an integer from 3 to 30.
[0070] [Compound A1]
[0071] Compound A1 is a compound of formula (A1) having an IOB value of 0.3 to 1.8 in an organic concept diagram and an Mw of 300 to 2500 as measured by GPC relative to a polystyrene standard.
[0072] In formula (A1), from the perspective of improving fluidity and freezing resistance and solubility of the PEG derivative in water, R is as defined above and each independently represents C 10 ~C 24 , preferably C 16 ~C 22 Examples of the monovalent hydrocarbon group R are as exemplified above.
[0073] In the formula (A1), from the viewpoint of improving the freezing resistance of the hydraulic composition, an ester bond (—COO—) is present, and n is as defined above.
[0074] Examples of compound A1 include polyethylene glycol monostearate (the average number of added moles of ethylene oxide (-C2H4O-) is 5, 10, 20, 30), polyethylene glycol monoisostearate (the average number of added moles of ethylene oxide (-C2H4O-) is 6, 8, 10, 12, 16), and polyethylene glycol monooleate (the average number of added moles of ethylene oxide (-C2H4O-) is 6, 10).
[0075] [Compound A2]
[0076] Compound A2 is a compound of formula (A2), and its IOB value in the organic concept diagram is 0.3 to 1.8, and its Mw measured by GPC relative to a polystyrene standard is 300 to 2500.
[0077] In formula (A2), from the perspective of improving fluidity and freezing resistance and the solubility of the PEG derivative in water, R is as defined above and each independently is C 10 ~C 24 , preferably C 16 ~C 22 Examples of the monovalent hydrocarbon group R are as exemplified above.
[0078] In the formula (A2), from the viewpoint of improving the freezing resistance, an ester bond (—COO—) is present.
[0079] In formula (A2), R 1The residue is a residue obtained by removing hydroxyl groups from a polyol having 2 to 5, preferably 2 or 3, hydroxyl groups, and the residue is a C2 to C5 straight-chain or branched hydrocarbon group having 2 to 5 valences, more preferably 2 or 3 valences. If the carbon number is less than 2 (i.e., equal to 1), the compound is difficult to synthesize. If the carbon number exceeds 5, the compound may have high hydrophobicity and be difficult to dissolve or disperse in water.
[0080] Examples of the polyol include dihydric alcohols (having 2 hydroxyl groups) such as 1,2-butanediol and 1,3-butanediol; trihydric alcohols (having 3 hydroxyl groups) such as glycerol and trimethylolpropane; tetrahydric alcohols (having 4 hydroxyl groups) such as diglycerol, erythritol, pentaerythritol, sorbitan and methyl glucoside; pentahydric alcohols (having 5 hydroxyl groups) such as xylitol and triglycerol. Among them, dihydric alcohols and trihydric alcohols are preferred, and 1,2-butanediol and 1,3-butanediol are more preferred from the viewpoint of preventing foaming of the hydraulic composition.
[0081] In formula (A2), t and u are each an integer of 1 to 4, and from the perspective of reducing bleeding, t is preferably 1, and from the perspective of preventing foaming of the hydraulic composition, u is preferably 1 or 2. The sum of t and u (i.e., t+u) is an integer of 2 to 5, which is equivalent to obtaining R 1 The sum of (t+u) is preferably 2 or 3, more preferably 2, from the perspective of preventing foaming of the hydraulic composition.
[0082] In formula (A2), n1 and n2 are each independently the average added molar number of ethyleneoxy (-C2H4O-), which is an integer greater than 0, and n1×t+n2×u is an integer from 3 to 30, preferably an integer from 5 to 30, more preferably an integer from 8 to 20, and further preferably an integer from 10 to 20.
[0083] Examples of compound (A2) include PEG-10BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 10), PEG-15BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 15), PEG-20BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 20), and PEG-25BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 25).
[0084] When the PEG derivative is in liquid form, it can be used, for example, for impregnation of a water-soluble porous powder. Even when the PEG derivative is in solid form, it can be used as long as it can be converted into a liquid by heating before impregnation of the water-soluble porous powder.
[0085] (Water-soluble porous powder)
[0086] The water-soluble porous powder is a carrier, and in this sense, the powder is impregnated with the PEG derivative, which means that the PEG derivative is loaded on the powder, and therefore, the PEG derivative can be handled in the form of a powder. The water-soluble porous powder is composed of porous water-soluble particles that can be impregnated with the PEG derivative, and is formed of a material that has no adverse effect on the properties of the hydraulic composition when dissolved in water. Examples of the material are water-soluble porous polysaccharides and sodium carbonate. In particular, water-soluble porous polysaccharides are preferred from the aspect of suppressing the alkali-silica reaction of the hydraulic composition.
[0087] Examples of water-soluble porous polysaccharides include water-soluble porous cellulose ethers, water-soluble porous maltodextrins and water-soluble porous dextrins. From the perspective of reducing the viscosity of the hydraulic composition and promoting the solubility during the preparation of the hydraulic composition (i.e., the exudation of the PEG derivative), water-soluble porous maltodextrin is preferred.
[0088] The water-soluble porous cellulose ether is selected from the group consisting of cellulose having a bulk density of preferably 0.10 to 0.25 g / cm 3 , more preferably 0.14 to 0.20 g / cm 3 Water-soluble cellulose ether in powder form.
[0089] The water-soluble porous cellulose ether is obtained by designing the water-soluble cellulose ether to be porous so as to be impregnated. From the viewpoint of the influence on the concrete composition, the water-soluble porous cellulose ether exerts the same effect as the water-soluble cellulose ether described below.
[0090] The water-soluble porous maltodextrin and the water-soluble porous dextrin are prepared from a solution of a starch decomposition product and / or a reduced starch decomposition product.
[0091] (Starch degradation products)
[0092] Starch decomposition products include products obtained by hydrolyzing starch by acid decomposition, alkali decomposition, enzyme decomposition, or roasting treatment and their combinations. Starch decomposition products may include one hydrolyzate or multiple hydrolyzates. Examples of starch used in this article include natural starch such as tapioca starch, sago starch, potato starch, wheat starch, rice starch, sweet potato starch, corn starch and waxy corn starch; modified starch such as acetylated distarch phosphate, acetylated oxidized starch, acetylated distarch adipate, sodium starch octenyl succinate, acetic starch, oxidized starch, hydroxypropyl distarch phosphate, hydroxypropyl starch, monostarch phosphate, distarch phosphate, phosphorylated distarch phosphate.
[0093] (Reduced starch degradation product)
[0094] The reduced starch degradation product is obtained by reducing the above-mentioned starch degradation product to a sugar alcohol form. The reduced starch degradation product may include one reduced starch degradation product or a plurality of reduced starch degradation products.
[0095] (Solution)
[0096] The solution of starch degradation product and / or reduced starch degradation product is obtained by dissolving at least one of starch degradation product and reduced starch degradation product in a solvent. The solvent used in this article is not particularly limited. For example, water, aqueous alcohol, etc. can be used, preferably water. The concentration of starch degradation product and / or reduced starch degradation product in the solvent is preferably 10 to 60% by weight of the total weight of the degradation product, more preferably 20 to 55% by weight, and further preferably 30 to 50% by weight. In particular, the solution of starch degradation product with low dextrose equivalent (DE) tends to increase in viscosity. Therefore, when using starch degradation product with low DE, it is preferred to set the concentration of the solution low to avoid excessive increase in the viscosity of the solution. For example, when DE is less than 6, the solution concentration is set to less than 50% by weight.
[0097] Water-soluble porous maltodextrin or water-soluble porous dextrin is prepared by drying the obtained solution with a drum dryer. The drum dryer used for the drying operation can be any known single-drum or double-drum drum dryer, preferably a double-drum drum dryer. As far as the operating conditions are concerned, there are no particular restrictions as long as acceptable water-soluble porous maltodextrin or dextrin is obtained. Although the usual temperature, pressure and number of revolutions can be used, the preferred drum internal pressure is 300-600 kPa, the temperature is 140-170° C., and the drum number of revolutions is 0.8-1.33 rpm. Generally, the higher the steam temperature in the drum, the more fluffy water-soluble porous maltodextrin or dextrin is obtained. Since too high a temperature may cause the powder to burn on the wall, it is recommended to appropriately select the drying conditions within the above range.
[0098] From the perspectives of ease of impregnation, workability, and cost, the bulk density of the water-soluble porous powder is preferably 0.10 to 0.25 g / cm 3 , more preferably 0.14 to 0.20 g / cm 3 .
[0099] The bulk density (or volume specific gravity) is determined by the following method (the same below). A fully dried measuring cylinder is statically filled with 10 g of the water-soluble porous powder to be measured. The volume (ml) of the powder is measured by the scale of the measuring cylinder. This operation is repeated 10 times. The average volume A (ml) is calculated from the measured volumes, and the bulk density is calculated according to the following equation.
[0100] Bulk density (g / cm 3 )=10 / A
[0101] In the cumulative molecular weight distribution of the water-soluble porous powder obtained by GPC analysis, the cumulative value of the concentration fraction of a molecular weight of 10,000 (i.e., the ratio of the peak area in the range of molecular weights below 10,000 relative to the total peak area in the differential molecular weight distribution obtained by GPC analysis) is preferably 30 to 90%, more preferably 45 to 85%, from the perspective of solubility and reduced exudation.
[0102] The determination of cumulative molecular weight distribution and differential molecular weight distribution is carried out as follows: the test solution is injected into a high performance liquid chromatography device (or GPC) using a size exclusion column, the dissolution time is measured, and the molecular weight is calculated based on the calibration curve of the standard solution. From these data, the cumulative value of the concentration fraction of the molecular weight 10000 in the cumulative molecular weight distribution can be determined. For example, according to the use of a GPC analyzer (Shodex GPC-101, manufactured by Showa Denko K.K.), a detector (differential refractometer RI-71S (manufactured by Showa Denko K.K.), a column (two TSKgel GMPW XL , φ7.8mm×300mm connected (Tosoh Corporation)) to analyze the cumulative molecular weight distribution of the water-soluble porous powder, and determine the cumulative value of the concentration fraction with a molecular weight of 10000 (the same below).
[0103] The dextrose equivalent (DE) of the water-soluble porous powder (particularly water-soluble porous maltodextrin or water-soluble porous dextrin) is preferably 2 to 18, more preferably 6 to 16, and even more preferably 9 to 15 from the viewpoint of solubility and reduction of bleeding.
[0104] As used herein, "dextrose equivalent" (DE) gives a percentage index of the degree of decomposition (or saccharification rate) of starch degradation products. It is an analytical value by a modified Somogyi method, and the reducing sugar in the sample is expressed as glucose (or D-glucose) by the following formula, and its percentage is calculated based on the solid (the same below).
[0105] DE = [(weight of direct reducing sugar (expressed as glucose)) / (weight of solids)] × 100
[0106] The maximum value of DE is 100, which means that all the solid components obtained from starch hydrolysis are glucose. When starch is completely decomposed, the decomposition product is 100% glucose, indicating a DE of 100. The smaller the DE, the lower the degree of decomposition.
[0107] The water-soluble porous powder used herein is not particularly limited as long as it satisfies the above characteristics. Commercially available products can be used, such as Pineflow (Matsuya Chemical Industry Co., Ltd.), which is a porous starch degradation product or porous dextrin, and Oil Q No. 50 (Nippon Chemical Co., Ltd.), which is a porous modified starch.
[0108] The method of impregnating the water-soluble porous powder with the PEG derivative is not particularly limited. Any known method of impregnating the powder with a liquid can be used. An exemplary method includes putting the water-soluble porous powder into the jacket of a compact stirring granulator, rotating the scraper and the chopper at the number of revolutions of the general granulation conditions, and dripping the PEG derivative into the jacket. When the PEG derivative is solid or semi-solid at room temperature, the PEG derivative is heated and melted to a liquid state before the PEG derivative is added for impregnation. In this case, the jacket is preferably controlled at a temperature near the melting point of the PEG derivative. Any known powder mixer can be used, such as a stirring granulator, a V-type mixer, a ribbon mixer, a Nota mixer, and a super mixer.
[0109] Preferably, the powder prepared by impregnating the water-soluble porous powder with the PEG derivative is then classified through a sieve with a mesh size of 300 μm, and the portion below the sieve is used as a powdery additive for a hydraulic composition.
[0110] The amount of the PEG derivative impregnated in the water-soluble porous powder can be determined to prevent the powdered additive from becoming sticky due to an excessive amount of the PEG derivative impregnated. Specifically, the weight ratio of the water-soluble porous powder to the PEG derivative is preferably 1.5 / 1 to 3.3 / 1, more preferably 2.0 / 1 to 2.5 / 1. Excessive PEG derivatives may make the powdered additive sticky and deteriorate the fluidity of the powder. Excessive water-soluble porous powder may cause a delay in the setting of the hydraulic composition and may cause seepage.
[0111] In the powdered additive, the weight ratio of the PEG derivative to the water-soluble porous powder is preferably 23.3:76.7 to 40:60, and more preferably 28.6:71.4 to 33.3:66.7, from the viewpoint of powder fluidity and reduction of bleeding due to delayed coagulation.
[0112] The average particle size of the water-soluble porous powder before impregnation with the PEG derivative, obtained by dry laser method, is preferably 10 to 230 μm, more preferably 10 to 150 μm, from the aspect of reduced fluidity of the hydraulic composition due to poor dissolution of the powdered additive. The volume ratio of particles with a particle size of 300 μm or more is preferably 0 to 10%, more preferably 0 to 5%. If the volume ratio of particles with a particle size of 300 μm or more exceeds 10%, it is preferred to classify the powder with a sieve with a mesh size of 300 μm and use the undersize fraction.
[0113] The average particle size of the powdery additive, i.e., the water-soluble porous powder impregnated with the PEG derivative, obtained by dry laser method is preferably 40 to 280 μm, more preferably 50 to 200 μm, and even more preferably 60 to 150 μm, from the viewpoint of decreased fluidity of the hydraulic composition due to poor dissolution of the powdery additive. The volume ratio of particles having a particle size of 300 μm or more is preferably 0 to 10%, and more preferably 0 to 3%.
[0114] The average particle size (D50 or median diameter) of the water-soluble porous powder and powdered additive and the volume ratio of particles with a particle size of 300 μm or more are determined by the following dry laser diffraction method: using the Master Sizer 3000 manufactured by Malvern Panalytical PLC of the United Kingdom or the HELOS device manufactured by Sympatec GmbH of Germany, the powder sample is sprayed with compressed air, irradiated with laser radiation, the diffraction intensity is measured, and the volume-based average particle size (the same below) is calculated accordingly.
[0115] When the powdery additive is formulated into the hydraulic composition, the additive may be mixed with the water-soluble cellulose ether to form a powdery thickener (described later) and mixed into the thickener. Alternatively, the powdery additive and the water-soluble cellulose ether may be formulated separately.
[0116] <Powdered Thickener>
[0117] Another embodiment of the present invention is a powdered thickener for a hydraulic composition, comprising the powdered additive defined above and a water-soluble cellulose ether.
[0118] The water-soluble cellulose ether used in this article is nonionic. Examples thereof include alkyl celluloses such as methyl cellulose; hydroxyalkyl celluloses such as hydroxyethyl cellulose and hydroxypropyl cellulose; and hydroxyalkyl alkyl celluloses such as hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose and hydroxyethyl ethyl cellulose. Depending on the specific purpose, the water-soluble cellulose ether can be used alone or in combination of two or more.
[0119] Among the alkylcelluloses, the DS of the methoxyl group of methylcellulose (MC) is preferably 1.00 to 2.20, more preferably 1.20 to 2.00.
[0120] Among hydroxyalkyl celluloses, the MS of the hydroxyethoxy group of hydroxyethyl cellulose (HEC) is preferably 0.30 to 3.00, and more preferably 0.50 to 2.80. The MS of the hydroxypropoxy group of hydroxypropyl cellulose (HPC) is preferably 0.30 to 3.30, and more preferably 0.50 to 3.00.
[0121] Among the hydroxyalkyl alkyl celluloses, the DS of the methoxyl groups of hydroxypropyl methyl cellulose (HPMC) is preferably 1.00 to 2.20, more preferably 1.30 to 1.90, and the MS of the hydroxypropoxyl groups is preferably 0.10 to 0.60, more preferably 0.10 to 0.50. The DS of the methoxyl groups of hydroxyethyl methyl cellulose (HEMC) is preferably 1.00 to 2.20, more preferably 1.30 to 1.90, and the MS of the hydroxyethoxyl groups is preferably 0.10 to 0.60, more preferably 0.20 to 0.40. The DS of the ethoxyl groups of hydroxyethyl ethyl cellulose (HEEC) is preferably 1.00 to 2.20, more preferably 1.20 to 2.00, and the MS of the hydroxyethoxyl groups is preferably 0.05 to 0.60, more preferably 0.10 to 0.50.
[0122] It should be noted that the degree of substitution (DS) refers to the average number of alkoxy groups per unit of anhydrous glucose. The molar substitution (MS) refers to the average number of moles of hydroxyalkoxy groups per mole of anhydrous glucose. The DS of alkoxy groups and the MS of hydroxyalkoxy groups in alkylcellulose, hydroxyalkylcellulose, and hydroxyalkylalkylcellulose are determined by converting the values that can be measured by analysis of the DS of hydroxypropylmethylcellulose (hydroxypropyl methylcellulose) described in the Japanese Pharmacopoeia (18th edition) (the same below).
[0123] From the perspective of imparting a desired viscosity to the hydraulic composition, the viscosity of a 2 wt % aqueous solution of a water-soluble cellulose ether at 20° C. is preferably 15 to 450,000 mPa·s, more preferably 50 to 370,000 mPa·s, and even more preferably 80 to 350,000 mPa·s. The viscosity of a 2 wt % aqueous solution of a water-soluble cellulose ether at 20° C. is measured using a single cylinder type rotational viscometer in accordance with the viscosity measurement method of the general test method described in the Japanese Pharmacopoeia (18th edition) when the viscosity is 600 mPa·s or more (hereinafter the same). When the viscosity is less than 600 mPa·s, it is measured using an Ubbelohde viscometer in accordance with the capillary viscometer method of the viscosity measurement method of the general test method described in the Japanese Pharmacopoeia (18th edition) (hereinafter the same).
[0124] In the case of a concrete composition with low fluidity such as ordinary concrete, cellulose ethers with low molecular weight or low viscosity are preferred from the perspective of reduced fluidity. In the case of a high-fluidity concrete composition that does not experience a phenomenon of reduced fluidity, cellulose ethers with high molecular weight or high viscosity are preferred from the perspective of cost. Specifically, for use in ordinary concrete compositions, the viscosity of a 2 wt % aqueous solution of cellulose ether at 20° C. is preferably 15 to 80,000 mPa·s, more preferably 50 to 50,000 mPa·s, and even more preferably 80 to 35,000 mPa·s. For use in high-fluidity concrete compositions, the viscosity of a 2 wt % aqueous solution of cellulose ether at 20° C. is preferably 50,000 to 450,000 mPa·s, more preferably 60,000 to 370,000 mPa·s, and even more preferably 70,000 to 350,000 mPa·s.
[0125] Among water-soluble cellulose ethers, hydroxyalkyl alkyl celluloses such as hydroxypropyl methyl cellulose (HPMC) and hydroxyethyl methyl cellulose (HEMC) are preferred from the viewpoint of satisfying both fluidity of the hydraulic composition and reduction of bleeding. Commercially available cellulose ethers or cellulose ethers produced by known methods can be used.
[0126] (Other ingredients)
[0127] In addition to the PEG derivative, the water-soluble porous powder, and the water-soluble cellulose ether, the powdered thickener may also contain other ingredients such as a water repellent, a gum, and a defoamer. The other ingredients may be introduced as contained in the hydraulic composition described later. In particular, when the other ingredients are liquids, they are preferably used as solutions or dispersions in water. Examples and addition amounts of defoamers are described below in conjunction with the hydraulic composition.
[0128] [Water repellent]
[0129] The water repellent used in this article is a substance that can increase the contact angle with water to impart water repellency. As long as it is a water repellent commonly used in the previous hydraulic composition, there is no particular restriction. Examples include hydrocarbons such as liquid paraffin, squalane, paraffin, and vaseline; waxes such as beeswax, jojoba oil, and carnauba wax; triglycerides such as triisostearate and tricaprylin; ester oils such as myristyl isocetyl and palmitic acid cetyl; higher alcohols such as cetyl alcohol and stearyl alcohol; vegetable oils such as olive oil and castor oil; fatty acids such as stearic acid; and fatty acid salts such as calcium stearate, sodium stearate, magnesium stearate, calcium isostearate, sodium isostearate, and magnesium isostearate. In particular, from the aspect of reducing the amount of addition, fatty acid salts are preferred, and calcium stearate is more preferred. For example, calcium stearate is commercially available from Fujifilm and Koku Pure Chemical Industries, Ltd.
[0130] From the viewpoint of handling, the water repellent is preferably added in the form of powder.
[0131] When used, the amount of the water repellent to be added to the powdered thickener is preferably 0.01 to 30% by weight, more preferably 1.8 to 20% by weight. When the thickener is added to a hydraulic composition (specifically, a concrete composition), from the perspective of imparting water repellency, the amount of the water repellent to be added to the powdered thickener is preferably 0.01 to 30% by weight, more preferably 1.8 to 20% by weight. 3 The amount of water repellent added to the hydraulic composition is preferably 0.05 to 200 g / m 3 , more preferably 10 to 100 g / m 3 .
[0132] [gum]
[0133] The gum used herein is not particularly limited as long as it is a substance used in the conventional hydraulic composition. Among them, diutan gum, welan gum, xanthan gum and gellan gum are preferred from the aspects of both the fluidity of the hydraulic composition and the reduction of exudation. The gum can be used alone or in combination.
[0134] Diutan gum is composed of D-glucose, D-glucuronic acid, D-glucose and L-rhamnose and 2 sugar units of L-rhamnose, and is commercially available from CP Kelco under the trade name KELCO-CRETE-DG-F, for example. Welan gum is a structure in which L-rhamnose or L-mannose side chains are bound to a backbone composed of D-glucose, D-glucuronic acid and L-rhamnose in a ratio of 2:2:1, and is commercially available from CP Kelco under the trade name CP KELCO K1A-96, for example. Xanthan gum, like cellulose, has a backbone of β-1,4-linked D-glucose, and a side chain composed of 2 mannoses and 1 glucuronic acid, and is commercially available from Sanjing Co., Ltd. under the trade name KELZAN, for example. Gellan gum is a heteropolysaccharide composed of four sugars, D-glucose, D-glucuronic acid and L-rhamnose, in a ratio of 2:1:1 as repeating units, and is commercially available from CP Kelco, for example, under the trade name KELCOGELAFT.
[0135] The gum may be added in the form of a powder or an aqueous solution. From the aspect of handling, it is preferably added in the form of a powder.
[0136] When used, the amount of gum added to the powdered thickener is preferably 0.01 to 4% by weight, more preferably 0.05 to 3% by weight. When the thickener is added to a hydraulic composition (specifically, a concrete composition), from the perspective of both fluidity and reduced bleeding, the amount of gum added to the hydraulic composition is preferably 0.01 to 4% by weight, more preferably 0.05 to 3% by weight. 3 ) The amount of gum added is preferably 0 to 100 g / m 3 , more preferably 0 to 30 g / m 3 .
[0137] In the powdered thickener, the amount of the PEG derivative is preferably 3 to 30% by weight, more preferably 5 to 28% by weight, and further preferably 7 to 27% by weight. The amount of the porous powder relative to the powdered thickener is preferably 6 to 60% by weight, more preferably 10 to 56% by weight, and further preferably 14 to 54% by weight. The weight ratio of the PEG derivative to the water-soluble porous powder is as described above, preferably 23.3:76.7 to 40:60, and more preferably 28.6:71.4 to 33.3:66.7. In other words, the weight ratio of the water-soluble porous powder to the PEG derivative is preferably 1.5 / 1 to 3.3 / 1, and more preferably 2.0 / 1 to 2.5 / 1.
[0138] The content of the water-soluble cellulose ether is preferably 20 to 90.9% by weight, more preferably 22 to 80% by weight, and further preferably 24 to 75% by weight. The total of the water-soluble cellulose ether, PEG derivative, water-soluble porous powder, and other components that may be added is 100% by weight.
[0139] When preparing the powdered thickener, a general mixing method for powders can be used. For example, a known powder mixer such as a stirring granulator, a V-type mixer, a ribbon mixer, a Nauta mixer, or a super mixer can be used. The powdered additive (i.e., the water-soluble porous powder impregnated with the PEG derivative), the water-soluble cellulose ether, and other ingredients that may be added are placed in a mixer and mixed and stirred at a standard rotation speed for tens of seconds to several minutes.
[0140] <Hydraulic composition>
[0141] In another aspect, the hydraulic composition provided by the present invention relates to the following three embodiments.
[0142] A hydraulic composition (i): comprising at least a powdery additive, a hydraulic substance (specifically, cement), and water;
[0143] A hydraulic composition (ii): comprising the hydraulic composition (i) and a water-soluble cellulose ether; and
[0144] Hydraulic composition (iii): It contains at least a powdery viscosity enhancer, a hydraulic substance (specifically, cement), and water.
[0145] Exemplary uses of hydraulic compositions include concrete compositions, mortar compositions, and grout compositions.
[0146] The concrete composition comprises fine aggregate (specifically, sand), coarse aggregate (specifically, gravel), and a water reducing agent, and a hydraulic composition (i), (ii) or (iii). Preferably, the concrete composition has a slump of 8 to 21 cm, more preferably 9 to 19 cm, as measured by the method of JIS A 1101, and a compressive strength of 18 to 45 N / mm2 at 28 days as measured by the method of JIS A 1108. 2 , more preferably 25 to 40 N / mm 2 .
[0147] Examples of concrete compositions include ordinary concrete, underwater concrete, blown-fill concrete, cold-season concrete, summer-season concrete, mass concrete, lightweight concrete, concrete subjected to seawater, short-fiber reinforced concrete, dam concrete, paving concrete, prestressed concrete, and the like.
[0148] The mortar composition comprises fine aggregate (specifically, sand) and a hydraulic composition (i), (ii) or (iii). Examples of the mortar include tiling mortar, repair mortar, self-leveling agent, and the like.
[0149] The grout composition is composed of the hydraulic composition (i), (ii) or (iii), and examples thereof include adhesives for tile-based inorganic building materials and grouting materials for filling gaps between components.
[0150] From the perspective of fluidity, seepage reduction and frost resistance, per cubic meter (m 3 ) in a hydraulic composition (specifically, a concrete composition), the amount of the powdered additive added to the hydraulic composition (i) or (ii), or the amount of the powdered thickener added to the hydraulic composition (iii), is preferably 0.025 to 10.0 kg / m 3 , more preferably 0.05 to 5.0 kg / m 3 .
[0151] From the perspective of fluidity, oozing reduction and frost resistance of hydraulic compositions, 3 The amount of the PEG derivative added to the hydraulic composition (specifically, the concrete composition) is preferably 10 to 300 g / m 3 , more preferably 10 to 150 g / m 3 .
[0152] Since the weight ratio of porous powder to PEG derivative is 1.5 to 3.3, 3 The amount of porous powder added to the hydraulic composition (specifically, the concrete composition) is preferably 15 to 990 g / m 3 , more preferably 15 to 495 g / m3 .
[0153] From the perspective of both fluidity and leakage reduction of the hydraulic composition, the volume per cubic meter (m 3 The amount of water-soluble cellulose ether added to the hydraulic composition (specifically, concrete composition) is preferably 10 to 1500 g / m 3 , more preferably 15 to 1000 g / m 3 .
[0154] Hydraulic material refers to cement and inorganic powder system mixed materials in the components matched when hydraulic composition is manufactured. Cement can be used alone or in combination with mixed materials, as long as the desired strength, durability and other properties can be obtained. Examples of cement include portland cement (e.g., ordinary portland cement, early strength portland cement, ultra early strength portland cement, medium heat portland cement), blended cement (e.g., blast furnace cement, silica cement, fly ash cement, etc.), special cement (e.g., alumina cement). Examples of mixed materials include slag, fly ash, silica fume, limestone powder.
[0155] When the hydraulic composition is a concrete composition, the amount of the hydraulic material added to the concrete composition is preferably 270 to 550 kg / m 3 When the hydraulic composition is a mortar composition, the amount of the hydraulic material added to the mortar composition is preferably 300 to 900 kg / m 3 When the hydraulic composition is a cement slurry composition, the amount of the hydraulic material added to the cement slurry composition is preferably 900 to 1600 kg / m 3 These amounts are preferred from the aspect of strength.
[0156] Examples of water include tap water, and "water other than tap water" as indicated in JIS A 5308. The unit amount of water in the concrete composition is preferably up to 185 kg / m 3 .
[0157] Taking segregation into consideration, the water / hydraulic material ratio in the hydraulic composition is preferably 30 to 70% by weight, more preferably 35 to 65% by weight.
[0158] The hydraulic composition may further comprise aggregate as required. Examples of suitable aggregates include fine aggregate and coarse aggregate. Examples of fine aggregate include river sand, mountain sand, land sand, crushed sand, silica sand. The particle size (maximum particle size) of fine aggregate is preferably up to 5 mm. Examples of coarse aggregate include river gravel, mountain gravel, land gravel, crushed stone, etc. The particle size (maximum particle size) of coarse aggregate is larger than the particle size of fine aggregate, preferably up to 40 mm, more preferably up to 25 mm.
[0159] When the hydraulic composition is a concrete composition, the content of fine aggregate is relative to m 3 The concrete composition is preferably 600 to 1100 kg, more preferably 700 to 1000 kg. When the hydraulic composition is a mortar composition, the content of the fine aggregate is 100 to 200 kg per m 3 The amount of the mortar is preferably 900 to 1600 kg, more preferably 1000 to 1400 kg.
[0160] When the hydraulic composition is a concrete composition, the content of the coarse aggregate is relative to 3 The concrete composition is preferably 600 to 1000 kg, more preferably 650 to 900 kg.
[0161] When the hydraulic composition is a concrete composition, in order to maintain fluidity or sufficient strength, the ratio of the fine aggregate defined below to the total volume of the aggregate is preferably 30 to 65% by volume, more preferably 35 to 60% by volume, and even more preferably 40 to 55% by volume.
[0162] Fine aggregate ratio (vol%) = (volume of fine aggregate) / (volume of fine aggregate+volume of coarse aggregate)×100.
[0163] Mixed materials may be added to the hydraulic composition as needed to suppress heat generation during hardening and improve durability after hardening. Suitable mixed materials include blast furnace slag and fly ash.
[0164] In addition, a water reducing agent can be added to the hydraulic composition as required to maintain high fluidity with a small amount of water. Suitable water reducing agents include lignin, polycarboxylic acids and melamine-based agents. Examples of lignin include lignin sulfonates and derivatives thereof. Examples of polycarboxylic acids include polycarboxylic acid ethers, complexes of polycarboxylic acid ethers and crosslinked polymers, complexes of polycarboxylic acid ethers and oriented polymers, complexes of polycarboxylic acid ethers and highly modified polymers, polyether carboxylic acid-based polymers, maleic acid copolymers, maleate copolymers, maleic acid derivative copolymers, polyethers containing carboxyl groups, polypolymers containing polycarboxylic acid groups with terminal sulfone groups, polycarboxylic acid-based graft copolymers, polycarboxylic acid-based compounds, and polycarboxylic acid ether-based polymers. Examples of melamine include melamine sulfonic acid formalin condensates, melamine sulfonate condensates, and melamine sulfonate polyol condensates.
[0165] per m 3 The amount of the water reducing agent in the hydraulic composition (specifically, the concrete composition) is relative to the amount of the water reducing agent per m 3 The unit cement amount is preferably 0.5 to 2.5 weight %, more preferably 0.5 to 1 weight %. In the case where the desired fluidity is not obtained, two or more water reducing agents can be used. If necessary, a liquid water reducing agent can be used.
[0166] Air entraining (AE) agents may be added to the hydraulic composition as required to provide the required amount of air and to make the hydraulic composition durable. Suitable AE agents include anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, and rosin-based surfactants. Examples of anionic surfactants include resinate type, carboxylic acid type, sulfate type, sulfonic acid type, and phosphate type surfactants. Examples of cationic surfactants include amine salt type, primary amine salt type, secondary amine salt type, tertiary amine salt type, and quaternary ammonium salt type surfactants. Examples of nonionic surfactants include ester type, ester-ether type, ether type, and alkanolamide type surfactants. Examples of amphoteric surfactants include amino acid type and sulfobetaine type surfactants. Examples of rosin-based surfactants include abietic acid, neoabietic acid, palustric acid, pimaric acid, isopimaric acid, and dehydroabietic acid.
[0167] The amount of AE agent used per cubic meter of hydraulic composition (particularly, concrete composition) is relative to the amount of AE agent used per cubic meter of hydraulic composition (particularly, concrete composition). 3 The unit cement amount is preferably 0.0001 to 0.050% by weight, more preferably 0.0001 to 0.01% by weight.
[0168] A defoamer may be added to the hydraulic composition (specifically, concrete composition) or powdered tackifier as needed to obtain the strength of the hydraulic composition. From the aspect of defoaming performance, suitable defoamers include oxyalkylene-based, silicone-based, alcohol-based, and fatty acid ester-based defoamers. In particular, from the aspect of frost resistance, oxyalkylene-based defoamers are preferred.
[0169] Examples of oxyalkylene defoaming agents include polyoxyalkylenes such as (poly)oxyethylene (poly)oxypropylene adducts; (poly)oxyalkylene alkyl ethers such as diethylene glycol heptyl ether, polyoxyethylene oleyl ether, polyoxypropylene butyl ether, polyoxyethylene polyoxypropylene 2-ethylhexyl ether, and oxyethylene propylene adducts with higher alcohols having 8 or more carbon atoms or secondary alcohols having 12 to 14 carbon atoms; (poly)oxyalkylene (alkyl) aryl ethers such as polyoxypropylene phenyl ether and polyoxyethylene nonylphenyl ether; oxyalkylenes and acetylene alcohols such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and 3-methyl-1-butyn-3-ol; (poly)oxyalkylene fatty acid esters such as diethylene glycol oleate, diethylene glycol laurate, and ethylene glycol distearate; (poly)oxyalkylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate and polyoxyethylene sorbitan trioleate; (poly)oxyalkylene alkyl (aryl) ether sulfates such as sodium polyoxypropylene methyl ether sulfate and sodium polyoxyethylene dodecylphenol ether sulfate; (poly)oxyalkylene alkyl phosphates such as (poly)oxyethylene stearic acid phosphate; (poly)oxyalkylene alkylamines such as polyoxyethylene laurylamine; and polyoxyalkylene amides.
[0170] Examples of the silicone-based defoaming agent include dimethyl silicone oil, silicone paste, silicone emulsion, organo-modified polysiloxane (ie, polyorganosiloxane such as dimethyl polysiloxane), and fluorosilicone oil.
[0171] Examples of the alcohol-based defoaming agent include octanol, 2-ethylhexanol, hexadecanol, acetylene alcohols, and glycols.
[0172] Examples of the fatty acid ester-based antifoaming agent include glyceryl monoricinoleate, alkenyl succinic acid derivatives, sorbitan monolaurate, sorbitan trioleate, and natural waxes.
[0173] When used, the amount of the defoamer added is preferably 0 to 16% by weight, more preferably 0.002 to 10% by weight relative to the water reducing agent. In another embodiment, the defoamer can be added to the powdered tackifier, and the content of the defoamer is preferably 0.01 to 10% by weight, more preferably 0.05 to 8% by weight relative to the powdered tackifier.
[0174] A setting accelerator such as calcium chloride, lithium chloride or calcium formate and a setting retarder such as sodium citrate or sodium gluconate may be added to the hydraulic composition as needed to control the physical properties of the hydraulic composition (fresh concrete, fresh mortar or fresh cement paste) just after mixing.
[0175] The amount of coagulation retarder used is relative to the amount of 3 The unit cement amount is preferably 0.3 to 1.2% by weight.
[0176] Furthermore, a hauyne-based or lime-based expansive material may be added to the hydraulic composition as necessary to prevent cracking caused by shrinkage and air entrainment during setting and drying, and cracking caused by thermal stress due to water and reaction heat in cement.
[0177] About the air void amount in hydraulic composition, in order to make the freezing resistance good, preferably reduce the large bubbles with a diameter exceeding 500 μm and below 2000 μm, increase the small bubbles with a diameter exceeding 50 μm and below 500 μm. As the evaluation index of the size of the bubble, the bubble spacing coefficient is used as an index. When it is believed that the bubble spacing coefficient is less than 250 μm, the freezing resistance becomes good. The bubble spacing coefficient can be measured by the air void analysis method described in the embodiment. When evaluating the bubble spacing coefficient, due to the increase or decrease of the air volume, the bubble spacing coefficient also changes, so it is preferred that the air volume of the concrete composition or the mortar composition is evaluated uniformly.
[0178] <Method for producing hydraulic composition>
[0179] The method for producing a hydraulic composition of the present invention comprises at least the step of mixing the components of the hydraulic composition, and further comprises the step of adding a powdered additive as defined herein or a powdered viscosity enhancer as defined herein to the step of mixing the components of the hydraulic composition. Specifically, the method of the present invention relates to the following three embodiments.
[0180] A method (I) for producing a hydraulic composition, which is a method for producing a hydraulic composition (i) comprising a hydraulic substance, water, and a polyethylene glycol derivative, the method comprising the step of adding a powdered additive during the step of mixing the components of the hydraulic composition.
[0181] A method for producing a hydraulic composition (II) comprising a hydraulic substance, water, a water-soluble cellulose ether, and a polyethylene glycol derivative, the method comprising the step of adding a powdered additive during the step of mixing the components of the hydraulic composition.
[0182] A method for producing a hydraulic composition (III) comprising a hydraulic substance, water, a water-soluble cellulose ether, and a polyethylene glycol derivative, the method comprising the step of adding a powdered thickener during the step of mixing the components of the hydraulic composition.
[0183] In the methods (I), (II) and (III) for producing a hydraulic composition of the present invention, the hydraulic composition is preferably a concrete composition further comprising a fine aggregate, a coarse aggregate and a water reducing agent, and the slump of the concrete composition measured by the method of JIS A 1101 is 8 to 21 cm, and the compressive strength of the concrete composition measured by the method of JIS A 1108 at 28 days is 18 to 45 N / mm 2 .
[0184] Also preferably, the step of mixing the ingredients of the hydraulic composition comprises dry mixing all the powdered ingredients except the liquid materials such as water, adding water and an optional liquid water reducing agent during dry mixing, and mixing the ingredients, and adding the powdered additive or powdered viscosity increasing agent to the dry mixing step.
[0185] For example, a powdered additive or powdered tackifier, a hydraulic material and optional aggregate (fine aggregate and coarse aggregate), and then an optional defoamer are placed in a forced twin-screw mixer, followed by dry mixing. Then, water is added for dry mixing to obtain a hydraulic composition (i) or (iii). Alternatively, a powdered additive, a water-soluble cellulose ether, a hydraulic material and optional aggregate (fine aggregate and coarse aggregate), and then an optional defoamer are placed in a forced twin-screw mixer, followed by dry mixing. Then, water is added for dry mixing to obtain a hydraulic composition (ii). The powdered additive or powdered tackifier used in these methods is in powdered form, so it is easy to handle, which ensures that hydraulic compositions (i), (ii) and (iii) are easily manufactured.
[0186] As described above, a powdery additive, a powdery thickener, and a hydraulic composition containing the additive or thickener are obtained that can improve the fluidity, bleeding, and frost damage resistance of a hydraulic composition. Example
[0187] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following examples.
[0188] I) Preparation of powdered additives and powdered tackifiers
[0189] The following ingredients were used to prepare a powdered additive and a powdered viscosity enhancing agent for a hydraulic composition.
[0190] <Ingredients>
[0191] (1) PEG derivatives: Details are shown in Table 1.
[0192] <Calculation of IOB value>
[0193] The IOB (Inorganic Organic Balance) value of the PEG derivative used was determined as follows.
[0194] The organic value (OV) and inorganic value (IV) of the compound of interest are determined by adding the predetermined values of the groups or sites on the compound in the entire molecule. For the predetermined values of each group or site of each compound, refer to "Methods for Emulsification Formulation Design Pages 2-9", Nippon Emulsion Co., Ltd., Emulsification Formulation Design of Organic Concept Diagram (Non-Patent Document 1), Page 2, Figure 2 "Calculation Method Example" and Appendix 1 "Inorganic Group, Organic Group and Organic / Inorganic Group Table".
[0195] Substitute the obtained IV and OV into the following formula to calculate the IOB value.
[0196] IOB value = IV / OV
[0197] A calculation example is shown below.
[0198] A1: In polyethylene glycol monostearate (C 17 H 35 COO(C2H4O) 10 H), by transforming -C2H4- in the first repeating unit (C2H4O) and -COO- bound thereto into (-COOR)-OCH2CH2 and COO(C2H4O) 10 -O-(C2H4O) in H 10-1 H transforms to -(OCH2CH2) 10-1 -OH, determine the structural formula such as "C 17 H 35 CO·OCH2CH2(OCH2CH2) 10-1 -OH".
[0199] OV = 38 (number of C) × 20 (OV of C) = 760
[0200] IV = 60 (IV of -COOR) + 75 (IV of -OCH2CH2) × 9 (number of -OCH2CH2) + 100 (IV of -OH) = 835
[0201] From the above values, we obtain an IOB value of 835 / 760≈1.10.
[0202] <Measurement of Mw>
[0203] Mw was measured as the weight average molecular weight by GPC analysis using a GPC system HLC-8220GPC (manufactured by Tosoh Corporation). The GPC system had a detector (differential refractometer RI-71S, manufactured by Showa Denko K.K.), columns (TSK-gel G5000HxL (7.8×300 mm)×1, G4000HxL (7.8×300 mm)×1, G3000HxL (7.8×300 mm)×1, G2000HxL (7.8×300 mm)×1 (manufactured by Tosoh Corporation)), tetrahydrofuran (THF) as a developing solvent, and the calculation was performed relative to a polystyrene standard.
[0204] By sampling an aliquot of about 0.01g of the PEG derivative, and adding about 10mL of THF to dissolve the PEG derivative, a test solution is prepared. Each (100 μL) of the test solution and a polystyrene standard (manufactured by Tosoh Corporation) is injected into the GPC system. THF is used for the mobile phase, and the column temperature is 40°C at a flow rate of 1.0mL / min. The results thus obtained are analyzed using a 480II data station GPC program (System Instruments Co., Ltd.). The molecular weight is calculated by AUTO fitting using the extrapolation curve method (once). The molecular weight is estimated using a calibration curve drawn based on the dissolution time and molecular weight of the polystyrene solution of the molecular weight standard.
[0205] (2) Water-soluble porous powder: Details are shown in Table 2.
[0206] <Cumulative value of the concentration fraction of molecular weight 10000 in the cumulative molecular weight distribution (%)>
[0207] How to determine the cumulative value of the concentration fraction (%) of a molecular weight of 10000 in the cumulative molecular weight distribution of the water-soluble porous powder used herein is shown.
[0208] The molecular weight distribution of the water-soluble porous fraction can be determined by injecting the test solution into a high performance liquid chromatography device (GPC system) with a size exclusion column, measuring the dissolution time, and calculating relative to the calibration curve of the standard solution. Based on the data, the cumulative value of the concentration fraction (%) of the molecular weight 10000 in the cumulative molecular weight distribution of the water-soluble porous powder can be determined. Specifically, a GPC analyzer (Shodex GPC-101, manufactured by Showa Denko K.K.), a detector (differential refractometer RI-71S (manufactured by Showa Denko K.K.)), a column (two TSKgel GMPW XL , φ7.8 mm×300 mm connection (manufactured by Tosoh Corporation)), and the measurement was performed as follows.
[0209] By sampling about 0.01g of water-soluble porous powder, it is added to about 100mL of 0.1mol / L sodium nitrate solution, the solution is allowed to stand overnight at room temperature, and the solution is filtered with a membrane filter with a pore size of 0.45μm, thereby preparing a test solution. Each 100μL of the test solution and the standard pullulan solution (Showa Denko Co., Ltd.) is injected into the GPC system. By using a 0.1mol / L sodium nitrate solution for the mobile phase, it is measured at a flow rate of 1.0mL / min and a column temperature of 40°C. The results thus obtained are analyzed using the 480II data station GPC program (System Instruments Co., Ltd.). In the peak curve thus obtained, a baseline is drawn, and after specifying the peak, the dissolution time is converted to a molecular weight using a calibration curve, the peak area is determined, and the concentration fraction of each dissolution time is calculated. By accumulating the concentration fractions in sequence, and drawing the molecular weight (logarithmic value) on the horizontal axis and the cumulative value of the concentration fraction on the vertical axis, the integral molecular weight distribution is completed. From the integrated molecular weight distribution, the cumulative value of the concentration fraction at a molecular weight of 10000 was obtained. This was performed using a calibration curve prepared based on the dissolution time and molecular weight of a standard pullulan solution.
[0210] <Bulk density>
[0211] The bulk density or bulk specific gravity is calculated as follows. Statically fill 10 g of the water-soluble porous powder to be measured into a fully dry measuring cylinder, and measure the volume (ml) of the powder from the scale of the measuring cylinder. Repeat this operation 10 times. Calculate the average volume A (ml) from the measured volumes. Substitute A into the equation: Bulk density (g / cm 3 )=10 / A, calculate the bulk density.
[0212] (3) Hydroxyalkyl alkyl cellulose (CE): Details are shown in Table 3.
[0213] (4) Calcium stearate (StCa): reagent (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0214] (5) Defoamer I (DF-1): Polyether defoamer I (silica impregnated with defoamer)
[0215] [Table 1]
[0216]
[0217] (PEG-10)C 17 H 35 COO(C2H4O) 10 H(PEG-20)C 17 H 35 COO(C2H4O) 20 H(PEG-6)iso-C 17 H35 COO(C2H4O)6H
[0218] (PEG-10BG)
[0219] [Table 2]
[0220]
[0221] [Table 3]
[0222]
[0223] (Preparation of powdered additive (Example 1) and powdered thickener (Examples 2 to 15))
[0224] The ingredients shown in Table 4A are combined to prepare a powdered additive for a hydraulic composition. Specifically, a vertical granulator FM-VG-05 (Powrex Corp.) is used as a compact stirring granulator. The water-soluble porous powder is weighed based on the mixing ratio (wt%) shown in Table 4A in such a way that the total weight of the water-soluble porous powder and the PEG derivative can be 200 g. The water-soluble porous powder is put into the jacket of the vertical granulator. The temperature in the jacket is adjusted to the melting point ±2°C of the PEG derivative when the PEG derivative is solid at room temperature (20°C (the same below)), and is adjusted to 20±2°C when the PEG derivative is liquid at room temperature. Then, the PEG derivative is weighed in a specified amount (the total weight of the water-soluble porous powder and the PEG derivative can be 200 g). In particular, when the PEG derivative is solid at room temperature, it is dissolved in a hot water bath before weighing. The PEG derivative is put into the funnel of the vertical granulator. The blade of the vertical granulator was set to 450 rpm, the chopper was set to 3000 rpm, and stirring was started. The valve of the funnel was opened, and the PEG derivative was added over 30 seconds. Furthermore, stirring was continued for 2.5 minutes. After the stirring was completed, the obtained powder was classified through a sieve with a mesh size of 300 μm to obtain a powdered additive.
[0225] A water-soluble cellulose ether is further added to the powdered additive to provide the mixing ratio (wt%) shown in Table 4A. A vertical granulator is used to mix for 30 seconds at the same rotation speed (blade 450 rpm, chopper 3000 rpm) as when the powdered additive is prepared to obtain a powdered thickener (thickener No. 2 to 12) (Examples 2 to 12). It should be noted that the PEG derivative in the powdered thickener of Example 2 (thickener No. 2) is changed to PEG-20 stearate to obtain Example 11 (thickener No. 11), and the PEG derivative in the powdered thickener of Example 2 (thickener No. 2) is changed to PEG-10BG isostearate to obtain Example 12 (thickener No. 12). Example 1 is a powdered additive (Additive No. 1) obtained by combining PEG-10 stearate and Pineflow, to which no water-soluble cellulose ether is added.
[0226] In addition, water-soluble cellulose ether and calcium stearate, or water-soluble cellulose ether and defoamer I were added to the powdered additive in the prescribed mixing ratio (wt%) shown in Table 4A. The mixture was mixed for 30 seconds using a vertical granulator at the same rotation speed (blade 450 rpm, chopper 3000 rpm) as in the preparation of the powdered additive to obtain a powdered thickener (thickener Nos. 13 to 15 of Examples 13 to 15).
[0227] The powdered additive of Example 1 (Additive No. 1) and the powdered thickeners of Examples 2 to 15 (Thickeners No. 2 to 15) are all powders that are not sticky and are easy to handle.
[0228] Comparative Example 1 (Comparative Additive No. 1) is composed of Defoamer I. Hydroxypropyl methylcellulose (HPMC-1) and Defoamer I were mixed for 30 seconds using a vertical granulator at the same rotation speed as in the preparation of the powdered additive to obtain Comparative Example 2 (Comparative Thickener No. 1).
[0229] II) Preparation of hydraulic composition (concrete composition)
[0230] Using the following ingredients, hydraulic compositions (concrete compositions) as shown in Table 4B were prepared.
[0231] <Ingredients>
[0232] (1) Powdered additives or powdered thickeners: Additive No. 1, Thickeners No. 2 to 15, Comparative Additive No. 1, Comparative Thickener No. 1 (see Table 4A)
[0233] (2) Water (W): tap water
[0234] (3) Cement (C): Ordinary Portland cement (density: 3.16 g / cm3 , Pacific Cement Co., Ltd.)
[0235] (4) AE water reducer (WR): lignin sulfonic acid (Master Pozzolith No. 70, manufactured by BASF Pozzolith, used in a 4-fold dilution)
[0236] (5) High-performance AE water reducer (superplasticizer SP): polycarboxylic acid copolymer (Chupole HP-11, manufactured by Takemoto Oil & Fats Co., Ltd.) (C x 0.85%)
[0237] (6) AE agent: resin acid salt type anionic surfactant (AE-300, manufactured by Takemoto Oil & Fats Co., Ltd., used in a 100-fold dilution: 1A = C x 0.001%)
[0238] (7) Fine aggregate (S): Land sand (produced in Shinano River, surface dry density: 2.60 g / cm 3 , water absorption rate: 2.07%, coarse particle rate: 2.79, solid volume percentage: 66.3%)
[0239] (8) Coarse aggregate (G): crushed stone (20-5 mm, surface dry density: 2.69 g / cm 3 , water absorption rate: 1.35%, coarse particle rate: 6.55, solid volume percentage: 58.5%)
[0240] The concrete mix shown in Table 5 was used for the test, i.e., under the following conditions: water / cement ratio 55.0%, fine aggregate ratio 52.9%, water 175 kg / m 3 、Cement 318kg / m 3 , fine aggregate 931kg / m 3 , coarse aggregate 861kg / m 3 As a unit quantity.
[0241] A hydraulic composition (concrete composition) was prepared using the concrete formulation (additive ingredients) shown in Table 4B. In Table 4B, the amount of PEG derivative, water-soluble porous powder, water-soluble cellulose ether, calcium stearate and defoaming agent added as a powdery additive or powdery thickener was expressed as 100 g / m3 of the concrete composition. 3 ) in grams (i.e. g / m 3 ); the addition amount of AE water reducer and high-efficiency water reducer is the amount (C×%) relative to the wt% of cement (C); the addition amount of AE agent is the recorded amount (unit A: 1A amount of 0.001wt% relative to cement (C)).
[0242] In particular, the amount of AE agent added was adjusted to provide an air amount of 4.5±0.5%.
[0243] In Example 11, in order to adjust the slump to 13.0±1.0 cm, the addition amount of the AE water reducer was changed in the formulation of Example 1. In Example 12, in order to adjust the slump to 20.0±1.0 cm, in the formulation of Example 1, a high-performance AE water reducer was further added as a liquid material to change the addition amount of the AE water reducer.
[0244] The concrete composition is prepared in a 60L forced twin-screw mixer (WHQ-60A (co., Kitagawa Iron Works)). First, the powder material is added. That is, cement, fine aggregate, coarse aggregate, powdered additives or powdered thickeners (additive No. 1, thickener No. 2 to 15, comparative additive No. 1, comparative thickener No. 1) shown in Table 4A are added as powder materials, followed by dry mixing for 10 seconds. Then, the liquid material is added. That is, AE water reducer, AE agent and water are added as liquid materials. Then, mixing is performed for 90 seconds to obtain a concrete composition. The concrete composition mixed in each batch is 50 liters. The amount of water added at this stage is the total weight of the liquid materials other than the necessary weight of water minus the water.
[0245] [Table 4A]
[0246]
[0247] [Table 4B]
[0248]
[0249] [Table 5]
[0250]
[0251] *Fine aggregate ratio (vol%) = (fine aggregate volume) / [(fine aggregate volume) + (coarse aggregate volume)] × 100
[0252] The obtained concrete compositions were tested under the following conditions.
[0253] <Fresh properties>
[0254] (Concrete temperature)
[0255] The material temperature was adjusted in such a way that the temperature of the concrete composition reached 20±3° C. at the end of mixing.
[0256] The sensor of a digital thermometer (model SN3200II, Thermo Scientific Corporation) was inserted into the concrete composition to measure the concrete temperature. All the concrete compositions showed a temperature within the range of 20±3°C.
[0257] (Slump)
[0258] The test was conducted in accordance with JIS A1101.
[0259] (Air volume test)
[0260] The amount of air (volume %) was measured in accordance with JIS A 1128 for the concrete composition just prepared (immediately after mixing).
[0261] (Exudation rate)
[0262] The exudation rate was measured in accordance with JIS A 1123 for the concrete composition just prepared (immediately after mixing).
[0263] (Air Void Analyzer (AVA) test or Bubble Spacing Factor)
[0264] Use an air void analyzer ( Glycerin (manufactured by German Instruments) and water were mixed in advance at a weight ratio of glycerin / water = 83 / 17 to prepare an AVA measurement solution.
[0265] The mixed concrete composition is passed through a sieve with a mesh size of 5 mm to collect the mortar composition for evaluating the bubble spacing coefficient. 20 ml of the sample is taken in a special syringe, about 2000 ml of water is injected into the measurement column, the bubbles attached to the column wall are removed with a brush, and 250 ml of the AVA measurement solution is injected into the bottom of the column using a special device. After injection, a culture dish for bubble sampling is set near the water surface of the column and fixed to the measurement part. After injecting 20 ml of the mortar composition taken in the syringe into the bottom of the column, the mortar composition is stirred for 30 seconds to fully release the air introduced into the mortar in the liquid. The bubble spacing coefficient is determined by measuring the released bubbles over time.
[0266] In calculating the air bubble spacing factor, in addition to the air volume of fresh concrete, the volume occupied by aggregates 5 mm or larger (i.e., mortar volume percentage) and the volume occupied by paste (paste volume percentage) need to be subtracted from the total volume of the mortar composition. The mortar volume percentage and the paste volume percentage are calculated by the following equations (I) and (II).
[0267] Mortar volume percentage (%) = [(V B +V W +V S ) / 1000]×100 (I)
[0268] Paste volume percentage (%) = [(V B +V W ) / 1000]×100 (II)
[0269] VB :Volume of cement (=Unit weight of cement (kg) / Specific gravity of cement)
[0270] V W : The volume of liquid additives including water, AE agent and water reducing agent (same as the unit water volume)
[0271] V S : Volume of aggregate with a size of 5 mm or less (=unit amount of fine aggregate / specific gravity of fine aggregate)
[0272] (Ratio of bubbles in each bubble diameter range)
[0273] When the air void analyzer is started according to the above steps, automatic measurement begins. Large bubbles rise faster in the column and are trapped under the petri dish, while small bubbles rise slower in the column. The bubble ratio in each bubble diameter range is automatically calculated by measuring the weight of the petri dish over time.
[0274] (Air volume %)
[0275] The sum of the bubble ratios in each bubble diameter range is the air amount (volume %).
[0276] <Curing properties>
[0277] (Compression Strength)
[0278] The compressive strength test was conducted on 28-day-old concrete according to JIS A 1108. The sample size was 10 cm (diameter) x 20 cm. The average value of three samples was used as the compressive strength of each level for evaluation.
[0279] (Freeze-thaw test)
[0280] The freeze-thaw test was carried out according to the A method in JIS A 1148-2010. The relative dynamic elastic coefficient was measured up to a maximum of 300 cycles. The size of the sample was 100 mm × 100 mm × 400 mm long. The average value of the three samples was used as the relative dynamic elastic coefficient of each level for evaluation. When the relative dynamic elastic coefficient became less than 60% before 300 cycles, the test was terminated at that cycle.
[0281] The durability index was calculated according to the following formula using the relative dynamic elastic coefficient and rounded off to an integer. A durability index of 60 or more was judged to be excellent in frost damage resistance.
[0282] Durability index = P × N / M
[0283] P: Relative dynamic elastic coefficient at N cycles (%), N: The smaller number between the number of cycles at which the relative dynamic elastic coefficient reaches 60% and 300 cycles, M: 300 cycles)
[0284] The above test results are shown in Tables 6A and 6B.
[0285] [Table 6A]
[0286]
[0287] [Table 6B]
[0288]
[0289] The following conclusions were drawn from the above results: Examples 1 to 9 demonstrate that even if the viscosity, DS, and / or chemical structure of the water-soluble cellulose ether is changed, the hydraulic composition can be advantageously improved in terms of fluidity, exudation, and frost resistance by adding a powdered additive in the form of a water-soluble porous powder impregnated with a PEG derivative.
[0290] Examples 10 to 12, 14, and 15 demonstrate that when the structure of the PEG derivative is changed or a defoaming agent is added, the three factors of fluidity, bleeding, and frost damage resistance of the hydraulic composition (specifically, concrete composition) are advantageously improved.
[0291] Example 13 demonstrates that the addition of calcium stearate further improves the frost resistance while maintaining the fluidity and improvement of the seepage of the hydraulic composition (concrete composition).
[0292] In an embodiment, the powdered additive or powdered tackifier can be used in a powder form for easy handling.
[0293] In Comparative Example 1 using defoamer I (DF-1): a polyether-based defoamer I in the form of silica impregnated with only the defoamer component, and Comparative Example 2 combining defoamer I with a water-soluble cellulose ether (HPMC-1), although they can be used in powder form and are easy to handle, no improvement was found in the three factors of fluidity, bleeding, and frost damage resistance.
[0294] It should be noted that the present invention is not limited to the above-mentioned embodiments. The embodiments are merely exemplary, and any embodiments having substantially the same structure as the technical concept described in the following claims and having equivalent functions and results are included in the spirit and scope of the present invention.
Claims
1. A powdered additive for a hydraulic composition, comprising a water-soluble porous powder impregnated with a polyethylene glycol derivative, wherein the polyethylene glycol derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw of 300 to 2500 measured by gel permeation chromatography relative to a polystyrene standard, and the polyethylene glycol derivative has at least one RCOO (C2H4O) in the molecule n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
2. The additive according to claim 1, wherein The polyethylene glycol derivative is at least one of the compounds represented by the general formulae (A1) and (A2): RCOO-(C2H4O) n -H(A1)(RCOO-(C2H4O) n1 ) t R 1 ((OC2H4) n2 -OH) u (A2) Wherein, R and n are as defined above, R 1 A residue obtained by removing a hydroxyl group from a polyol having 2 to 5 hydroxyl groups, wherein the residue is a 2- to 5-valent C2-C5 straight-chain or branched hydrocarbon group, t and u are each an integer of 1 to 4, the sum of t and u is an integer of 2 to 5, n1 and n2 are each an integer greater than 0, and n1×t+n2×u is an integer of 3 to 30.
3. The additive according to claim 1 or 2, wherein The water-soluble porous powder is a water-soluble porous polysaccharide.
4. The additive according to claim 1 or 2, wherein The volume density of the water-soluble porous powder is 0.10-0.25 g / cm 3 .
5. The additive according to claim 1 or 2, wherein In the cumulative molecular weight distribution of the water-soluble porous powder measured by gel permeation chromatography, the cumulative value of the concentration fraction of a molecular weight of 10,000 is 30 to 90%.
6. The additive according to claim 1 or 2, wherein The dextrose equivalent (DE) of the water-soluble porous powder is 2-18.
7. The additive according to claim 1 or 2, wherein In the particle size distribution of the water-soluble porous body measured by a dry laser method, the average particle size of the water-soluble porous powder is 10 to 230 μm and the volume ratio of particles with a particle size of 300 μm or more is 0 to 10%.
8. The additive according to claim 1 or 2, wherein In the particle size distribution of the additive measured by a dry laser method, the average particle size of the additive is 40 to 280 μm, and the volume ratio of particles with a particle size of 300 μm or more is 0 to 10%.
9. A powdery thickener for a hydraulic composition, comprising the powdery additive according to any one of claims 1 to 8 and a water-soluble cellulose ether.
10. The thickener according to claim 9, wherein The water-soluble cellulose ether is hydroxyalkyl alkyl cellulose.
11. The thickener according to claim 9, wherein The viscosity of a 2 wt % aqueous solution of the water-soluble cellulose ether at 20° C. is 15 to 450,000 mPa·s.
12. The tackifier according to claim 9, further comprising a water repellent.
13. A hydraulic composition comprising the powdery additive according to any one of claims 1 to 8, a hydraulic substance, and water.
14. The hydraulic composition of claim 13, further comprising a water-soluble cellulose ether.
15. The hydraulic composition of claim 13, further comprising a water repellent.
16. The hydraulic composition according to claim 13, which is a concrete composition further comprising fine aggregate, coarse aggregate, and a water reducing agent, in, The concrete composition has a slump of 8 to 21 cm as measured by the method of JIS A 1101, and a compressive strength of 18 to 45 N / mm2 as measured by the method of JIS A 1108 at 28 days. 2 .
17. A hydraulic composition comprising the powdery thickener according to any one of claims 9 to 12, a hydraulic substance, and water.
18. The hydraulic composition according to claim 17, which is a concrete composition further comprising fine aggregate, coarse aggregate, and a water reducing agent, in, The concrete composition has a slump of 8 to 21 cm as measured by the method of JIS A 1101, and a compressive strength of 18 to 45 N / mm2 as measured by the method of JIS A 1108 at 28 days. 2 .
19. A method for producing a hydraulic composition, wherein: The hydraulic composition comprises a hydraulic substance, water and a polyethylene glycol derivative, The method comprises the step of adding the powdered additive according to any one of claims 1 to 8 to the step of mixing the components of the hydraulic composition.
20. The method of claim 19, wherein: The hydraulic composition further comprises fine aggregate, coarse aggregate, and a water reducing agent to form a concrete composition. The concrete composition has a slump of 8 to 21 cm as measured by the method of JIS A 1101, and a compressive strength of 18 to 45 N / mm2 as measured by the method of JIS A 1108 at 28 days. 2 .
21. A method for producing a hydraulic composition, wherein: The hydraulic composition comprises a hydraulic substance, water, a water-soluble cellulose ether and a polyethylene glycol derivative. The method comprises the step of adding the powdered additive according to any one of claims 9 to 12 to the step of mixing the components of the hydraulic composition.
22. The method of claim 21, wherein: The hydraulic composition further comprises fine aggregate, coarse aggregate, and a water reducing agent to constitute a concrete composition. The concrete composition has a slump of 8 to 21 cm as measured by the method of JIS A 1101, and a compressive strength of 18 to 45 N / mm as measured by the method of JIS A 1108 at 28 days. 2 .