Catalyst, preparation method and application in polycarbonate diol synthesis
By using potassium modified magnesium aluminum hydrotalcite catalyst, the problems of wide molecular weight distribution and unstable alcohol hydroxyl value of polycarbonate diol are solved, the separation of catalysts and the improvement of polyurethane properties are achieved, and the mechanical strength and resistance of the material are improved. Chemically corrosive.
Patent Information
- Application Number
- CN202411078955.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-12-06
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of chemical material production, and in particular relates to a catalyst, a preparation method and an application in the synthesis of polycarbonate diol. Background Art
[0002] Polyurethane is a general term for a class of polymer compounds containing carbamate segments (-NHCOO-) in the main chain. It is usually synthesized from diisocyanate, a hard segment raw material, and diol, a soft segment oligomer. Among them, polycarbonate polyurethane synthesized with polycarbonate diol (PCDL) as an oligomer has excellent mechanical properties, hydrolysis resistance, heat resistance, oxidation resistance and wear resistance. Therefore, with the widespread use of new polycarbonate polyurethane materials in production practice, polycarbonate diol products have also received attention from academia and industry.
[0003] At present, methods such as phosgene method, carbon dioxide epoxide regulation copolymerization method, ring-opening polymerization method of cyclic carbonate, and small molecule carbonate transesterification method have been developed to synthesize polycarbonate diols. The main synthesis method currently adopted in industry is: polycarbonate diols are obtained by polycondensation reaction of dimethyl carbonate and dihydroxy compounds under the action of catalysts. However, in the actual production process, it is usually difficult to effectively separate the catalyst and the product, resulting in low quality of polycarbonate diols. The residue of strong alkaline catalysts will not only make the hydroxyl value of polycarbonate diols unstable and the molecular weight distribution wide, but also make the physical properties and chemical corrosion resistance of the synthesized polyurethane elastomers low, and even cannot be used as raw materials to synthesize polyurethane elastomers.
[0004] Therefore, it has become an urgent problem to be solved by technical personnel in this field to develop a catalyst, a preparation method and its application in the synthesis of polycarbonate diols to solve the technical defects in the prior art, such as wide molecular weight distribution of the prepared polycarbonate diols, unstable hydroxyl value and difficulty in separating from the catalyst used in the preparation process. Summary of the invention
[0005] Based on this, it is necessary to provide a catalyst, a preparation method and its application in the synthesis of polycarbonate diols to address the technical defects of the existing technology, such as the wide molecular weight distribution of the prepared polycarbonate diols, the unstable hydroxyl value and the difficulty in separating them from the catalyst used in the preparation process.
[0006] The present application provides a catalyst for transesterification reaction and / or polycondensation reaction, wherein the catalyst is potassium-modified magnesium-aluminum hydrotalcite.
[0007] In one embodiment, the ratio of magnesium element to aluminum element in the catalyst is (1-4):1 by mole.
[0008] In one embodiment, the ratio of magnesium element to aluminum element in the catalyst is (2-3):1 by mole.
[0009] In one embodiment, in the catalyst, the molar ratio of the total molar amount of magnesium and aluminum to the molar amount of potassium is (5-8):1.
[0010] In one embodiment, in the catalyst, the molar ratio of the total molar amount of magnesium element and aluminum element to the molar amount of potassium element is (0.5-10):1, calculated by molar parts.
[0011] In one embodiment, in the catalyst, the potassium source of the potassium element is selected from any one or more of potassium chloride, potassium nitrate, potassium carbonate and potassium hydroxide.
[0012] In one embodiment, in the catalyst, the magnesium source of the magnesium element is selected from any one or more of magnesium chloride, magnesium nitrate, magnesium carbonate and magnesium hydroxide.
[0013] In one embodiment, in the catalyst, the aluminum source of the aluminum element is selected from any one or more of aluminum chloride, aluminum nitrate, aluminum carbonate and aluminum hydroxide.
[0014] The present application also provides a method for preparing the catalyst comprising any one of the above, wherein the preparation method is: a precipitation method or an impregnation method;
[0015] The precipitation method is as follows: magnesium source, aluminum source and potassium source are simultaneously precipitated under weak alkaline conditions to obtain potassium-modified magnesium aluminum hydrotalcite;
[0016] and / or,
[0017] The impregnation method is as follows: after calcining the aluminum-magnesium hydrotalcite precursor, potassium element is loaded by impregnation to obtain potassium-modified magnesium-aluminum hydrotalcite.
[0018] In one embodiment, the precipitation method is as follows: a magnesium source, an aluminum source and a potassium source are prepared into a mixed solution, a weak alkaline solution is added dropwise and the mixture is allowed to stand for crystallization, the intermediate obtained is filtered and washed, and then dried and calcined in sequence to obtain potassium-modified magnesium-aluminum hydrotalcite.
[0019] In one embodiment, the weak alkaline solution is selected from any one or more of ammonia water, ethanolamine, diethanolamine and triethanolamine, and the concentration of the weak alkaline solution is 5 to 25 mol / L.
[0020] In one embodiment, the drying temperature is 80-120° C., and the drying time is 6-12 hours.
[0021] In one embodiment, the calcination temperature is 300-800° C., and the calcination time is 3-8 hours.
[0022] In one embodiment, the impregnation method is:
[0023] Step 1: preparing a mixed solution of a magnesium source and an aluminum source, dropping a weak alkaline solution and standing the mixture for crystallization, filtering and washing the obtained intermediate, and performing a first drying and a first calcination to obtain a magnesium aluminum hydrotalcite precursor;
[0024] Step 2: The magnesium aluminum hydrotalcite precursor is impregnated in a potassium source solution, and after the impregnation is completed, it is dried for a second time and calcined for a second time to obtain potassium-modified magnesium aluminum hydrotalcite.
[0025] In one embodiment, the weak alkaline solution is selected from any one or more of ammonia water, ethanolamine, diethanolamine and triethanolamine, and the concentration of the weak alkaline solution is 5 to 25 mol / L.
[0026] In one embodiment, in step 1, the temperature of the first drying is 80-120° C., and the time of the first drying is 6-12 hours.
[0027] In one of the embodiments, in step 1, the temperature of the first calcination is 300-800° C., and the time of the first calcination is 3-8 hours.
[0028] In one embodiment, in step 2, the temperature of the second drying is 80-120° C., and the time of the second drying is 6-12 hours.
[0029] In one of the embodiments, in step 1, the temperature of the second calcination is 300-800° C., and the time of the second calcination is 3-8 hours.
[0030] In one embodiment, in step 2, the immersion temperature is 10-80° C., and the immersion time is 3-12 hours.
[0031] The present application also provides an application of a catalyst comprising any one of the above or a product obtained by any one of the above preparation methods in the synthesis of bio-based polycarbonate diol.
[0032] In one embodiment, the synthesis method of the bio-based polycarbonate diol is as follows: diol, carbonate and potassium-modified magnesium aluminum hydrotalcite are mixed, and then transesterification reaction and polycondensation reaction are carried out in sequence to obtain bio-based polycarbonate diol;
[0033] The diols include bio-based diols and / or petroleum-based diols.
[0034] In one of the embodiments, the feed ratio of the bio-based glycol to the petroleum-based glycol is (1-5):1.
[0035] In one embodiment, the bio-based diol is selected from any one or more of 1,3-propylene glycol, 1,4-propylene glycol, 1,5-pentanediol and isosorbide.
[0036] In one embodiment, the petroleum-based diol is selected from: any one or more of 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, tricyclodecane dimethanol, pentacyclopentadecanedimethanol, 2,6-decahydronaphthalene dimethanol, 1,5-decahydronaphthalene dimethanol, 2,3-decahydronaphthalene dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol and 1,3-adamantanedimethanol.
[0037] In one embodiment, the carbonate is selected from any one or more of dimethyl carbonate, diethyl carbonate and dibutyl carbonate.
[0038] In one embodiment, the transesterification reaction is carried out under the protection of a nitrogen atmosphere, the reaction pressure of the transesterification reaction is 50 to 200 KPa, the reaction temperature of the transesterification reaction is 140 to 200° C., and the reaction time of the transesterification reaction is 1 to 5 h.
[0039] In one of the embodiments, the polycondensation reaction is carried out under vacuum conditions, the reaction pressure of the polycondensation reaction is 5 to 30 KPa, the reaction temperature of the polycondensation reaction is 160 to 220° C., and the reaction time of the polycondensation reaction is 2 to 6 hours.
[0040] In one of the embodiments, the feeding amount of the potassium-modified magnesium-aluminum hydrotalcite is 0.001w% to 1w%.
[0041] In one embodiment, the feed ratio of the diol to the carbonate is (0.6-1.5):1.0 in molar parts.
[0042] In one embodiment, the synthesis method further comprises: refining, wherein the refining is performed after the polycondensation reaction;
[0043] The refining method is as follows: the reaction system after the polycondensation reaction is distilled and filtered in sequence to obtain the bio-based polycarbonate diol.
[0044] In summary, the present application provides a catalyst for transesterification reaction and / or polycondensation reaction, which is: potassium-modified magnesium aluminum hydrotalcite. The present application also provides a method for preparing the above catalyst, which is: precipitation method or impregnation method; the present application also provides an application of the above catalyst or the product obtained by the above preparation method in the synthesis of bio-based polycarbonate diol. According to experimental measurements, the bio-based polycarbonate diol prepared by the technical solution provided by the present application has a narrow number average molecular weight distribution, a stable alcohol hydroxyl value, and the catalyst used is a heterogeneous catalyst, which can be separated by filtration. The catalyst, preparation method and application in the synthesis of polycarbonate diol provided by the present application solve the technical defects in the prior art that the prepared polycarbonate diol has a wide molecular weight distribution, an unstable alcohol hydroxyl value and is not easy to separate from the catalyst used in the preparation process. DETAILED DESCRIPTION
[0045] The embodiments of the present application provide a catalyst, a preparation method and an application in the synthesis of polycarbonate diol, which are used to solve the technical defects in the prior art that the prepared polycarbonate diol has a wide molecular weight distribution, an unstable hydroxyl value and is difficult to separate from the catalyst used in the preparation process.
[0046] In order to make the above-mentioned purpose, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0047] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the embodiments, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0048] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0049] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0050] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0051] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0052] Example 1
[0053] 1.1 Catalyst preparation (one-pot method)
[0054] In this embodiment, the catalyst is prepared by a one-pot process.
[0055] 0.1 mol of magnesium chloride, 0.1 mol of aluminum chloride and 0.025 mol of potassium chloride were dissolved in 0.1 L of deionized water to prepare a solution. 0.3 L of 0.2 mol / L ammonia solution was added dropwise to the solution. After the addition was completed, the solution was allowed to stand for crystallization. After filtration, a white powder was obtained. The powder was washed with deionized water for 5 times. The intermediate obtained by washing was dried at 80 ° C for 12 h, and then calcined at 500 ° C for 3 h to obtain a potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst.
[0056] 1.2 Transesterification reaction
[0057] 1,4-Butanediol (0.12 mol), 1,5-pentanediol (0.21 mol), 1,6-hexanediol (0.12 mol) and dimethyl carbonate (0.59 mol) were added into a four-necked flask, and potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.01 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 180°C, and the reflux reaction was maintained for 4 hours to complete the ester exchange reaction.
[0058] 1.3 Polycondensation
[0059] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 50 KPa, the temperature was raised to 200° C., and the polycondensation reaction was completed after 3 h of polycondensation.
[0060] 1.4 Refining
[0061] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, and solids are filtered out to obtain a bio-based polycarbonate diol product.
[0062] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1022 g / mol, a hydroxyl value of 92.7 mg KOH / g, and an acid value of 0.015 mg KOH / g.
[0063] Example 2
[0064] 2.1 Catalyst preparation (one-pot method)
[0065] In this embodiment, the catalyst is prepared by a one-pot process.
[0066] 0.2 mol of magnesium chloride, 0.1 mol of aluminum chloride and 0.03 mol of potassium chloride were dissolved in 0.1 L of deionized water to prepare a solution. 0.3 L of 0.3 mol / L ammonia solution was added dropwise to the solution. After the addition was completed, the solution was allowed to stand for crystallization. After filtration, a white powder was obtained. The powder was washed with deionized water for 5 times. The intermediate obtained by washing was dried at 80 ° C for 12 h, and then calcined at 500 ° C for 3 h to obtain a potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst.
[0067] 2.2 Transesterification reaction
[0068] 1,4-Butanediol (0.21 mol), isosorbide (0.11 mol), 1,6-hexanediol (0.12 mol) and dimethyl carbonate (0.61 mol) were added into a four-necked flask, and potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.02 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 160°C, and the reaction was refluxed for 4 hours to complete the ester exchange reaction.
[0069] 2.3 Polycondensation
[0070] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 60 KPa, the temperature was raised to 210° C., and the polycondensation reaction was completed after 3 h of polycondensation.
[0071] 2.4 Refining
[0072] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, and solids are filtered out to obtain bio-based polycarbonate diol.
[0073] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1057 g / mol, a hydroxyl value of 96.8 mg KOH / g, and an acid value of 0.019 mg KOH / g.
[0074] Example 3
[0075] 3.1 Catalyst preparation (one-pot method)
[0076] In this embodiment, the catalyst is prepared by a one-pot process.
[0077] 0.3 mol of magnesium chloride, 0.1 mol of aluminum chloride and 0.04 mol of potassium chloride were dissolved in 0.1 L of deionized water to prepare a solution. 0.3 L of 0.4 mol / L ammonia solution was added dropwise to the solution. After the addition was completed, the solution was allowed to stand for crystallization. After filtration, a white powder was obtained. The powder was washed with deionized water for 5 times. The intermediate obtained by washing was dried at 80 ° C for 6 h, and then calcined at 500 ° C for 8 h to obtain a potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst.
[0078] 3.2 Transesterification
[0079] 1,4-Butanediol (0.23 mol), 1,6-hexanediol (0.22 mol) and dimethyl carbonate (0.60 mol) were added into a four-necked flask, and potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.01 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 180°C, and the reflux reaction was maintained for 4 hours to complete the ester exchange reaction.
[0080] 3.3 Polycondensation
[0081] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 50 KPa, the temperature was raised to 200° C., and the polycondensation reaction was completed after 4 hours of polycondensation.
[0082] 3.4 Refining
[0083] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, and solids are filtered out to obtain bio-based polycarbonate diol.
[0084] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1123 g / mol, a hydroxyl value of 111.8 mg KOH / g, and an acid value of 0.023 mg KOH / g.
[0085] Example 4
[0086] 4.1 Catalyst preparation (impregnation method)
[0087] In this embodiment, the catalyst is prepared by impregnation.
[0088] 0.1 mol of magnesium chloride and 0.1 mol of aluminum chloride were dissolved in 0.1 L of deionized water to prepare a solution, and 0.3 L of 0.2 mol / L ammonia solution was added dropwise to the solution. After the addition was completed, the mixture was allowed to stand for crystallization and filtered to obtain a white powder. The powder was washed five times, and the intermediate obtained by washing was dried at 80 ° C for 8 h, and then calcined at 500 ° C for 3 h to obtain Mg-Al-O magnesium aluminum hydrotalcite.
[0089] 1 wt% potassium chloride was prepared into a solution of 0.074 L, and the Mg-Al-O magnesium aluminum hydrotalcite obtained above was impregnated at 60°C for 12 hours. After the impregnation was completed, it was dried at 80°C for 24 hours and continued to be calcined at 600°C for 5 hours to obtain potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O).
[0090] 4.2 Transesterification
[0091] 1,4-Butanediol (0.11 mol), 1,5-pentanediol (0.22 mol), 1,6-hexanediol (0.13 mol) and dimethyl carbonate (0.61 mol) were added into a four-necked flask, and potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.01 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 180°C, and the reflux reaction was maintained for 4 hours to complete the ester exchange reaction.
[0092] 4.3 Polycondensation
[0093] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 50 KPa, the temperature was raised to 200° C., and the polycondensation reaction was completed after 3 h of polycondensation.
[0094] 4.4 Refining
[0095] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, and solids are filtered out to obtain bio-based polycarbonate diol.
[0096] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1134 g / mol, a hydroxyl value of 108.5 mg KOH / g, and an acid value of 0.022 mg KOH / g.
[0097] Example 5
[0098] 5.1 Catalyst preparation (impregnation method)
[0099] In this embodiment, the catalyst is prepared by impregnation.
[0100] 0.2 mol of magnesium chloride and 0.1 mol of aluminum chloride were dissolved in 0.1 L of deionized water to prepare a solution, and 0.3 L of 0.3 mol / L ammonia solution was added dropwise to the solution. After the addition was completed, the solution was allowed to stand for crystallization and filtered to obtain a white powder. The powder was washed five times, and the intermediate obtained by washing was dried at 80 ° C for 8 h, and then calcined at 500 ° C for 5 h to obtain Mg-Al-O magnesium aluminum hydrotalcite.
[0101] 1 wt% potassium chloride was prepared into a solution of 0.158 L, and the Mg-Al-O magnesium aluminum hydrotalcite obtained above was impregnated at 60°C for 3 hours. After the impregnation was completed, it was dried at 80°C for 24 hours and continued to be calcined at 600°C for 5 hours to obtain potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O).
[0102] 5.2 Transesterification
[0103] 1,4-Butanediol (0.21 mol), 1,6-hexanediol (0.22 mol) and dimethyl carbonate (0.58 mol) were added into a four-necked flask, and potassium-modified magnesium-aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.01 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 180°C, and the reflux reaction was maintained for 4 hours to complete the ester exchange reaction.
[0104] 5.3 Polycondensation
[0105] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 50 KPa, the temperature was raised to 200° C., and the polycondensation reaction was completed after 3 h of polycondensation.
[0106] 5.4 Refining
[0107] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, and solids are filtered out to obtain bio-based polycarbonate diol.
[0108] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1197 g / mol, a hydroxyl value of 111.3 mg KOH / g, and an acid value of 0.029 mg KOH / g.
[0109] Example 6
[0110] 6.1 Catalyst preparation (impregnation method)
[0111] In this embodiment, the catalyst is prepared by impregnation.
[0112] 0.3 mol of magnesium chloride and 0.1 mol of aluminum chloride were dissolved in 0.1 L of deionized water to prepare a solution, and 0.3 L of 0.4 mol / L ammonia solution was added dropwise to the solution. After the addition was completed, the solution was allowed to stand for crystallization and filtered to obtain a white powder. The powder was washed 5 times, and the intermediate obtained by washing was dried at 80 ° C for 8 h, and then calcined at 500 ° C for 5 h to obtain Mg-Al-O magnesium aluminum hydrotalcite.
[0113] 1 wt% potassium chloride was prepared into a solution of 0.158 L, and the Mg-Al-O magnesium aluminum hydrotalcite obtained above was impregnated at 60°C for 12 hours. After the impregnation was completed, it was dried at 80°C for 24 hours and continued to be calcined at 600°C for 5 hours to obtain potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O).
[0114] 6.2 Transesterification
[0115] 1,5-pentanediol (0.21 mol), 1,6-hexanediol (0.22 mol) and dimethyl carbonate (0.57 mol) were added into a four-necked flask, and potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.01 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 180°C, and the reflux reaction was maintained for 4 hours to complete the ester exchange reaction.
[0116] 6.3 Polycondensation
[0117] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 30 KPa, the temperature was raised to 220°C, and the polycondensation reaction was completed after 2 hours of polycondensation.
[0118] 6.4 Refining
[0119] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, the monomers and low molecular weight polycarbonate are distilled to remove the monomers and low molecular weight polycarbonate, and the solid matter is filtered out to obtain bio-based polycarbonate diol.
[0120] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1189 g / mol, a hydroxyl value of 116.4 mg KOH / g, and an acid value of 0.031 mg KOH / g.
[0121] Example 7
[0122] 7.1 Catalyst preparation
[0123] In this embodiment, the catalyst used is the catalyst shown in 1.1.
[0124] 7.2 Transesterification
[0125] 1,5-pentanediol (0.35 mol), 1,6-hexanediol (0.07 mol) and dimethyl carbonate (0.57 mol) were added into a four-necked flask, and potassium-modified magnesium aluminum hydrotalcite (K-Mg-Al-O) catalyst was added at 0.01 wt% of the total material mass. Under nitrogen protection, the pressure in the reactor was adjusted to 80 KPa, the temperature was raised to 180°C, and the reflux reaction was maintained for 4 hours to complete the ester exchange reaction.
[0126] 7.3 Polycondensation
[0127] After the ester exchange reaction was completed, the vacuum degree in the reactor was adjusted to 30 KPa, the temperature was raised to 220°C, and the polycondensation reaction was completed after 2 hours of polycondensation.
[0128] 7.4 Refining
[0129] The reaction system after the polycondensation reaction is distilled to remove monomers and low molecular weight polycarbonate, the monomers and low molecular weight polycarbonate are distilled to remove the monomers and low molecular weight polycarbonate, and the solid matter is filtered out to obtain bio-based polycarbonate diol.
[0130] After testing, the bio-based polycarbonate diol obtained in this example has a number average molecular weight of 1233 g / mol, a hydroxyl value of 118.2 mg KOH / g, and an acid value of 0.051 mg KOH / g.
[0131] Comparative Example 1
[0132] In this comparative example, the technical solution of Example 2 is adopted, which is different from the technical solution of Example 2 in that magnesium aluminum hydrotalcite is directly used as a catalyst.
[0133] After testing, the bio-based polycarbonate diol prepared in this comparative example has a number average molecular weight of 597 g / mol, a hydroxyl value of 161.1 mg KOH / g, and an acid value of 0.046 mg KOH / g.
[0134] Comparative Example 2
[0135] In this comparative example, the technical solution of Example 2 is adopted, which is different from the technical solution of Example 2 in that sodium methoxide is used as a catalyst.
[0136] After testing, the bio-based polycarbonate diol prepared in this comparative example has a number average molecular weight of 1407, a hydroxyl value of 89.7 mgKOH / g, and an acid value of 0.003 mgKOH / g.
[0137] The polycarbonate diol prepared by the technical solution provided by the present application has the advantages of stable hydroxyl value, narrow molecular weight and low acid value. The use of polycarbonate diol with stable hydroxyl value, narrow molecular weight and low acid value to prepare polyurethane has a significant effect on the performance of polyurethane. Among them, stable hydroxyl value and narrow molecular weight can significantly improve the crosslinking density and molecular weight of polyurethane, thereby improving the mechanical strength, weather resistance and chemical corrosion resistance of the material. The acid value has a lot of influence on the performance of polyurethane, which is manifested in affecting the polymerization reaction speed. When the acid value is low, the polymerization reaction speed is faster, and as the acid value increases, the polymerization reaction speed slows down and the viscosity stability time is extended; at the same time, it also affects the hydrolysis resistance. With the increase of acid value, the modulus, tensile strength and elongation at break of the resin are reduced to varying degrees; the greater the alcohol acid value of polycarbonate diol, the greater its adverse effect on the hydrolysis resistance of polyurethane; and it also affects the physical properties of polyurethane. The acid value not only affects the synthesis process of polyurethane, but also directly affects its final physical properties. For example, water resistance and chemical resistance are all affected by the acid value. Polyurethane synthesized from polycarbonate diols with low acid values performs better in terms of hydrolysis resistance and aging resistance.
[0138] In summary, the present application provides a catalyst for transesterification reaction and / or polycondensation reaction, which is: potassium-modified magnesium aluminum hydrotalcite. The present application also provides a method for preparing the above catalyst, which is: precipitation method or impregnation method; the present application also provides an application of the above catalyst or the product obtained by the above preparation method in the synthesis of bio-based polycarbonate diol. According to experimental measurements, the bio-based polycarbonate diol prepared by the technical solution provided by the present application has a narrow number average molecular weight distribution, a stable alcohol hydroxyl value, and the catalyst used is a heterogeneous catalyst, which can be separated by filtration. The catalyst, preparation method and application in the synthesis of polycarbonate diol provided by the present application solve the technical defects in the prior art that the prepared polycarbonate diol has a wide molecular weight distribution, an unstable alcohol hydroxyl value and is not easy to separate from the catalyst used in the preparation process.
[0139] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. At the same time, other implementation methods can be derived from the above-mentioned embodiments, so that structural and logical replacements and changes can be made without departing from the scope of this disclosure.
[0140] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A catalyst for transesterification and / or polycondensation reaction, characterized in that: The catalyst is potassium-modified magnesium-aluminum hydrotalcite.
2. The catalyst according to claim 1, characterized in that In terms of molar parts, the ratio of magnesium element to aluminum element in the catalyst is (1-4):
1.
3. The catalyst according to claim 1 or 2, characterized in that In terms of molar parts, in the catalyst, the molar ratio of the total molar amount of magnesium element and aluminum element to the molar amount of potassium element is (0.5-10):
1.
4. The catalyst according to any one of claims 1 to 3, characterized in that In the catalyst, the potassium source of the potassium element is selected from any one or more of potassium chloride, potassium nitrate, potassium carbonate and potassium hydroxide.
5. The catalyst according to any one of claims 1 to 3, characterized in that In the catalyst, the magnesium source of the magnesium element is selected from any one or more of magnesium chloride, magnesium nitrate, magnesium carbonate and magnesium hydroxide.
6. The catalyst according to any one of claims 1 to 3, characterized in that In the catalyst, the aluminum source of the aluminum element is selected from any one or more of aluminum chloride, aluminum nitrate, aluminum carbonate and aluminum hydroxide.
7. A method for preparing the catalyst according to any one of claims 1 to 6, characterized in that: The preparation method is: precipitation method or impregnation method; The precipitation method is as follows: magnesium source, aluminum source and potassium source are simultaneously precipitated under weak alkaline conditions to obtain potassium-modified magnesium aluminum hydrotalcite; and / or, The impregnation method is as follows: after calcining the aluminum-magnesium hydrotalcite precursor, potassium element is loaded by impregnation to obtain potassium-modified magnesium-aluminum hydrotalcite.
8. The preparation method according to claim 7, characterized in that: The precipitation method comprises the following steps: preparing a mixed solution of magnesium source, aluminum source and potassium source, dropping a weak alkaline solution and standing the mixture for crystallization, filtering and washing the obtained intermediate, and sequentially drying and roasting the intermediate to obtain potassium-modified magnesium aluminum hydrotalcite.
9. The preparation method according to claim 8, characterized in that: The weak alkaline solution is selected from any one or more of ammonia water, ethanolamine, diethanolamine and triethanolamine, and the concentration of the weak alkaline solution is 5-25 mol / L.
10. The preparation method according to claim 8 or 9, characterized in that: The drying temperature is 80-120° C., and the drying time is 6-12 hours.
11. The preparation method according to claim 8 or 9, characterized in that: The calcination temperature is 300-800° C., and the calcination time is 3-8 hours.
12. The preparation method according to claim 7, characterized in that: The method of the impregnation method is: Step 1: preparing a mixed solution of a magnesium source and an aluminum source, dropping a weak alkaline solution and standing the mixture for crystallization, filtering and washing the obtained intermediate, and performing a first drying and a first calcination to obtain a magnesium aluminum hydrotalcite precursor; Step 2: The magnesium aluminum hydrotalcite precursor is impregnated in a potassium source solution, and after the impregnation is completed, it is dried for a second time and calcined for a second time to obtain potassium-modified magnesium aluminum hydrotalcite.
13. The preparation method according to claim 12, characterized in that: The weak alkaline solution is selected from any one or more of ethanolamine, diethanolamine and triethanolamine, and the concentration of the weak alkaline solution is 5-25 mol / L.
14. The preparation method according to claim 12 or 13, characterized in that: In step 1, the temperature of the first drying is 80-120° C., and the time of the first drying is 6-12 hours.
15. The preparation method according to claim 12 or 13, characterized in that: In step 1, the temperature of the first calcination is 300-800° C., and the time of the first calcination is 3-8 hours.
16. The preparation method according to claim 12 or 13, characterized in that: In step 2, the temperature of the second drying is 80-120° C., and the time of the second drying is 6-12 hours.
17. The preparation method according to claim 12 or 13, characterized in that: In step 1, the temperature of the second calcination is 300-800° C., and the time of the second calcination is 3-8 hours.
18. The preparation method according to claim 12 or 13, characterized in that: In step 2, the immersion temperature is 10 to 80° C., and the immersion time is 3 to 12 hours.
19. Use of the catalyst according to any one of claims 1 to 6 or the product obtained by the preparation method according to any one of claims 7 to 18 in the synthesis of bio-based polycarbonate diol.
20. The use according to claim 19, characterized in that The synthesis method of the bio-based polycarbonate diol comprises: mixing diol, carbonate and potassium-modified magnesium aluminum hydrotalcite, and sequentially performing transesterification reaction and polycondensation reaction to obtain the bio-based polycarbonate diol; The diols include bio-based diols and / or petroleum-based diols.
21. The use according to claim 20, characterized in that Calculated by molar parts, the feed ratio of the bio-based diol to the petroleum-based diol is (1-5):
1.
22. The use according to claim 20 or 21, characterized in that The bio-based diol is selected from any one or more of 1,3-propylene glycol, 1,4-propylene glycol, 1,5-pentanediol and isosorbide.
23. The use according to claim 20 or 21, characterized in that The petroleum-based diol is selected from any one or more of 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, tricyclodecane dimethanol, pentacyclopentadecanedimethanol, 2,6-decahydronaphthalene dimethanol, 1,5-decahydronaphthalene dimethanol, 2,3-decahydronaphthalene dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol and 1,3-adamantanedimethanol.
24. The use according to claim 20 or 21, characterized in that The carbonate is selected from any one or more of dimethyl carbonate, diethyl carbonate and dibutyl carbonate.
25. The use according to any one of claims 20 to 24, characterized in that The transesterification reaction is carried out under the protection of nitrogen atmosphere, the reaction pressure of the transesterification reaction is 50-200 KPa, the reaction temperature of the transesterification reaction is 140-200° C., and the reaction time of the transesterification reaction is 1-5 hours.
26. The use according to any one of claims 20 to 24, characterized in that The polycondensation reaction is carried out under vacuum conditions, the reaction pressure of the polycondensation reaction is 5 to 30 KPa, the reaction temperature of the polycondensation reaction is 160 to 220° C., and the reaction time of the polycondensation reaction is 2 to 6 hours.
27. The use according to any one of claims 20 to 24, characterized in that The feeding amount of the potassium-modified magnesium-aluminum hydrotalcite is 0.001w% to 1w%.
28. The use according to any one of claims 20 to 24, characterized in that Calculated by molar parts, the feed ratio of the diol to the carbonate is (0.6-1.5):1.
0.
29. The use according to claim 20, characterized in that The synthesis method further comprises: refining, wherein the refining is performed after the polycondensation reaction; The refining method is as follows: the reaction system after the polycondensation reaction is distilled and filtered in sequence to obtain the bio-based polycarbonate diol.