Flame-retardant nylon and preparation method thereof
By integrating a novel structural flame retardant monomer into the nylon chain and converting amino groups into amide bonds, the method addresses heat resistance and degradation issues, achieving high flame retardancy and mechanical strength in nylon products.
Patent Information
- Application Number
- CN202411405039.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for preparing flame-retardant nylon suffer from poor heat resistance, degradation at high temperatures, and precipitation of additives, resulting in yellowish appearance and low mechanical properties, failing to meet the higher flame retardant requirements of UL94 V-0 and LOI > 29%.
A method involving a novel structural reaction flame retardant monomer, P-[3-[(4,6-diamino-1,3,5-triazine-2-yl)amino]-3-oxopropyl]-p-phenylphosphinic acid (HPPMEL), is integrated into the nylon main chain through a two-stage reaction under inert conditions, converting amino groups into amide bonds to enhance stability and heat resistance, forming a chemically grafted modified nylon with improved flame retardant properties.
The resulting nylon exhibits a high limiting oxygen index (>35%), excellent flame retardancy, good tensile strength, and suitable melting point, with a white product that maintains comprehensive performance advantages.
Smart Images

Figure BDA0005076305030000021 
Figure BDA0005076305030000022 
Figure BDA0005076305030000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nylon preparation, and particularly relates to flame-retardant nylon and a preparation method thereof. Background Art
[0002] Nylon (PA) is a thermoplastic engineering plastic containing an amide bond (-NHCO-) in the main chain of the molecule. Since it was introduced by DuPont in the United States in 1930, PA has been widely used in the automotive industry, electronic appliances, synthetic fibers, construction and other fields due to its advantages such as heat resistance, wear resistance, chemical resistance and self-lubrication, becoming one of the engineering plastics with the largest output and the widest application range in the world today.
[0003] The combustion grade of nylon material is UL94 V-2, and the limiting oxygen index (LOI) is about 24%, which has certain flame retardant properties. However, with the continuous expansion of the scope of application, fields such as electronics and construction have put forward higher requirements for the flame retardant properties of nylon, requiring the vertical combustion grade to reach UL94 V-0 and the LOI to reach more than 29%.
[0004] Prior art CN106633043A discloses a method for preparing a halogen-free flame-retardant nylon 66 polymer, wherein DDP is selected as a reactive flame retardant to polymerize with nylon 66 salt to obtain a flame-retardant nylon 66 resin. The disadvantage of this method is that DDP itself has poor heat resistance and is easily decarboxylated at high temperatures. Under the conditions of this preparation process, DDP does not undergo random copolymerization with nylon 66 salt. It is actually an additive blending process, which is easy to precipitate during use. Prior art CN 106633043 A discloses a method for preparing a halogen-free flame-retardant nylon 6, wherein an additive flame retardant is first polymerized with caprolactam in situ, and then a DPP reactive flame retardant is added at 235°C to finally obtain a flame-retardant nylon resin. The disadvantage of this method is also that DDP itself has poor heat resistance and is easily decarboxylated at high temperatures. Under the conditions of 235°C, the DPP salt has been degraded, and what is obtained is a blend of two additive flame retardants, which is easy to precipitate during use. In addition, due to the degradation of DDP flame retardant, the resins obtained by these two methods have a yellowish appearance and low mechanical properties. Summary of the invention
[0005] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:
[0006] One of the objects of the present invention is to provide a method for preparing flame retardant nylon, comprising:
[0007] Under inert atmosphere conditions, a first mixed reaction system containing P-[3-[(4,6-diamino-1,3,5-triazine-2-yl)amino]-3-oxopropyl]-p-phenylphosphinic acid, a first dibasic acid and a first catalyst is subjected to a first reaction at 150-200° C. to obtain a flame retardant prepolymer;
[0008] Under inert atmosphere conditions, a second mixed reaction system containing the flame retardant prepolymer, reactive monomers and a second catalyst is subjected to a second reaction to obtain flame retardant nylon, wherein the reactive monomers include a second dibasic acid and a diamine, or the reactive monomers include lactam.
[0009] The chemical structure of P-[3-[(4,6-diamino-1,3,5-triazine-2-yl)amino]-3-oxopropyl]-p-phenylphosphinic acid (HPPMEL) is as follows:
[0010]
[0011] The preparation method provided by the present invention introduces a novel structural reaction flame retardant monomer into the main chain of nylon molecules to obtain chemically grafted modified nylon, and the nylon product exhibits a higher limiting oxygen index, excellent flame retardant properties, good tensile strength, suitable melting point and viscosity, and the product is white; since the heat resistance of HPPMEL is slightly poor and the amino groups contained are easily oxidized, the present invention first reacts HPPMEL with a first dibasic acid to prepare a flame retardant prepolymer, and converts the amino groups therein into amide bonds, so that the flame retardant prepolymer has good stability and heat resistance, thereby being more conducive to obtaining a nylon material with excellent comprehensive performance.
[0012] The reaction temperature has a certain influence on the reaction effect. In the preparation process of the flame retardant prepolymer, if the reaction temperature is lower than 150°C, the flame retardant and the first dibasic acid will not react or the reaction effect will be poor. If it is higher than 200°C, the prepolymerization reaction will easily cause the flame retardant to degrade.
[0013] The equation for the reaction of HPPMEL with the first dibasic acid is as follows:
[0014]
[0015] In some embodiments, the molar ratio of the P-[3-[(4,6-diamino-1,3,5-triazine-2-yl)amino]-3-oxopropyl]-p-phenylphosphinic acid to the first dibasic acid is 1.0-1.05:1.
[0016] In some embodiments, the first reaction time is 4-8 hours. If the reaction time is less than 4 hours, the HPPMEL and the first dibasic acid do not react fully, and if the reaction time is more than 8 hours, the HPPMEL has completely formed a prepolymer, which increases energy consumption and production costs.
[0017] In some embodiments, the second reaction specifically includes: firstly raising the temperature of the second mixed reaction to 150-200°C and maintaining for 1-6 hours, then raising the temperature to 200-220°C and maintaining for 2-4 hours, then adjusting the vacuum degree to below 50Pa, raising the temperature to 220-320°C and maintaining for 0.1-4 hours. In the first stage (150-200°C), the flame retardant prepolymer and the reaction monomer form oligomers, and the diacid decarboxylation and diamine loss will occur if the temperature is too high; in the second stage (200-220°C), the molecular weight of the oligomer gradually increases, and the heat resistance of the material in the kettle is improved; in the third stage (220-320°C), the molecular weight of the polymer is further increased, and finally a high polymer is formed.
[0018] In some embodiments, in the second mixed reaction system, the mass of the flame retardant prepolymer is 0.1-99% of the total mass of the flame retardant prepolymer and the reaction monomer, preferably 0.1-20%, more preferably 0.2-10%, and particularly preferably 0.5-3%. If the mass ratio of the flame retardant prepolymer is lower than 0.1%, the flame retardant effect is not obvious, and if it exceeds 20%, the molecular weight of the polymer will be low and the production cost will increase.
[0019] In some embodiments, when the reactive monomer includes a second dibasic acid and a diamine, the molar ratio of the second dibasic acid to the diamine is 1:1.0-1.05.
[0020] In some embodiments, the first dibasic acid and the second dibasic acid include one or more of aliphatic dibasic acid, aromatic dibasic acid, alicyclic dicarboxylic acid or heterocyclic dibasic acid, and the first dibasic acid and the second dibasic acid are the same or different.
[0021] In some embodiments, the aliphatic dibasic acid comprises C4 to C 14 The aromatic dibasic acid includes one or more of a monocyclic aromatic dibasic acid, a polycyclic aromatic dibasic acid containing two or more benzene rings, or a naphthyl dibasic acid, and the alicyclic dicarboxylic acid includes C4 to C 14 The heterocyclic dicarboxylic acid comprises one or more of a furanyl dicarboxylic acid or a pyridyl dicarboxylic acid, but is not limited thereto.
[0022] In some embodiments, the aliphatic dibasic acid includes one or more of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid or tetradecanedioic acid, but is not limited thereto.
[0023] In some embodiments, the aromatic dibasic acid includes one or more of phthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid or diphenyl sulfone-4,4'-dicarboxylic acid, but is not limited thereto.
[0024] In some embodiments, the alicyclic dicarboxylic acid includes one or a combination of 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid, but is not limited thereto.
[0025] In some embodiments, the heterocyclic dicarboxylic acid includes one or a combination of furandicarboxylic acid and pyridinedicarboxylic acid, but is not limited thereto.
[0026] In some preferred embodiments, the first dibasic acid and the second dibasic acid include adipic acid. The present invention finds that the polymer prepared using adipic acid has better comprehensive properties.
[0027] In some embodiments, the diamine includes an aliphatic diamine, preferably one or more of diamine selected from ...
[0028] In some embodiments, the lactam includes one or a combination of caprolactam and laurolactam.
[0029] In some embodiments, the first catalyst and the second catalyst include one or more of potassium hypophosphite, sodium hypophosphite, magnesium hypophosphite, calcium hypophosphite or zinc hypophosphite, and the first catalyst and the second catalyst are the same or different. Preferably, the first catalyst and the second catalyst are preferably sodium hypophosphite.
[0030] In some embodiments, the first mixed reaction system further includes a first solvent, and / or the second mixed reaction system further includes a second solvent, the first solvent and the second solvent include but are not limited to a combination of one or more of water, alcohol solvents, amide solvents or sulfoxide solvents, and the first solvent and the second solvent are the same or different.
[0031] In some embodiments, the alcohol solvent includes one or more combinations of methanol, ethanol, propanol, butanol, pentanol, hexanol, octanol, decanol, hexanediol or glycerol, but not limited thereto. The amide solvent includes one or more combinations of N,N-dimethylformamide and N,N-dimethylacetamide, but not limited thereto. The sulfoxide solvent includes dimethyl sulfoxide, but not limited thereto.
[0032] In some preferred embodiments, the first solvent and the second solvent are water.
[0033] A second object of the present invention is to provide a flame retardant nylon prepared according to any of the methods described above.
[0034] In some embodiments, the limiting oxygen index of the flame retardant nylon is greater than 35%.
[0035] Compared with the prior art, the present invention has at least the following beneficial effects: the preparation method provided by the present invention introduces a novel structural reactive flame-retardant monomer into the main chain of the nylon molecule to obtain chemically grafted modified nylon, the nylon product exhibits a relatively high limiting oxygen index, excellent flame retardant properties, and the product is white; since the heat resistance of HPPMEL is slightly poor and the amino groups contained therein are easily oxidized, the present invention first reacts HPPMEL with a first dibasic acid to prepare a flame-retardant prepolymer, and converts the amino groups therein into amide bonds, so that the flame-retardant prepolymer has good stability and heat resistance, which is more conducive to obtaining a nylon material with excellent comprehensive properties. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0037] Unless otherwise specified, the raw materials and reagents used in the present invention are all commercially available. The test method used in the present invention is as follows:
[0038] 1. Relative viscosity η r
[0039] The tested samples were dissolved in concentrated sulfuric acid to obtain a concentration of 1 g / dl, and the relative viscosity η of the solution was measured at 25°C. r :
[0040] η r =t1 / t0
[0041] Where t0 represents the time for solvent to flow out (s), t1 represents the time for sample solution to flow out (s), and η r Indicates relative viscosity.
[0042] 2. Melting point
[0043] The melting point of the sample was determined using a Mettler-Toledo DSC1 instrument. Under a nitrogen atmosphere, the temperature was raised from room temperature to 340°C at a rate of 10°C / min, maintained for 5 min, then cooled to room temperature at a rate of 10°C / min, and then raised to 340°C at a rate of 10°C / min. The endothermic peak temperature at this time was the melting point of the polymer.
[0044] 3. Mechanical properties
[0045] The prepared injection molding test specimens were tested for tensile strength according to GB / T1040.2 standard.
[0046] 4. Limiting oxygen index
[0047] The limiting oxygen index is tested according to GB / T2406-2009 standard.
[0048] Example 1
[0049] Preparation of flame retardant prepolymer: HPPMEL, adipic acid, sodium hypophosphite and water are added to a reaction kettle (wherein HPPMEL and adipic acid are equimolar), nitrogen is replaced three times in the kettle, and stirring is started under nitrogen protection, the temperature is raised to 180° C., and stirring is performed for 6 hours; exhaust and cooling are performed to obtain a flame retardant prepolymer;
[0050] Preparation of flame-retardant nylon 66 resin: Add 2 parts of flame retardant prepolymer prepared above, 100 parts of reaction monomers (reaction monomers are adipic acid and hexamethylenediamine, both are equimolar), water, and sodium hypophosphite into a reactor, seal the reactor, and gradually heat to 180°C in a nitrogen atmosphere for 2 hours; continue to heat to 210°C and react for 3 hours; start exhausting for 4 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 280°C, vacuum ≤50Pa, react at this temperature for 2 hours, and discharge to obtain flame-retardant nylon 66 resin.
[0051] Its relative viscosity is 2.7, tensile strength is 83 MPa, melting point is 265°C, and limiting oxygen index is 38%.
[0052] Example 2
[0053] Preparation of flame retardant prepolymer: Add equimolar HPPMEL, adipic acid, sodium hypophosphite and water into a reaction kettle (wherein HPPMEL and adipic acid are equimolar), replace nitrogen in the kettle three times, and start stirring under nitrogen protection, heat to 180°C, stir for 6 hours; exhaust and cool to obtain flame retardant prepolymer;
[0054] Preparation of flame-retardant nylon 6 resin: Add 2 parts of flame retardant prepolymer prepared above, 100 parts of reaction monomer caprolactam, water and sodium hypophosphite into a reactor, seal the reactor, gradually heat to 180°C under nitrogen atmosphere, and react for 4 hours; continue to heat to 210°C and react for 3 hours; start exhausting for 2 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 235°C, vacuum ≤50Pa, react at this temperature for 2 hours, discharge, and obtain flame-retardant nylon 6 resin.
[0055] Its relative viscosity is 2.5, tensile strength is 75 MPa, melting point is 220°C, and limiting oxygen index is 37%.
[0056] Example 3
[0057] Preparation of flame retardant prepolymer: HPPMEL, adipic acid, sodium hypophosphite and water are added to a reaction kettle (wherein HPPMEL and adipic acid are equimolar), nitrogen is replaced three times in the kettle, and stirring is started under nitrogen protection, the temperature is raised to 180°C, and stirring is performed for 6 hours; exhaust and cooling are performed to obtain a flame retardant prepolymer;
[0058] Preparation of flame-retardant nylon 56 resin: 2 parts of the flame retardant prepolymer prepared above, 100 parts of reaction monomers (reaction monomers are adipic acid and pentamethylenediamine, both are equimolar), water, and sodium hypophosphite are added to a reactor, the reactor is sealed, and the temperature is gradually raised to 180°C under a nitrogen atmosphere for 2 hours; the temperature is continued to be raised to 210°C and the reaction is carried out for 3 hours; exhaust is started for 4 hours, and the temperature in the reactor is increased while exhausting, and the temperature in the reactor is raised to 275°C, and vacuum is drawn. ≤ 50Pa, react at this temperature for 2h, discharge the material, and obtain flame retardant nylon 56 resin.
[0059] Its relative viscosity is 2.65, tensile strength is 80 MPa, melting point is 258°C, and limiting oxygen index is 39%.
[0060] Example 4
[0061] Preparation of flame retardant prepolymer: HPPMEL, adipic acid, sodium hypophosphite and water are added to a reaction kettle (wherein HPPMEL and adipic acid are equimolar), nitrogen is replaced three times in the kettle, and stirring is started under nitrogen protection, the temperature is raised to 180°C, and stirring is performed for 6 hours; exhaust and cooling are performed to obtain a flame retardant prepolymer;
[0062] Preparation of flame retardant nylon 66 resin: 1 part of flame retardant prepolymer, 100 parts of reactive monomer (reactive monomers are adipic acid and hexamethylenediamine, both are equimolar), water, and sodium hypophosphite are added to a reactor, the reactor is sealed, and the temperature is gradually raised to 180°C under a nitrogen atmosphere, and the reaction is carried out for 2 hours; the temperature is continued to be raised to 210°C, and the reaction is carried out for 3 hours; exhaust is started for 4 hours, and the temperature in the reactor is increased while exhausting, and the temperature in the reactor is raised to 280°C, and vacuum is drawn ≤50Pa, and the reaction is carried out at this temperature for 2 hours, and the material is discharged to obtain flame retardant nylon 66 resin. Obtain flame retardant nylon 66 resin.
[0063] The relative viscosity is 2.7, the tensile strength is 80 MPa, the melting point is 265°C, and the limiting oxygen index is 36%.
[0064] Example 5
[0065] Preparation of flame retardant prepolymer: HPPMEL, adipic acid, sodium hypophosphite and water are added to a reaction kettle (wherein HPPMEL and adipic acid are equimolar), nitrogen is replaced three times in the kettle, and stirring is started under nitrogen protection, the temperature is raised to 180°C, and stirring is performed for 6 hours; exhaust and cooling are performed to obtain a flame retardant prepolymer;
[0066] Preparation of flame retardant nylon 6 resin: 1 part of flame retardant prepolymer, 100 parts of reactive monomer (caprolactam), water and sodium hypophosphite are added to a reactor, the reactor is sealed, and the temperature is gradually raised to 180°C under a nitrogen atmosphere, and the reaction is carried out for 4 hours; the temperature is continued to be raised to 210°C and the reaction is carried out for 3 hours; exhaust is started for 2 hours, and the temperature in the reactor is increased while exhausting, and the temperature in the reactor is raised to 235°C, and a vacuum is drawn to ≤50Pa. The reaction is carried out at this temperature for 2 hours, and the material is discharged to obtain flame retardant nylon 6 resin.
[0067] The relative viscosity is 2.5, the tensile strength is 73 MPa, the melting point is 220°C, and the limiting oxygen index is 35%.
[0068] Example 6
[0069] Preparation of flame retardant prepolymer: HPPMEL, adipic acid, sodium hypophosphite and water are added to a reaction kettle (wherein HPPMEL and adipic acid are equimolar), nitrogen is replaced three times in the kettle, and stirring is started under nitrogen protection, the temperature is raised to 180°C, and stirring is performed for 6 hours; exhaust and cooling are performed to obtain a flame retardant prepolymer;
[0070] Preparation of flame-retardant nylon 66 resin: 3 parts of flame retardant prepolymer, 100 parts of reactive monomer (reactive monomers are adipic acid and hexamethylenediamine, both of which are equimolar), water, and sodium hypophosphite are added to the reactor, the reactor is sealed, and the temperature is gradually raised to 180°C under nitrogen atmosphere for 2 hours; the temperature is continued to rise to 210°C and the reaction is carried out for 3 hours; exhaust is started for 4 hours, and the temperature in the reactor is raised while exhausting, and the temperature in the reactor is raised to 280°C, and vacuum is drawn. ≤50Pa, react at this temperature for 2h, discharge, and obtain flame retardant nylon 66 resin.
[0071] Its relative viscosity is 2.7, tensile strength is 85 MPa, melting point is 265°C, and limiting oxygen index is 40%.
[0072] Example 7
[0073] Preparation of flame retardant prepolymer: HPPMEL, adipic acid, sodium hypophosphite and water are added to a reaction kettle (wherein HPPMEL and adipic acid are equimolar), nitrogen is replaced three times in the kettle, and stirring is started under nitrogen protection, the temperature is raised to 180°C, and stirring is performed for 6 hours; exhaust and cooling are performed to obtain a flame retardant prepolymer;
[0074] Preparation of flame retardant nylon 6 resin: 3 parts of flame retardant prepolymer, 100 parts of reactive monomer (caprolactam), water and sodium hypophosphite are added to a reactor, the reactor is sealed, and the temperature is gradually raised to 180°C under a nitrogen atmosphere, and the reaction is carried out for 4 hours; the temperature is continued to be raised to 210°C and the reaction is carried out for 3 hours; exhaust is started for 2 hours, and the temperature in the reactor is increased while exhausting, and the temperature in the reactor is raised to 235°C, and a vacuum is drawn to ≤50 Pa. The reaction is carried out at this temperature for 2 hours, and the material is discharged to obtain flame retardant nylon 6 resin.
[0075] Its relative viscosity is 2.5, tensile strength is 78 MPa, melting point is 220°C, and limiting oxygen index is 39%.
[0076] Embodiments 8 to 16
[0077] The difference between Examples 8 to 16 and Example 1 is that the raw materials and their amounts are changed as shown in Table 1, and the rest is implemented in the same way as Example 1.
[0078] Comparative Example 1
[0079] Preparation of nylon 66 resin: Add equimolar adipic acid, hexamethylenediamine, water and sodium hypophosphite to a reactor, seal the reactor, gradually heat to 180°C under nitrogen atmosphere, and react for 2 hours; continue to heat to 210°C and react for 3 hours; start exhausting for 4 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 280°C, vacuumize ≤50 Pa, react at this temperature for 2 hours, discharge, and obtain nylon 66 resin.
[0080] Its relative viscosity is 2.7, tensile strength is 74 MPa, melting point is 265°C, and limiting oxygen index is 23%.
[0081] Comparative Example 2
[0082] Preparation of nylon 6 resin: add caprolactam, water and sodium hypophosphite to the reactor, seal the reactor, gradually heat up to 180°C under nitrogen atmosphere, and react for 4 hours; continue to heat up to 210°C and react for 3 hours; start exhausting for 2 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 235°C, vacuumize ≤50 Pa, react at this temperature for 2 hours, discharge the material, and obtain flame-retardant nylon 6 resin.
[0083] Its relative viscosity is 2.5, tensile strength is 68 MPa, melting point is 220°C, and limiting oxygen index is 22%.
[0084] Comparative Example 3
[0085] Preparation of nylon 56 resin: add equimolar adipic acid, pentamethylenediamine, water and sodium hypophosphite into a reactor, seal the reactor, gradually heat to 180°C under nitrogen atmosphere, and react for 2 hours; continue to heat to 210°C and react for 3 hours; start exhausting for 4 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 275°C, vacuumize ≤50Pa, react at this temperature for 2 hours, discharge the material, and obtain flame-retardant nylon 56 resin.
[0086] Its relative viscosity is 2.65, tensile strength is 72 MPa, melting point is 258°C, and limiting oxygen index is 24%.
[0087] Comparative Example 4
[0088] The difference between Comparative Example 4 and Example 1 is that HPPMEL is used to directly prepare nylon 66, as follows:
[0089] Preparation of nylon 66 resin: 2 parts of HPPMEL, 100 parts of reaction monomers (the reaction monomers are adipic acid and hexamethylenediamine, both of which are equimolar), water, and sodium hypophosphite are added to a reactor, the reactor is sealed, and the temperature is gradually raised to 180°C under a nitrogen atmosphere, and the reaction is carried out for 2 hours; the temperature is continued to be raised to 210°C and the reaction is carried out for 3 hours; exhaust is started for 4 hours, and the temperature in the reactor is increased while exhausting, the temperature in the reactor is raised to 280°C, and a vacuum is drawn ≤50Pa. The reaction is carried out at this temperature for 2 hours, and the material is discharged to obtain nylon 66 resin.
[0090] Comparative Example 5
[0091] The difference between Comparative Example 5 and Example 2 is that HPPMEL is used to directly prepare nylon 6, as follows:
[0092] Preparation of nylon 6 resin: Add 2 parts of HPPMEL, 100 parts of reaction monomer caprolactam, water and sodium hypophosphite into a reactor, seal the reactor, gradually heat to 180°C under nitrogen atmosphere, and react for 4 hours; continue to heat to 210°C and react for 3 hours; start exhausting for 2 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 235°C, vacuum ≤50Pa, react at this temperature for 2 hours, discharge, and obtain nylon 6 resin.
[0093] Comparative Example 6
[0094] The difference between Comparative Example 6 and Example 3 is that HPPMEL is used to directly prepare nylon 56, as follows:
[0095] Add the above 2 parts of HPPMEL, 100 parts of reaction monomers (the reaction monomers are adipic acid and pentamethylenediamine, both of which are equimolar), water and sodium hypophosphite into the reactor, seal the reactor, and gradually heat to 180°C under nitrogen atmosphere, and react for 2 hours; continue to heat to 210°C and react for 3 hours; start exhausting for 4 hours, while increasing the temperature in the reactor, the temperature in the reactor is increased to 275°C, vacuumize ≤50Pa, react at this temperature for 2 hours, and discharge to obtain nylon 56 resin.
[0096] Table 1 Raw materials and dosage used in the examples and comparative examples
[0097]
[0098]
[0099] Table 2 Various properties of nylon resin obtained in Examples and Comparative Examples
[0100]
[0101]
[0102] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0103] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0104] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.
Claims
1. A method for preparing flame retardant nylon, characterized in that: include: Under inert atmosphere conditions, a first mixed reaction system containing P-[3-[(4,6-diamino-1,3,5-triazine-2-yl)amino]-3-oxopropyl]-p-phenylphosphinic acid, a first dibasic acid and a first catalyst is subjected to a first reaction at 150-200° C. to obtain a flame retardant prepolymer; Under inert atmosphere conditions, a second mixed reaction system containing the flame retardant prepolymer, reactive monomers and a second catalyst is subjected to a second reaction to obtain flame retardant nylon, wherein the reactive monomers include a second dibasic acid and a diamine, or the reactive monomers include lactam.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the P-[3-[(4,6-diamino-1,3,5-triazine-2-yl)amino]-3-oxopropyl]-p-phenylphosphinic acid to the first dibasic acid is 1.0 to 1.05:1; And / or, the first reaction time is 4-8h.
3. The preparation method according to claim 1, characterized in that: The second reaction specifically includes: firstly raising the temperature of the second mixed reaction to 150-200°C and maintaining for 1-6h, then raising the temperature to 200-220°C and maintaining for 2-4h, and then adjusting the vacuum degree to below 50Pa, raising the temperature to 220-320°C and maintaining for 0.1-4h.
4. The preparation method according to claim 1 or 3, characterized in that: In the second mixed reaction system, the mass of the flame retardant prepolymer is 0.1 to 99% of the total mass of the flame retardant prepolymer and the reaction monomer, preferably 0.1 to 20%, more preferably 0.2 to 10%, and particularly preferably 0.5 to 3%; And / or, when the reaction monomer comprises a second dibasic acid and a diamine, the molar ratio of the second dibasic acid to the diamine is 1:1.0-1.
05.
5. The preparation method according to claim 1, characterized in that: The first dibasic acid and the second dibasic acid include one or more of an aliphatic dibasic acid, an aromatic dibasic acid, an alicyclic dicarboxylic acid or a heterocyclic dibasic acid, and the first dibasic acid and the second dibasic acid are the same or different; Preferably, the aliphatic dibasic acid includes C4 to C 14 The aromatic dibasic acid includes one or more of a monocyclic aromatic dibasic acid, a polycyclic aromatic dibasic acid containing two or more benzene rings, or a naphthyl dibasic acid, and the alicyclic dicarboxylic acid includes C4 to C 14 alicyclic dicarboxylic acid, wherein the heterocyclic dicarboxylic acid comprises one or more of furanyl dicarboxylic acid or pyridyl dicarboxylic acid; More preferably, the aliphatic dibasic acid includes one or more combinations of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane dicarboxylic acid, dodecanedioic acid, tridecanedioic acid or tetradecanedioic acid; the aromatic dibasic acid includes one or more combinations of phthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid or diphenyl sulfone-4,4'-dicarboxylic acid; the alicyclic dicarboxylic acid includes one or two combinations of 1,3-cyclopentane dicarboxylic acid and 1,4-cyclohexane dicarboxylic acid; the heterocyclic dicarboxylic acid includes one or two combinations of furandicarboxylic acid and pyridine dicarboxylic acid; Particularly preferably, the first dibasic acid and the second dibasic acid include adipic acid.
6. The preparation method according to claim 1, characterized in that: The diamine includes an aliphatic diamine, preferably includes one or more of diamine selected from diamine selected from butanediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine or decamethylenediamine, more preferably includes one or two of diamine selected from diamine selected from pentamethylenediamine and hexamethylenediamine; And / or, the lactam includes one or a combination of caprolactam and lauryl lactam.
7. The preparation method according to claim 1, characterized in that: The first catalyst and the second catalyst include one or more of potassium hypophosphite, sodium hypophosphite, magnesium hypophosphite, calcium hypophosphite or zinc hypophosphite, and the first catalyst and the second catalyst are the same or different.
8. The preparation method according to claim 1, characterized in that: The first mixed reaction system further includes a first solvent, and / or the second mixed reaction system further includes a second solvent; the first solvent and the second solvent include one or more of water, an alcohol solvent, an amide solvent or a sulfoxide solvent, and the first solvent and the second solvent are the same or different; Preferably, the alcohol solvent includes one or more combinations of methanol, ethanol, propanol, butanol, pentanol, hexanol, octanol, decanol, hexanediol or glycerol; the amide solvent includes one or more combinations of N,N-dimethylformamide and N,N-dimethylacetamide; and the sulfoxide solvent includes dimethyl sulfoxide.
9. The flame retardant nylon prepared according to the method according to any one of claims 1 to 8.
10. The flame retardant nylon according to claim 9, characterized in that: The limiting oxygen index of the flame retardant nylon is above 35%.
Citation Information
Patent Citations
Halogen-free flame-retardant polyamide 6 and preparation method thereof
CN106633043A
Melamine carboxethyl phenylphosphinic acid condensation product and preparation method thereof
CN102344570A
Novel organic phosphorus-nitrogen flame retardant as well as preparation method and application thereof
CN105153228A
Flame-retardant polyamide and preparation method and application thereof
CN105175717A
Copolymerized flame-retardant polyamide fiber and preparation method thereof
CN112048779A