Membrane material for heat exchange core as well as preparation method and application of membrane material

By using film materials of aromatic diamine, aromatic anhydride, fluorosilane and carbon materials, combined with fluoro-containing metal complexes and sulfonic acid catalysts, the problems of insufficient thermal conductivity, perspective performance and strength of existing heat exchange core materials are solved, and the problem of insufficient thermal conductivity, perspective performance and strength of existing heat exchange core materials is achieved. Highly efficient heat transfer and equipment stability.

CN119081113AInactive Publication Date: 2024-12-06ZHONGSHAN FORTUNE WAY ENVIRONMENTAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411220909.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing film materials for heat exchange cores have shortcomings in thermal conductivity, perspective performance and mechanical strength, resulting in poor heat transfer efficiency and equipment reliability problems.

Method used

The film material consisting of aromatic diamine, aromatic anhydride, fluoro-containing silane and carbon materials is prepared by heating polymerization to form a high thermal conductivity, high moisture permeability and high strength film material, and the introduction of fluoro-containing metal complexes and sulfonates Acid catalyst, optimize polymerization reaction to improve material stability and interface adhesion.

Benefits of technology

The film materials with high thermal conductivity, high moisture permeability and high mechanical strength are achieved, which significantly improves the heat exchange efficiency and equipment reliability, ensuring stable performance in high temperature and high pressure environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023000260000181
    Figure BDA0005023000260000181
  • Figure BDA0005023000260000191
    Figure BDA0005023000260000191
Patent Text Reader

Abstract

The invention discloses a membrane material for a heat exchange core as well as a preparation method and application of the membrane material. Relates to the technical field of heat exchange cores. The raw materials of the membrane material comprise the following components: aromatic diamine; aromatic anhydride; a fluorine-containing silane; and a carbon material. The membrane material disclosed by the invention is a membrane material with high heat conductivity, high moisture permeability and high strength. Wherein the aromatic diamine and the aromatic anhydride are used as raw materials of the base material, and excellent thermal conductivity and mechanical strength are provided for the membrane material. The introduction of fluorine-containing silane improves the thermal conductivity and moisture permeability of the membrane material. The carbon material is used as a filler, so that the thermal conductivity and the electrical conductivity of the film are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane materials, and in particular to a membrane material for a heat exchange core and a preparation method and application thereof. Background Art

[0002] Heat exchange refers to the process of transferring and exchanging heat between two or more fluids through a certain medium or device. This process is crucial in many industrial and daily applications, such as in air conditioning systems, cooling systems, energy recovery and other fields. Its basic principle is to transfer heat from one fluid to another fluid through heat conduction, convection or radiation, so as to achieve effective utilization or regulation of heat. The design and performance of heat exchange devices directly affect the efficiency and energy saving effect of the system, so it has received widespread attention in the engineering field.

[0003] In a heat exchange system, the heat exchange core is one of the core components. The heat exchange core is a component specially designed to enhance the efficiency of heat exchange. It is usually composed of multiple layers of materials through which heat can be efficiently transferred between fluids. The design of the heat exchange core takes into account factors such as fluid flow, thermal conductivity, surface area, etc. to achieve the best heat exchange effect. Common heat exchange core forms include plate heat exchangers, shell and tube heat exchangers, and fin heat exchangers. These design solutions are all aimed at improving heat exchange efficiency and reducing the size and weight of the device.

[0004] Membrane materials for heat exchange cores are key materials that make up the heat exchange core. Their main function is to provide an effective heat transfer medium. These membrane materials usually have high thermal conductivity to ensure that heat can be quickly transferred from one fluid to another. In addition, membrane materials also need to have good mechanical strength and corrosion resistance to cope with operating conditions under different working conditions. The choice of membrane materials directly affects the overall performance of the heat exchange core, so the development and optimization of these materials is an important area to improve the performance of heat exchange equipment.

[0005] However, there are some problems with the existing membrane materials for heat exchange cores in practical applications. First, poor thermal conductivity is a major problem. Although some membrane materials have high thermal conductivity, in practical applications, the thermal conductivity of the material may be affected by factors such as the manufacturing process, material thickness, and fluid flow mode, resulting in heat transfer efficiency that is not as expected. Secondly, poor perspective performance is also a problem. During the heat exchange process, the membrane material requires not only good thermal conductivity, but also sufficient transparency to ensure that heat can effectively penetrate the membrane layer. If the perspective performance of the membrane material is insufficient, it may cause uneven heat transfer, thereby affecting the overall heat exchange efficiency. In addition, the strength of the membrane material is also an issue that needs attention. In order to work stably in high pressure, high temperature or corrosive environments, the membrane material needs to have sufficient mechanical strength and durability. However, existing membrane materials often have deficiencies in strength, which may cause aging, breakage and other problems in the material during use, thereby affecting the reliability and service life of the heat exchange equipment.

[0006] The root of these problems is usually related to material selection and processing technology. The thermal conductivity, perspective performance and strength of the material are closely related to its chemical composition, microstructure and manufacturing process. For example, some membrane materials may contain more fillers or impurities, resulting in reduced thermal conductivity. Or during the manufacturing process, the material structure may be non-uniform, resulting in reduced efficiency of heat transfer.

[0007] Based on this, it is urgent to develop a new type of membrane material for heat exchange core to solve the above problems. Summary of the invention

[0008] The object of the present invention is to provide a membrane material for a heat exchange core having high thermal conductivity, high moisture permeability and high strength.

[0009] The first aspect of the present invention is:

[0010] A membrane material is provided.

[0011] The second aspect of the present invention is:

[0012] Provided is a method for preparing a membrane material.

[0013] The third aspect of the present invention is:

[0014] Application of the membrane material.

[0015] The invention also provides a heat exchange core.

[0016] Specifically, the technical solution adopted according to the first aspect of the present invention is:

[0017] A membrane material, the raw materials of which include the following components:

[0018] Aromatic diamines;

[0019] Aromatic anhydrides;

[0020] Fluorinated silanes;

[0021] Carbon material.

[0022] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0023] The membrane material of the present invention is a membrane material with high thermal conductivity, high moisture permeability and high strength. Among them, aromatic diamine and aromatic anhydride are used as raw materials of the base material to provide excellent thermal conductivity and mechanical strength for the membrane material. The introduction of fluorine-containing silane improves the thermal conductivity and moisture permeability of the membrane material. Carbon material is used as a filler to further improve the thermal conductivity and electrical conductivity of the membrane.

[0024] According to one embodiment of the present invention, the raw materials of the membrane material include the following components in parts by weight:

[0025] Aromatic diamine, 50-60 parts;

[0026] Aromatic anhydride, 70-100 parts;

[0027] Fluorine-containing silane, 2-10 parts;

[0028] Carbon material, 5-15 parts.

[0029] The appropriate amount of raw materials ensures that a three-dimensional heat conduction channel is constructed in the membrane material.

[0030] According to one embodiment of the present invention, the aromatic diamine includes at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminobenzene, 2,2'-diaminobenzene, 1,3-phenylenediamine and 1,4-phenylenediamine.

[0031] According to one embodiment of the present invention, the aromatic anhydride includes at least one of terephthalic anhydride, pyromellitic anhydride, phthalic anhydride and benzoic anhydride.

[0032] According to one embodiment of the present invention, the fluorine-containing silane includes at least one of (trifluoromethyl)trimethylsilane, fluorophenylsilane, fluoroaminosilane, perfluorosilane and fluorinated dimethylsilane.

[0033] According to one embodiment of the present invention, the fluorine-containing silane includes (trifluoromethyl)trimethylsilane.

[0034] The membrane material of the present invention uses aromatic diamine and aromatic anhydride to construct a base membrane material containing polyimide, and the membrane material has a certain thermal conductivity. On this basis, the present invention introduces fluorine-containing silane to further improve the thermal conductivity of the membrane material of the present invention and impart a certain moisture permeability.

[0035] According to one embodiment of the present invention, the carbon material includes at least one of graphene oxide, graphene, carbon nanotubes and acetylene black.

[0036] According to one embodiment of the present invention, the carbon material includes graphene oxide. Graphene oxide has a higher specific surface area and excellent dispersibility, and can be evenly distributed in the matrix material, thereby significantly improving the thermal conductivity of the film. In addition, graphene oxide has more surface functional groups, such as hydroxyl groups, which can effectively improve the interface contact of the material, thereby promoting the conduction of heat.

[0037] According to one embodiment of the present invention, the raw material of the membrane material further includes the following components: a fluorine-containing metal complex.

[0038] After the introduction of fluorine-containing silane into the membrane material of the present invention, although the thermal conductivity of the membrane material is further improved, the thermal stability of the membrane material will be affected. For example, when the fluorine-containing silane is preferably (trifluoromethyl)trimethylsilane, although the thermal conductivity of the membrane material of the present invention is excellent, the trifluoromethyl group (-CF3) in (trifluoromethyl)trimethylsilane has a very strong electron-attracting property. This strong electron-attracting effect will make the adjacent chemical bonds more easily broken in a high temperature environment, thereby affecting the stability of the membrane material.

[0039] Therefore, by adding a fluorine-containing metal complex, it is possible to effectively coordinate with fluorine-containing silanes such as (trifluoromethyl)trimethylsilane and form a complex, thereby affecting the electronic effect of (trifluoromethyl)trimethylsilane through coordination. This coordination will shield the electronic effect of the trifluoromethyl group to a certain extent.

[0040] In addition, the fluoride ions in the fluorine-containing metal complex can react with the hydroxyl groups on the surface of the carbon material, improve the interfacial adhesion of the carbon material, and enhance the bonding strength between the filler (carbon material) and the matrix (polyimide). Stronger interfacial adhesion can better transfer the reinforcing effect of the carbon material to the matrix.

[0041] According to one embodiment of the present invention, the fluorine-containing metal complex includes at least one of tetraaminocopper (II) fluoride complex, copper (II) chloride fluoride complex, iron (III) hexafluoride complex, aluminum (III) tetrafluoride complex, magnesium (II) tetrafluoride complex, titanium (IV) tetrafluoride complex and potassium fluoride (I) complex.

[0042] According to one embodiment of the present invention, the raw material of the membrane material further includes the following components: sulfonic acid and a catalyst.

[0043] According to one embodiment of the present invention, the sulfonic acid includes at least one of p-nitrobenzenesulfonic acid and p-toluenesulfonic acid. The introduction of sulfonic acid can promote the imidization reaction during the polymerization process, increase the reaction rate, help adjust the acid-base environment of the reaction, and optimize the performance of the polymer.

[0044] According to one embodiment of the present invention, the catalyst includes at least one of isoquinoline, aminopyridine, pyridine and furan. The introduction of the catalyst can promote the polymerization reaction and improve the molecular weight of the polymer and the uniformity of the reaction.

[0045] Specifically, the technical solution adopted according to the second aspect of the present invention is:

[0046] A method for preparing the membrane material comprises the following steps:

[0047] S1 mixes aromatic diamine and aromatic anhydride to obtain a mixture;

[0048] S2: adding carbon material and fluorine-containing silane to the mixture, and subjecting the mixture to a heating polymerization reaction to obtain the membrane material.

[0049] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0050] The preparation method of the present invention significantly improves the thermal conductivity of the film by mixing aromatic diamine and aromatic anhydride, adding carbon material and fluorine-containing silane, and then performing a heating polymerization reaction. The addition of carbon material enhances the thermal conductivity of the film, making the heat exchange efficiency higher, and also improves the mechanical strength and toughness of the film. The polyamide structure formed by aromatic diamine and aromatic anhydride provides a solid matrix to ensure the durability of the film. The introduction of fluorine-containing silane further improves the thermal conductivity of the film.

[0051] According to one embodiment of the present invention, the temperature of the heating polymerization reaction is 80-180°C.

[0052] According to one embodiment of the present invention, the heating polymerization reaction has a reaction time of 8-24 hours.

[0053] According to one embodiment of the present invention, the.

[0054] Another aspect of the present invention further provides a heat exchange core, including the membrane material as described in the first embodiment. Since the application adopts all the technical solutions of the membrane material, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.

[0055] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION

[0056] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0057] In the description of the present invention, it should be understood that descriptions involving orientation, such as orientation or positional relationship indicated as up, down, etc., are based on the orientation or positional relationship shown in the embodiments, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0058] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0059] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0060] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0061] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0062] In the embodiment and comparative example, the preparation method of Cu(NH3)2F2 comprises the following steps: mixing CuO and H2SiF6 solution, reacting overnight, filtering and collecting the product copper (II) fluoride. Taking 1 part by weight of copper (II) fluoride, adding it into water to obtain a copper (II) fluoride aqueous solution, slowly adding the copper (II) fluoride aqueous solution into 25% ammonia water, stirring until a precipitate is completely formed, and drying to obtain Cu(NH3)2F2.

[0063] In the embodiment, the preparation method of Cu(Cl2)F2 comprises the following steps: mixing CuO and H2SiF6 solution, reacting overnight, filtering and collecting the product copper (II) fluoride. Taking 1 part by weight of copper (II) fluoride, adding it into water to obtain a copper (II) fluoride aqueous solution, dropping a 40% hydrogen fluoride solution into the copper (II) fluoride aqueous solution, stirring until a precipitate is completely formed, and drying to obtain Cu(Cl2)F2.

[0064] Example 1

[0065] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0066] Aromatic diamine, 50 parts;

[0067] Aromatic anhydride, 70 parts;

[0068] Fluorosilane, 3.5 parts;

[0069] Carbon material, 5 parts.

[0070] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0071] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0072] Wherein, the carbon material is graphene oxide.

[0073] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0074] The method for preparing the above-mentioned membrane material comprises the following steps:

[0075] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0076] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid and 2.5 parts of (trifluoromethyl)trimethylsilane to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained a membrane material.

[0077] Example 2

[0078] The difference between Example 2 and Example 1 is that the fluorine-containing silane is different. The fluorine-containing silane in Example 2 is trityl fluorosilane.

[0079] Specific:

[0080] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0081] Aromatic diamine, 50 parts;

[0082] Aromatic anhydride, 70 parts;

[0083] Fluorosilane, 3.5 parts;

[0084] Carbon material, 5 parts.

[0085] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0086] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0087] Among them, the carbon material is graphene oxide.

[0088] The fluorine-containing silane is trityl fluorosilane.

[0089] The method for preparing the above-mentioned membrane material comprises the following steps:

[0090] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0091] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid and 2.5 parts of trityl fluorosilane to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained a membrane material.

[0092] Example 3

[0093] The difference between Example 3 and Example 1 is that in Example 3, the raw material of the membrane material also includes a fluorine-containing metal complex.

[0094] Specific:

[0095] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0096] Aromatic diamine, 50 parts;

[0097] Aromatic anhydride, 70 parts;

[0098] Fluorosilane, 3.5 parts;

[0099] Carbon material, 5 parts;

[0100] Fluorine-containing metal complex, 0.8 parts.

[0101] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0102] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0103] Among them, the carbon material is graphene oxide.

[0104] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0105] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0106] The method for preparing the above-mentioned membrane material comprises the following steps:

[0107] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0108] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0109] Example 4

[0110] The difference between Example 4 and Example 3 is that the fluorine-containing metal complex is different. The fluorine-containing metal complex in Example 4 is Cu(Cl2)F2.

[0111] Specific:

[0112] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0113] Aromatic diamine, 50 parts;

[0114] Aromatic anhydride, 70 parts;

[0115] Fluorosilane, 3.5 parts;

[0116] Carbon material, 5 parts;

[0117] Fluorine-containing metal complex, 0.8 parts.

[0118] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0119] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0120] Among them, the carbon material is graphene oxide.

[0121] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0122] Wherein, the fluorine-containing metal complex is Cu(Cl2)F2.

[0123] The method for preparing the above-mentioned membrane material comprises the following steps:

[0124] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0125] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of Cu(Cl2)F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0126] Example 5

[0127] The difference between Example 5 and Example 3 is that the carbon material is different, and the carbon material in Example 5 is graphene.

[0128] Specific:

[0129] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0130] Aromatic diamine, 50 parts;

[0131] Aromatic anhydride, 70 parts;

[0132] Fluorosilane, 3.5 parts;

[0133] Carbon material, 5 parts;

[0134] Fluorine-containing metal complex, 0.8 parts.

[0135] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0136] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0137] Among them, the carbon material is graphene.

[0138] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0139] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0140] The method for preparing the above-mentioned membrane material comprises the following steps:

[0141] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0142] S2 added 5 parts of graphene, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of copper (II) fluoride complex to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0143] Example 6

[0144] The difference between Example 6 and Example 3 is that the carbon material is different. The carbon material of Example 6 is carbon nanotube.

[0145] Specific:

[0146] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0147] Aromatic diamine, 50 parts;

[0148] Aromatic anhydride, 70 parts;

[0149] Fluorosilane, 3.5 parts;

[0150] Carbon material, 5 parts;

[0151] Fluorine-containing metal complex, 0.8 parts.

[0152] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0153] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0154] Among them, the carbon material is carbon nanotube.

[0155] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0156] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0157] The method for preparing the above-mentioned membrane material comprises the following steps:

[0158] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0159] S2 added 5 parts of carbon nanotubes, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of copper (II) fluoride complex to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0160] Example 7

[0161] The difference between Example 7 and Example 3 is that the carbon material is different. The carbon material in Example 7 is acetylene black.

[0162] Specific:

[0163] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0164] Aromatic diamine, 50 parts;

[0165] Aromatic anhydride, 70 parts;

[0166] Fluorosilane, 3.5 parts;

[0167] Carbon material, 5 parts;

[0168] Fluorine-containing metal complex, 0.8 parts.

[0169] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0170] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0171] Wherein, the carbon material is acetylene black.

[0172] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0173] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0174] The method for preparing the above-mentioned membrane material comprises the following steps:

[0175] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0176] S2 added 5 parts of acetylene black, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of copper (II) fluoride complex to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0177] Example 8

[0178] The difference between Example 8 and Example 3 is that the amounts of components are different.

[0179] Specific:

[0180] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0181] Aromatic diamine, 60 parts;

[0182] Aromatic anhydride, 100 parts;

[0183] Fluorosilane, 3.5 parts;

[0184] Carbon material, 5 parts;

[0185] Fluorine-containing metal complex, 0.8 parts.

[0186] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0187] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0188] Among them, the carbon material is graphene oxide.

[0189] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0190] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0191] The method for preparing the above-mentioned membrane material comprises the following steps:

[0192] S1: dissolving 60 parts of pyromellitic anhydride and 100 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0193] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0194] Example 9

[0195] The difference between Example 9 and Example 3 is that the amounts of components are different.

[0196] Specific:

[0197] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0198] Aromatic diamine, 50 parts;

[0199] Aromatic anhydride, 70 parts;

[0200] Fluorosilane, 5 parts;

[0201] Carbon material, 5 parts;

[0202] Fluorine-containing metal complex, 0.8 parts.

[0203] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0204] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0205] Among them, the carbon material is graphene oxide.

[0206] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0207] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0208] The method for preparing the above-mentioned membrane material comprises the following steps:

[0209] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0210] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 5 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0211] Example 10

[0212] The difference between Example 10 and Example 3 is that the amounts of components are different.

[0213] Specific:

[0214] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0215] Aromatic diamine, 50 parts;

[0216] Aromatic anhydride, 70 parts;

[0217] Fluorosilane, 3.5 parts;

[0218] Carbon material, 8 parts;

[0219] Fluorine-containing metal complex, 1.2 parts.

[0220] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0221] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0222] Among them, the carbon material is graphene oxide.

[0223] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0224] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0225] The method for preparing the above-mentioned membrane material comprises the following steps:

[0226] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0227] S2 added 8 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2.5 parts of (trifluoromethyl)trimethylsilane and 1.2 parts of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0228] Embodiment 11

[0229] The difference between Example 11 and Example 3 is that the amounts of components are different.

[0230] Specific:

[0231] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0232] Aromatic diamine, 50 parts;

[0233] Aromatic anhydride, 70 parts;

[0234] Fluorosilane, 5 parts;

[0235] Carbon material, 8 parts;

[0236] Fluorine-containing metal complex, 1.2 parts.

[0237] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0238] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0239] Among them, the carbon material is graphene oxide.

[0240] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0241] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0242] The method for preparing the above-mentioned membrane material comprises the following steps:

[0243] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0244] S2 added 8 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 5 parts of (trifluoromethyl)trimethylsilane and 1.2 parts of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0245] Example 12

[0246] The difference between Example 12 and Example 3 is that the amounts of components are different.

[0247] Specific:

[0248] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0249] Aromatic diamine, 60 parts;

[0250] Aromatic anhydride, 80 parts;

[0251] Fluorosilane, 2 parts;

[0252] Carbon material, 5 parts;

[0253] Fluorine-containing metal complex, 0.8 parts.

[0254] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0255] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0256] Among them, the carbon material is graphene oxide.

[0257] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0258] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0259] The method for preparing the above-mentioned membrane material comprises the following steps:

[0260] S1: dissolving 60 parts of pyromellitic anhydride and 80 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0261] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 2 parts of (trifluoromethyl)trimethylsilane and 0.8 parts of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0262] Embodiment 13

[0263] The difference between Example 13 and Example 7 is that the amounts of components are different.

[0264] Specific:

[0265] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0266] Aromatic diamine, 50 parts;

[0267] Aromatic anhydride, 70 parts;

[0268] Fluorosilane, 4.5 parts;

[0269] Carbon material, 6 parts;

[0270] Fluorinated metal complex, 1 part.

[0271] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0272] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0273] Among them, the carbon material is graphene oxide.

[0274] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0275] Wherein, the fluorine-containing metal complex is Cu(NH3)2]F2.

[0276] The method for preparing the above-mentioned membrane material comprises the following steps:

[0277] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0278] S2 added 6 parts of graphene oxide, 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid, 4.5 parts of (trifluoromethyl)trimethylsilane and 1 part of Cu(NH3)2]F2 to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained the membrane material.

[0279] Comparative Example 1

[0280] The difference between Comparative Example 1 and Example 1 is that the raw material of the membrane material of Comparative Example 1 does not contain carbon material.

[0281] Specific:

[0282] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0283] Aromatic diamine, 50 parts;

[0284] Aromatic anhydride, 70 parts;

[0285] Fluorosilane, 3.5 parts.

[0286] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0287] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0288] Among them, the fluorine-containing silane is (trifluoromethyl)trimethylsilane.

[0289] The method for preparing the above-mentioned membrane material comprises the following steps:

[0290] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0291] S2: add 3 parts of isoquinoline, 3 parts of p-toluenesulfonic acid and 2.5 parts of (trifluoromethyl)trimethylsilane to the mixture, raise the temperature to 80°C, carry out polymerization reaction for 7 hours, raise the temperature to 180°C, react for 12 hours, and obtain a membrane material.

[0292] Comparative Example 2

[0293] The difference between Comparative Example 2 and Example 1 is that the raw material of the membrane material of Comparative Example 2 does not contain fluorine-containing silane.

[0294] Specific:

[0295] A membrane material, wherein the raw materials of the membrane material include the following components in parts by weight:

[0296] Aromatic diamine, 50 parts;

[0297] Aromatic anhydride, 70 parts;

[0298] Carbon material, 5 parts.

[0299] Wherein, the aromatic diamine is 4,4'-diaminodiphenyl ether.

[0300] Wherein, the aromatic anhydride is pyromellitic dianhydride.

[0301] Among them, the carbon material is graphene oxide.

[0302] The method for preparing the above-mentioned membrane material comprises the following steps:

[0303] S1: dissolving 70 parts of pyromellitic anhydride and 50 parts of 4,4'-diaminodiphenyl ether in 520 parts of N-methylpyrrolidone to obtain a mixture;

[0304] S2 added 5 parts of graphene oxide, 3 parts of isoquinoline, and 3 parts of p-toluenesulfonic acid to the mixture, raised the temperature to 80°C, carried out polymerization reaction for 7 hours, raised the temperature to 180°C, reacted for 12 hours, and obtained a membrane material.

[0305] Performance Test:

[0306] The membrane materials prepared in Examples 1-14 and Comparative Examples 1-2 were coated and dried on a template to form a film with a thickness of 100 μm. The films were taken for the following tests. The test results are shown in Table 1. The instrument used for the test was a Hot Disk thermal conductivity meter.

[0307] Table 1

[0308]

[0309]

[0310] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A membrane material, characterized in that: The raw materials of the membrane material include the following components: Aromatic diamines; Aromatic anhydrides; Fluorinated silanes; Carbon material.

2. A membrane material according to claim 1, characterized in that: The raw materials of the membrane material include the following components in parts by weight: Aromatic diamine, 50-60 parts; Aromatic anhydride, 70-100 parts; Fluorine-containing silane, 2-10 parts; Carbon material, 5-15 parts.

3. A membrane material according to claim 1, characterized in that: The aromatic diamine includes at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminobenzene, 2,2'-diaminobenzene, 1,3-phenylenediamine and 1,4-phenylenediamine.

4. A membrane material according to claim 1, characterized in that: The aromatic anhydride includes at least one of terephthalic anhydride, pyromellitic anhydride, phthalic anhydride and benzoic anhydride.

5. A membrane material according to claim 1, characterized in that: The fluorine-containing silane includes at least one of (trifluoromethyl)trimethylsilane, fluorophenylsilane, fluoroaminosilane, perfluorosilane and fluorinated dimethylsilane.

6. A membrane material according to claim 1, characterized in that: The carbon material includes at least one of graphene oxide, graphene, carbon nanotubes and acetylene black.

7. A membrane material according to claim 1, characterized in that: The raw materials of the membrane material also include the following components: fluorine-containing metal complex.

8. A membrane material according to claim 7, characterized in that: The fluorine-containing metal complex includes at least one of tetraaminocopper(II) fluoride complex, copper(II) chloride fluoride complex, iron(III) hexafluoride complex, aluminum(III) tetrafluoride complex, magnesium(II) tetrafluoride complex, titanium(IV) tetrafluoride complex and potassium(I) fluoride complex.

9. A method for preparing a membrane material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1 mixes aromatic diamine and aromatic anhydride to obtain a mixture; S2: adding carbon material and fluorine-containing silane to the mixture, and subjecting the mixture to a heating polymerization reaction to obtain the membrane material.

10. A heat exchange core, characterized in that: The invention comprises a membrane material as claimed in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method for graphene-polyimide composite film

    CN103665866A

  • Production method of high-heat conduction polyimide film

    CN106496611A

  • Graphene-containing heat conducting polyimide film and preparation method thereof

    CN109957126A

  • Heat-conducting silicone grease as well as preparation method and application of heat-conducting silicone grease

    CN116254000A

  • Ultrahigh specific energy cathode material for lithium ion battery and production method thereof