Fully biodegradable PGA foaming material and preparation method thereof
By combining a blending system of polyglycolic acid (PGA) with glass fibers with twin screw extrusion and supercritical CO2 foaming, a fully biodegradable PGA foaming material with high hardness and uniform pore size was prepared, and the existing technology was solved. The problem of insufficient mechanical properties of PGA foaming materials in China has achieved the goal of replacing non-degradable foam plastics and is used to solve the problem of "white pollution".
Patent Information
- Application Number
- CN202310663535.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
The existing fully biodegradable foaming materials have shortcomings in terms of mechanical properties and pore size uniformity, and it is difficult to replace non-degradable foam plastics. Especially foaming materials with pure polyglycolic acid (PGA) as the matrix have not been fully explored in terms of performance. .
A blended system formed by polyglycolic acid (PGA) and glass fibers is prepared by twin screw extrusion and supercritical CO2 foaming process. The formula includes 45-93% PGA, 0.5-5% melt reinforcement, 5 -50% glass fiber, 0.5-3% compatibility agent and 0.5-1.5% antioxidant, the mass ratio of glass fiber to PGA is 2:8-5:5, and the melt reinforcement contains epoxy functional groups. The copolymer and polyisocyanate compounds of the same, the compatible agent is maleic anhydride graft polymer, and the antioxidant is phosphite esters.
It has prepared a fully biodegradable PGA foaming material with high hardness, light weight, small pore size and uniformity. It has excellent mechanical properties and can replace non-degradable foam plastics for disposable foaming tableware and transportation packaging, which solves the problem of " White pollution problem.
Smart Images

Figure BDA0004270117630000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of foaming materials, and in particular relates to a fully biodegradable PGA foaming material and a preparation method thereof. Background Art
[0002] Non-degradable plastic bags, disposable plastic tableware, express delivery plastic packaging, etc. are included in the scope of plastic products that are prohibited or restricted. In addition, as people's pace of life accelerates, the demand for disposable foam plastic packaging is increasing day by day.
[0003] If a fully biodegradable foam material is developed that is light in weight, has small and uniform pore size, and has excellent mechanical properties, it can replace most of the non-degradable and difficult-to-recycle foam plastics currently in use, and is an important way to solve the "white pollution".
[0004] Patent document CN107541031A discloses a fully biodegradable foaming material of modified PGA or PLGA and a preparation method thereof, comprising components: 30-80 parts of PGA or PLGA, 20-60 parts of PBAT, 0.1-0.5 parts of a cross-linking agent, 3-10 parts of a chemical foaming agent, 0.05-0.1 parts of an antioxidant, 0.1-0.5 parts of a lubricant, and a product is obtained by screw extrusion foaming. The foaming material in the patent uses a cross-linker-modified PGA mixture, and is a mixture of PGA and PBAT, and does not conduct an in-depth study of the foaming material with pure PGA as the base resin.
[0005] Patent document CN109651783A discloses a micro-foamed natural fiber reinforced polylactic acid composite material and its preparation method, comprising: 10-89.8% natural fiber, 10-89.8% polylactic acid, 0.1-10% epoxy chain extender, 0.1-2% initiator, 0.1-10% maleic anhydride, 0.1-2% other additives, and obtaining a foamed material with fine pores through an extrusion processing method. This patent is mainly for foaming with PLA as the matrix, and the natural fiber used therein has poor temperature resistance, which will have an adverse effect on the performance of the obtained foamed material.
[0006] In view of this, how to use pure polyglycolic acid (PGA) resin as the base resin and form a blending system with glass fiber to foam and prepare a foamed material with light weight, small and uniform pore size, and excellent mechanical properties has become a direction worthy of research. Summary of the invention
[0007] The purpose of the present invention is to provide a fully biodegradable PGA foam material and a preparation method thereof in view of the problems existing in the existing fully biodegradable foam materials, so as to obtain a fully biodegradable PGA foam material with light weight, small and uniform pores and high mechanical properties.
[0008] In order to achieve the above object, the technical solution of the present invention is as follows:
[0009] In a first aspect, a fully biodegradable PGA foam material is provided, which is prepared by foaming the following raw material components, based on the total weight of each component:
[0010] Polyglycolic acid (PGA) is 45-93 parts by weight (e.g., 50 parts by weight, 60 parts by weight, 65 parts by weight, 72 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight), preferably 70-88 parts by weight;
[0011] The melt enhancer is 0.5-5 parts by weight (such as 0.8 parts by weight, 1.2 parts by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 4 parts by weight), preferably 1-3 parts by weight;
[0012] The glass fiber masterbatch is 5-50 parts by weight (such as 8 parts by weight, 12 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight), preferably 10-25 parts by weight;
[0013] The compatibilizer is 0.5-3 parts by weight (such as 0.8 parts by weight, 1.2 parts by weight, 1.5 parts by weight, 1.8 parts by weight, 2.5 parts by weight), preferably 1-2 parts by weight;
[0014] The antioxidant is 0.5-1.5 parts by weight (such as 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1.2 parts by weight, 1.4 parts by weight), preferably 0.5-1 parts by weight;
[0015] Wherein, in the glass fiber masterbatch, the mass ratio of glass fiber to polyglycolic acid (PGA) is 2:8-5:5 (eg, 4:6), preferably 3:7-5:5.
[0016] The glass fiber masterbatch includes glass fiber and PGA. In the formula of raw material components, for example, when the mass ratio of glass fiber to PGA in the glass fiber masterbatch is 4:6, the glass fiber content in the PGA foaming material can be converted into 2-20 parts by weight (3 parts by weight, 5 parts by weight, 12 parts by weight, 15 parts by weight, 18 parts by weight), preferably 5-10 parts by weight.
[0017] According to the PGA foam material provided by the present invention, in some embodiments, the weight average molecular weight of the polyglycolic acid is greater than or equal to 50,000 and less than or equal to 500,000 (for example, 60,000, 80,000, 90,000, 100,000, 120,000, 150,000, 180,000, 220,000, 300,000, 400,000); the melt index at 240°C and 2.16kg is 5-70g / min (for example, 8g / min, 12g / min, 15g / min, 20g / min, 25g / min, 40g / min, 50g / min, 60g / min), preferably 10-30g / 10min.
[0018] In some embodiments, the diameter of the glass fiber is 5-20 μm (e.g., 6 μm, 8 μm, 12 μm, 14 μm, 18 μm), preferably 10-15 μm; the aspect ratio is 300: 1-1000: 1 (e.g., 350: 1, 400: 1, 450: 1, 600: 1, 750: 1, 850: 1, 900: 1), preferably 500: 1-800: 1. The present invention selects the range of the diameter and aspect ratio of the glass fiber. If the fiber length is too long, the processing will be cut off due to granulation, which will bring inconvenience to the processing technology; if the fiber length is too short, it cannot play a good supporting role for the foamed cells and can only play the role of a nucleating agent; in addition, considering the thickness of the cell wall of the foaming material, if the fiber diameter is too large, the compatibility between the foaming cells and the cell wall is poor, and the fiber is easily pulled out, resulting in poor cell airtightness; if the fiber diameter is too small, there will also be a defect of poor supporting force.
[0019] In some embodiments, the melt enhancer is a copolymer containing epoxy functional groups and / or a polyisocyanate compound, preferably a compound of a copolymer containing epoxy functional groups and a polyisocyanate compound.
[0020] In some embodiments, in the composite, the mass ratio of the copolymer containing epoxy functional groups to the polyisocyanate compound is (2-4):1 (such as 2.5:1, 3:1, 3.5:1), preferably 2:1.
[0021] In some embodiments, the copolymer containing epoxy functional groups is selected from styrene-acrylonitrile-glycidyl methacrylate copolymer and ethylene-methyl acrylate-glycidyl methacrylate copolymer.
[0022] In some embodiments, the polyisocyanate compound is selected from at least one of toluene-2,4-diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, lysine diisocyanate and polyisocyanate.
[0023] In some embodiments, the compatibilizer is a maleic anhydride grafted polymer, preferably at least one selected from ethylene-maleic anhydride grafted copolymer, polyolefin thermoplastic elastomer-maleic anhydride grafted copolymer and propylene-maleic anhydride grafted copolymer.
[0024] In some embodiments, the grafting rate of the maleic anhydride grafted polymer is 0.2-5 wt% (eg, 0.5 wt%, 0.8 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 3.0 wt%, 4.0 wt%).
[0025] In some embodiments, the antioxidant is a phosphite antioxidant, preferably one or more selected from antioxidant 168, antioxidant 1010, antioxidant 626 and antioxidant 9228.
[0026] In a second aspect, a method for preparing the fully biodegradable PGA foam material as described above is provided, comprising the following steps:
[0027] The raw material components are weighed respectively by mass and dried for later use; the dried materials are mixed evenly, extruded and granulated by a twin-screw extruder, and then foamed by a supercritical CO2 foaming process to obtain the fully biodegradable PGA foaming material.
[0028] In some embodiments, the drying temperature is 60-80° C. (eg, 70° C., 75° C.), and the drying time is 2-5 hours (eg, 3 hours, 4 hours).
[0029] In some embodiments, the extrusion granulation adopts a twin-screw extruder; the feeding section temperature of the twin-screw extruder is 180-210°C (such as 190°C, 200°C), the plasticizing section temperature is 200-230°C (such as 210°C, 220°C), the homogenizing section temperature is 220-235°C (such as 225°C, 230°C), the extrusion die temperature is 225-235°C (such as 230°C), the extrusion die pressure is 1-10MPa (such as 2MPa, 4MPa, 6MPa, 8MPa); the screw speed is 70-110rpm (such as 80rpm, 90rpm, 100rpm).
[0030] In some embodiments, the supercritical CO2 foaming process is to press the blend particles obtained by extrusion granulation into blend sheets and then foam them using supercritical CO2 gas.
[0031] In some embodiments, the process conditions of supercritical CO2 foaming include: foaming temperature of 224-230°C (such as 225°C, 228°C), foaming pressure of 5-20MPa (such as 6MPa, 10MPa, 15MPa), and foaming holding time of 0.5-3h (such as 1h, 2h, 2.5h).
[0032] The invention first modifies the blend formed by PGA and other components such as glass fiber, melt enhancer, compatibilizer, etc. by reaction extrusion, and then obtains a high-performance PGA foam material by chemical foaming. The foam material has high hardness, light weight, small and uniform pore size, and excellent mechanical properties. It is a fully biodegradable material that can be used for disposable foam tableware and transportation packaging, etc. It can replace most of the currently used non-degradable and difficult to recycle foam plastics, and is an important way to solve "white pollution".
[0033] The added glass fiber can play the role and effect of nucleation and cell support reinforcement when foaming in the blend. If the amount of glass fiber added is too little, there will be no nucleation and cell support reinforcement effect; if the amount of glass fiber added is too much, the dispersion uniformity of the glass fiber will deteriorate, which will lead to poor air retention and easy air leakage in the aggregated area formed by the glass fiber, resulting in foam collapse and poor foaming effect. Therefore, the appropriate range of glass fiber dosage should be selected according to the interaction with other components in the ratio.
[0034] Compared with other reinforcing fillers, glass fiber itself has a certain strength and a rod-like structure. This structure can play a supporting role in all directions of the bubbles during the foaming and shaping process of the blend, reducing the collapse of the bubbles. Other commonly used inorganic fillers (such as talcum powder, calcium carbonate, etc.) can only play a nucleating role and will not play a supporting role. The bubbles are still likely to shrink severely.
[0035] The present invention selects glass fiber as a nucleating agent and a cell supporting agent, and blends and extrude the glass fiber with a PGA resin in the form of a glass fiber masterbatch. In addition to the synergistic effect of compounding a copolymer containing an epoxy functional group and an isocyanate melt strengthener, the glass fiber can simultaneously exert a synergistic effect with the epoxy and isocyanate melt strengtheners, thereby effectively enhancing the expandability, supporting properties and nucleation properties of the polyglycolic acid, and obtaining a high-performance foaming material with small and uniform cells. DETAILED DESCRIPTION
[0036] In order to understand the technical features and contents of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described here.
[0037] <Source of raw materials>
[0038] Polyglycolic acid (PGA), weight average molecular weight of 220,000, melt index of 30 g / 10 min at 240°C and 2.16 kg, purchased from Shanghai Pujing;
[0039] Glass fiber, with a diameter of 10 μm and an aspect ratio of 300:1, was purchased from Taishan Glass Fiber Co., Ltd.;
[0040] Polyisocyanate (PMDI), PM200 produced by Wanhua Chemical (viscosity of 150-250 mPa.s at 25°C, -NCO content of 30.2-32% by weight, functionality of 2.6-2.7);
[0041] Copolymer containing epoxy functional groups: BASF ADR-4468 (GMA content is 10 wt %, weight average molecular weight is about 6680);
[0042] Antioxidant 168 and antioxidant 1010 were purchased from BASF;
[0043] Maleic anhydride grafted POE (compatibilizer), GR216, grafting rate 0.5wt%, Dow Chemical.
[0044] <Detection method>
[0045] 1. Foaming ratio test process: the density of the sample before foaming is marked as P1, and the density of the sample after foaming is marked as P2. P1 divided by P2 is the final foaming ratio;
[0046] 2. Test process of average pore diameter: Cut the cross section of the foam material sample with a paper cutter, observe the pore morphology under SEM, and use Image software to measure and count the pores in the SEM picture;
[0047] 3. Cell density test process: Cut a piece of foam material sample and measure its mass as A1, then press the whole sample into water and measure its mass as A2, and use A1 / A2 to get the foam density;
[0048] 4. Compression modulus test process: Cut the foam material into test samples with a length and width of 5 cm each, measure the thickness of the test sample, and use a mechanical measuring instrument to compress the thickness by 20% to obtain the compression modulus.
[0049] Preparation of glass fiber masterbatch with 40wt% content
[0050] The glass fiber and PGA are blended in a weight ratio of 4:6, and then the blend is melt-extruded in a twin-screw extruder and granulated to obtain a glass fiber masterbatch; wherein the melt extrusion process conditions are: the temperature of each zone of the screw extrusion is 220-235°C, and the screw speed is 80-100rpm.
[0051] Embodiment 1:
[0052] The preparation method of the fully biodegradable PGA foam material is as follows:
[0053] (1) drying polyglycolic acid (PGA), the glass fiber masterbatch prepared as above, melt enhancer (in the compound, the mass ratio of BASF ADR-4468 to polyisocyanate PMDI is 2:1), compatibilizer, antioxidant and other raw materials for use at a drying temperature of 80° C. for 5 hours;
[0054] (2) According to the formula ratio shown in Table 1, the dried raw material components are mixed uniformly, and then the mixed material is put into a twin-screw extruder for melting and extrusion; the feeding section temperature of the twin-screw extruder is 180-210° C., the plasticizing section temperature is 200-230° C., the homogenizing section temperature is 220-235° C., the extrusion die temperature is 225-235° C., the extrusion die pressure is 1-3 MPa, and the screw speed is 90 rpm; extrusion granulation is performed to obtain blend particles;
[0055] (3) The blend particles obtained in step (2) were tableted to obtain a blend sheet, which was then placed in a molded supercritical CO2 device for CO2 supercritical foaming, with the supercritical foaming temperature set to 228°C and the supercritical foaming pressure set to 20 MPa. The foaming was carried out at a constant temperature for 1 hour under these foaming conditions to obtain a foamed material. The test results of the foamed material properties are shown in Table 2.
[0056] Embodiment 2-4:
[0057] The operation process of Example 1 is referred to, except that the formula of the raw material components is different, and the ingredients are prepared as shown in Table 1. The test results of the foaming material properties are shown in Table 2.
[0058] Comparative Examples 1-3:
[0059] The operation process of Example 1 was followed, except that the formula of the raw material components was different, and the ingredients were prepared as shown in Table 1. The test results of the foaming material properties are shown in Table 2.
[0060] Table 1 Raw material formula of each embodiment and comparative example
[0061] PGA Glass fiber masterbatch Fiberglass Melt Enhancer Compatibilizer Antioxidants Example 1 90 6 / 2 1 1 Example 2 47 50 / 1 1 1 Example 3 75 20 / 3 1 1 Example 4 85 10 / 3 1 1 Comparative Example 1 78 20 / / 1 1 Comparative Example 2 98 / / 1 / 1 Comparative Example 3 86 / 10 2 1 1
[0062] Table 2 Performance test of foamed materials obtained in various embodiments and comparative examples
[0063]
[0064]
[0065] It can be seen from the experimental results that the foamed material prepared by the present invention can play a synergistic role with epoxy and isocyanate melt enhancers because it contains glass fiber as a nucleating agent and a pore supporting agent, effectively enhancing the expandability and nucleation of polyglycolic acid, and can obtain a light-weight, small-pore and uniform foamed material. At the same time, the hardness and compression modulus (as an indicator of hardness, the higher the compression modulus, the higher the hardness) of the foamed material are excellent.
[0066] In the raw material formula of Comparative Example 1, no melt enhancer is added. Although the glass fiber contained therein can play a certain nucleation and pore supporting role, the effect is not good. The pores of the foamed material are broken, making the foamed material unusable; in the raw material formula of Comparative Example 2, no glass fiber masterbatch and compatibilizer are added. Although the presence of the melt enhancer can play a certain reinforcing role on the foamed material, the melt enhancer has poor compatibility with the matrix resin, which has an adverse effect on the comprehensive performance of the foamed material. In addition, the synergistic reinforcement effect of the glass fiber and the melt enhancer cannot be achieved; in the raw material formula of Comparative Example 3, glass fiber is not added in the form of glass fiber masterbatch, so the glass fiber as a nucleating agent and pore supporting agent has a poor effect on improving the performance of the foamed material, and the comprehensive performance is poor.
[0067] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the spirit of the present invention.
Claims
1. A fully biodegradable PGA foaming material, It is characterized in that Based on the total weight of each component, the following raw material components are foamed: Polyglycolic acid is 45-93 parts by weight, preferably 70-88 parts by weight; The melt enhancer is 0.5-5 parts by weight, preferably 1-3 parts by weight; The glass fiber masterbatch is 5-50 parts by weight, preferably 10-25 parts by weight; The compatibilizer is 0.5-3 parts by weight, preferably 1-2 parts by weight; The antioxidant is 0.5-1.5 parts by weight, preferably 0.5-1 parts by weight; Wherein, in the glass fiber masterbatch, the mass ratio of glass fiber to polyglycolic acid is 2:8-5:5, preferably 3:7-5:
5.
2. The PGA foam material according to claim 1, It is characterized in that The weight average molecular weight of the polyglycolic acid is greater than or equal to 50,000 and less than or equal to 500,000; the melt index at 240° C. and 2.16 kg is 5-70 g / min, preferably 10-30 g / 10 min.
3. The PGA foam material according to claim 1, It is characterized in that The diameter of the glass fiber is 5-20 μm, preferably 10-15 μm; the aspect ratio is 300:1-1000:1, preferably 500:1-800:
1.
4. The PGA foam material according to claim 1, It is characterized in that The melt enhancer is a copolymer containing epoxy functional groups and / or a polyisocyanate compound, preferably a compound of a copolymer containing epoxy functional groups and a polyisocyanate compound; In the compound, the mass ratio of the copolymer containing epoxy functional groups to the polyisocyanate compound is (2-4):
1.
5. The PGA foam material according to claim 4, It is characterized in that The copolymer containing epoxy functional groups is selected from styrene-acrylonitrile-glycidyl methacrylate copolymer, ethylene-methyl acrylate-glycidyl methacrylate copolymer; and / or The polyisocyanate compound is selected from at least one of toluene-2,4-diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, lysine diisocyanate and polyisocyanate.
6. The PGA foam material according to claim 1, It is characterized in that The compatibilizer is a maleic anhydride grafted polymer, preferably at least one selected from ethylene-maleic anhydride grafted copolymer, polyolefin thermoplastic elastomer-maleic anhydride grafted copolymer and propylene-maleic anhydride grafted copolymer; Preferably, the grafting rate of the maleic anhydride grafted polymer is 0.2-5 wt %.
7. The PGA foam material according to claim 1, It is characterized in that The antioxidant is a phosphite antioxidant, preferably one or more selected from the group consisting of antioxidant 168, antioxidant 1010, antioxidant 626 and antioxidant 9228.
8. The method for preparing the fully biodegradable PGA foam material according to any one of claims 1 to 7, It is characterized in that The steps include: Weigh each raw material component by mass and dry it for later use; mix the dried materials evenly, extrude and granulate them through a twin-screw extruder, and then pass through a supercritical CO 2 The foaming process is used to foam the PGA to obtain the fully biodegradable PGA foaming material.
9. The preparation method according to claim 8, It is characterized in that The drying temperature is 60-80° C. and the drying time is 2-5 hours.
10. The preparation method according to claim 8, It is characterized in that The extrusion granulation adopts a twin-screw extruder; the feeding section temperature of the twin-screw extruder is 180-210°C, the plasticizing section temperature is 200-230°C, the homogenizing section temperature is 220-235°C, the extrusion die temperature is 225-235°C, the extrusion die pressure is 1-10MPa; the screw speed is 70-110rpm; and / or The supercritical CO 2 The foaming process is to press the blend particles obtained by extrusion granulation into blend sheets and then use supercritical CO 2 Gas for foaming; Preferably, the supercritical CO 2 The foaming process conditions include: foaming temperature of 224-230° C., foaming pressure of 5-20 MPa, and foaming pressure holding time of 0.5-3 h.
Citation Information
Patent Citations
A modified completely-biodegradable PGA or PLGA foaming material and a preparing method thereof
CN107541031A
Microcellular foamed natural fiber reinforced polylactic acid composite material and preparation method thereof
CN109651783A