Silica sol coating and preparation method thereof
Through the treatment of sodium silicate solution made of quartz sand and caustic soda and cation exchange resin, combined with antifouling agent and gel agent, the complex and susceptible preparation of silica sol coatings is solved, achieving high gloss, anti-pollution and Wear-resistant silicone sol coating ensures that the product is not prone to cracking and impact resistance after spraying.
Patent Information
- Application Number
- CN202411543148.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2024-12-06
AI Technical Summary
The existing silicon sol coating preparation methods are complex and susceptible to contamination, and cannot ensure anti-pollution and stability, resulting in the sprayed product being prone to cracking and impacting the blocks.
Sodium silicate solution is made through quartz sand and caustic soda, and sodium ions are replaced by strong acid cation exchange resin to form a combined hydrated silica sol, and antifouling agent, gel agent and dispersant are added, and polycondensation and pyrolysis reaction is carried out by a ball mill. , crystals are formed to improve adhesion.
The prepared silicone sol coating has high gloss, excellent decorative properties, good pollution resistance and wear resistance, and is not easy to crack and impact and remove blocks, improving the product performance after spraying.
Smart Images

Figure CN119081456A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a silica sol coating and a preparation method thereof. Background Art
[0002] Silica sol coatings were studied abroad in the 1960s, mainly by companies in the United States, Japan and South Korea. DuPont successfully developed nano-ceramic coatings for daily necessities such as non-stick pans, automobile exhaust pipes and electric irons. Kim, Johng Ha and others in South Korea developed inorganic ceramic coatings that can be applied to the surface of aluminum alloy substrates and galvanized sheets. KFCC in South Korea developed ceramic coatings that can be applied to aluminum alloy building curtain walls and subway vehicle interior decorative coatings, replacing the previous fluorocarbon curtain wall coatings. TRITON SYSTEMS and FREECOM in the United States have developed nano-ceramic coatings for glass surfaces.
[0003] In China, it started in the 1980s, with the KNT brand ceramic coatings developed by Shanghai Jinlitai Chemical Co., Ltd. and South Korea's KFCC Company. Shanghai Yicilong New Materials Technology Co., Ltd., Beijing Kairui Jiecheng Co., Ltd., Shenzhen Yilong Technology Co., Ltd. and Zhejiang Zhu Paint Co., Ltd. successively developed various silica sol coatings, which have been applied in corresponding occasions. Although the performance of silica sol coatings is particularly excellent, many coating companies in various regions have successfully developed them. For example, Chinese patent application number CN202410686264.0, published on October 1, 2024, discloses a method for preparing an aqueous silica sol, the method comprising the following steps: adding 10 to 15 parts by mass of sodium hydroxide to 40 to 60 parts by mass of ionized water and stirring; After stirring evenly, a sodium hydroxide solution is obtained. Under stirring conditions, 5 to 10 parts by weight of the sodium hydroxide solution are added to 40 to 60 parts by weight of deionized water, and the solution temperature is raised to 50 to 60° C. Then, under stirring conditions and under the protection of a nitrogen atmosphere, 40 to 60 parts by weight of an ethanol solution of methyl orthosilicate is added dropwise at a rate of 30 to 40 ml / min, and then stirred and aged to obtain an aqueous silica sol.
[0004] The above method is to add methyl orthosilicate ethanol solution into sodium hydroxide. Since methyl orthosilicate ethanol solution is easy to deliquesce, it needs to be added under the protection of nitrogen atmosphere, which makes the whole operation process complicated, makes the subsequent appearance easy to be contaminated, and cannot ensure anti-pollution and stability. Summary of the invention
[0005] The invention provides a silica sol coating and a preparation method thereof. The silica sol coating has high gloss, excellent decorative properties, excellent anti-pollution properties, and is not prone to cracking.
[0006] In order to achieve the above object, the present invention provides a method for preparing a silica sol coating, the specific steps of which include: S1 Preparation of associated hydrated silica sol.
[0007] (1) Quartz sand is weighed according to the weight ratio of quartz sand and caustic soda and placed in a furnace. Caustic soda is added and heated to form solid sodium silicate.
[0008] (2) The sodium silicate solid is dissolved by hot water method to obtain sodium silicate liquid.
[0009] (3) A strong acid cation exchange resin is added to the sodium silicate liquid in a weight ratio of 1:1, and the sodium ions are replaced by the hydrogen ions of the cation exchange resin to form a silicic acid solution.
[0010] (4) Adding the catalyst to the silicic acid solution according to the weight ratio of the silicic acid solution to the catalyst to prepare an associated hydrated silica sol.
[0011] S2: 140-160 parts of the associated hydrated silica sol are placed in a reactor and stirred.
[0012] S3: slowly add 90-110 parts of gelling agent, 0.4-0.6 parts of dispersant, 0.2-0.4 parts of wetting agent and 1.0-1.4 parts of antifouling agent in sequence during stirring to obtain a mixed material.
[0013] S4: placing the mixed material in a ball mill for polycondensation and pyrolysis reaction to obtain a silica sol coating.
[0014] The above method first prepares quartz sand into associated hydrated silica sol, and then adds antifouling agent, gelling agent and dispersant. Since a sodium silicate solution of a certain concentration is prepared by quartz sand and caustic soda, a silicic acid solution is formed, and then a strong acid cation exchange resin is used to pass a certain concentration of sodium silicate through the resin layer, and the sodium ions are replaced by hydrogen ions to form silicic acid, and a catalyst is used to obtain multi-molecular associated colloidal hydrated silica. After the hydrogen ions on the cation resin are replaced by sodium ions, the efficiency decreases, and hydrochloric acid must be used for regeneration. For continued use, various impurity anions such as sulfate and hydrochloride are removed by cation exchange resin, and the anions are regenerated by caustic soda solution to obtain associated hydrated silica sol, thereby forming crystals, so that the prepared silica sol has strong adhesion, so that when the silica sol is sprayed, the sprayed product is not easy to crack and resist impact and fall off.
[0015] Furthermore, after step S4, step S6 is specifically included to prepare white slurry.
[0016] S61: weigh all-red titanium dioxide, ultrafine talcum powder, barite powder, white carbon black and a dispersant, put them into isopropanol, stir and mix them to obtain an isopropanol mixture.
[0017] S62: The isopropyl alcohol mixture is placed on a sand mill for grinding to obtain a white slurry.
[0018] S63: placing the white slurry in the silica sol coating for mixing, and obtaining the white silica sol coating after the mixing is completed.
[0019] Furthermore, step S62 specifically includes grinding the isopropyl alcohol mixture to less than 25 microns on a grinder.
[0020] Furthermore, in step S4, the rotation speed of the ball mill is 30-50 rpm, and the reaction time is 3-5 hours.
[0021] Furthermore, in step S5, the drying temperature is 170°-190°, and the drying time is 15-25 minutes.
[0022] The silica sol coating prepared by the above method has high gloss, excellent decorative properties, improved flexibility, is not easy to crack and fall off due to impact, and has particularly excellent anti-pollution and wear resistance.
[0023] On the other hand, the present invention provides a technical solution: a silica sol coating, comprising the following raw materials in parts by weight: 140-160 parts of associated hydrated silica sol, 90-110 parts of a gelling agent, 0.4-0.6 parts of a dispersant, 0.2-0.4 parts of a wetting agent and 1.0-1.4 parts of an antifouling agent; the associated hydrated silica sol is prepared by adding 0.8-1.2 parts by weight of a catalyst to a silicic acid solution made of quartz sand and caustic soda, the catalyst is prepared by 0.3-0.5 parts by weight of dilute sulfuric acid and 0.5-0.7 parts by weight of dilute hydrochloric acid, and the weight ratio of the silicic acid solution to the catalyst is 149:1.
[0024] In the above arrangement, the use of quartz sand can ensure that the final coating has a good gloss, and the use of antifouling agents can ensure a good antifouling effect, so that the silica sol has a good antifouling and easy-to-clean function. A sodium silicate solution of a certain concentration is made by quartz sand and caustic soda, and then a silicic acid solution is formed. Then, after the hydrogen ions on the cationic resin are replaced by sodium ions through a catalyst, the efficiency decreases, and then hydrochloric acid is used for regeneration to obtain an associated hydrated silica sol, thereby forming crystals, so that the produced silica sol has a strong adhesion, so that when the silica sol is sprayed, the sprayed product is not easy to crack and resist impact and fall off.
[0025] Furthermore, the weight ratio of the quartz sand to the caustic soda is 3:2.
[0026] Further, it also includes 90-110 parts of white slurry; the white slurry is made of 20-40 parts of all-red titanium dioxide, 8-12 parts of ultrafine talc, 12-17 parts of ultrafine barite powder, 1-3 parts of white carbon black, 41-42 parts of isopropanol and 1.2-1.7 parts of dispersant; specifically, it also includes 100 parts of white slurry, which is made of 30 parts of all-red titanium dioxide, 10 parts of ultrafine talc, 15 parts of ultrafine barite powder, 2 parts of white carbon black, 41.5 parts of isopropanol and 1.5 parts of dispersant.
[0027] The above arrangement can form a white coating by adding white slurry, and the color effect is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a use effect diagram of the silica sol coating of the present invention applied to an artistic background wall.
[0029] Figure 2 This is a diagram showing the effect of the silica sol coating of the present invention being applied to a load-bearing column.
[0030] Figure 3 This is a diagram showing the effect of using the silica sol coating of the present invention on a subway platform DETAILED DESCRIPTION The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Example 1.
[0032] A method for preparing a silica sol coating, the specific steps comprising: S1 Preparation of associated hydrated silica sol.
[0033] (1) Quartz sand is weighed and placed in a furnace according to the weight ratio of quartz sand and caustic soda, and caustic soda is added and heated to prepare solid sodium silicate. Specifically, the weight ratio of quartz sand and caustic soda is 3:2.
[0034] (2) The sodium silicate solid is dissolved by hot water method to obtain sodium silicate liquid.
[0035] (3) A strong acid cation exchange resin is added to the sodium silicate liquid in a weight ratio of 1:1, and the sodium ions are replaced by the hydrogen ions of the cation exchange resin to form a silicic acid solution.
[0036] (4) Adding the catalyst to the silicic acid solution according to the weight ratio of the silicic acid solution to the catalyst to prepare an associated hydrated silica sol.
[0037] S2: Weigh 140 parts of the combined hydrated silica sol and place it in a reactor for stirring.
[0038] S3: 90 parts of gelling agent, 0.4 parts of dispersant, 0.2 parts of wetting agent and 1.0 parts of antifouling agent were slowly added in sequence during stirring to obtain a mixed material.
[0039] S4: placing the mixed material in a ball mill for polycondensation and pyrolysis reaction to obtain a silica sol coating.
[0040] The rotation speed of the ball mill was 30 rpm, and the reaction time was 3 hours.
[0041] The drying temperature is 170° and the drying time is 15 minutes.
[0042] Example 2.
[0043] A method for preparing a silica sol coating, the specific steps comprising: S1 Preparation of associated hydrated silica sol.
[0044] (1) Quartz sand is weighed and placed in a furnace according to the weight ratio of quartz sand and caustic soda, and caustic soda is added and heated to prepare solid sodium silicate. Specifically, the weight ratio of quartz sand and caustic soda is 3:2.
[0045] (2) The sodium silicate solid is dissolved by hot water method to obtain sodium silicate liquid.
[0046] (3) A strong acid cation exchange resin is added to the sodium silicate liquid in a weight ratio of 1:1, and the sodium ions are replaced by the hydrogen ions of the cation exchange resin to form a silicic acid solution.
[0047] (4) Adding the catalyst to the silicic acid solution according to the weight ratio of the silicic acid solution to the catalyst to prepare an associated hydrated silica sol.
[0048] S2: Weigh 150 parts of the combined hydrated silica sol and place it in a reactor for stirring.
[0049] S3: 100 parts of gelling agent, 0.5 parts of dispersant, 0.3 parts of wetting agent and 1.2 parts of antifouling agent are slowly added in sequence during stirring to obtain a mixed material.
[0050] S4: placing the mixed material in a ball mill for polycondensation and pyrolysis reaction to obtain a silica sol coating.
[0051] The rotation speed of the ball mill was 40 rpm, and the reaction time was 4 hours.
[0052] The drying temperature is 180° and the drying time is 20 minutes.
[0053] Example 3.
[0054] A method for preparing a silica sol coating, the specific steps comprising: S1 Preparation of associated hydrated silica sol.
[0055] (1) Quartz sand is weighed and placed in a furnace according to the weight ratio of quartz sand and caustic soda, and caustic soda is added and heated to prepare solid sodium silicate. Specifically, the weight ratio of quartz sand and caustic soda is 3:2.
[0056] (2) The sodium silicate solid is dissolved by hot water method to obtain sodium silicate liquid.
[0057] (3) A strong acid cation exchange resin is added to the sodium silicate liquid in a weight ratio of 1:1, and the sodium ions are replaced by the hydrogen ions of the cation exchange resin to form a silicic acid solution.
[0058] (4) Add a stabilizer and a catalyst to the silicic acid solution to obtain an associated hydrated silica sol.
[0059] S2: Weigh 160 parts of the combined hydrated silica sol and place it in a reactor for stirring.
[0060] S3: 110 parts of gelling agent, 0.6 parts of dispersant, 0.4 parts of wetting agent and 1.4 parts of antifouling agent were slowly added in sequence during stirring to obtain a mixed material.
[0061] S4: adding the catalyst to the silicic acid solution according to the weight ratio of the silicic acid solution to the catalyst to obtain an associated hydrated silica sol.
[0062] The rotation speed of the ball mill was 50 rpm, and the reaction time was 5 hours.
[0063] S5 uses an oven to spray the silica sol coating onto the metal surface and dry it, and the product is solidified and formed.
[0064] The drying temperature is 190° and the drying time is 25 minutes.
[0065] Example 4.
[0066] White pulp is added on the basis of the above three embodiments, and the specific steps of preparing the white pulp include: S61 Weigh 30 parts of all-red titanium dioxide, 10 parts of ultrafine talc, 15 parts of ultrafine barite powder, 2 parts of white carbon black and 1.5 parts of dispersant into 41.5 parts of isopropanol, stir and mix to obtain an isopropanol mixture.
[0067] S62: grinding the isopropyl alcohol mixture on a sand mill to obtain a white slurry. Specifically, grinding the isopropyl alcohol mixture on the grinder to less than 25 microns.
[0068] S63: placing the white slurry in the silica sol coating for mixing, and obtaining the white silica sol coating after the mixing is completed.
[0069] In another embodiment, the specific steps of preparing the white pulp include: S61 Weigh 20 parts of all-red titanium dioxide, 8 parts of ultrafine talc, 12 parts of ultrafine barite powder, 1 part of white carbon black and 1.2 parts of dispersant into 41 parts of isopropanol, stir and mix to obtain an isopropanol mixture.
[0070] S62: grinding the isopropyl alcohol mixture on a sand mill to obtain a white slurry. Specifically, grinding the isopropyl alcohol mixture on the grinder to less than 25 microns.
[0071] S63: placing the white slurry in the silica sol coating for mixing, and obtaining the white silica sol coating after the mixing is completed.
[0072] In another embodiment, the specific steps of preparing the white pulp include: S61 Weigh 40 parts of all-red titanium dioxide, 12 parts of ultrafine talc, 17 parts of ultrafine barite powder, 3 parts of white carbon black and 1.7 parts of dispersant into 42 parts of isopropanol, stir and mix to obtain an isopropanol mixture.
[0073] S62: grinding the isopropyl alcohol mixture on a sand mill to obtain a white slurry. Specifically, grinding the isopropyl alcohol mixture on the grinder to less than 25 microns.
[0074] S63: placing the white slurry in the silica sol coating for mixing, and obtaining the white silica sol coating after the mixing is completed.
[0075] Example 5.
[0076] The invention provides a method for preparing an associated hydrated silica sol.
[0077] High-grade quartz sand (such as Hunan Shimen Baisha) is heated in a furnace with caustic soda to form sodium silicate solid, which is then dissolved into sodium silicate liquid using hot water. Alternatively, concentrated alkali solution can be directly reacted with quartz sand in a reactor under heating and stirring to form sodium silicate solution.
[0078] Using strong acid cation exchange resin, the sodium ions of sodium silicate are replaced by hydrogen ions of cation exchange resin to form silicic acid. Using stabilizer and catalyst to mix, multi-molecule associated colloidal hydrated silica is obtained. Using spectrum circle detection. Combined with thermal differential analyzer, it can be known that it is not crystalline silica. Its typical molecular formula is , the structural formula of associated hydrated silicon dioxide is:
[0079] Example 6 In this embodiment, the formula of the silica sol coating is shown in Table 1 below.
[0080]
[0081] Table 1 The silica sol coating was sprayed on a steel plate, and the performance test results are shown in Table 2 below.
[0082]
[0083] Table 2 The performance of silica sol coating was compared with that of various coatings, and the results are shown in Table 3 below.
[0084]
[0085] Table 3 It can be seen from Tables 2 and 3 above that the steel plates sprayed with silica sol coating have excellent properties such as fastness, aging resistance and corrosion resistance.
[0086] In the field of building decoration, silica sol coating combines the advantages of ceramic tiles, rock panels, and decorative panels, and introduces the advantages of easy decoration and flexibility of coating, making it more convenient to use. The use of silica sol coating decoration on energy-saving and environmentally friendly building panels such as calcium silicate boards and ecological boards, which are currently widely used, has greatly improved their grade and can be made into large curtain wall panels, background walls, art boards, etc. It can be made into elegant thermal insulation wall tiles with hollow boards, foam magnesium boards, and foam tiles, and can be made into sterilization boards, infrared heating boards, insect and mosquito-proof curtain wall panels, etc. with functional materials.
[0087] Underground projects such as subways have extremely high fire protection requirements, and ordinary paints are not allowed to be used. Tiles can be used on the ground, but tiles cannot be used in areas such as large Roman columns, tops, and special-shaped areas. That is, silica sol paint (inorganic flame retardant) can be sprayed on aluminum plates and flexible magnesium oxide plates to make composite plates that can be decorated on load-bearing columns (such as Figure 2 As shown), artistic background wall (such as Figure 1 as shown), platform (as shown Figure 3 As shown in the figure), corridors, carriages and other places. Silica sol coating is heat-resistant and highly wear-resistant. It can be used for aerospace shells, and can also be used in various heat-resistant equipment such as non-stick pans, hairpins, fireplaces, etc.
[0088] The method of the present invention comprises the following steps: firstly preparing quartz sand into associated hydrated silica sol, then adding an antifouling agent, a gelling agent and a dispersant, preparing a sodium silicate solution of a certain concentration by means of quartz sand and caustic soda, and then forming a silicic acid solution, and then using a strong acid type cation exchange resin to pass a certain concentration of sodium silicate through a resin layer, wherein sodium ions are replaced by hydrogen ions to form silicic acid, and using a catalyst to obtain multi-molecule associated colloidal hydrated silica, after hydrogen ions on the cation resin are replaced by sodium ions, the efficiency is reduced, and hydrochloric acid must be used for regeneration, and for continued use, various impurity anions such as sulfate and hydrochloride are removed by means of the cation exchange resin, and the anions are regenerated by means of a caustic soda solution to obtain associated hydrated silica sol, thereby forming a crystal, so that the prepared silica sol has a relatively strong adhesion, so that when the silica sol is sprayed, the sprayed product is not prone to cracking and falling off due to impact.
Claims
1. A method for preparing a silica sol coating, characterized in that: The specific steps include: S1 prepares associated hydrated silica sol; (1) Weighing quartz sand according to the weight ratio of quartz sand and caustic soda and placing it in a furnace, adding caustic soda and heating it to prepare sodium silicate solid; (2) dissolving sodium silicate solid by hot water method to obtain sodium silicate liquid; (3) adding a strong acid cation exchange resin to the sodium silicate liquid in a weight ratio of 1:1, and replacing the sodium ions with the hydrogen ions of the cation exchange resin to form a silicic acid solution; (4) adding the catalyst to the silicic acid solution according to the weight ratio of the silicic acid solution to the catalyst to prepare an associated hydrated silica sol; S2: placing 140-160 parts of the associated hydrated silica sol in a reactor and stirring; S3. Slowly add 90-110 parts of gelling agent, 0.4-0.6 parts of dispersant, 0.2-0.4 parts of wetting agent and 1.0-1.4 parts of antifouling agent in sequence during stirring to obtain a mixed material; S4: placing the mixed material in a ball mill for polycondensation and pyrolysis reaction to obtain a silica sol coating.
2. The method for preparing a silica sol coating according to claim 4, characterized in that: After step S4, the step further includes S6 preparing white pulp; S61 Weigh all-red titanium dioxide, ultrafine talcum powder, barite powder, white carbon black and a dispersant into isopropanol, stir and mix to obtain an isopropanol mixture; S62 placing the isopropyl alcohol mixture on a sand mill for grinding to obtain a white slurry; S63: placing the white slurry in the silica sol coating for mixing, and obtaining the white silica sol coating after the mixing is completed.
3. The method for preparing a silica sol coating according to claim 1, characterized in that: Step S62 specifically includes grinding the isopropyl alcohol mixture to less than 25 microns on a grinder.
4. The method for preparing a silica sol coating according to claim 1, characterized in that: In step S4, the rotation speed of the ball mill is 30-50 rpm, and the reaction time is 3-5 hours.
5. The method for preparing a silica sol coating according to claim 1, characterized in that: The drying temperature in step S5 is 170°-190°, and the drying time is 15-25 minutes.
6. A silica sol coating according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 140-160 parts of associated hydrated silica sol, 90-110 parts of gelling agent, 0.4-0.6 parts of dispersant, 0.2-0.4 parts of wetting agent and 1.0-1.4 parts of antifouling agent; the associated hydrated silica sol is prepared by adding 0.8-1.2 parts by weight of catalyst to a silicic acid solution prepared from quartz sand and caustic soda, the catalyst is prepared from 0.3-0.5 parts by weight of dilute sulfuric acid and 0.5-0.7 parts by weight of dilute hydrochloric acid, and the weight ratio of the silicic acid solution to the catalyst is 149:
1.
7. The silica sol coating according to claim 1, characterized in that: The weight ratio of the quartz sand to the caustic soda is 3:
2.
8. The silica sol coating according to claim 1, characterized in that: It also includes 90-110 parts of white slurry; the white slurry is made of 20-40 parts of full-rutile titanium dioxide, 8-12 parts of ultrafine talc powder, 12-17 parts of ultrafine barite powder, 1-3 parts of white carbon black, 41-42 parts of isopropanol and 1.2-1.7 parts of dispersant.
Citation Information
Patent Citations
Preparation method of silicon sol
CN103145133A
Aqueous high-temperature-resistant enamel paint, and preparation method and construction method thereof
CN104403382A
Production process of high-modulus liquid sodium silicate
CN105271276A
Preparation method of ludox for acrylonitrile catalyst
CN105329906A
Environment-friendly nanometer ceramic paint, coating and coating technology
CN110205022A