Anti-corrosion and wear-resistant coating with pH response and preparation method of anti-corrosion and wear-resistant coating
By combining a composite nano container with a two-dimensional MXene nanosheet and a zeolite imidazole ester skeleton with a polymer resin, an anti-corrosion and wear-resistant coating with pH response was solved, and the problems of corrosion and peeling of the polymer coating in the marine environment were achieved. Efficient corrosion and wear resistance.
Patent Information
- Application Number
- CN202411352690.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-26
AI Technical Summary
Polymer coatings are prone to microcracks and micropores during marine service, resulting in local corrosion and peeling. The existing inhibitors have problems of environmental toxicity or low efficiency. It is urgent to develop anti-corrosion and wear-resistant coatings with local corrosion response to achieve High environmental adaptability for long-term anti-corrosion applications.
A composite nano container composed of two-dimensional MXene nanosheets and zeolite imidazole ester skeleton is combined with polymer resin to form a anti-corrosion and wear-resistant coating with pH response. It is prepared by etching reaction and modification process and embedded in the polymer coating. Extend the permeation path of corrosive media and release inhibitors under local acidification conditions.
The coating exhibits excellent physiological barrier and intelligent protection in extreme environments, effectively extending the penetration path of corrosive media, inhibiting corrosion expansion of the coating/metal interface, and significantly improving corrosion resistance and wear resistance.
Smart Images

Figure CN119081508A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional coatings, and in particular relates to a pH-responsive anticorrosion and wear-resistant coating and a preparation method thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] In the severe marine service process, polymer coatings will inevitably produce microcracks and micropores, which will cause local corrosion, and the continuous scouring of seawater will lead to coating peeling failure, economic losses and even safety accidents. Therefore, it is very necessary to develop composite coatings that are synergistic with local corrosion response and anti-corrosion and wear resistance.
[0004] In response to the above situation, various corrosion inhibitors have been developed for corrosion protection of metals or alloys. It is reported that inhibitors can affect the kinetics of electrochemical reactions in the corrosion process, thereby slowing down metal dissolution. Existing inhibitors (corrosion inhibitors) can be divided into two categories: organic corrosion inhibitors and inorganic corrosion inhibitors. However, it has been proven that traditional inorganic corrosion inhibitors (such as chromates, nitrates, and metal oxides) generally exhibit environmental toxicity, while most organic corrosion inhibitors are inefficient and expensive. Therefore, new corrosion inhibitors and a new generation of organic-inorganic composite corrosion inhibitors have received much attention in recent years. At this stage, technicians are in urgent need of developing a new strategy to construct anti-corrosion and wear-resistant coatings with local corrosion response to achieve high environmental adaptability for long-term anti-corrosion applications.
[0005] Metal-organic framework compounds (MOFs) have an ideal structure and function due to their bottom-up structural properties generated by selecting appropriate metals and organic ligands, so MOFs with corrosion inhibition ability have become a cutting-edge topic. When corrosive substances penetrate into the MOF structure, the corrosion inhibition process begins, causing the metal ions and organic ligands to detach, further releasing the inhibitor to achieve corrosion protection. Among them, zeolitic imidazolate framework materials (ZIFs) are a typical MOFs with pH responsiveness and good compatibility with polymers, showing great potential in smart protection applications. Summary of the invention
[0006] In response to the needs of the prior art, the purpose of the present invention is to provide a pH-responsive anti-corrosion and wear-resistant coating and a preparation method thereof, so as to expand the application of polymer coatings in the deep sea.
[0007] Specifically, the present invention provides the following technical solutions:
[0008] In a first aspect of the present invention, a pH-responsive anticorrosion and wear-resistant coating is provided, wherein the pH-responsive anticorrosion and wear-resistant coating is composed of a composite nanocontainer and a polymer resin, wherein the composite nanocontainer is composed of a two-dimensional MXene nanosheet and a zeolite imidazolate skeleton;
[0009] Wherein, the mass ratio of the composite nanocontainer to the polymer resin is 1:200 to 1:30;
[0010] The mass ratio of the zeolite imidazolate framework to the two-dimensional MXene nanosheet in the composite nanocontainer is 1:2 to 1:10.
[0011] The two-dimensional MXene nanosheets are selected from Ti3C2T x 、V2CT x 、Nb2CT x One or more of;
[0012] The zeolite imidazolate framework is selected from one or more of ZIF-7, ZIF-8, and ZIF-62;
[0013] The polymer resin is selected from one or more of polyurethane resin, silicone resin, epoxy resin and fluorocarbon resin.
[0014] The second aspect of the present invention provides a method for preparing the above-mentioned pH-responsive anticorrosion and wear-resistant coating, comprising the following steps:
[0015] S1, adding MAX powder into etching solution to carry out etching reaction to obtain MXene nanosheets;
[0016] S2, modifying MXene nanosheets with zeolite imidazolate framework to prepare composite nanocontainers;
[0017] S3, mixing the composite nanocontainer with a polymer resin to form a composite coating.
[0018] Preferably, in step S1, the MAX powder is selected from one or more of Ti3AlC2, V2AlC and Nb2AlC; and the etching solution is selected from one or more of HF, HCl and LiF.
[0019] Preferably, in step S1, the etching reaction time is 12 to 36 hours; further preferably, the etching reaction time is 24 hours; the mixture obtained after the etching reaction needs to be washed with deionized water, centrifuged, filtered and freeze-dried in sequence;
[0020] Wherein, the centrifugal speed is set to 3300-3700 rpm; preferably, the speed is set to 3500 rpm;
[0021] The pH value of the supernatant after centrifugation is not less than 6;
[0022] The filtration is vacuum-assisted filtration using a polyvinylidene fluoride (PVDF) membrane with a pore size of 0.22 μm, and then the MXene deposits are re-washed with deionized water;
[0023] The freeze-drying time is 20 to 26 hours; preferably, the freeze-drying time is 24 hours.
[0024] Preferably, in step S2, the zeolite imidazolate framework is obtained by dissolving Zn(NO3)2·6H2O and benzimidazole separately, mixing and reacting, and then centrifuging, washing and drying in sequence;
[0025] Wherein, the molar ratio of Zn(NO3)2·6H2O to benzimidazole is 1:7;
[0026] The Zn(NO3)2·6H2O is dissolved in DMF, and the benzimidazole is dissolved in anhydrous methanol;
[0027] The mixing reaction time is 12 to 36 hours; preferably, the mixing reaction time is 24 hours;
[0028] The washing is performed 2 to 4 times with an organic solvent; preferably, the organic solvent is methanol;
[0029] The drying temperature is 35-45° C., and the drying time is 20-26 hours; preferably, the drying temperature is 40° C., and the drying time is 24 hours.
[0030] Preferably, in step S2, the composite nanocontainer is obtained by dissolving MXene nanosheets and zeolite imidazolate framework in ethanol respectively for mixing reaction, and then centrifuging and drying in sequence;
[0031] Wherein, the mass ratio of the MXene nanosheets to the zeolite imidazolate skeleton is 1:1 to 3:1; preferably, the mass ratio of the MXene nanosheets to the zeolite imidazolate skeleton is 2:1;
[0032] The mixing reaction time is 20 to 26 hours; preferably, the mixing reaction time is 24 hours;
[0033] The drying temperature is 35-45° C., and the drying time is 8-15 hours; preferably, the drying temperature is 40° C., and the drying time is 12 hours.
[0034] Preferably, in step S3, the composite coating is obtained by reacting an alcohol suspension of a composite nanocontainer, an aqueous curing agent, and a polymer resin, followed by degassing, electrode coating, and electrode curing in sequence;
[0035] Wherein, the mass ratio of the water-based curing agent and the polymer resin of the composite nanocontainer is 3:1 to 1:1; preferably, the mass ratio of the water-based curing agent and the polymer resin of the composite nanocontainer is 3:2;
[0036] The alcohol suspension is preferably an ethanol suspension; the concentration of the ethanol suspension is 8 to 12 mg / mL; preferably, the concentration of the ethanol suspension is 10 mg / mL;
[0037] The degassing treatment time is 5 to 15 minutes; preferably, the degassing treatment time is 10 minutes;
[0038] The water-based curing agent is selected from one or more of polyetheramine D230, polyetheramine D400, and polyetheramine D2000;
[0039] The specific operation of the coating is: using a wire rod coater to coat the composite coating on the surface of the pretreated carbon steel electrode with a thickness of 80±5 μm;
[0040] Preferably, the specific operation of curing is to first cure the coated electrode at 25-30°C for 8-12 hours, and then heat it to 40-80°C for curing for 8-12 hours; further preferably, the coated electrode is first cured at 25°C for 12 hours, and then heat it to 60°C for curing for 12 hours.
[0041] The third aspect of the present invention provides an application of the above-mentioned pH-responsive anti-corrosion and wear-resistant coating in the deep sea.
[0042] The beneficial effects achieved by one or more of the above technical solutions of the present invention are as follows:
[0043] (1) The present invention first uses MXene as a substrate and ZIF-7 as a modified particle to synthesize a two-dimensional composite nanocontainer, and then embeds it into a polymer coating through a simple preparation method. In the early stage of service, the two-dimensional composite nanocontainer can effectively extend the penetration path of the corrosive medium and exhibit an excellent passive physical barrier effect;
[0044] When early local corrosion occurs, due to its stimulus-responsive characteristics, local acidification of the anode area leads to the decomposition of the two-dimensional composite nanocontainer, resulting in the rapid release of a large amount of benzimidazole (BIM), which effectively inhibits the corrosion extension of the coating / metal interface.
[0045] (2) The present invention relates to the multifunctionality of two-dimensional composite nanocontainers embedded in coatings. The designed intelligent system can be used to construct a new generation of intelligent protective materials that can serve in extremely harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0047] Figure 1 The scanning electron microscope images of the ZIF-7 nanoparticles and the two-dimensional composite nanocontainer loaded with ZIF-7 in Example 1 of the present invention (wherein a1 is the ZIF-7 nanoparticles; a2 is the enlarged view of the ZIF-7 nanoparticles; b1 is the two-dimensional composite nanocontainer loaded with ZIF-7; b2 is the enlarged view of the two-dimensional composite nanocontainer loaded with ZIF-7);
[0048] Figure 2 The solubility photos and adsorption kinetic curves of ZIF-7 in solutions with different pH values in Example 1 of the present invention are shown;
[0049] Figure 3 Impedance diagram, phase angle diagram and Nyquist diagram of carbon steel after immersion in 3.5wt% NaCl solution with and without nanocontainers (500mg / L) for different time periods;
[0050] Figure 4 Schematic diagram of the synergistic protection mechanism of the pH-responsive anti-corrosion and wear-resistant coatings of Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0051] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0052] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0053] Example 1 : This embodiment provides a method for preparing a pH-responsive anti-corrosion and wear-resistant coating.
[0054] S1, 1.5g Ti3C2T X The powder was slowly added to 30 mL of a mixed etching solution of HCl and LiF and magnetically stirred for 5 to 30 minutes at room temperature. Then the reaction was allowed to proceed for 24 hours at room temperature. The mixture was washed with deionized water and centrifuged several times at 3500 rpm until the pH value of the supernatant was not less than 6. Vacuum-assisted filtration was then performed using a 0.22 μm pore size polyvinylidene fluoride (PVDF) membrane, and the MXene deposit was rewashed with deionized water. Finally, the deposit was freeze-dried under vacuum for 24 hours to obtain pure Ti3C2T XMXene nanosheets;
[0055] S2. Dissolve 3.2 g Zn(NO3)2·6H2O in 100 mL DMF and 9 g benzimidazole in 100 mL anhydrous methanol. After ultrasonic dissolution, gradually mix the two and stir them at 25 °C with a constant temperature heated magnetic stirrer for 24 h, then centrifuge at 8000 rpm and remove the supernatant. Wash the final product with methanol, then repeat the centrifugation three times with a high-speed centrifuge, and wash with methanol each time. Dry the final product in a vacuum oven at 40 °C for 24 h to obtain pure white ZIF-7 powder;
[0056] S3, take 0.5g Ti3C2T X MXene nanosheets and 0.25 g ZIF-7 nanoparticles were dissolved in 50 mL ethanol and then mixed and stirred for 24 h. The mixture was centrifuged at 3000 rpm for 2 min, and the final product was placed in a vacuum oven (40 °C) for 12 h to obtain the MXene@ZIF-7 two-dimensional composite nanocontainer.
[0057] S4. Mix 5 mL of ethanol suspension (10 mg / mL) of MXene@ZIF-7 two-dimensional composite nanocontainer with 3 g of aqueous curing agent mixed with polyetheramine D400 and polyetheramine D2000. The mixture was ultrasonically treated for 5 min and stirred with a glass rod for 10 min. Then 2 g of EP resin (E-51) was added and stirred for 20 min. In order to ensure the compactness of the coating, the mixture was degassed in a vacuum oven at room temperature for 10 min. Finally, the composite coating was coated on the surface of the pretreated carbon steel electrode using a wire rod coater with a thickness of 80 ± 5 μm. The coated electrode was cured at room temperature for 12 h and then placed in a 60 ° C oven for 12 h. It was named MXene@ZIF-7 / EP coating.
[0058] Example 2 : This embodiment provides a method for preparing a pH-responsive anti-corrosion and wear-resistant coating.
[0059] S1, 1.5g Ti3C2T X The powder was slowly added to 30 mL of a mixed etching solution of HCl and LiF and magnetically stirred for 5 to 30 minutes at room temperature. Then the reaction was allowed to proceed for 24 hours at room temperature. The mixture was washed with deionized water and centrifuged several times at 3500 rpm until the pH value of the supernatant was not less than 6. Vacuum-assisted filtration was then performed using a 0.22 μm pore size polyvinylidene fluoride (PVDF) membrane, and the MXene deposit was rewashed with deionized water. Finally, the deposit was freeze-dried under vacuum for 24 hours to obtain pure Ti3C2T X MXene nanosheets;
[0060] S2. Dissolve 3.2 g Zn(NO3)2·6H2O in 100 mL DMF and 9 g benzimidazole in 100 mL anhydrous methanol. After ultrasonic dissolution, gradually mix the two and stir them at 25 °C with a constant temperature heated magnetic stirrer for 24 h, then centrifuge at 8000 rpm and remove the supernatant. Wash the final product with methanol, then repeat the centrifugation three times with a high-speed centrifuge, and wash with methanol each time. Dry the final product in a vacuum oven at 40 °C for 24 h to obtain pure white ZIF-7 powder;
[0061] S3, take 0.5g Ti3C2T X MXene nanosheets and 0.1 g ZIF-7 nanoparticles were dissolved in 50 mL ethanol and then mixed and stirred for 24 h. The mixture was centrifuged at 3000 rpm for 2 min, and the final product was placed in a vacuum oven (40 °C) for 12 h to obtain a MXene@ZIF-7 two-dimensional composite nanocontainer.
[0062] S4. Mix 5 mL of MXene@ZIF-7 two-dimensional composite nanocontainer ethanol suspension (10 mg / mL) with 3 g of water-based curing agent mixed with polyetheramine D400 and polyetheramine D2000. The mixture was ultrasonically treated for 5 min and stirred with a glass rod for 10 min. Then 2 g of EP resin (E-51) was added and stirred for 20 min. In order to ensure the compactness of the coating, the mixture was degassed in a vacuum oven at room temperature for 10 min. Finally, the composite coating was coated on the pretreated carbon steel electrode surface using a wire rod coater with a thickness of 80 ± 5 μm. The coated electrode was cured at room temperature for 12 h and then placed in a 60 ° C oven for 12 h. It was named MXene@ZIF-7 / EP coating.
[0063] Example 3 : This embodiment provides a method for preparing a pH-responsive anti-corrosion and wear-resistant coating.
[0064] S1, 1.5g Ti3C2T X The powder was slowly added to 30 mL of a mixed etching solution of HCl and LiF and magnetically stirred for 5 to 30 minutes at room temperature. Then the reaction was allowed to proceed for 24 hours at room temperature. The mixture was washed with deionized water and centrifuged several times at 3500 rpm until the pH value of the supernatant was not less than 6. Vacuum-assisted filtration was then performed using a 0.22 μm pore size polyvinylidene fluoride (PVDF) membrane, and the MXene deposit was rewashed with deionized water. Finally, the deposit was freeze-dried under vacuum for 24 hours to obtain pure Ti3C2T X MXene nanosheets;
[0065] S2. Dissolve 3.2 g Zn(NO3)2·6H2O in 100 mL DMF and 9 g benzimidazole in 100 mL anhydrous methanol. After ultrasonic dissolution, gradually mix the two and stir them at 25°C with a constant temperature heated magnetic stirrer for 24 h, then centrifuge at 8000 rpm and remove the supernatant. Wash the final product with methanol, then repeat the centrifugation three times with a high-speed centrifuge, and wash with methanol each time. Dry the final product in a vacuum oven at 40°C for 24 h to obtain pure white ZIF-7 powder;
[0066] S3, take 0.5g Ti3C2T X MXene nanosheets and 0.05 g ZIF-7 nanoparticles were dissolved in 50 mL ethanol and then mixed and stirred for 24 h. The mixture was centrifuged at 3000 rpm for 2 min, and the final product was placed in a vacuum oven (40 °C) for 12 h to obtain a MXene@ZIF-7 two-dimensional composite nanocontainer.
[0067] S4. Mix 5 mL of MXene@ZIF-7 two-dimensional composite nanocontainer ethanol suspension (10 mg / mL) with 3 g of water-based curing agent mixed with polyetheramine D400 and polyetheramine D2000. The mixture was ultrasonically treated for 5 min and stirred with a glass rod for 10 min. Then 2 g of EP resin (E-51) was added and stirred for 20 min. In order to ensure the compactness of the coating, the mixture was degassed in a vacuum oven at room temperature for 10 min. Finally, the composite coating was coated on the pretreated carbon steel electrode surface using a wire rod coater with a thickness of 80 ± 5 μm. The coated electrode was cured at room temperature for 12 h and then placed in a 60 ° C oven for 12 h. It was named MXene@ZIF-7 / EP coating.
[0068] Comparative Example 1
[0069] Compared with Example 1, this comparative example uses a two-dimensional composite nanocontainer without ZIF-7 loading.
[0070] S1, 1.5g Ti3C2T X The powder was slowly added to 30 mL of a mixed etching solution of HCl and LiF and magnetically stirred for 5 to 30 minutes at room temperature. Then the reaction was allowed to proceed for 24 hours at room temperature. The mixture was washed with deionized water and centrifuged several times at 3500 rpm until the pH value of the supernatant was not less than 6. Vacuum-assisted filtration was then performed using a 0.22 μm pore size polyvinylidene fluoride (PVDF) membrane, and the MXene deposit was rewashed with deionized water. Finally, the deposit was freeze-dried under vacuum for 24 hours to obtain pure Ti3C2T X MXene nanosheets;
[0071] S2, 5mL Ti3C2T X An ethanol suspension of MXene nanosheets (10 mg / mL) was mixed with an aqueous curing agent of 3 g of polyetheramine D400 and polyetheramine D2000. The mixture was ultrasonically treated for 5 min and stirred with a glass rod for 10 min. Subsequently, 2 g of EP resin (E-51) was added and then stirred for 20 min. In order to ensure the compactness of the coating, the mixture was degassed in a vacuum oven at room temperature for 10 min. Finally, the composite coating was applied to the pretreated carbon steel electrode surface using a wire rod coater with a thickness of 80 ± 5 μm. The coated electrode was cured at room temperature for 12 h and then placed in a 60 ° C oven for 12 h, which was named MXene / EP coating.
[0072] Comparative Example 2 : This comparative example provides a method for preparing an EP coating.
[0073] S1. 2 g of EP resin (E-51) was mixed with 3 g of a water-based curing agent mixed with polyetheramine D400 and polyetheramine D2000, and then stirred for 20 min. To ensure the compactness of the coating, the mixture was degassed in a vacuum oven at room temperature for 10 min. Finally, the composite coating was applied to the pretreated carbon steel electrode surface using a wire rod coater with a thickness of 80 ± 5 μm.
[0074] S2. The coated electrode was cured at room temperature for 12 h, and then placed in a 60°C oven for 12 h, which was named EP coating.
[0075] Test Example 1
[0076] In this test example, electrochemical impedance spectroscopy (EIS) was used to study the corrosion inhibition performance of MXene@ZIF-7 two-dimensional composite nanocontainer on steel electrode.
[0077] Figure 3 The impedance graph of carbon steel in 3.5 wt% NaCl solution with and without nanocontainers (500 mg / L) is shown as a function of time. In general, electrochemical reactivity can be measured by the impedance modulus (Z f =0.01 Hz). Therefore, this test example evaluates the interaction between the two-dimensional composite nanocontainer and the electrode surface by collecting the change in impedance.
[0078] like Figure 3 As shown in a1, the steel electrode exhibited a lower impedance value (impedance value lower than 569.4Ωcm) in the pure 3.5wt% NaCl solution during the 12h test. 2, log value is 2.76). For carbon steel substrates, the interaction with the electrolyte easily leads to the formation of microcouples. The metal substrate is oxidized, losing electrons to produce metal ions. The metal ions then undergo a hydrolysis reaction, resulting in acidification of the anodic region.
[0079] like Figure 3 As shown in b1, the impedance value of the steel electrode is slightly improved in the NaCl solution containing only MXene.
[0080] In contrast, Figure 3 As shown in c1, in the NaCl solution containing the MXene@ZIF-7 two-dimensional composite nanocontainer prepared in Example 1 of the present application, the typical impedance modulus of steel increased from 667.2 (log value is 2.82, 1h) to 1600Ωcm 2 (log value is 3.20, 12h), which indicates that the metal oxidation process has been effectively inhibited by the two-dimensional composite nanocontainer.
[0081] In addition, the corrosion degree and failure process of different samples can be analyzed by the changes in phase angle diagram and Nyquist diagram. In general, the microscopic corrosion of the coating is related to the breakpoint frequency (f b ) is closely related, f b Defined as the frequency at -45° in the phase angle diagram. Figure 3 As can be seen from a2, b2, and c2, the f containing the two-dimensional nanocontainer b Minimum. From Figure 3 As can be seen from a3, b3 and c3, the electrochemical results of the two-dimensional nanocontainer always maintain the largest capacitive reactance arc radius during the entire immersion cycle, indicating that the two-dimensional nanocontainer prepared by the present invention has relatively excellent corrosion inhibition performance.
[0082] Based on the above discussion, it can be concluded that the synthesized MXene@ZIF-7 two-dimensional composite nanocontainer has pH-responsive properties. In other words, local acidification stimulates the dissociation of the nanosensor to produce BIM, which can act as an inhibitor to protect the metal substrate from corrosion.
[0083] Test Example 2
[0084] In this test example, the changes in the corrosion inhibition performance (impedance value) of the two-dimensional composite nanocontainer formed by ZIF-7, ZIF-8 and ZIF-62 in the test in 3.5wt% NaCl solution were tested and compared. The test results are shown in Table 1.
[0085] Table 1 Sustained release performance test results
[0086]
[0087] As can be seen from Table 1, compared with the two-dimensional composite nanocontainers formed by ZIF-8 and ZIF-62, the change in the typical impedance modulus value of steel in the NaCl solution of the two-dimensional composite nanocontainer formed by ZIF-7 shows that it has a better corrosion inhibition effect.
[0088] The organic ligand of ZIF-7 is benzimidazole. This type of corrosion inhibitor is an adsorption-type corrosion inhibitor. Its functional groups can bond with the metal surface through molecular interface adsorption, inhibition effect, group covering effect and hydrogen bonding effect, so that the benzimidazole molecules are adsorbed on the metal surface and form a dense passivation film. In addition, due to its higher porosity, ZIF-7 responds more quickly to pH values, thereby achieving a more excellent corrosion inhibition effect. The organic ligand of ZIF-8 is 2-methylimidazole. Due to its higher bond energy, it is not conducive to its release of corrosion inhibitor molecules, resulting in its insensitive response to pH values. The ligands of ZIF-62 are imidazole and benzimidazole. Due to the special structure of imidazole, it has certain hydrophobic properties, which seriously hinders its dissolution in aqueous solution, thereby reducing its corrosion inhibition performance.
[0089] Test Example 3
[0090] In this test example, the friction coefficient of the coatings of Examples 1 to 3 and Comparative Examples 1 to 2 was tested, specifically by using an Rtec MFT-5000 multifunctional friction and wear tester, in a reciprocating friction form, setting the loading force to 10N for 20 minutes. The test results are shown in Table 2.
[0091] Table 2 Friction coefficient test results
[0092] Example / Comparative Example Friction coefficient Wear rate Example 1 0.18 0.005 Example 2 0.2 0.013 Example 3 0.24 0.022 Comparative Example 1 0.21 0.018 Comparative Example 2 0.43 0.197
[0093] It can be seen from Table 2 that Ti3C2T x MXene nanosheets can resist severe plastic deformation, thus reducing the wear rate of C-MXene. x MXene nanosheets easily slide relative to each other, thereby reducing the friction coefficient of the coating.
[0094] The anti-corrosion mechanism of the composite coatings of Examples 1 to 3 is as follows: Figure 4 As shown in the figure, in the early stage of service, the applied coating mainly plays its barrier role and prolongs the diffusion path of the electrolyte. After a long period of service, the corrosive medium will inevitably penetrate the coating and contact the metal substrate, thus generating a galvanic cell at the metal / coating interface. At this time, due to the hydrolysis of metal ions, a local acidic environment can be established in the anode area, which dissociates the two-dimensional composite nanocontainer and causes the ZIF-7 loaded on the MXene sheet to respond and generate Zn 2+Ions and BIM active molecules. The generated iron ions can be quickly captured by the detached BIM, so the free BIM can act as an inhibitor to effectively inhibit the further spread of local corrosion.
[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A pH-responsive anticorrosion and wear-resistant coating, characterized in that: The pH-responsive anticorrosion and wear-resistant coating is composed of a composite nanocontainer and a polymer resin, wherein the composite nanocontainer is composed of a two-dimensional MXene nanosheet and a zeolite imidazolate skeleton; Wherein, the mass ratio of the composite nanocontainer to the polymer resin is 1:200 to 1:30; The mass ratio of the zeolite imidazolate framework to the two-dimensional MXene nanosheet in the composite nanocontainer is 1:2 to 1:
10. The two-dimensional MXene nanosheets are selected from Ti3C2T x 、V2CT x 、Nb2CT x One or more of; The zeolite imidazolate framework is selected from one or more of ZIF-7, ZIF-8, and ZIF-62; The polymer resin is selected from one or more of polyurethane resin, silicone resin, epoxy resin and fluorocarbon resin.
2. A method for preparing a pH-responsive anticorrosion and wear-resistant coating as claimed in claim 1, characterized in that: The steps include: S1, adding MAX powder into etching solution to carry out etching reaction to obtain MXene nanosheets; S2, modifying MXene nanosheets with zeolite imidazolate framework to prepare composite nanocontainers; S3, mixing the composite nanocontainer with a polymer resin to form a composite coating.
3. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 2, characterized in that: In step S1, the MAX powder is selected from one or more of Ti3AlC2, V2AlC and Nb2AlC; the etching solution is selected from one or more of HF, HCl and LiF; Preferably, the etching reaction time is 12 to 36 hours; further preferably, the etching reaction time is 24 hours; the mixture obtained after the etching reaction needs to be washed with deionized water, centrifuged, filtered and freeze-dried in sequence.
4. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 3, characterized in that: The centrifugal speed is set to 3300-3700 rpm; preferably, the speed is set to 3500 rpm; Preferably, the pH value of the supernatant after centrifugation is not less than 6; Preferably, the filtration is vacuum-assisted filtration using a polyvinylidene fluoride membrane with a pore size of 0.22 μm, and then the MXene deposit is re-washed with deionized water; Preferably, the freeze-drying time is 20 to 26 hours; further preferably, the freeze-drying time is 24 hours.
5. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 2, characterized in that: In step S2, the zeolite imidazolate framework is obtained by dissolving Zn(NO3)2·6H2O and benzimidazole respectively, mixing and reacting, and then centrifuging, washing and drying in sequence; Preferably, the molar ratio of Zn(NO3)2·6H2O to benzimidazole is 1:7; Preferably, the Zn(NO3)2·6H2O is dissolved in DMF, and the benzimidazole is dissolved in anhydrous methanol; Preferably, the mixing reaction time is 12 to 36 hours; further preferably, the mixing reaction time is 24 hours; Preferably, the washing is performed 2 to 4 times with an organic solvent; more preferably, the organic solvent is methanol; Preferably, the drying temperature is 35-45° C., and the drying time is 20-26 h; preferably, the drying temperature is 40° C., and the drying time is 24 h.
6. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 2, characterized in that: In step S2, the composite nanocontainer is obtained by dissolving MXene nanosheets and zeolite imidazolate framework in ethanol respectively for mixing reaction, and then centrifuging and drying in sequence.
7. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 6, characterized in that: The mass ratio of the MXene nanosheets to the zeolite imidazolate skeleton is 1:1 to 3:1; preferably, the mass ratio of the MXene nanosheets to the zeolite imidazolate skeleton is 2:1; Preferably, the mixing reaction time is 20 to 26 hours; further preferably, the mixing reaction time is 24 hours; Preferably, the drying temperature is 35-45° C., and the drying time is 8-15 h; further preferably, the drying temperature is 40° C., and the drying time is 12 h.
8. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 2, characterized in that: In step S3, the composite coating is obtained by reacting an alcohol suspension of a composite nanocontainer, an aqueous curing agent, and a polymer resin, followed by degassing, electrode coating, and electrode curing.
9. The method for preparing a pH-responsive anticorrosion and wear-resistant coating according to claim 8, characterized in that: The mass ratio of the water-based curing agent and the polymer resin of the composite nanocontainer is 3:1 to 1:1; preferably, the mass ratio of the water-based curing agent and the polymer resin of the composite nanocontainer is 3:2; Preferably, the alcohol suspension is preferably an ethanol suspension; the concentration of the ethanol suspension is 8 to 12 mg / mL; further preferably, the concentration of the ethanol suspension is 10 mg / mL; Preferably, the degassing time is 5 to 15 minutes; more preferably, the degassing time is 10 minutes; Preferably, the water-based curing agent is selected from one or more of polyetheramine D230, polyetheramine D400, and polyetheramine D2000; Preferably, the specific operation of coating is: using a wire rod coater to coat the composite coating on the surface of the pretreated carbon steel electrode with a thickness of 80±5 μm; Preferably, the specific operation of curing is to first cure the coated electrode at 25-30°C for 8-12 hours, and then heat it to 40-80°C for curing for 8-12 hours; further preferably, the coated electrode is first cured at 25°C for 12 hours, and then heat it to 60°C for curing for 12 hours.
10. Use of the pH-responsive anticorrosion and wear-resistant coating according to claim 1 in the deep sea.
Citation Information
Patent Citations
Interface passivation type heavy anti-corrosion powder coating as well as preparation method and application thereof
CN115895394A
Preparation method and application of MBM-ZIF-8-LDH modified epoxy resin anticorrosive paint
CN116716010A
Multifunctional lubricating anticorrosive material as well as preparation method and application thereof
CN118460068A
Composite ZIF modified multifunctional coating and preparation method thereof
CN118685096A
Heat-conducting wave-absorbing auxiliary agent, low-temperature curing coating, heavy corrosion-resistant coating, and preparation method therefor and use thereof
WO2024149031A1
Cited By
Wear-resistant anticorrosive coating and preparation method thereof
CN119775889A
A wear-resistant anticorrosive coating and a method for preparing the same
CN119775889B