VAR smelting method for improving component uniformity of large-size titanium alloy cast ingot

Through computer numerical simulation and forward and reverse arc stabilization smelting technology, the problem of poor composition uniformity of large-scale titanium alloy ingots is solved, and low-cost and efficient composition uniformity improvement and process window expansion is achieved. It is suitable for titanium grades 4000~8000kg Alloy ingots.

CN119082514APending Publication Date: 2024-12-06西部超导材料科技股份有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411137482.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Large-sized titanium alloy ingots have component segregation and tissue defects during vacuum consumable arc smelting, resulting in poor composition uniformity. The existing methods will increase the smelting time and cost when improving composition uniformity, and the process window range is narrow.

Method used

The numerical model of titanium alloy ingot was established by computer numerical simulation method. Through the forward and reverse arc stable arc smelting process and the design of self-consumed electrodes, the flow intensity of the melt pool was controlled to ensure that the clockwise and counterclockwise flow were equal, and three smelting was performed to improve the composition. Uniformity, including current control, melting speed control and forward and reverse arc stabilization.

Benefits of technology

On the basis of maintaining the smelting time and cost, the composition uniformity of large-scale titanium alloy ingots has been significantly improved, the process window scope has been expanded, product quality and batch stability have been improved, and it is suitable for 4000~8000kg grade titanium alloys Ingot cast.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082514A_ABST
    Figure CN119082514A_ABST
Patent Text Reader

Abstract

The invention discloses a VAR smelting method for improving the component uniformity of a large-size titanium alloy cast ingot. The VAR smelting method comprises the steps that 1, a titanium alloy cast ingot numerical model is established through a computer numerical simulation method; step 2, simulating the smelting process to obtain a steady arc period in which the clockwise and anticlockwise liquid flowing intensities of a molten pool are equal, namely a forward and reverse steady arc smelting process; step 3, preparing a consumable electrode; and 4, the consumable electrode obtained in the step 3 is placed in a vacuum consumable electric arc furnace to be smelted for the third time, and the titanium alloy cast ingot is obtained. The large-specification (4000kg-8000kg) titanium alloy cast ingot prepared by the method disclosed by the invention is high in component uniformity and low in production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy processing methods, and in particular relates to a VAR smelting method for improving the uniformity of components of large-size titanium alloy ingots. Background Art

[0002] Titanium alloys have been widely used in aviation, aerospace, medical and other fields due to their high specific strength, high temperature resistance and good biocompatibility. Among them, vacuum consumable arc melting (VAR) technology has always been the main method for melting titanium alloys. A large number of studies have shown that titanium alloy ingots prepared by VAR technology have problems such as component segregation and structural defects. The existence of these defects often has a great impact on the quality and performance of titanium alloy components. With the development of industries such as aviation and electric power, the demand for large-scale titanium alloy ingots has gradually increased, so the preparation of large-scale ingots is imminent. However, due to the poor thermal conductivity of titanium alloys themselves, the degree of element segregation is aggravated and the uniformity of the ingot composition is reduced after the ingot size is enlarged.

[0003] A Chinese patent with a publication date of August 11, 2020 and a publication number of CN111519066 A discloses a preparation method for improving the uniformity of the composition of large-sized titanium alloy ingots. The method achieves the purpose of uniformity of the composition of the ingot by reducing the input power of the molten pool (i.e., reducing the melting rate). However, after actual production verification, although the smelting method can improve the uniformity of the composition of the ingot to a certain extent, it has the following problems: (1) The smelting time and smelting cost of the entire ingot are significantly increased; (2) The process window range is narrow: the arc stabilization period needs to be maintained at a high level, otherwise it is easy to have annual ring-like and streamline-like banded segregation. In view of this, the present invention proposes a VAR smelting method for improving the uniformity of the composition of large-sized titanium alloy ingots to overcome the defects of the prior art. Summary of the invention

[0004] The purpose of the present invention is to provide a VAR smelting method for improving the composition uniformity of large-sized titanium alloy ingots. The method improves the composition uniformity of large-sized (4000-8000kg) titanium alloy ingots while maintaining the smelting cost and smelting time without increasing the smelting cost, and the process window range is relatively wide.

[0005] The technical solution adopted by the present invention is a VAR smelting method for improving the uniformity of the composition of large-sized titanium alloy ingots, which is specifically implemented according to the following steps:

[0006] Step 1: Establishing a numerical model of titanium alloy ingot by computer numerical simulation method;

[0007] Step 2, simulating the melting process to obtain an arc stabilization cycle that makes the liquid flow intensity of the molten pool equal in clockwise and counterclockwise directions, that is, a forward and reverse arc stabilization melting process;

[0008] Step 3, preparing a consumable electrode;

[0009] Step 4: Place the consumable electrode obtained in step 3 in a vacuum consumable arc furnace and perform smelting three times to obtain a titanium alloy ingot.

[0010] The present invention is also characterized in that:

[0011] Step 3 is as follows:

[0012] The titanium sponge and the intermediate alloy required for preparing the titanium alloy ingot are proportioned, uniformly mixed, and pressed into a plurality of electrode blocks, which are then welded into consumable electrodes in an argon-protected plasma welding box.

[0013] The total ingot feed amount in step 3 is 4000-8000kg.

[0014] In step 4, the first two smelting processes are specifically as follows:

[0015] The first smelting is controlled by electric current, and the surface of the ingot is polished after it comes out of the furnace;

[0016] The second smelting adopts melting rate control, and the melting rate is 15kg / min~26kg / min.

[0017] In step 4, the third smelting adopts the forward and reverse stable arc smelting process, specifically:

[0018] The vacuum degree is controlled below 1.0Pa, the melting speed is 10kg / min-25kg / min, and when the consumable electrode is melted to a remaining weight of 15%-20% of the initial weight, the forward arc stabilization period is set to 10-18s, and the reverse arc stabilization period is set to 13-25s. When the remaining weight of the consumable electrode accounts for 4%-6% of the initial weight, the feeding stage begins, and the current is gradually reduced to lift the riser. The total feeding time is not less than 100-200min.

[0019] The titanium alloy ingot is TC4 or TC17 alloy.

[0020] The beneficial effects of the present invention are:

[0021] The method of the present invention uses a computer numerical simulation method to establish a numerical model of titanium alloy ingots, optimizes process parameters, and adopts a vacuum consumable arc melting method (VAR) to melt the consumable electrode. During the melting process, different arc stabilization periods are set in two directions (AC+ / AC-) to compensate for the inherent rotation of the molten pool, and ensure that the flow intensity of the molten pool in the horizontal direction is equal in the clockwise and counterclockwise directions, thereby improving the composition uniformity of the ingots, solving the problems of poor composition uniformity and low batch stability in large-scale titanium alloy ingots, and achieving a more ideal balance between product quality and manufacturing cost. Compared with the existing smelting methods, the method of the present invention has lower smelting time and smelting cost, the prepared ingot has high composition uniformity, and the process window range is wider, and the arc stabilization period does not need to be maintained at a high level. In addition, the preparation process of the present invention can be extended to the ingot melting of other alloys such as TB6 and TC18 alloys, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram comparing the molten pool flow strength required for the smelting process in the method of the present invention and the molten pool flow strength required for the traditional smelting process;

[0023] Figure 2 Schematic diagram of sampling positions for sampling five points longitudinally on the surface of a titanium alloy ingot in an embodiment of the present invention;

[0024] Figure 3 Schematic diagram of sampling positions for sampling nine points of the transverse cross section of the middle of a titanium alloy ingot in an embodiment of the present invention;

[0025] Figure 4 is a main element content distribution diagram obtained by sampling at five points in the longitudinal direction of the ingot prepared in Example 1 of the present invention;

[0026] Figure 5 is a main element content distribution diagram obtained by sampling nine points of the transverse cross section of the ingot prepared in Example 1 of the present invention;

[0027] Figure 6 is a main element content distribution diagram obtained by sampling at five points in the longitudinal direction of the ingot prepared in Example 2 of the present invention;

[0028] Figure 7 is a main element content distribution diagram obtained by sampling nine points of the transverse cross section of the ingot prepared in Example 2 of the present invention;

[0029] Figure 8 is a main element content distribution diagram obtained by sampling at five points in the longitudinal direction of the ingot prepared in Example 3 of the present invention;

[0030] Fig. 9 This is a main element content distribution diagram obtained by sampling at nine points on the transverse cross section of the ingot prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] The VAR smelting method of the present invention for improving the uniformity of the composition of large-sized titanium alloy ingots is specifically implemented according to the following steps:

[0033] Step 1: Establishing a numerical model of titanium alloy ingot by computer numerical simulation method;

[0034] Step 2: simulate the smelting process, such as Figure 1 As shown, a stable arc cycle is obtained that makes the liquid flow intensity of the molten pool equal in clockwise and counterclockwise directions, that is, a forward and reverse stable arc melting process;

[0035] Step 3: Preparation of consumable electrode:

[0036] The titanium sponge and the master alloy required for preparing the titanium alloy ingot are batched, uniformly mixed, and pressed into a plurality of electrode blocks, which are then welded into consumable electrodes in an argon-protected plasma welding box for standby use; wherein the total ingot feed amount is 4000-8000kg;

[0037] Step 4: Ingot melting:

[0038] The consumable electrode obtained in step 3 is placed in a vacuum consumable arc furnace for three smeltings to obtain a titanium alloy ingot, which includes a TC4 or TC17 alloy.

[0039] Among them, the three smelting processes are specifically as follows:

[0040] The first smelting is controlled by electric current, and the surface of the ingot is polished after it comes out of the furnace;

[0041] The second smelting adopts melting rate control, and the melting rate is 15kg / min~26kg / min;

[0042] The third smelting adopts the forward and reverse stable arc smelting process obtained in step 2, specifically:

[0043] The vacuum degree is controlled below 1.0Pa, the melting speed is 10kg / min-25kg / min, and when the consumable electrode is melted to a remaining weight of 15%-20% of the initial weight, the forward (AC+) arc stabilization period is set to 10-18s, and the reverse (AC-) arc stabilization period is set to 13-25s. When the remaining weight of the consumable electrode accounts for 4%-6% of the initial weight, the feeding stage begins, and the current is gradually reduced to lift the riser. The total feeding time is not less than 100-200min.

[0044] Example 1

[0045] Step 1: Establishing a numerical model of titanium alloy ingot by computer numerical simulation method;

[0046] Step 2, simulating the melting process to obtain an arc stabilization cycle that makes the liquid flow intensity of the molten pool equal in clockwise and counterclockwise directions, that is, a forward and reverse arc stabilization melting process;

[0047] Step 3: Preparation of consumable electrode:

[0048] The titanium sponge, VAl, TiSi and Al alloys required for the preparation of TC4-DT ingots are uniformly mixed and pressed into multiple electrode blocks, which are then welded into consumable electrodes in an argon-protected plasma welding box for standby use. The total ingot feed amount is 5000kg;

[0049] Step 4: Place the consumable electrode obtained in step 3 in a vacuum consumable arc furnace and perform smelting three times to obtain a titanium alloy ingot.

[0050] The first smelting is controlled by electric current, and the surface of the ingot is polished after it comes out of the furnace;

[0051] The second smelting adopts melting rate control, and the melting rate is 19kg / min;

[0052] The third smelting adopts the forward and reverse stable arc smelting process, specifically:

[0053] A Φ720mm crucible is used, the vacuum degree is controlled below 1.0Pa, the melting speed is 23kg / min, and when the consumable electrode is melted to 1000kg, the forward (AC+) arc stabilization period is set to 15s, and the reverse (AC-) arc stabilization period is set to 21s. When the remaining weight of the consumable electrode is 200kg, the feeding stage is entered, and the current is reduced step by step to lift the riser. The total feeding time is not less than 130min.

[0054] The Φ720 mm TC4-DT titanium alloy ingot melted in this embodiment was sampled, and the location of the sampling point was as follows: Figure 2 and Figure 3 As shown, five points of sampling are carried out longitudinally on the surface ( Figure 2 ), the sampling sites were named head, top, middle, bottom and tail; nine points of sampling were carried out on the middle transverse section ( Figure 3 ), the sampling locations were named 1-9, and the overall composition uniformity of TC4-DT titanium alloy ingot was analyzed. The test results are shown in Table 1 and Figure 4 , Figure 5 shown.

[0055] Table 1 Main element content of TC4-DT ingot prepared in Example 1 (wt%)

[0056]

[0057]

[0058] Depend on Figure 4 , Figure 5 As shown in Table 1, the main element content of the TC4-DT titanium alloy ingot prepared in this embodiment meets the standard requirements of GB / T3620.1, the transverse and longitudinal composition uniformity is good, and the main element deviation of 9 points in the middle transverse direction is within 800ppm.

[0059] Example 2

[0060] Step 1: Establishing a numerical model of titanium alloy ingot by computer numerical simulation method;

[0061] Step 2, simulating the melting process to obtain an arc stabilization cycle that makes the liquid flow intensity of the molten pool equal in clockwise and counterclockwise directions, that is, a forward and reverse arc stabilization melting process;

[0062] Step 3: Preparation of consumable electrodes

[0063] The titanium sponge, HZr, CrAl, MoAl and Al alloys required for TC17 ingot casting are uniformly mixed and pressed into multiple electrode blocks, which are then welded into consumable electrodes in an argon-protected plasma welding box for standby use. The total ingot casting feedstock is 6000kg;

[0064] Step 4: Place the consumable electrode obtained in step 3 in a vacuum consumable arc furnace and perform smelting three times to obtain a titanium alloy ingot.

[0065] The first smelting is controlled by electric current, and the surface of the ingot is polished after it comes out of the furnace;

[0066] The second smelting adopts melting rate control, and the melting rate is 18kg / min;

[0067] The third smelting adopts the forward and reverse stable arc smelting process, specifically:

[0068] A Φ720mm crucible is used, the vacuum degree is controlled below 1.0Pa, the melting speed is 12kg / min, and when the consumable electrode is melted to 1000kg, the forward (AC+) arc stabilization period is set to 12s, and the reverse (AC-) arc stabilization period is set to 16s. When the remaining weight of the consumable electrode is 250kg, the feeding stage is entered, and the current is reduced step by step to lift the riser. The total feeding time is not less than 110min.

[0069] The Φ720 mm TC17 titanium alloy ingot melted in this embodiment was sampled, and the sampling points were the same as those in Example 1. The overall composition uniformity of the TC17 titanium alloy ingot was analyzed. The test results are shown in Tables 2 and Figure 6 , Figure 7 shown.

[0070] Table 2 Main element content of TC17 ingot prepared in Example 2 (wt%)

[0071]

[0072] Depend on Figure 6 , Figure 7 As can be seen from Table 2, the main element content of the TC17 titanium alloy ingot prepared in this embodiment meets the standard requirements of GB / T3620.1, the transverse and longitudinal composition uniformity is good, and the main element deviation of 9 points in the middle transverse direction is within 1200ppm.

[0073] Example 3

[0074] Step 1: Establishing a numerical model of titanium alloy ingot by computer numerical simulation method;

[0075] Step 2, simulating the melting process to obtain an arc stabilization cycle that makes the liquid flow intensity of the molten pool equal in clockwise and counterclockwise directions, that is, a forward and reverse arc stabilization melting process;

[0076] Step 3: Preparation of consumable electrodes

[0077] The titanium sponge, VAl, TiSi and Al alloys required for TC4-DT ingot casting are uniformly mixed and pressed into multiple electrode blocks, which are then welded into consumable electrodes in an argon-protected plasma welding box for standby use. The total ingot casting material is 7000kg;

[0078] Step 4: Place the consumable electrode obtained in step 3 in a vacuum consumable arc furnace and perform smelting three times to obtain a titanium alloy ingot.

[0079] The first smelting is controlled by electric current, and the surface of the ingot is polished after it comes out of the furnace;

[0080] The second smelting adopts melting rate control, and the melting rate is 22kg / min;

[0081] The third smelting adopts the forward and reverse stable arc smelting process, specifically:

[0082] A Φ920mm crucible is used, the vacuum degree is controlled below 1.0Pa, the melting speed is 20kg / min, and when the consumable electrode is melted to 1400kg, the forward (AC+) arc stabilization period is 18s, and the reverse (AC-) arc stabilization period is 24s. When the remaining weight of the consumable electrode is 450kg, the current is gradually reduced to lift the riser, and the total shrinkage time is not less than 200min.

[0083] The Φ920 mm TC4-DT titanium alloy ingot melted in this embodiment was sampled, and the sampling points were the same as those in Example 1. The overall composition uniformity of the TC17 titanium alloy ingot was analyzed. The test results are shown in Tables 3 and Figure 8 , Fig. 9 shown.

[0084] Table 3 Main element content of TC4-DT ingot prepared in Example 3 (wt%)

[0085]

[0086]

[0087] Depend on Figure 8 , Fig. 9 As shown in Table 3, the main element content of the TC4-DT titanium alloy ingot prepared in this embodiment meets the standard requirements of GB / T3620.1, the transverse and longitudinal composition uniformity is good, and the main element deviation of 9 points in the middle transverse direction is within 800ppm.

Claims

1. VAR melting method to improve the composition uniformity of large-size titanium alloy ingots, It is characterized in that Follow the steps below to implement it: Step 1: Establishing a numerical model of titanium alloy ingot by computer numerical simulation method; Step 2, simulating the melting process to obtain an arc stabilization cycle that makes the liquid flow intensity of the molten pool equal in clockwise and counterclockwise directions, that is, a forward and reverse arc stabilization melting process; Step 3, preparing a consumable electrode; Step 4: Place the consumable electrode obtained in step 3 in a vacuum consumable arc furnace and perform smelting three times to obtain a titanium alloy ingot.

2. The VAR smelting method for improving the composition uniformity of large-sized titanium alloy ingots according to claim 1, It is characterized in that Step 3 is as follows: The titanium sponge and the intermediate alloy required for preparing the titanium alloy ingot are proportioned, uniformly mixed, and pressed into a plurality of electrode blocks, which are then welded into consumable electrodes in an argon-protected plasma welding box.

3. The VAR smelting method for improving the composition uniformity of large-sized titanium alloy ingots according to claim 1, It is characterized in that The total ingot feed amount in step 3 is 4000-8000kg.

4. The VAR smelting method for improving the composition uniformity of large-sized titanium alloy ingots according to claim 1, It is characterized in that In step 4, the first two smelting processes are specifically as follows: The first smelting is controlled by electric current, and the surface of the ingot is polished after it comes out of the furnace; The second smelting adopts melting rate control, and the melting rate is 15kg / min~26kg / min.

5. The VAR smelting method for improving the composition uniformity of large-sized titanium alloy ingots according to claim 1, It is characterized in that In step 4, the third smelting adopts the forward and reverse stable arc smelting process, specifically: The vacuum degree is controlled below 1.0Pa, the melting speed is 10kg / min-25kg / min, and when the consumable electrode is melted to a remaining weight of 15%-20% of the initial weight, the forward arc stabilization period is set to 10-18s, and the reverse arc stabilization period is set to 13-25s. When the remaining weight of the consumable electrode accounts for 4%-6% of the initial weight, the feeding stage begins, and the current is gradually reduced to lift the riser. The total feeding time is not less than 100-200min.

6. The VAR smelting method for improving the composition uniformity of large-sized titanium alloy ingots according to claim 1, It is characterized in that The titanium alloy ingot is TC4 or TC17 alloy.

Citation Information

Cited By

  • Titanium alloy cast ingot preparation method capable of cooperatively controlling melting speed and cooling speed