Steel suitable for high heat input welding, preparation method thereof and steel product
By introducing TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions into steel, refining the austenite grains, the problem of poor crack-absorbing performance of traditional steel plates in super-large line energy welding is solved, and high-line The good effect of energy welding meets the high thickness and crack-resistance requirements of marine steel plates.
Patent Information
- Application Number
- CN202411090778.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-12-06
AI Technical Summary
In super-large line energy welding, the high-temperature platform period of the welded joints and heat-affected zones is relatively long, resulting in rapid coarsing of ferrite and austenite grains in the microstructure, resulting in large-area stress concentration, reducing thick plates. The crack-resistance performance is difficult to meet the requirements of marine steel plates in terms of high thickness and crack-resistance performance.
Steel materials containing specific element components and TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions are used to form needle-shaped ferrite through smelting and rolling, and austenite grains are refined and welding heat is enhanced. The microstructure of the affected area improves the crack-resistance performance of steel.
Under high-line energy welding conditions, the impact work, tensile strength and brittle crack-resistance toughness of the welding heat-affected zone of steel are significantly improved, meeting the high thickness and crack-resistance performance requirements of marine steel plates.
Smart Images

Figure CN119082598A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel, and in particular to a steel material suitable for large-line energy welding, a preparation method thereof, and a steel product. Background Art
[0002] Marine engineering steel receives a large amount of energy during welding, and the low-temperature toughness of the heat-affected zone is stable, thus improving welding efficiency. Crack arrest performance is an indicator of the ability to resist crack propagation. Excellent crack arrest performance indicates excellent resistance to crack propagation and better prevention of brittle fracture, thereby ensuring the safety of parts or components.
[0003] As container ships have become larger and larger in recent years, the load on the container deck has become larger and larger, so the required steel plate thickness has increased significantly. The current maximum thickness can reach 100mm, and it needs to withstand an ultra-large welding line energy of 700KJ / cm. However, in ultra-large line energy welding of traditional steel plates, such as when the welding line energy is higher than 500KJ / cm, the high-temperature plateau period of the weld joint and the heat-affected zone is relatively long, resulting in rapid coarsening of the ferrite and austenite grains in the microstructure. Especially for thick plates with a thickness of more than 80mm, the difference between the structure of the surface and the core is large under high line energy welding, resulting in large-area stress concentration, making it very easy for cracks to initiate and proliferate, reducing the crack arrest performance of the thick plate, and it is difficult to meet the requirements of shipbuilding steel plates in terms of high thickness and crack arrest performance. Summary of the invention
[0004] Based on this, it is necessary to provide a steel material suitable for high-energy line welding with good crack arrestability, a preparation method thereof, and a steel product.
[0005] In a first aspect, the present application provides a steel material suitable for high-energy-input welding, which comprises the following element components by mass percentage: C: 0.06%~0.1%, Si: 0.15%~0.30%, S: 0.001%~0.0054%, Mn: 1.0%~2.0%, Ti: 0.005%~0.05%, P: 0.001%~0.012%, Cu: 0.01%~0.5%, Ni: 0.01%~0. 5%, Cr: 0.01%~0.5%, Ca: 0.0015%~0.0025%, B: 0.0003%~0.0015%, N: 0.003%~0.01%, O: 0.002%~0.004%, Al: 0.001%~0.035%, Mg: 0.005%~0.05%; Mo: 0~0.01%, Nb: 0~0.04%, V: 0~0.01% and the balance Fe;
[0006] The steel material contains inclusions, wherein the inclusions with an average particle size of 0.1 μm to 5 μm include inclusions containing MgO components, and the inclusions containing MgO components include TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions.
[0007] The steel contains various element components in a specific ratio, and forms TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions of a specific particle size in the steel. The composite inclusions serve as the nucleation core of the primary austenite phase, increase the nucleation efficiency of the needle-shaped ferrite in the austenite crystal, promote the heterogeneous nucleation of the molten steel, refine the austenite grain size, and enhance the crack arrest performance. At the same time, the microstructure of the welding heat affected zone is significantly refined, and a good ultra-large line energy welding effect is achieved.
[0008] In some embodiments, the steel meets at least one of the following conditions:
[0009] (1) Among the inclusions with an average particle size of 0.1 μm to 5 μm, the number of inclusions containing MgO components accounts for 30% to 50%;
[0010] (2) Among the inclusions with an average particle size of 0.1 μm to 5 μm and containing MgO components, the number of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 0.5 μm to 5 μm accounts for ≥50%;
[0011] (3) The carbon equivalent Ceq in the steel is 0.23~0.60, and the calculation formula of Ceq is:
[0012] Ceq=ω C +ω Mn / 6+(ω Cr +ω Mo +ω V ) / 5+(ω Ni +ω Cu ) / 15,
[0013] In the formula, ω C ,ω Mn ,ω Cr ,ω Mo ,ω V ,ω Ni and Cu It indicates the mass percentage of each element component in the steel.
[0014] In some embodiments, the mass percentage of V is 0.004% to 0.008%; and / or,
[0015] The mass percentage of Nb is 0.025% to 0.036%; and / or,
[0016] The mass percentage of Mo is 0.001%~0.005%.
[0017] In some embodiments, the steel material is a profile, and the thickness of the profile is 70 mm to 110 mm.
[0018] In some embodiments, the welded steel obtained by welding the steel material under the welding condition of a welding line energy of 700 KJ / cm satisfies at least one of the following conditions:
[0019] (1) The impact energy of the welding heat affected zone at -40°C is ≥45J;
[0020] (2) The tensile strength of the welding heat affected zone is ≥550MPa;
[0021] (3) Brittle crack arrest toughness Kca value at -10℃ ≥8800N / mm 1.5 .
[0022] In some embodiments, the weld heat affected zone of the weld steel contains TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm, and the mass ratio of Ca to Al in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm is 0.11 to 0.14; and / or,
[0023] The ratio of the sum of the total mass of Al and Mg to the mass of Ti is 6.25 to 11.12; and / or,
[0024] The mass ratio of Mg to Al is 0.41~0.50.
[0025] The second aspect of the present application provides a method for preparing the above-mentioned steel material, comprising the following preparation steps:
[0026] Providing raw materials according to the elemental composition of the steel, smelting the raw materials, and then casting them to obtain ingots;
[0027] The cast slab is subjected to a rolling process and then cooled.
[0028] In some embodiments, the rolling process includes rolling in a recrystallized region and rolling in a non-recrystallized region performed sequentially;
[0029] The starting rolling temperature of the recrystallization zone rolling is 1010°C~1150°C, the single-pass reduction rate is ≥14%, and the cumulative reduction rate is ≥40%;
[0030] The starting rolling temperature of the non-recrystallization zone rolling is 710°C to 850°C, the single-pass reduction rate is ≥10%, and the cumulative reduction rate is ≥60%; and / or,
[0031] The final rolling temperature of the non-recrystallization zone rolling is 20°C to 50°C above Ar3°C; wherein Ar3 is calculated as follows:
[0032] Ar3=910-310×ω C -80×ω Mn -20×ω Cu -15×ω Cr -55×ω Ni -80×ω Mo -0.35×(H-8),
[0033] In the formula, ω C ,ω Mn ,ω Cu ,ω Cr ,ω Ni and Mo It represents the mass percentage of each element component in the steel; H in the formula is the thickness of the steel plate, in mm.
[0034] In some embodiments, the cooling step includes: cooling the rolled steel to 25°C to 40°C above Ar1°C at a rate of ≥10°C / s, and then air cooling to below 300°C; wherein Ar1 is the temperature at which austenite transforms to pearlite during cooling, and Ar1 is calculated as follows:
[0035] Ar1=630-45×ω Mn -40×ω V -35×ω Si -30×ω Cr -25×ω Mo -20×ω Ni -15×w W ,
[0036] In the formula, ω Mn ,ω V ,ω Si ,ω C ,ω Mo ,ω Ni and W It represents the mass percentage of each element component in the steel, and the element component not contained in the steel is 0.
[0037] A third aspect of the present application provides a steel product, which is prepared by the above-mentioned steel material. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are merely embodiments of the present application, and ordinary technicians in this field can obtain other drawings based on the disclosed drawings without paying any creative work.
[0039] Figure 1 The SEM and element distribution diagram of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions in the steel plate prepared in Example 1.
[0040] Figure 2 This is a metallographic image of the welded joint area of the welded plate obtained under the welding condition of 700KJ / cm for the steel plate prepared in Example 1. DETAILED DESCRIPTION
[0041] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0043] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0044] In one embodiment of the present application, a steel material suitable for high-energy line welding is provided, which includes the following element components by mass percentage: C: 0.06%~0.1%, Si: 0.15%~0.30%, S: 0.001%~0.0054%, Mn: 1.0%~2.0%, Ti: 0.005%~0.05%, P: 0.001%~0.012%, Cu: 0.01%~0.5%, Ni: 0.01%~0 .5%, Cr: 0.01%~0.5%, Ca: 0.0015%~0.0025%, B: 0.0003%~0.0015%, N: 0.003%~0.01%, O: 0.002%~0.004%, Al: 0.001%~0.035%, Mg: 0.005%~0.05%; Mo: 0~0.01%, Nb: 0~0.04%, V: 0~0.01% and the balance of Fe;
[0045] The steel material contains inclusions, wherein the inclusions with an average particle size of 0.1 μm to 5 μm include inclusions containing MgO components, and the inclusions containing MgO components include TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions.
[0046] The inclusions containing MgO components are composite inclusions in which MgO components and other components are stacked together, wherein the other components include but are not limited to TiOx, Al2O3 and (Mn, Ca) S. As an example, TiOx-MgO-Al2O3-(Mn, Ca)S composite inclusions are also a type of MgO inclusions.
[0047] The above-mentioned TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions refer to composite inclusions in which TiOx, MgO, Al2O3, MnS and CaS are piled together.
[0048] The steel contains various element components in a specific ratio, and forms TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions of a specific particle size in the steel. The composite inclusions serve as the nucleation core of the primary austenite phase, increase the nucleation efficiency of the needle-shaped ferrite in the austenite crystal, promote the heterogeneous nucleation of the molten steel, refine the austenite grain size, and enhance the crack arrest performance. At the same time, the microstructure of the welding heat affected zone is significantly refined, and a good ultra-large line energy welding effect is achieved.
[0049] The above "Mg: 0.005% to 0.05%" can be understood as the mass percentage of Mg in the steel can be 0.005%, 0.006%, 0.008%, 0.01%, 0.012%, 0.015%, 0.016%, 0.018%, 0.02%, 0.022%, 0.025%, 0.030%, 0.035%, 0.04%, 0.045% and 0.05%. Further, the mass percentage of Mg in the steel can be a range value consisting of any two of the above point values as end values. Preferably, the mass percentage of Mg in the steel is 0.024% to 0.042%.
[0050] The above "Mo: 0-0.01%" can be understood as the mass percentage of Mo in the steel can be 0%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009% or 0.01%. Further, the mass percentage of Mo in the steel can be a range value consisting of any two of the above point values as end values. Preferably, the mass percentage of Mo in the steel is 0.001%-0.005%.
[0051] The above "Nb: 0-0.04%" can be understood as the mass percentage of Nb in the steel can be 0%, 0.001%, 0.005%, 0.006%, 0.008%, 0.01%, 0.012%, 0.015%, 0.016%, 0.018%, 0.02%, 0.022%, 0.025%, 0.030%, 0.035% or 0.04%. Further, the mass percentage of Nb in the steel can be a range value consisting of any two of the above point values as end values. Preferably, the mass percentage of Nb in the steel is 0.025%-0.036%.
[0052] The above "V: 0~0.01%" can be understood as the mass percentage of V in the steel can be 0%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009% or 0.01%. Further, the mass percentage of V in the steel can be a range value consisting of any two of the above point values as end values. Preferably, the mass percentage of V in the steel is 0.004%~0.008%. V can improve the hardenability and temper softening resistance, and further controlling V helps to improve the strength of the heat affected zone of large line energy welding.
[0053] In some embodiments, the steel comprises the following element components, measured by mass percentage: C: 0.06%~0.1%, Si: 0.15%~0.30%, S: 0.001%~0.0054%, Mn: 1.0%~2.0%, Ti: 0.005%~0.05%, P: 0.001%~0.012%, Cu: 0.01%~0.5%, Ni: 0.01%~0.5%, Cr: 0.01%~0.5 %, Ca: 0.0015%~0.0025%, B: 0.0003%~0.0015%, N: 0.003%~0.01%, O: 0.002%~0.004%, Al: 0.001%~0.035%, Mg: 0.005%~0.05%; Mo: 0.001%~0.005%, Nb: 0.025%~0.036%, V: 0.004%~0.008% and the balance of Fe.
[0054] In some embodiments, the steel material comprises the following element components by weight percentage:
[0055] C: 0.064%~0.07%, Si: 0.17%~0.19%, S: 0.003%~0.004%, Mn: 1.35%~1.65%, Ti: 0.026%~0.03 6%, P: 0.002%~0.005%, Cu: 0.07%~0.09%, Ni: 0.16%~0.25%, Cr: 0.02%~0.03%, Ca: 0.0019%~ 0.0022%, B: 0.0003%~0.0007%, N: 0.003%~0.008%, O: 0.003%~0.006%, Al: 0.023%~0.031%, Mg: 0.024%~0.042%; Mo: 0.001%~0.005%, Nb: 0.025%~0.036%, V: 0.004%~0.008% and the balance of Fe.
[0056] In some embodiments, the steel material further contains necessary impurities.
[0057] In some embodiments, among the inclusions with an average particle size of 0.1 μm to 5 μm, the number of inclusions containing MgO components accounts for 30% to 50%. It can be understood that the average particle size of the inclusions containing MgO components in the above-mentioned steel can be 0.1 μm to 5 μm, or it can be other sizes. Among them, among the inclusions with an average particle size of 0.1 μm to 5 μm, the number of inclusions containing MgO components can account for 30%, 35%, 40%, 45% or 50%. Controlling the number of magnesium oxide inclusions at a specific particle size is conducive to promoting the nucleation of acicular ferrite with higher efficiency, effectively hindering the coarsening of the grains of the steel after welding, thereby improving the impact toughness of the heat affected zone after welding.
[0058] In some embodiments, among the inclusions with an average particle size of 0.1 μm to 5 μm and containing MgO components, the number of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 0.5 μm to 5 μm accounts for ≥50%. It can be understood that in the above-mentioned steel, among the inclusions with an average particle size of 0.1 μm to 5 μm containing MgO components, there are also composite inclusions in which TiOx, MgO, Al2O3, MnS and CaS are piled together. Among them, the number of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 0.5 μm to 5 μm can account for 50%, 55%, 60%, 65%, 70%, 75% or other numbers greater than 50%. Furthermore, among the inclusions containing MgO components with a size of 0.1 μm to 5 μm, the number of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 0.5 μm to 5 μm accounts for 50% to 80%. Controlling the number of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions at a specific particle size is conducive to promoting the nucleation of acicular ferrite with higher efficiency, effectively hindering the grain coarsening of the steel after welding, thereby improving the impact toughness of the heat-affected zone after welding.
[0059] In some embodiments, the carbon equivalent Ceq in the steel is 0.23-0.60, and the calculation formula of Ceq is:
[0060] Ceq=ω C +ω Mn / 6+(ω Cr +ω Mo +ω V ) / 5+(ω Ni +ω Cu ) / 15,
[0061] In the formula, ω C ,ω Mn ,ω Cr ,ω Mo ,ωV ,ω Ni and Cu Indicates the mass percentage of each element component in the steel. Further, when the steel does not contain the corresponding component, its value is 0.
[0062] Further, the carbon equivalent Ceq in the steel can be 0.23, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55 or 0.60. The carbon equivalent Ceq can also be a range value consisting of any two of the above point values as end values. Preferably, the carbon equivalent Ceq is 0.30~0.55. More preferably, the carbon equivalent Ceq is 0.31~0.40. Further preferably, the carbon equivalent Ceq is 0.31~0.37. Controlling the carbon equivalent is beneficial to improving the strength and toughness of the steel, while reducing the low-temperature brittleness and work hardening of the steel.
[0063] In some embodiments, the yield strength of the steel is ≥440 MPa. Further, the yield strength of the steel is 440 MPa-520 MPa.
[0064] In some embodiments, the tensile strength of the steel is 570 MPa-720 MPa.
[0065] In some embodiments, the elongation at break of the steel is ≥ 17%. Further, the elongation at break of the steel is 17% to 21%.
[0066] In some embodiments, the impact energy of the steel material at -40°C is ≥75 J. Further, the impact energy of the steel material at -40°C is 75 J to 186 J.
[0067] In some embodiments, the steel material is a profile, and the thickness of the profile is 70 mm to 110 mm.
[0068] In some embodiments, the profile comprises a plate.
[0069] In some embodiments, the impact energy of the weld heat affected zone of the welded plate obtained under the welding condition of the steel material with a welding line energy of 700KJ / cm at -40°C is ≥45J. As an example, the impact energy of the weld heat affected zone of the welded plate at -40°C may be 45J, 50J, 58J, 60J, 69J, 70J, 80J, 85J, 87J, 100J, 103J, 106J, 110J, 116J, 120J, 125J, 130J or 132J. Further, the impact energy of the weld heat affected zone of the welded plate at -40°C may be any other value greater than 45J. Preferably, the impact energy of the weld heat affected zone of the welded plate at -40°C is 45J~132J.
[0070] In some embodiments, the tensile strength of the weld heat affected zone of the welded steel obtained under the welding condition of 700KJ / cm of welding line energy is ≥550MPa. The above-mentioned weld heat affected zone refers to the area where the parent material in the solid state on both sides of the weld undergoes obvious changes in structure and properties under the action of welding heat cycle. Further, the tensile strength of the weld heat affected zone of the welded plate is 559MPa~630MPa.
[0071] In some embodiments, the -10°C brittle crack arrest toughness Kca value of the welded plate is ≥8800N / mm1.5. As an example, the -10°C brittle crack arrest toughness Kca value of the welded plate may be 8800N / mm1.5, 8840N / mm1.5, 9000N / mm1.5, 9050N / mm1.5, 9100N / mm1.5, 9150N / mm1.5, 9200N / mm1.5, 9250N / mm1.5, 9300N / mm1.5, 9320N / mm1.5 or 9400N / mm1.5, or any other value greater than 8800N / mm1.5. Further, the -10°C brittle crack arrest toughness Kca value of the welded plate is 8840N / mm1.5~9500N / mm1.5.
[0072] In some embodiments, the welding heat affected zone of the welding plate contains composite inclusions with an average particle size of 1 μm to 4 μm, and the mass ratio of Ca to Al in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm is 0.11 to 0.14. It can be understood that the mass ratio of Ca to Al in the composite inclusions with an average particle size of 1 μm to 4 μm can be 0.11, 0.12, 0.13 or 0.14. Further, the mass ratio of Ca to Al in the composite inclusions with an average particle size of 1 μm to 4 μm can be a range value composed of any two of the above point values as point values. Controlling the mass ratio of Ca to Al in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions can prevent the generation of excessive CaS on the surface of the composite inclusions, thereby hindering the IAF nucleation under the manganese-poor zone mechanism of Ti2O3.
[0073] In some embodiments, the ratio of the sum of the total mass of Al and Mg to the mass of Ti in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm is 6.25 to 11.12. It can be understood that the ratio of the sum of the total mass of Al and Mg to the mass of Ti in the composite inclusions with an average particle size of 1 μm to 4 μm can be 6.25, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11 or 11.12. Further, the ratio of the sum of the total mass of Al and Mg to the mass of Ti in the composite inclusions with an average particle size of 1 μm to 4 μm can be a range value composed of any two of the above point values as point values. Controlling the ratio of the sum of the total mass of Al and Mg to the mass of Ti in the composite inclusions can promote the precipitation of Ti2O3 inclusions, thereby promoting IAF nucleation and improving the impact toughness of the heat affected zone.
[0074] In some embodiments, the mass ratio of Mg to Al in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm is 0.41 to 0.50. It can be understood that the mass ratio of Mg to Al in the composite inclusions with an average particle size of 1 μm to 4 μm is 0.41, 0.42, 0.43, 0.45, 0.46, 0.47, 0.48, 0.49 or 5.0. Further, the mass ratio of Mg to Al in the composite inclusions with an average particle size of 1 μm to 4 μm is a range value that can be composed of any two of the above point values as point values. Controlling the Mg / Al ratio in the heat affected zone of the welded steel can promote the formation of magnesium-aluminum spinel MgAlO4, which can promote IAF nucleation under a low mismatch mechanism and improve the impact toughness of the heat affected zone.
[0075] In one embodiment, a method for preparing the above steel is provided, comprising the following preparation steps:
[0076] S10, providing raw materials according to the elemental composition of the steel, smelting the raw materials, and then casting them to obtain ingots;
[0077] S20, rolling the ingot and then cooling it.
[0078] In some embodiments, the step of smelting the raw material includes:
[0079] S11, smelting molten iron, scrap steel, ferromanganese, ferrosilicon and lime at 1300° C. to 1340° C., tapping steel to obtain a first melt;
[0080] S12, transferring the first melt to the LF furnace, adjusting the elemental composition of the melt in the LF furnace until the elemental composition of the melt meets the elemental composition requirements of the above-mentioned steel material, tapping the steel, and obtaining the second melt.
[0081] S13, transferring the second melt to the RH furnace, adding magnesium-calcium cored wire to the second melt, adding ultra-low carbonized rice husk for heat preservation before tapping, and obtaining the third melt.
[0082] In some embodiments, the casting process is a continuous casting process.
[0083] In some embodiments, the casting temperature of the continuous casting process is 1540°C to 1560°C.
[0084] In some embodiments, the casting speed of the continuous casting process is controlled to be 0.8 m / min to 1.5 m / min.
[0085] In some embodiments, the rolling process includes rolling in a recrystallized region and rolling in a non-recrystallized region performed sequentially.
[0086] In some embodiments, the start rolling temperature of the recrystallization zone rolling is 1010°C to 1150°C.
[0087] In some embodiments, the single pass reduction rate during the recrystallization zone rolling process is ≥14%, and the cumulative reduction rate is ≥40%. Further, the single pass reduction rate during the recrystallization zone rolling process is 14% to 16%, and the cumulative reduction rate is 42% to 48%. By controlling the single pass reduction rate, on the one hand, the casting meets the overall reduction quality and size requirements, and on the other hand, the controlled reduction amount is gradually reduced, thereby reducing the phenomenon of steel plate cracking caused by lower rolling plate temperature and increased deformation.
[0088] In some embodiments, the starting rolling temperature of the non-recrystallization zone rolling is 710°C to 850°C.
[0089] In some embodiments, during the rolling process in the non-recrystallization zone, the single-pass reduction rate is ≥10%, and the cumulative reduction rate is ≥60%. Further, during the rolling process in the non-recrystallization zone, the single-pass reduction rate is 10%-13%, and the cumulative reduction rate is 60%-78%.
[0090] In some embodiments, the final rolling temperature of the non-recrystallized region rolling is 20°C to 50°C above Ar3°C; wherein Ar3 is calculated as follows:
[0091] Ar3=910-310×ω C -80×ω Mn -20×ω Cu -15×ω Cr -55×ω Ni -80×ω Mo -0.35×(H-8),
[0092] In the formula, ω C ,ω Mn ,ω Cu ,ω Cr ,ω Ni and Mo Indicates the mass percentage of each element component in the steel;
[0093] Where H is the thickness of the steel plate in mm.
[0094] In some embodiments, the cooling step includes: cooling the rolled steel at a rate of ≥10°C / s to 25°C to 40°C above Ar1°C, and then air cooling to below 300°C; wherein Ar1 is calculated as: Ar1=630-45×ω Mn -40×ω V -35×ω Si -30×ω Cr -25×ω Mo -20×ω Ni -15×ω W ,
[0095] In the formula, ω Mn ,ω V ,ω Si ,ω C ,ω Mo ,ω Ni and W It represents the mass percentage of each element component in the steel, and the element component not contained in the steel is 0.
[0096] In some embodiments, the rolled steel is cooled at a rate of 10°C / s to 11°C / s to 25°C to 40°C above Ar1°C. For thick steel plates used for welding, the core of the steel plate dissipates heat slowly. By controlling the cooling rate during cooling, the temperature difference between the internal and surface structures of the steel plate can be reduced, the macrosegregation of alloy elements and carbon elements can be reduced, and the longitudinal mechanical properties of the steel plate can be improved.
[0097] In one embodiment, a steel product is provided. The steel product is prepared by using the above-mentioned steel material.
[0098] In some embodiments, the steel product comprises marine grade EH47.
[0099] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0100] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.
[0101] Example 1
[0102] The present embodiment provides a steel plate, the chemical composition of the steel plate including, by weight percentage, C: 0.064%, S: 0.003%, P: 0.002%, O: 0.006%, N: 0.003%, V: 0.006%, Si: 0.17%, Mn: 1.65%, Nb: 0.034%, Cu: 0.07%, Ni: 0.25%, Ti: 0.026%, Cr: 0.02%, Mo: 0.003%, Ca: 0.0019%, B: 0.0007%, Al: 0.023%, Mg: 0.024%, carbon equivalent Ceq: 0.366, and the rest is Fe and unavoidable impurities.
[0103] The manufacturing method of the above-mentioned steel plate comprises the following steps:
[0104] (1) Smelting stage:
[0105] a) Converter smelting: Mix molten iron and clean scrap steel in a ratio of 6:1, smelt the molten iron at 1300℃~1340℃, then add ferromanganese, ferrosilicon and lime to the molten iron in turn for smelting, and tap the steel after smelting.
[0106] b) LF furnace refining: After steel is tapped, Mn, Cr, Ni, Cu, Ti, and Mg elements are added to the molten steel according to the elemental composition of the above steel plate, and the temperature is measured and samples are taken. Steel is tapped after the above elements meet the elemental composition requirements of the welding steel plate.
[0107] c) RH furnace refining: During the RH refining process, magnesium-calcium cored wire is added to the molten steel, and ultra-low carbonized rice husk is added for heat preservation before tapping.
[0108] d) Continuous casting: The casting temperature was controlled at 1500°C and the pulling speed was controlled at 1.1 m / min to produce a continuous casting slab with a thickness of 345 mm.
[0109] (2) Rolling stage:
[0110] The slab obtained in the smelting stage was heated at 1160°C for 300 minutes, and after heating, it was rolled in the recrystallization zone. The start rolling temperature of the recrystallization zone rolling was 970°C, the single pass reduction rate was 14%, and the rolling was repeated 3 times. The final rolling temperature of the recrystallization zone rolling was 900°C. Then, the non-recrystallization zone rolling was carried out. The start rolling temperature of the non-recrystallization zone rolling was 820°C, the single pass reduction rate was 10%, and the rolling was repeated 6 times. The final rolling temperature of the non-recrystallization zone rolling was 780°C, and a steel plate with a thickness of 80 mm was obtained.
[0111] (3) Cooling stage:
[0112] After rolling, the steel plate is transported to the ACC equipment at the maximum transport speed of the roller. After the ACC equipment cools the steel plate to 490°C at a cooling rate of 10.1°C / s, the steel plate is air-cooled to below 300°C.
[0113] Example 2
[0114] The present embodiment provides a steel plate, the elemental composition of the steel plate comprising, by weight percentage, C: 0.066%, S: 0.004%, P: 0.003%, O: 0.005%, N: 0.003%, V: 0.006%, Si: 0.19%, Mn: 1.57%, Nb: 0.028%, Cu: 0.09%, Ni: 0.17%, Ti: 0.033%, Cr: 0.02%, Mo: 0.003%, Ca: 0.0021%, B: 0.0007%, Al: 0.028%, Mg: 0.037%, carbon equivalent Ceq: 0.412, and the rest is Fe and unavoidable impurities.
[0115] The manufacturing method of the steel plate comprises the following steps:
[0116] (1) Smelting stage:
[0117] a) Converter smelting: Mix molten iron and clean scrap steel in a ratio of 5:1, smelt the molten iron at 1300℃~1340℃, then add ferromanganese, ferrosilicon and lime to the molten iron in turn for smelting, and tap the steel after smelting.
[0118] b) LF furnace refining: After steel is tapped, Mn, Cr, Ni, Cu, Ti, and Mg are added to the molten steel according to the elemental composition of the above steel plate, and the temperature is measured and samples are taken. Steel is tapped after the above elements meet the chemical composition requirements of the welding steel plate.
[0119] c) RH furnace refining: During the RH refining process, magnesium-calcium cored wire is added to the molten steel, and ultra-low carbonized rice husk is added for heat preservation before tapping.
[0120] d) Continuous casting: The casting temperature was controlled at 1520°C and the pulling speed was controlled at 1.3 m / min to produce a continuous casting slab with a thickness of 390 mm.
[0121] (2) Rolling stage:
[0122] The slab obtained in the smelting stage is heated at 1160℃ for 300min, and after heating is completed, it is rolled in the recrystallization zone. The starting rolling temperature of the recrystallization zone rolling is 970℃, the single-pass reduction rate is 14%, and the rolling is performed 3 times. The final rolling temperature of the recrystallization zone rolling is 910℃; then it is rolled in the non-recrystallization zone. The starting rolling temperature of the non-recrystallization zone rolling is 820℃, the single-pass reduction rate is 10%, and the rolling is performed 6 times. The final rolling temperature of the non-recrystallization zone rolling is 770℃, and a steel plate with a thickness of 90mm is obtained.
[0123] (3) Cooling stage:
[0124] After rolling, the steel plate is transported to the ACC equipment at the maximum transport speed of the roller. After the ACC equipment cools the steel plate to 490°C at a cooling rate of 10.3°C / s, the steel plate is air-cooled to below 300°C.
[0125] Example 3
[0126] The present embodiment provides a steel plate, the chemical composition of the steel plate including, by weight percentage, C: 0.069%, S: 0.003%, P: 0.005%, O: 0.006%, N: 0.003%, V: 0.006%, Si: 0.17%, Mn: 1.35%, Nb: 0.028%, Cu: 0.09%, Ni: 0.16%, Ti: 0.036%, Cr: 0.03%, Mo: 0.003%, Ca: 0.0022%, B: 0.0007%, Al: 0.031%, Mg: 0.042%, carbon equivalent Ceq: 0.469, and the rest is Fe and unavoidable impurities.
[0127] The manufacturing method of the steel plate comprises the following steps:
[0128] (1) Smelting stage:
[0129] a) Converter smelting: Mix molten iron and clean scrap steel in a ratio of 7:1, smelt the molten iron at 1300℃~1340℃, then add ferromanganese, ferrosilicon and lime into the molten iron for smelting, and tap the steel after smelting.
[0130] b) LF furnace refining: After steel is tapped, the chemical composition of the welded steel plate in Table 1 is added with Mn, Cr, Ni, Cu, Ti, and Mg elements into the molten steel, and the temperature is measured and samples are taken. Steel is tapped after the above elements meet the chemical composition requirements of the welded steel plate.
[0131] c) RH furnace refining: During the RH refining process, magnesium-calcium cored wire is added to the molten steel, and ultra-low carbonized rice husk is added for heat preservation before tapping.
[0132] d) Continuous casting: The casting temperature is controlled at 1530°C and the pulling speed is controlled at 1.2 m / min to produce a continuous casting slab with a thickness of 430 mm.
[0133] (2) Rolling stage:
[0134] The slab obtained in the smelting stage is heated at 1160℃ for 300min, and after heating is completed, it is rolled in the recrystallization zone. The starting rolling temperature of the recrystallization zone rolling is 970℃, the single-pass reduction rate is 14%, and the rolling is performed 3 times. The final rolling temperature of the recrystallization zone rolling is 920℃; then it is rolled in the non-recrystallization zone. The starting rolling temperature of the non-recrystallization zone rolling is 820℃, the single-pass reduction rate is 10%, and the rolling is performed 6 times. The final rolling temperature of the non-recrystallization zone rolling is 790℃, and a steel plate with a thickness of 100mm is obtained.
[0135] (3) Cooling stage:
[0136] After rolling, the steel plate is transported to the ACC equipment at the maximum transport speed of the roller. After the ACC equipment cools the steel plate to 490°C at a cooling rate of 10.5°C / s, the steel plate is air-cooled to below 300°C.
[0137] Embodiments 4 to 8
[0138] The preparation methods of Examples 4 to 8 are basically the same as those of Example 3, and the main difference is that the elemental composition of the steel plates is different. The elemental composition of the steel plates prepared in Examples 4 to 8 is shown in Table 1. The other preparation steps are the same as those in Example 3.
[0139] Example 9
[0140] The preparation method of this embodiment is basically the same as the preparation method of embodiment 3, and the only difference is that the cooling speed in the cooling stage of the preparation process is different. The cooling stage of step (3) of this embodiment is as follows: after rolling is completed, the steel plate is transported to the ACC equipment at the maximum transport speed of the roller. After the ACC equipment cools the steel plate to 490°C at a cooling speed of 11°C / s, the steel plate is air-cooled to below 300°C.
[0141] Comparative Example 1
[0142] The preparation method of this comparative example is basically the same as that of Example 3, the only difference being that the element components in the steel plate are different. The element composition ratio in this comparative example is shown in Table 1.
[0143] Comparative Example 2
[0144] The preparation method of this comparative example is basically the same as that of Example 3, the only difference being that the element components in the steel plate are different. The element composition ratios in this comparative example are shown in Tables 1 and 2.
[0145] The element compositions of the steel plates in the embodiments and comparative examples are shown in Tables 1 and 2.
[0146] Table 1
[0147]
[0148] Table 2
[0149]
[0150] Note: In Table 1 and Table 2, the element composition in each embodiment also includes the balance of Fe and unavoidable impurity components.
[0151] Performance Testing:
[0152] The welded plates prepared in each embodiment and comparative example are obtained by single-sided welding of three types of thick steel plates of 80mm, 90mm and 100mm produced in industrial trials with a line energy of 700kJ / cm. The yield strength, tensile strength, elongation after fracture, brittle crack arrest toughness and -40℃ impact energy of the samples prepared in each embodiment and comparative example are measured according to the method specified in Materials and Welding 2021 of China Classification Society (CCS).
[0153] The SEM test method and EDS spectrometer were used to observe the particle size and element composition of the inclusions in the steel plates prepared in each embodiment and comparative example.
[0154] The performance test data of each embodiment and comparative example are shown in Table 3 and Table 4.
[0155] Table 3
[0156]
[0157] Table 4
[0158]
[0159] See also Figure 1 , Figure 1 The SEM image and element distribution diagram of a TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusion in the steel plate prepared in Example 1, wherein Figure 1 Figure a is the SEM image of the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusion, and the others are element distribution diagrams of Fe, Al, O, Ti, Mg, Mn, S and Ca in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusion.
[0160] See also Figure 2 , Figure 2This is a metallographic image of the welded joint area of the welded plate obtained under 700KJ / cm welding conditions for the steel plate prepared in Example 1, wherein the HAZ area is the welding heat affected zone, the FL line is the fusion line, and the WD area is the weld area. As can be seen from the figure, the grains in the HAZ welding heat affected zone are relatively coarse, but a lot of acicular ferrite formed inside the grains is promoted by inclusions. The acicular ferrite structure is slender and mostly radial. The acicular ferrite cuts and refines the overall grain structure of the HAZ welding heat affected zone, and also fixes the grains to prevent further coarsening of the grains, thereby improving the strength and impact toughness of the HAZ.
[0161] It can be seen from Table 3 that among the inclusions with an average particle size of 0.1~0.5μm in the steel plate base material, the average size of MgO type inclusions is 0.3μm~0.5μm, accounting for 36%~45%; among the inclusions with an average particle size of 0.5μm~5μm in the steel plate base material, the average size of TiOx-MgO-Al2O 3- The average particle size of (Mn,Ca)S composite inclusions is 1.8μm~2.5μm, accounting for more than 60% of the total; among the 1μm~4μm composite inclusions in the HAZ of welded steel plates, Ca / Al is controlled at 0.11~0.14, (Al+Mg) / Ti is controlled at 6.25~11.12, and Mg / Al is controlled at 0.41~0.50.
[0162] From Table 4, it can be seen that the yield strength of the 80mm~100mm thick steel plates prepared by the technical solution of the present application in Examples 1~9 reaches 442MPa~510MPa, the tensile strength reaches 592MPa~685MPa, the elongation after fracture reaches 17%~21%, and the impact energy at -40℃ reaches 95J~186J, which has good mechanical properties. Under the condition of welding line energy of 700kJ / cm, the tensile strength of the heat-affected zone is 559MPa~630MPa, the longitudinal impact at -40℃ is 45J~132J, and the crack arrest toughness of the welded plate at -10℃ is 8840N / mm 1.5 ~9320N / mm 1.5 , which can meet the requirements of marine steel plates.
[0163] The Mg content in the element composition of the steel prepared in Comparative Example 1 is not within the scope of the present application, and the TiO x-MgO-Al2O3-(Mn,Ca)S composite inclusions have an average particle size of 1.5μm, accounting for only 55% of the inclusions with an average particle size of 0.5μm~5μm. The yield strength of the steel plate is only 477MPa, the tensile strength is 550MPa, and the elongation after fracture is 18%, which is lower than the strength of the steel plate prepared in Example 3. Under the condition of welding line energy of 700kJ / cm, the steel plate prepared in Comparative Example 1 has a tensile strength of 338MPa in the heat affected zone, a longitudinal impact of 34J at -40℃, and a crack arrest toughness of 4930N / mm at -10℃. 1.5 It can be seen that the performance of the steel plate of Comparative Example 1 after welding with a welding line energy of 700 kJ / cm is not as good as that of Example 3.
[0164] The carbon equivalent Ceq in the elemental composition of the steel prepared in Comparative Example 2 is not within the scope of the present application, and the TiO x -MgO-Al2O3-(Mn,Ca)S composite inclusions have an average particle size of 1.3μm, accounting for only 43% of the inclusions with an average particle size of 0.5μm~5μm. The yield strength of the steel plate is only 480MPa, the tensile strength is 535MPa, and the elongation after fracture is 16%, which is lower than the strength of the steel plate prepared in Example 3. Under the condition of welding line energy of 700kJ / cm, the steel plate prepared in Comparative Example 2 has a tensile strength of 310MPa in the heat affected zone, a longitudinal impact of 27J at -40℃, and a crack arrest toughness of 5020N / mm at -10℃. 1.5 It can be seen that the performance of the steel plate of Comparative Example 2 after welding with a welding line energy of 700 kJ / cm is not as good as that of Example 3.
[0165] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0166] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A steel material suitable for high-energy line welding, characterized in that: In terms of mass percentage, it includes the following element components: C: 0.06%~0.1%, Si: 0.15%~0.30%, S: 0.001%~0.0054%, Mn: 1.0%~2.0%, Ti: 0.005%~0.05%, P: 0.001%~0.012%, Cu: 0.01%~0.5%, Ni: 0.01%~0.5%, Cr: 0.01%~ 0.5%, Ca: 0.0015%~0.0025%, B: 0.0003%~0.0015%, N: 0.003%~0.01%, O: 0.002%~0.004%, Al: 0.001%~0.035%, Mg: 0.005%~0.05%; Mo: 0~0.01%, Nb: 0~0.04%, V: 0~0.01% and the balance of Fe; The steel material contains inclusions, wherein the inclusions with an average particle size of 0.1 μm to 5 μm include inclusions containing MgO components, and the inclusions containing MgO components include TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions.
2. The steel material according to claim 1, characterized in that: The steel material meets at least one of the following conditions: (1) Among the inclusions with an average particle size of 0.1 μm to 5 μm, the number of inclusions containing MgO components accounts for 30% to 50%; (2) Among the inclusions with an average particle size of 0.1 μm to 5 μm and containing MgO components, the number of TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 0.5 μm to 5 μm accounts for ≥50%; (3) The carbon equivalent Ceq in the steel is 0.23 to 0.60, and the calculation formula of Ceq is: Ceq=ω C +oh Mn / 6+(ω Cr +oh Mo +oh V ) / 5+(ω Ni +oh Cu ) / 15, In the formula, ω C ,ω Mn ,ω Cr ,ω Mo ,ω V ,ω Ni and Cu It indicates the mass percentage of each element component in the steel.
3. The steel material according to any one of claims 1 to 2, characterized in that: The mass percentage of V is 0.004%~0.008%; and / or, The mass percentage of Nb is 0.025% to 0.036%; and / or, The mass percentage of Mo is 0.001%~0.005%.
4. The steel material according to any one of claims 1 to 2, characterized in that: The steel material is a profile, and the thickness of the profile is 70mm~110mm.
5. The steel material according to claim 4, characterized in that: The welded plate obtained by welding the steel material under the welding condition of a welding line energy of 700 KJ / cm satisfies at least one of the following conditions: (1) The impact energy of the welding heat affected zone at -40°C is ≥45J; (2) The tensile strength of the welding heat affected zone is ≥550MPa; (3) Brittle crack arrest toughness Kca value at -10℃ ≥8800N / mm 1.5 .
6. The steel material according to claim 5, characterized in that: The welding heat affected zone of the welding plate contains TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm, and the mass ratio of Ca to Al in the TiOx-MgO-Al2O3-(Mn,Ca)S composite inclusions with an average particle size of 1 μm to 4 μm is 0.11 to 0.14; and / or, The ratio of the sum of the total mass of Al and Mg to the mass of Ti is 6.25 to 11.12; and / or, The mass ratio of Mg to Al is 0.41~0.
50.
7. The method for preparing the steel material according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: Providing raw materials according to the elemental composition of the steel, smelting the raw materials, and then casting them to obtain ingots; The cast slab is subjected to a rolling process and then cooled.
8. The preparation method according to claim 7, characterized in that: The rolling process includes recrystallization zone rolling and non-recrystallization zone rolling performed sequentially; The starting rolling temperature of the recrystallization zone rolling is 1010°C~1150°C, the single-pass reduction rate is ≥14%, and the cumulative reduction rate is ≥40%; The starting rolling temperature of the non-recrystallization zone rolling is 710°C to 850°C, the single-pass reduction rate is ≥10%, and the cumulative reduction rate is ≥60%; and / or, The final rolling temperature of the non-recrystallization zone rolling is 20°C to 50°C above Ar3°C; wherein Ar3 is calculated as follows: Ar3=910-310×ω C -80×ω Mn -20×ω Cu -15×ω Cr -55×ω Ni -80×ω Mo -0.35×(H-8), In the formula, ω C ,ω Mn ,ω Cu ,ω Cr ,ω Ni and Mo It represents the mass percentage of each element component in the steel; H in the formula is the thickness of the steel plate, in mm.
9. The preparation method according to any one of claims 7 to 8, characterized in that The cooling step comprises: cooling the rolled steel to 25°C to 40°C above Ar1°C at a speed of ≥10°C / s, and then air cooling to below 300°C; wherein Ar1 is calculated as follows: Ar1=630-45×ω Mn -40×ω V -35×ω Si -30×ω Cr -25×ω Mo -20×ω Ni -15×ω W , In the formula, ω Mn ,ω V ,ω Si ,ω C ,ω Mo ,ω Ni and W It represents the mass percentage of each element component in the steel, and the element component not contained in the steel is 0.
10. A steel product, characterized in that: The steel product is prepared by the steel material as claimed in any one of claims 1 to 6.