Heat-treated and cold-rolled steel sheet, manufacturing method and use thereof, and vehicle
By rationally formulating elements in steel plates and using heat treatment cold rolling technology to form high bainite microstructure and internal oxide layer, the problem of insufficient strength and formability of steel plates in the prior art is solved, and high tensile strength and Good phosphating properties, suitable for high-performance steel plate manufacturing of automotive parts.
Patent Information
- Application Number
- CN202411271255.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-12-19
- Filing Date
- 2018-11-05
- Publication Date
- 2024-12-06
AI Technical Summary
It is difficult for the prior art to manufacture steel plates that can meet the assembly standards for complex components of automobile components and reduce the weight of the vehicle while maintaining high strength and high formability, especially failing to meet the tensile strength and good phosphating properties of 1000 MPa.
Steel plates containing elements such as 0.18% to 0.24% carbon, 1.5% to 2.5% manganese, 1.2% to 2% silicon, 0.01% to 0.06% aluminum, 0.2% to 0.5% chromium, etc., and are formed by heat treatment and cold rolling process. At least 55% bainite microstructure and an internal oxide layer of 3 microns or less is formed on the surface, combined with appropriate annealing and cooling treatment, achieve a tensile strength above 1000MPa and a phosphating coverage of more than 96% Rate.
The steel plate is achieved with high tensile strength, good phosphating properties and forming adaptability, and is especially suitable for rolling with good weldability and coating, meeting the strength and durability requirements of automotive parts, while reducing vehicle weight.
Smart Images

Figure BDA0005038784230000131 
Figure BDA0005038784230000141 
Figure BDA0005038784230000142
Abstract
Description
[0001] This application is a divisional application of an invention patent application with an application date of November 5, 2018, application number 201880077389.6 (PCT / IB2018 / 058669), and invention name “Cold-rolled and heat-treated steel plate and its manufacturing method”. Technical Field
[0002] The present invention relates to a cold-rolled and heat-treated steel sheet suitable for use as a steel sheet for vehicles. Background Art
[0003] Auto parts need to meet two inconsistent requirements, that is, easy to form and have strength, but in recent years, in consideration of global environmental issues, a third requirement for improving fuel consumption has been given to automobiles. Therefore, now auto parts must be made of materials with high formability in order to meet the standard of easy assembly of complex automobile components, and at the same time must be improved in strength for vehicle crash resistance and durability, while reducing the weight of the vehicle to improve fuel efficiency.
[0004] Therefore, a great deal of research and development efforts have been made to reduce the amount of material used in automobiles by increasing the strength of the material. Conversely, an increase in the strength of a steel sheet reduces formability, and therefore a material having both high strength and high formability must be developed.
[0005] Early research and development in the field of high strength and high formability steel sheets has resulted in several methods for producing high strength and high formability steel sheets, some of which are listed herein for an overall understanding of the present invention.
[0006] US 9 074 272 describes a steel having the following chemical composition: 0.1% to 0.28% C, 1.0% to 2.0% Si, 1.0% to 3.0% Mn, the remainder consisting of iron and unavoidable impurities. The microstructure contains 5% to 20% of retained austenite, 40% to 65% of bainitic ferrite, 30% to 50% of polygonal ferrite, and less than 5% of martensite. US 9 074 272 relates to cold rolled steel sheets with excellent elongation, but the invention described therein fails to achieve a strength of 900 MPa as a requirement for reducing weight while maintaining the robustness of complex automotive parts.
[0007] US2015 / 0152533 discloses a method for producing high-strength steel, which contains: C: 0.12% to 0.18%, Si: 0.05% to 0.2%, Mn: 1.9% to 2.2%, Al: 0.2% to 0.5%, Cr: 0.05% to 0.2%, Nb: 0.01% to 0.06%, P: ≤0.02%, S: ≤0.003%, N: ≤0.008%, Mo: ≤0.1%, B: ≤0.0007%, Ti: ≤0.01%, Ni: ≤0.1%, Cu: ≤0.1%, and iron and inevitable impurities as the remainder. The steel sheet produced by the method described in patent application US2015 / 0152533 should have a microstructure consisting of 50% to 90% by volume of ferrite (including bainitic ferrite), 5% to 40% by volume of martensite, up to 15% by volume of retained austenite, and up to 10% by volume of other structural components. Although US2015 / 0152533 contains a large amount of martensite (i.e., up to 40%), it still fails to reach a tensile strength level of 900 MPa.
[0008] US2014 / 170439 provides a cold-rolled steel sheet. The steel sheet has a strength greater than 1000 MPa, a uniform elongation greater than 12%, and a V-shaped bendability greater than 90°. The composition of the steel sheet, expressed in weight percentage, includes: 0.15% ≤ C ≤ 0.25%, 1.8% ≤ Mn ≤ 3.0%, 1.2% ≤ Si ≤ 2%, 0% ≤ Al ≤ 0.10%, 0% ≤ Cr ≤ 0.50%, 0% ≤ Cu ≤ 1%, 0% ≤ Ni ≤ 1%, 0% ≤ S ≤ 0.005%, 0% ≤ P ≤ 0.020%, Nb ≤ 0.015%, Ti ≤ 0.020%, V ≤ 0.015%, Co ≤ 1%, N ≤ 0.008%, B ≤ 0.001%, wherein Mn + Ni + Cu ≤ 3%. The remainder of the composition is composed of iron and unavoidable impurities generated by processing. The microstructure contains, by area percentage, 5% to 20% polygonal ferrite, 10% to 15% retained austenite, 5% to 15% martensite and the balance bainite. The bainite is in the form of laths and contains carbides between the laths. The number N of inter-lath carbides greater than 0.1 micrometers per unit surface area is less than or equal to 50,000 / mm 2 A manufacturing method and a motor vehicle are also provided. However, US2014 / 170439 does not mention the phosphatability of steel.
[0009] Since the known prior art related to the manufacture of high strength and high formability steel sheets has one or another drawback, there is a need for cold rolled steel sheets having a strength greater than 1000 MPa and a method for manufacturing the same. Summary of the invention
[0010] The object of the present invention is to solve these problems by making a usable cold rolled steel sheet having the following characteristics at the same time:
[0011] - an ultimate tensile strength greater than or equal to 1000 MPa, and preferably higher than 1180 MPa, or even higher than 1220 MPa,
[0012] -Good phosphatizability to at least 96% of the surface.
[0013] According to one aspect of the present invention, there is provided a heat-treated and cold-rolled steel sheet, the steel comprising, by weight percentage: 0.18%≤carbon≤0.24%, 1.5%≤manganese≤2.5%, 1.2%≤silicon≤2%, 0.01%≤aluminum≤0.06%, 0.2%≤chromium≤0.5%, phosphorus≤0.02%, sulfur≤0.03%, and optionally one or more of the following elements: niobium≤0.06%, titanium≤0.08%, vanadium≤0.1%, calcium≤0.005%, and the remainder comprising iron and unavoidable impurities, the steel sheet also having, by area fraction, a microstructure comprising: 0% to 15% of tempered martensite, 10% to 15% of retained austenite, and optionally up to 30% of ferrite, the remainder being composed of bainite, the bainite content being at least 55% and having an internal oxide layer of 3 μm or less on both surfaces of the steel sheet.
[0014] Optionally, the steel plate composition includes 2.0% to 2.3% manganese.
[0015] Optionally, the steel sheet composition contains a maximum of 0.013% phosphorus.
[0016] Optionally, the microstructure of the steel plate comprises greater than 60% bainite.
[0017] Optionally, the carbon concentration of the retained austenite in the steel plate is 0.9% to 1.15%.
[0018] Optionally, the steel sheet exhibits a tensile strength of greater than or equal to 1000 MPa and a phosphate coverage of 96% or more.
[0019] Optionally, the steel sheet exhibits a tensile strength of greater than or equal to 1050 MPa and a phosphate coverage of 98% or more.
[0020] Optionally, the steel sheet has an internal oxide layer on both surfaces having a thickness of up to 2 microns or less.
[0021] Optionally, the steel sheet has an internal oxide layer on both surfaces having a thickness of up to 1 micron or less.
[0022] In a preferred embodiment, the steel sheet according to the present invention may have a yield strength value greater than or higher than 700 MPa.
[0023] Preferably, such a steel may also have good formability, especially for rolling with good weldability and paintability.
[0024] Another object of the invention is also to provide a method for manufacturing these panels which is compatible with conventional industrial applications while being robust to manufacturing parameter variations.
[0025] According to another aspect of the present invention, there is provided a method for manufacturing a heat-treated and cold-rolled steel sheet, comprising the following consecutive steps:
[0026] - providing a steel composition according to one aspect of the invention to obtain a semi-finished product,
[0027] - reheating the semi-finished product to a temperature of 1000° C. to 1280° C.;
[0028] - rolling the semi-finished product completely in the austenitic range to obtain a hot rolled steel sheet, wherein the hot rolling final rolling temperature is greater than or equal to 850°C;
[0029] - cooling the plate to a temperature lower than or equal to 500°C at a cooling rate higher than 30°C / second; and coiling the hot rolled plate and maintaining the temperature of the coiled plate lower than 570°C;
[0030] - cooling the hot rolled sheet;
[0031] - performing a descaling process on the hot rolled steel sheet;
[0032] - subjecting the hot rolled steel sheet to annealing at a temperature of 500° C. to 750° C. for a period of 1 hour to 96 hours;
[0033] - subjecting the hot rolled annealed steel sheet to an optional descaling process;
[0034] - cold rolling the hot rolled steel sheet at a reduction ratio of 35% to 90% to obtain a cold rolled steel sheet;
[0035] - then annealing the cold rolled steel sheet continuously for at least 100 seconds at a rate of 1°C / s to 20°C / s to a soaking temperature of Ac1 to Ac3+50°C, the temperature and time being selected to obtain a minimum percentage of 70% austenite;
[0036] - the plate is then cooled at a rate greater than 10°C / second to a temperature of Ms-20°C to Ms+40°C, where Ms is the Ms temperature of the initial austenite before cooling, and then
[0037] - the cold rolled steel sheet is maintained at 350°C to 450°C for a period of 200 seconds to 1000 seconds; then
[0038] - The plate is cooled to room temperature at a cooling rate of no more than 200°C / sec.
[0039] According to another aspect of the present invention, there is provided a method for manufacturing a heat-treated and cold-rolled steel sheet, comprising the following consecutive steps:
[0040] - providing a steel composition according to one aspect of the invention to obtain a semi-finished product,
[0041] - reheating the semi-finished product to a temperature of 1000° C. to 1280° C.;
[0042] - rolling the semi-finished product completely in the austenitic range to obtain a hot rolled steel sheet, wherein the hot rolling final rolling temperature is greater than or equal to 850°C;
[0043] - cooling the plate at a cooling rate higher than 30°C / second to a cooling temperature lower than or equal to 500°C; and coiling the hot rolled plate and maintaining the temperature of the coiled plate lower than 570°C;
[0044] - cooling the hot rolled sheet;
[0045] - subjecting the hot rolled steel sheet to annealing at a temperature of 350° C. to 500° C. for a period of 1 hour to 96 hours;
[0046] - performing at least one descaling process on the hot rolled steel sheet before or after annealing of the hot rolled steel sheet;
[0047] - cold rolling the hot rolled steel sheet at a reduction ratio of 35% to 90% to obtain a cold rolled steel sheet;
[0048] - then annealing the cold rolled steel sheet continuously for at least 100 seconds at a rate of 1°C / s to 20°C / s to a soaking temperature of Ac1 to Ac3+50°C, the temperature and time being selected to obtain a minimum percentage of 70% austenite;
[0049] - the plate is then cooled at a rate greater than 10°C / second to a temperature of Ms-20°C to Ms+40°C, where Ms is the Ms temperature of the initial austenite before cooling, and then
[0050] - the cold rolled steel sheet is maintained at 350°C to 450°C for a period of 200 seconds to 1000 seconds; then
[0051] - The plate is cooled to room temperature at a cooling rate of no more than 200°C / sec.
[0052] Optionally, the cooling temperature of the steel plate is set to 150°C to 500°C.
[0053] Optionally, the steel sheet is continuously annealed at 800° C. to 900° C. for 100 seconds to 1000 seconds.
[0054] The cold rolled heat-treated steel sheet of the present invention may be optionally coated with zinc or a zinc alloy, or with aluminum or an aluminum alloy to improve its corrosion resistance.
[0055] According to yet another aspect of the present invention, there is provided use of the steel sheet or the steel sheet produced according to the manufacturing method for manufacturing a structural component or a safety component of a vehicle.
[0056] According to yet another aspect of the present invention, there is provided a vehicle comprising a component obtained according to the above use. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 Not according to the invention. Figure 1 FIG. 1 is a micrograph showing cracks formed due to internal oxides on the surface of a cold-rolled steel sheet and an internal oxide layer formed thereby. In order to illustrate the cracks, one of the cracks is marked as 10. The cold-rolled steel sheet belongs to steel grade 7 of Table 1.
[0058] Figure 2 FIG. 2 is a micrograph showing the surface of a cold-rolled steel sheet according to the present invention. The cold-rolled steel sheet has no internal oxide layer and belongs to steel type 2 in Table 1.
[0059] Figure 3 Not according to the invention. Figure 3 FIG. 2 is a micrograph showing cracks formed due to internal oxides and internal oxide layers formed therefrom on the surface of a cold-rolled and heat-treated steel sheet. In order to illustrate the cracks, one of the cracks is marked as 20. The cold-rolled steel sheet belongs to steel grade 7 of Table 1.
[0060] Figure 4 FIG. 2 is a micrograph showing the surface of a cold-rolled and heat-treated steel sheet according to the present invention. The cold-rolled steel sheet has an internal oxide layer of less than 3 micrometers. The cold-rolled steel sheet belongs to steel type 2 of Table 1.
[0061] Figure 5 Figure 2 shows a micrograph of phosphating on a cold rolled and heat treated steel sheet not according to the invention. Figure 5 Porosity is shown over the coverage area. One of the porosity markers is highlighted as 30. Figure 5 Belongs to steel grade 7 in Table 1.
[0062] Figure 6 The following is a micrograph showing phosphate treatment on a cold rolled and heat treated steel sheet according to the invention. The steel sheet shown belongs to steel grade 2 of Table 1 and has a phosphate coverage of 100%. DETAILED DESCRIPTION
[0063] Other features and advantages of the present invention will become apparent from the following detailed description of the invention.
[0064] Carbon is present in steel at 0.18% to 0.24%. Carbon is an element necessary to improve the strength of steel sheets by producing low temperature transformation phases such as martensite. In addition, carbon also plays a key role in austenite stabilization. A content of less than 0.18% does not stabilize austenite, thereby reducing strength as well as ductility. On the other hand, when the carbon content exceeds 0.24%, the weld zone and heat-affected zone are significantly hardened, and thus the mechanical properties of the weld zone are impaired.
[0065] The manganese content of the steel of the present invention is 1.5% to 2.5%. Manganese is an element that both imparts strength and stabilizes austenite to obtain retained austenite. It has been found that manganese in an amount of at least about 1.5% by weight is used to provide strength and hardenability of the steel sheet and to stabilize austenite. Therefore, higher percentages of manganese, such as 1.9% to 2.2%, are preferred. However, when manganese is greater than 2.5%, this produces adverse effects such as slowing down the transformation of austenite to bainite during isothermal holding for bainite transformation, resulting in reduced ductility. In addition, manganese contents above 2.5% also reduce the weldability of the steel of the present invention.
[0066] The silicon content of the steel of the present invention is 1.2% to 2%. Silicon as a component hinders the precipitation of carbon from austenite. Therefore, due to the presence of 1.2% of silicon, the carbon-rich austenite is stable at room temperature. However, adding more than 2% of silicon does not improve the mentioned effect and causes problems such as hot rolling embrittlement. Therefore, the concentration is controlled within the upper limit of 2%.
[0067] The aluminum content of the steel of the present invention is 0.01% to 0.06%. Within such a range, the aluminum in the steel combines with nitrogen to form aluminum nitride, thereby reducing the size of the grains. However, when the aluminum content exceeds 0.06% in the present invention, the Ac3 point is increased, thereby reducing productivity.
[0068] The steel of the present invention has a chromium content of 0.2% to 0.5%. Chromium is an essential element for providing strength and hardening to steel, but above 0.5% it impairs the surface finish of the steel when used.
[0069] The phosphorus content of the steel of the invention is limited to 0.02%. Phosphorus is an element that hardens in solid solution and also interferes with the formation of carbides. Therefore, small amounts of at least 0.002% phosphorus can be advantageous, but phosphorus also has its adverse effects, such as a reduction in spot weldability and hot ductility, especially due to its tendency to segregate at grain boundaries or co-segregate with manganese. For these reasons, the phosphorus content is preferably limited to a maximum of 0.015%.
[0070] Sulfur is not an essential element but may be contained in the steel as an impurity. From the viewpoint of manufacturing cost, the sulfur content is preferably as low as possible, but is 0.03% or less, and preferably at most 0.003%. In addition, if higher sulfur is present in the steel, sulfur combines with Mn and Ti in particular to form sulfides and reduces their beneficial effects on the present invention.
[0071] Niobium is an optional element that can be added to the steel in an amount of 0% to 0.06%, preferably 0.0010% to 0.06%. Niobium is suitable for forming carbonitrides by precipitation hardening to impart strength to the steel according to the invention. Since niobium delays recrystallization during heating, the microstructure formed at the end of the holding temperature and therefore after full annealing is finer, which leads to a hardening of the product. However, when the niobium content is above 0.06%, the amount of carbonitrides is disadvantageous for the invention, since a large amount of carbonitrides tends to reduce the ductility of the steel.
[0072] Titanium is an optional element that can be added to the steel of the invention in an amount of 0% to 0.08%, preferably 0.001% to 0.08%. Like niobium, it participates in carbonitrides and therefore plays a role in hardening. However, titanium also participates in the formation of TiN that occurs during solidification of the cast product. The amount of Ti is therefore limited to 0.08% in order to avoid coarse TiN that is detrimental to hole expansion. In the case of a titanium content below 0.001%, titanium does not have any effect on the steel of the invention.
[0073] Vanadium is an optional element that can be added to the steel of the invention in an amount of 0% to 0.1%, preferably 0.001% to 0.01%. Like niobium, it participates in carbonitrides and therefore plays a role in hardening. However, vanadium also participates in the formation of VN that occurs during solidification of the cast product. The amount of V is therefore limited to 0.1% in order to avoid coarse VN that is detrimental to hole expansion. In the case of a vanadium content below 0.001%, vanadium does not have any effect on the steel of the invention.
[0074] Calcium is an optional element that can be added to the steel of the present invention at 0% to 0.005%, preferably 0.001% to 0.005%. Calcium is added to the steel of the present invention as an optional element, especially during inclusion treatment. Calcium aids in the refining of steel by capturing harmful sulfur content during the spheroidizing treatment of the steel.
[0075] Other elements such as cerium, boron, magnesium or zirconium may be added alone or in combination in the following proportions: Ce≤0.1%, B≤0.01%, Mg≤0.05% and Zr≤0.05%. Up to the maximum content levels shown, these elements enable grain refinement during solidification.
[0076] Among the alloying elements present in the steel of the present invention, silicon, manganese, aluminum and chromium are more oxidizable than iron and it is well known that during coiling, hot strip annealing, annealing and during other similar heat treatment processes, the elements mentioned except iron also undergo selective oxidation, forming internal oxides.
[0077] Figure 1 The following is a micrograph of a cold rolled steel sheet not according to the invention, which has an inner oxide layer, wherein these selective oxides are formed during coiling of the hot rolled steel sheet due to the reduced oxygen partial pressure, and these selective oxides also lead to cracks at the grain boundaries during cold rolling of the cold rolled steel sheet. Figure 1 In the figure, cracks on the surface of the cold rolled steel sheet are also shown (10). Figure 1 Internal oxides with a thickness greater than 1 micron on the surface of the cold rolled steel sheet are also shown. Similarly, selective oxidation also occurs during annealing.
[0078] Figure 2 FIG. 1 is a micrograph showing a cold-rolled steel sheet according to the present invention, wherein the cold-rolled steel sheet has no internal oxide.
[0079] Figure 3 To show a micrograph of a heat-treated cold-rolled steel sheet not according to the invention, which has an internal oxide layer, wherein these selective oxides are formed during coiling of the hot-rolled steel sheet or during hot-zone annealing of the hot-rolled steel sheet or during annealing of the cold-rolled steel sheet due to the reduced oxygen partial pressure, and these selective oxides also lead to cracks at grain boundaries during cold rolling of the cold-rolled steel sheet, which are aggravated during annealing. Figure 3 In FIG. 2 , cracks on the surface of a heat-treated cold-rolled steel sheet are also shown ( 20 ). Figure 3 Internal oxides with a thickness greater than 3 microns on the surface of the cold rolled steel sheet are also shown.
[0080] Figure 4 The micrograph of a heat-treated cold rolled steel sheet according to the present invention is shown, wherein the heat-treated cold rolled steel sheet has an internal oxide layer, and according to the present invention, an oxide layer with a thickness of up to 3 microns is acceptable on the heat-treated cold rolled steel sheet.
[0081] Therefore, the present invention contemplates the implementation of specific process parameters, such as maintaining the coiling temperature below 500°C and performing at least one forced pickling before cold rolling to control the formation of internal oxides. The present invention maintains an internal oxide layer of up to 3 microns on the final cold rolled and heat treated steel sheet. In a preferred embodiment, such a layer is formed of iron, silicon, manganese and chromium.
[0082] In another embodiment, it is preferred that an inner oxide layer having a thickness of 1 micrometer or less is present on the cold rolled sheet after cold rolling.
[0083] The remainder of the steel's composition consists of iron and unavoidable impurities resulting from processing.
[0084] The microstructure of the steel sheet according to the present invention comprises, by area fraction, 0 to 15% tempered martensite, 10 to 15% retained austenite, and optionally up to 30% ferrite, the remainder consisting of bainite, the bainite content being at least 55%.
[0085] Bainite is the matrix of the steel and is contained in a minimum of 55%, preferably 60%. Within the framework of the present invention, bainite includes lath bainite and granular bainite. Granular bainite is bainite with a very low density of carbides, which means that the steel contains less than 100 carbides / 100 μm. 2 The lath bainite is in the form of thin ferrite laths, with carbides formed between the laths. The size of the carbides present between the laths is such that the number of carbides larger than 0.1 micrometer is less than 50,000 / mm 2 The lath bainite provides the steel with adequate hole expansion, while the granular bainite provides improved elongation.
[0086] Tempered martensite is contained in an amount of 0% to 15%. It is preferred to have such a content of tempered martensite to achieve a strength level of 1000 MPa or more, and if the amount of martensite reaches more than 15%, ductility will be adversely affected.
[0087] Retained austenite is included in an amount of 10% to 15%. It is known that the solubility of carbon in retained austenite is higher than that in bainite and therefore acts as an effective carbon sink, thereby delaying the formation of carbides in bainite. The retained austenite of the present invention preferably contains 0.9% to 1.15% carbon, with the average carbon content in the austenite being 1.00%. Austenite also imparts ductility to the steel of the present invention.
[0088] Martensite and austenite may preferably be present in the steel according to the invention as separate phases or in the form of martensite-austenite islands.
[0089] Ferrite may be present in the steel at 0% to 30%. Such ferrite may include polygonal ferrite, lath ferrite, acicular ferrite, plate ferrite or epitaxial ferrite. The presence of ferrite in the present invention may impart formability and elongation to the steel. The presence of ferrite has a negative effect due to the fact that ferrite increases the hardness gap and reduces local ductility through hard phases such as martensite and bainite. If the presence of ferrite is above 30%, the target tensile strength cannot be achieved.
[0090] The steel sheet according to the invention can be produced by any suitable method. A preferred method comprises providing a semi-finished casting of a steel having a chemical composition according to the invention. The casting can be made into an ingot or continuously into the form of a thin slab or a thin strip, i.e., a thickness ranging from about 220 mm for a slab to tens of millimeters for a thin strip.
[0091] For example, a slab will be considered as a semi-finished product. The slab having the above chemical composition is produced by continuous casting, wherein the slab preferably undergoes a direct slight reduction during casting to ensure elimination of center segregation and reduction of porosity. The slab provided by the continuous casting process can be used directly at high temperature after continuous casting, or can be first cooled to room temperature and then heated for hot rolling.
[0092] The temperature of the slab subjected to hot rolling is preferably at least 1000°C, preferably higher than 1200°C and must be lower than 1280°C. In the case where the temperature of the slab is lower than 1000°C, an excessive load is imposed on the rolling mill, and furthermore, the temperature of the steel may decrease to the ferrite transformation temperature during finish rolling, whereby the steel will be rolled in a state containing transformation ferrite in the structure. Furthermore, the temperature must not be higher than 1280°C, because there will be a risk of the formation of coarse ferrite grains leading to coarse ferrite grains, which reduces the ability of these grains to recrystallize during hot rolling. The larger the initial ferrite grain size, the less likely it is to recrystallize, which means that reheating temperatures higher than 1280°C must be avoided, because this is industrially expensive and disadvantageous in terms of the recrystallization of ferrite.
[0093] The temperature of the slab is preferably high enough so that hot rolling can be completed completely in the austenite range, and the hot rolling final rolling temperature is kept above 850°C and preferably above 900°C. Final rolling must be performed above 850°C because the steel sheet shows a significant drop in rollability below this temperature. A final rolling temperature between 900°C and 950°C is preferred to have a structure that is conducive to recrystallization and rolling.
[0094] The plate obtained in this way is then cooled to a temperature below 500°C at a cooling rate higher than 30°C / sec. The cooling temperature is kept below 500°C to avoid selective oxidation of alloying elements such as manganese, silicon and chromium. Preferably, the cooling rate will be less than or equal to 65°C / sec and higher than 35°C / sec. Thereafter, the hot rolled steel sheet is coiled, and during the time that the hot rolled sheet remains coiled, a transformation of austenite to bainite occurs, and the temperature of the coiled hot rolled sheet increases due to recalendering. The temperature of the coiled hot rolled steel sheet must be kept below 570°C to avoid selective internal oxidation of silicon, manganese, aluminum and chromium on the surface of the hot rolled coil, because these oxides form cracks on the surface of the hot rolled steel sheet. Thereafter, the coiled hot rolled steel sheet is cooled to room temperature. The hot rolled steel sheet is then subjected to a descaling process such as pickling to remove the scale formed during hot rolling and to ensure that there is no scale on the surface of the hot rolled steel sheet before the hot rolled steel sheet is subjected to tropical annealing.
[0095] The hot rolled sheet is then subjected to tropical annealing at a temperature of 350°C to 750°C for a period of 1 hour to 96 hours. The temperature and time of such tropical annealing are selected to ensure softening of the hot rolled sheet to facilitate cold rolling of the hot rolled steel sheet. In addition, the atmosphere of the tropical annealing is controlled to avoid oxidation during the tropical annealing. If the tropical annealing is performed between a temperature range of 350°C to 500°C for a period of 1 hour to 96 hours, the descaling process before the tropical annealing is not mandatory, because in this temperature range, the possibility of increasing the thickness of the oxide layer is very small. However, if the tropical annealing is performed between 500°C to 750°C, it is mandatory to perform the descaling process before such annealing.
[0096] The hot rolled steel sheet is then cooled to room temperature to obtain an annealed hot rolled sheet. Thereafter, the annealed hot rolled sheet may be subjected to an optional descaling process. According to the present invention, at least one descaling process must be performed before cold rolling.
[0097] The annealed hot-rolled sheet is then cold-rolled at a thickness reduction ratio of 35% to 70% to obtain a cold-rolled steel sheet having substantially no internal oxide.
[0098] Figure 2 The micrograph of a cold rolled steel sheet according to the invention is shown, wherein the cold rolled steel sheet has no internal oxide, but according to the invention an oxide layer up to 1 micron thick on the cold rolled sheet after pickling and HBA is acceptable.
[0099] The cold rolled steel sheet is then subjected to annealing to impart the target microstructure and mechanical properties to the steel of the present invention.
[0100] In order to continuously anneal the cold rolled steel sheet, the cold rolled steel sheet is first heated to a soaking temperature of Ac1 to Ac3+50°C at a heating rate of 1°C / s to 20°C / s, preferably greater than 3°C / s, during at least 100 seconds and preferably not more than 1000 seconds to ensure sufficient recrystallization and transformation to obtain a minimum 70% austenite microstructure. Ac1 of the steel according to the invention is generally 680°C to 750°C. Ac3 of the steel according to the invention is generally 820°C to 900°C.
[0101] The plate is then cooled at a cooling rate greater than 10°C / second to a cooling temperature range between Ms-20°C and Ms+40°C, where Ms is calculated according to the following formula:
[0102] Ms=565-(31*[Mn]+13*[Si]+10*[Cr]+18*[Ni]+12*[Mo])-600*(1-EXP(-0,96*[C]))
[0103] In a preferred embodiment, the cooling rate is greater than 30°C / second.
[0104] The temperature of the cold rolled steel sheet is then brought to a temperature range of Ms+10°C to Ms+100°C, which is typically 350°C to 450°C, and maintained at this temperature for at least 200 seconds but not more than 1000 seconds. This isothermal overaging stabilizes the carbon-rich austenite and contributes to the formation and stabilization of the low-density carbide bainite, thereby imparting the target mechanical properties to the steel of the present invention.
[0105] The cold rolled steel sheet is then cooled to room temperature at a cooling rate not exceeding 200° C. / sec. During this cooling, unstable retained austenite may be transformed into fresh martensite in the form of MA islands.
[0106] An optional skin pass rolling or leveling operation with a reduction ratio of less than 0.8% may be performed at this stage.
[0107] Figure 4 The micrograph of a heat-treated cold rolled steel sheet according to the present invention is shown, which belongs to Steel Sample 2, wherein the heat-treated cold rolled steel sheet according to the present invention has an internal oxide layer of less than 3 micrometers.
[0108] The heat treated cold rolled sheet may then optionally be coated by electrodeposition or vacuum coating or any other suitable process.
[0109] A post-batch annealing may optionally be carried out after annealing for the uncoated product or after coating for the coated product, preferably at 170 to 210° C. for 12 to 30 hours, to reduce the hardness gradient between the phases and ensure degassing of the coated product.
[0110] Example
[0111] The following tests and examples provided herein are non-limiting in nature and must be considered for illustrative purposes only, and will demonstrate the advantageous features of the present invention and illustrate the importance of parameters selected by the inventors after extensive experimentation, and further determined the properties that can be achieved by the steel according to the present invention.
[0112] Steel sheet samples according to the invention and according to some comparative grades were prepared with the compositions summarized in Table 1 and the process parameters are summarized in Table 2. The corresponding microstructures of these steel sheets are summarized in Table 3 and the properties in Table 4.
[0113] Table 1 depicts steels having compositions expressed in weight percent.
[0114] Table 1: Composition of the trial
[0115] Steel Type C Mn Si Al Cr P S N Nb Ti v Ca 1 0.212 2.09 1.512 0.042 0.352 0.011 0.002 0.007 0.001 0.005 - - 2 0.213 2.08 1.490 0.034 0.357 0.01 0.001 0.004 0.002 0.005 0.002 0.001 3 0.211 2.11 1.473 0.042 0.368 0.012 0.003 0.004 0.001 0.004 0.002 - 4 0.197 2.215 1.472 0.043 0.200 0.0126 0.0004 0.005 0.002 0.01 0.004 - 5 0.212 2.09 1.514 0.042 0.352 0.011 0.002 0.007 0.001 0.005 0.002 - 6 0.212 2.09 1.492 0.042 0.355 0.011 0.002 0.007 0.001 0.004 0.002 - 7 0.211 2.08 1.480 0.041 0.351 0.011 0.002 0.007 0.001 0.004 0.002 - 8 0.212 2.094 1.490 0.042 0.354 0.01 0.002 0.007 0.001 0.004 0.002 - 9 0.202 2.211 1.503 0.056 0.198 0.013 0.0022 0.0038 0.0007 0.006 0.0007 - 10 0.212 2.092 1.535 0.042 0.352 0.011 0.002 0.007 0.008 0.004 0.002 -
[0116] Table 2 summarizes the annealing process parameters implemented on the steels in Table 1.
[0117] Table 1 also shows the bainite transformation temperature Bs and the martensite transformation temperature Ms of the steel of the present invention and the reference steel. The calculation of Bs and Ms is completed by using the Van Bohemen formula published in Materials Science and Technology (2012), Vol. 28, No. 4, pp. 487-495, and the formula is as follows:
[0118] Bs=839-(86*[Mn]+23*[Si]+67*[Cr]+33*[Ni]+75*[Mo])-270*(1-EXP(-1,33*[C]))
[0119] Ms=565-(31*[Mn]+13*[Si]+10*[Cr]+18*[Ni]+12*[Mo])-600*(1-EXP(-0,96*[C]))
[0120] Furthermore, before the annealing treatment of the steel according to the present invention and the reference steel, the samples were heated to a temperature of 1000°C to 1280°C and then hot rolled at a finishing temperature of more than 850°C.
[0121]
[0122] Table 3 summarizes the results of tests carried out according to standards on different microscopes, such as a scanning electron microscope, to determine the microstructural composition of both the steel tests of the invention and the reference tests.
[0123] Table 3: Microstructure of the test
[0124]
[0125] Table 4 summarizes the mechanical and surface properties of both the inventive steel and the reference steel. The tensile strength and yield strength were determined according to the JIS Z2241 standard.
[0126] Table 4: Tested mechanical and surface properties
[0127]
[0128] I = according to the invention; R = reference; underlined values: not according to the invention.
[0129] The examples show that the steel sheet according to the invention is the only one which exhibits all the targeted properties due to its specific composition and microstructure.
Claims
1. A heat-treated and cold-rolled steel sheet, the steel comprising, by weight percentage: 0.18%≤Carbon≤0.24%, 1.5%≤Manganese≤2.5%, 1.2%≤Silicon≤2%, 0.01%≤Aluminum≤0.06%, 0.2%≤Chromium≤0.5%, Phosphorus ≤ 0.02%, Sulfur ≤ 0.03%, and optionally one or more of the following elements: Niobium ≤ 0.06%, Titanium ≤ 0.08%, Vanadium ≤ 0.1%, Calcium ≤ 0.005% The steel sheet has a microstructure comprising, by area fraction, 0% to 15% of tempered martensite, 10% to 15% of retained austenite, and optionally up to 30% of ferrite, the balance being bainite, the bainite content being at least 55% and having an internal oxide layer of 3 μm or less on both surfaces of the steel sheet.
2. The heat-treated and cold-rolled steel sheet according to claim 1, wherein the composition contains 2.0% to 2.3% manganese.
3. The heat-treated and cold-rolled steel sheet according to claim 1 or 2, wherein the composition contains a maximum of 0.013% phosphorus.
4. The heat treated and cold rolled steel sheet according to any one of claims 1 to 3, wherein the microstructure comprises greater than 60% bainite.
5. The heat-treated and cold-rolled steel sheet according to any one of claims 1 to 4, wherein the carbon concentration of the retained austenite is 0.9% to 1.15%.
6. The heat-treated and cold-rolled steel sheet according to any one of claims 1 to 5, which exhibits a tensile strength of greater than or equal to 1000 MPa and a phosphating coverage of 96% or more.
7. The heat-treated and cold-rolled steel sheet according to claims 1 to 6, which exhibits a tensile strength of greater than or equal to 1050 MPa and a phosphating coverage of 98% or more.
8. The heat-treated and cold-rolled steel sheet according to claims 1 to 7, having an inner oxide layer having a thickness of up to 2 micrometers or less on both surfaces.
9. The heat-treated and cold-rolled steel sheet according to claim 8, having an inner oxide layer having a thickness of up to 1 micrometer or less on both surfaces.
10. A method for manufacturing a heat-treated and cold-rolled steel sheet, comprising the following consecutive steps: - providing a steel composition according to any one of claims 1 to 3 to obtain a semi-finished product, - reheating the semi-finished product to a temperature of 1000° C. to 1280° C.; - rolling the semi-finished product completely in the austenitic range to obtain a hot rolled steel sheet, wherein the hot rolling final rolling temperature is greater than or equal to 850° C.; - cooling the plate to a temperature lower than or equal to 500°C at a cooling rate higher than 30°C / second; and coiling the hot rolled plate and maintaining the temperature of the coiled plate lower than 570°C; - cooling the hot rolled sheet; - performing a scale removal process on the hot rolled steel sheet; - subjecting the hot rolled steel sheet to annealing at a temperature of 500° C. to 750° C. for a period of 1 hour to 96 hours; - subjecting the hot rolled annealed steel sheet to an optional descaling process; - cold rolling the hot rolled steel sheet at a reduction ratio of 35% to 90% to obtain a cold rolled steel sheet; - then annealing the cold rolled steel sheet continuously for at least 100 seconds at a rate of 1°C / s to 20°C / s to a soaking temperature of Ac1 to Ac3+50°C, the temperature and time being selected to obtain a minimum percentage of 70% austenite; - the plate is then cooled at a rate greater than 10°C / second to a temperature of Ms-20°C to Ms+40°C, where Ms is the Ms temperature of the initial austenite before cooling, and then - Maintaining the cold rolled steel sheet at 350°C to 450°C for 200 seconds to 1000 seconds; and then - The plate is cooled to room temperature at a cooling rate of no more than 200°C / second.
11. A method for manufacturing a heat-treated and cold-rolled steel sheet, comprising the following consecutive steps: - providing a steel composition according to any one of claims 1 to 3 to obtain a semi-finished product, - reheating the semi-finished product to a temperature of 1000° C. to 1280° C.; - rolling the semi-finished product completely in the austenitic range to obtain a hot rolled steel sheet, wherein the hot rolling final rolling temperature is greater than or equal to 850° C.; - cooling the plate to a cooling temperature lower than or equal to 500°C at a cooling rate higher than 30°C / second; and coiling the hot rolled plate and maintaining the temperature of the coiled plate lower than 570°C; - cooling the hot rolled sheet; - subjecting the hot rolled steel sheet to annealing at a temperature of 350° C. to 500° C. for a period of 1 hour to 96 hours; - performing at least one descaling process on the hot rolled steel sheet before or after annealing of the hot rolled steel sheet; - cold rolling the hot rolled steel sheet at a reduction ratio of 35% to 90% to obtain a cold rolled steel sheet; - then annealing the cold rolled steel sheet continuously for at least 100 seconds at a rate of 1°C / s to 20°C / s to a soaking temperature of Ac1 to Ac3+50°C, the temperature and time being selected to obtain a minimum percentage of 70% austenite; - the plate is then cooled at a rate greater than 10°C / second to a temperature of Ms-20°C to Ms+40°C, where Ms is the Ms temperature of the initial austenite before cooling, and then - Maintaining the cold rolled steel sheet at 350°C to 450°C for 200 seconds to 1000 seconds; and then - The plate is cooled to room temperature at a cooling rate of no more than 200°C / second.
12. The method according to claim 10 or 11, wherein the cooling temperature of the hot-rolled steel sheet is set to 150°C to 500°C.
13. The method according to any one of claims 10 to 12, wherein the cold rolled steel sheet is continuously annealed at 800°C to 900°C for 100 seconds to 1000 seconds.
14. The method according to any one of claims 10 to 13, wherein the cold rolled steel sheet is further coated with zinc or a zinc based alloy.
15. Use of the steel sheet according to any one of claims 1 to 9 or the steel sheet produced according to the method according to claims 10 to 14 for manufacturing structural parts or safety parts of a vehicle.
16. A vehicle comprising a component obtained according to claim 15.