Ozone dispersion strengthened (ODS) steel with orderly distributed oxide nanoparticles and preparation method thereof

By introducing Y2O3 nanoparticles into ODS steel and using mechanical ball milling and thermal isostatic pressing processes, the orderly distribution of oxide nanoparticles is achieved, which solves the problem of insufficient creep resistance and radiation resistance of ODS steel at high temperatures, significantly improves the The mechanical properties of the material.

CN119082619APending Publication Date: 2024-12-06ZHONGBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411214608.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-01
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The random distribution of oxide nanoparticles in existing ODS steels leads to insufficient high-temperature creep resistance and radiation resistance. The existing process of orderly distribution of carbides in low-carbon microalloy high-strength steels is not suitable for ODS steels.

Method used

By introducing Y2O3 nanoparticles into raw materials such as Cr, Mn, Fe, etc., and using mechanical ball milling and thermal isostatic pressing processes, the distribution of oxide nanoparticles is controlled to achieve their orderly distribution in ODS steel.

Benefits of technology

It improves the high-temperature creep strength and radiation resistance of ODS steel, with low cost and simple process, and is of great technical significance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082619A_ABST
    Figure CN119082619A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oxide dispersion strengthened steel preparation, in particular to oxide nano-particle ordered distribution ODS steel and a preparation method thereof.The preparation method comprises the following steps that pre-alloyed powder is prepared with Cr, Mn and Fe as main raw materials, the pre-alloyed powder and Y2O3 nano-particles are subjected to mechanical ball milling in a ball mill, and the pre-alloyed powder is obtained; the method comprises the following steps: ball-milling mixed powder to obtain ball-milled mixed powder, filling the ball-milled mixed powder into a stainless steel sheath, degassing the mixed powder in the stainless steel sheath, sealing and welding the stainless steel sheath, putting the stainless steel sheath into hot isostatic pressing equipment for curing and forming, and cooling to room temperature along with a furnace to obtain the ODS steel with orderly distributed oxide nanoparticles. The problems that the ODS steel prepared through an existing heat treatment technology is single in microstructure characteristic, and ordered distribution of oxide nanoparticles cannot be achieved are solved, and a new technical route is provided for research and development of the ODS steel with high performance and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oxide dispersion strengthened steel preparation, in particular to an ODS steel with orderly distributed oxide nanoparticles and a preparation method thereof. Background Art

[0002] In order to meet the growing global demand for sustainable energy, reduce dependence on fossil fuels while maintaining economic benefits and energy system reliability, countries around the world have begun to pay attention to advanced fission energy systems. The demand for new clean energy has also accelerated the research on fusion energy. Low-activated martensitic steel has become the main candidate structural material for fast neutron reactors and fusion reactors because of its low radiation swelling and thermal expansion coefficient, high thermal conductivity and good resistance to liquid metal corrosion. However, this type of material still has problems such as insufficient high-temperature strength, low service temperature, and helium embrittlement.

[0003] In order to solve these problems, highly thermally stable oxide nanoparticles dispersed in the martensite or ferrite matrix are introduced to effectively pin dislocations and grain boundaries, thereby greatly improving the material's high-temperature creep strength and radiation resistance. This material is called high-performance oxide dispersion strengthened (ODS) steel, especially when applied to a martensite or ferrite matrix, it is called ODS martensitic steel or ODS ferritic steel, which is of great significance for the safe and efficient use of nuclear energy in the future.

[0004] The oxide nanoparticles in ODS steel prepared by existing heat treatment processes are usually randomly distributed in the matrix of ODS steel. Although the orderly distribution of carbides has been achieved in low-carbon microalloyed high-strength steel, the composition design principle and preparation process for achieving orderly distribution of carbides in low-carbon microalloyed high-strength steel are not applicable to ODS steel due to the differences in thermal stability and solid solubility between carbides and oxides in steel.

[0005] In view of this, the present invention aims to solve the problems existing in the prior art, and proposes an ODS steel capable of achieving orderly distribution of oxide nanoparticles and a preparation method thereof, so as to improve the mechanical properties of the ODS steel and provide new technical means. Summary of the invention

[0006] In order to solve the problem that the microstructure characteristics of ODS steel prepared by the existing heat treatment process are single and the oxide nanoparticles cannot be orderly distributed, the present invention provides an ODS steel with orderly distributed oxide nanoparticles and a preparation method thereof.

[0007] The present invention is achieved by adopting the following technical solutions:

[0008] A method for preparing ODS steel with orderly distributed oxide nanoparticles comprises the following steps:

[0009] S1: Pre-alloyed powder is prepared with Cr, Mn and Fe as main raw materials, and the mass percentage of the main raw materials of the pre-alloyed powder is 8% to 10% of Cr, 2% to 3% of Mn, and the balance is Fe. The pre-alloyed powder and Y2O3 nanoparticles are mechanically ball-milled in a ball mill, and argon gas is used for protection to obtain a mixed powder after ball milling, wherein the mass percentage of Y2O3 nanoparticles in the mixed powder after ball milling is 0.35% to 0.5%;

[0010] S2: The ball-milled mixed powder is placed in a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;

[0011] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 5℃~10℃ / min, the molding temperature is 1150℃, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, ODS steel with orderly distribution of oxide nanoparticles is obtained.

[0012] Furthermore, the raw material of the pre-alloyed powder also includes Ti, and the mass percentage of Ti is 0.05% to 0.2%.

[0013] Furthermore, the ball-to-material ratio in the ball mill is 10:1.

[0014] Furthermore, the ball milling speed in the ball mill is 250 r / min.

[0015] Furthermore, the ball milling time in the ball mill is 30 h.

[0016] An ODS steel with orderly distributed oxide nanoparticles is obtained based on the above-mentioned preparation method of the ODS steel with orderly distributed oxide nanoparticles.

[0017] The key to the present invention lies in the raw material composition design of the pre-alloyed powder and the process parameters of hot isostatic pressing. The main raw materials and mass percentages of the pre-alloyed powder are Cr: 8% to 10%, Mn: 2% to 3%, and the balance is Fe, which determines that the mixed powder after ball milling and degassing will undergo austenite phase transformation through the high-temperature heating process during the hot isostatic pressing process, and ferrite phase transformation and martensite phase transformation through the cooling process; different from the previous ODS steel alloy composition, the Mn content is increased to 2% to 3% in the present invention, which has an important impact on the movement rate of the phase interface during the phase transformation process. The raw material composition design of the pre-alloyed powder determines whether the austenite phase transformation can occur during the hot isostatic pressing process and how fast the austenite phase transformation occurs, and the heating rate during the hot isostatic pressing process determines the length of the residence time in the austenite-ferrite two-phase region during the heating process, which affects the speed of the austenite phase transformation. The slower the austenite phase transformation, the lower the migration rate of the austenite / ferrite interface, which is more conducive to the dissolution of oxide nanoparticles at the interface front. The dissolved yttrium atoms and oxygen atoms are segregated on the moving interface. When the dissolved yttrium atoms and oxygen atoms reach saturation, they re-precipitate in the form of oxide nanoparticles, forming an ordered distribution of oxide nanoparticles.

[0018] The present invention can obtain ODS steel with orderly distribution of oxide nanoparticles by performing certain raw material composition design and preparation process adjustment on ODS steel in the early stage. The invention has low cost, simple process and strong purpose. It provides a new technical means for regulating the distribution state of oxide nanoparticles in ODS steel, which is of great significance for further improving the high temperature strength and radiation resistance of ODS steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a scanning electron microscopy (SEM) photograph of orderly distribution of oxide nanoparticles in the ODS steel obtained in Example 1 of the present invention.

[0020] Figure 2 It is a tensile property curve diagram of the ODS steel obtained in Example 1 of the present invention at room temperature and 650°C.

[0021] Figure 3 This is a scanning electron microscopy (SEM) photograph of orderly distribution of oxide nanoparticles in the ODS steel obtained in Example 2 of the present invention.

[0022] Figure 4 It is a tensile property curve diagram of the ODS steel obtained in Example 2 of the present invention at room temperature and 650°C. DETAILED DESCRIPTION

[0023] A method for preparing ODS steel with orderly distributed oxide nanoparticles comprises the following steps:

[0024] S1: Pre-alloyed powder is prepared with Cr, Mn and Fe as main raw materials, and the mass percentage of the main raw materials of the pre-alloyed powder is 8% to 10% of Cr, 2% to 3% of Mn, and the balance is Fe. The pre-alloyed powder and Y2O3 nanoparticles are mechanically ball-milled in a ball mill with a ball-to-material ratio of 10:1, a ball milling speed of 250 r / min, a ball milling time of 30 h, and argon protection is used to obtain a mixed powder after ball milling, wherein the mass percentage of Y2O3 nanoparticles in the mixed powder after ball milling is 0.35% to 0.5%, and the particle size range of the Y2O3 nanoparticles is 30nm to 50nm;

[0025] S2: The ball-milled mixed powder is placed in a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;

[0026] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 5℃~10℃ / min, the molding temperature is 1150℃, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, ODS steel with orderly distribution of oxide nanoparticles is obtained.

[0027] The following are specific embodiments of the present invention, but the present invention is not limited to the following embodiments.

[0028] Example 1

[0029] S1: Pre-alloyed powder is prepared with Cr, Mn and Fe as main raw materials, and the mass percentage of the main raw materials of the pre-alloyed powder is 8.7% Cr, 2.2% Mn, and the balance is Fe. The pre-alloyed powder and Y2O3 nanoparticles are mechanically ball-milled in a QM-3SP4 planetary ball mill, with a ball-to-material ratio of 10:1, a ball milling speed of 250 r / min, a ball milling time of 30 h, and argon protection to obtain a ball-milled mixed powder, wherein the mass percentage of Y2O3 nanoparticles in the ball-milled mixed powder is 0.35%, and the particle size range of the Y2O3 nanoparticles is 30 nm to 50 nm;

[0030] S2: The ball-milled mixed powder is placed in a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;

[0031] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 8°C / min, the molding temperature is 1150°C, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, ODS steel with orderly distribution of oxide nanoparticles is obtained.

[0032] Figure 1 : is a scanning electron microscopy (SEM) photograph of the orderly distribution of oxide nanoparticles in the ODS steel obtained in this example. It can be seen from the figure that the oxide nanoparticles are orderly distributed in stripes on the ferrite matrix. Figure 2 The tensile properties of the ODS steel obtained in this embodiment at room temperature and 650°C are shown in FIG. At room temperature, its tensile strength is 867MPa and its elongation is 17.3%; at 650°C, its tensile strength is 204MPa and its elongation is 7.2%. Different from the traditional ODS steel alloy composition, the ODS steel obtained in this embodiment does not contain W element, but it still exhibits good mechanical properties at room temperature and 650°C, which illustrates the beneficial effect of the ordering of oxide nanoparticles on the mechanical properties of ODS steel.

[0033] Example 2

[0034] S1: Pre-alloyed powder is prepared with Cr, Mn, Fe and Ti as raw materials, and the mass percentages of the raw materials of the pre-alloyed powder are 8.7% Cr, 2.2% Mn, 0.1% Ti, and the balance is Fe. The pre-alloyed powder and Y2O3 nanoparticles are mechanically ball-milled in a QM-3SP4 planetary ball mill, with a ball-to-material ratio of 10:1, a ball milling speed of 250 r / min, a ball milling time of 30 h, and argon protection is used to obtain a ball-milled mixed powder, wherein the mass percentage of Y2O3 nanoparticles in the ball-milled mixed powder is 0.35%, and the particle size range of the Y2O3 nanoparticles is 30 nm to 50 nm;

[0035] S2: The ball-milled mixed powder is placed in a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;

[0036] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 8°C / min, the molding temperature is 1150°C, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, ODS steel with orderly distribution of oxide nanoparticles is obtained.

[0037] Comparative Example 1, Figure 3This is a scanning electron microscopy (SEM) photograph of the orderly distribution of oxide nanoparticles in the ODS steel obtained in this example. It can be seen from the figure that after adding a certain amount of Ti, the orderly distribution of oxide nanoparticles can still be obtained on the ferrite matrix. Figure 4 This is a tensile property curve of the ODS steel obtained in this embodiment at room temperature and 650°C. At room temperature, its tensile strength is 670MPa and its elongation is 29%; at 650°C, its tensile strength is 191MPa and its elongation is 7.9%. Due to the addition of Ti, the room temperature plasticity of the ODS steel obtained in this embodiment is significantly improved, which is convenient for cold processing.

[0038] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing ODS steel with orderly distributed oxide nanoparticles, Features: The following steps are involved: S1: Prepare pre-alloyed powder with Cr, Mn and Fe as main raw materials, and the mass percentage of the main raw materials of the pre-alloyed powder is Cr: 8% to 10%, Mn: 2% to 3%, and the balance is Fe. 2 O 3 The nanoparticles were mechanically milled in a ball mill under argon protection to obtain a mixed powder after ball milling, wherein Y 2 O 3 The mass percentage of the nanoparticles in the mixed powder after ball milling is 0.35% to 0.5%; S2: The ball-milled mixed powder is placed in a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa; S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 5℃~10℃ / min, the molding temperature is 1150℃, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, ODS steel with orderly distribution of oxide nanoparticles is obtained.

2. The method for preparing ODS steel with orderly distributed oxide nanoparticles according to claim 1, Features: In step S1: the raw material of the pre-alloyed powder also includes Ti, and the mass percentage of Ti is 0.05% to 0.2%.

3. The method for preparing ODS steel with orderly distributed oxide nanoparticles according to claim 1, Features: In step S1: the ball-to-material ratio in the ball mill is 10:

1.

4. The method for preparing ODS steel with orderly distributed oxide nanoparticles according to claim 1, Features: In step S1: the ball milling speed is 250 r / min.

5. The method for preparing ODS steel with orderly distributed oxide nanoparticles according to claim 1, Features: In step S1: the ball milling time in the ball mill is 30 hours.

6. An ODS steel with orderly distributed oxide nanoparticles, the ODS steel being obtained based on the preparation method of an ODS steel with orderly distributed oxide nanoparticles according to any one of claims 1 to 5.