Composition, preparation method and application of composition in white cardboard

By using compositions of needle pulp, chemical pulp, mechanical pulp and damaged paper reuse pulp in white cardboard, combined with specific slurry concentration and additives, the printing and flowering problem is solved, and high printing suitability and Effective utilization of resources.

CN119083227APending Publication Date: 2024-12-06GUANGXI SUN PAPER BOARD CO LTD +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411297093.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing white cardboard has uneven printing color blocks and imperfect hair due to the rough paper surface. It is called printing hair, which affects the visual effect and causes waste of resources.

Method used

A composition is adopted, including a surface slurry, a core slurry and a base slurry, which consists of needle slurry, chemical slurry, mechanical slurry and paper-destroying recycle slurry, and is subjected to a specific slurry concentration and additives. Addition and preparation process to control the optical roughness of the paper and avoid printing and floral.

Benefits of technology

It significantly reduces the optical roughness of the paper, improves printing suitability, avoids uneven printing color blocks and flaws, and reduces the waste of white paper and printing dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083227A_ABST
    Figure CN119083227A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of papermaking, and particularly relates to a composition, a preparation method and application of the composition in white cardboard. The composition comprises surface layer pulp, core layer pulp and bottom layer pulp, the surface layer pulp is composed of softwood pulp and chemical pulp, the core layer pulp is composed of mechanical pulp and broken paper recycling pulp, and the bottom layer pulp is composed of softwood pulp and chemical pulp. The invention also provides a preparation method of the composition, and also provides application of the composition or a product obtained by the preparation method in white cardboard. According to the technical scheme provided by the invention, the pulping degree of the pulp is controlled, the dehydration amount of each step and the moisture of the product are controlled in combination with the preparation process, and the addition amount of the auxiliary agent is matched, so that the optical roughness of the prepared product is remarkably reduced, and the product has high printability and does not have the problem of printing floating when being applied to the white cardboard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of papermaking, and in particular relates to a composition, a preparation method and an application thereof in white cardboard. Background Art

[0002] With the development of social economy and the improvement of people's living standards, the use of paper is becoming more and more extensive. Among them, white cardboard, as a high-end packaging material, is mainly used for the outer packaging of small high-end commodities and high value-added products such as daily necessities, cosmetics, food, medicines, cigarettes, electronic communication products, etc., and in the non-packaging field, it is also commonly used as greeting card covers, business cards, certificates, invitations, desk calendars and postal postcards.

[0003] The white card paper in the prior art has a rough surface, which will cause uneven and blurred printing color blocks, poor visual effects, and is called printing blooming. It cannot be processed later and becomes waste, resulting in a great waste of white card paper and printing dyes.

[0004] Therefore, a composition, a preparation method and its application in white cardboard are developed to solve the technical defect of printing blur in the prior art of white cardboard printing, which has become an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0005] Based on this, it is necessary to provide a composition, a preparation method and its application in white cardboard in view of the technical defect of printing flowery white cardboard in the existing technology.

[0006] The present application provides a composition, wherein the raw materials of the composition include: a surface layer pulp, a core layer pulp and a bottom layer pulp, wherein the surface layer pulp is composed of coniferous pulp and chemical pulp, the core layer pulp is composed of mechanical pulp and broken paper recycling pulp, and the bottom layer pulp is composed of coniferous pulp and chemical pulp;

[0007] Among them, the refining concentration of the chemical pulp is 4.0%-5.0%, and the freeness of the chemical pulp is 380-400CSF; the refining concentration of the coniferous pulp is 4.0%-5.0%, and the freeness of the coniferous pulp is 400-420CSF; the refining concentration of the mechanical pulp is 3.5%-4.5%, and the freeness of the mechanical pulp is 380-400CSF; the refining concentration of the broken paper recycled pulp is 3.0%-4.0%, and the freeness of the broken paper recycled pulp is 280-300CSF.

[0008] In one embodiment, based on 100% of the surface layer pulp, the surface layer pulp includes 60% to 70% of coniferous pulp, and the remaining component is chemical pulp.

[0009] In one of the embodiments, based on 100% of the core layer pulp, the core layer pulp includes 70% to 80% of mechanical pulp, and the remaining component is broken paper recycled pulp.

[0010] In one embodiment, based on 100% of the bottom slurry, the bottom slurry includes 60% to 70% of coniferous pulp, and the remaining component is chemical pulp.

[0011] In one embodiment, the raw materials of the composition include, by weight: 20 to 23 parts of surface layer slurry, 60 to 65 parts of core layer slurry and 12 to 20 parts of bottom layer slurry.

[0012] In one embodiment, the raw materials of the composition further include: an auxiliary agent, and the auxiliary agent is selected from: any one or more of a dry strength agent, a cationic starch, a brightener, a retention and drainage aid, a bactericide and a defoaming agent.

[0013] In one embodiment, the dry strength agent is added in an amount of 10-20 kg / t of the composition, and the dry strength agent is selected from any one or more of cationic polyacrylamide, anionic polyacrylamide and polyacrylamide.

[0014] In one embodiment, the feeding amount of the cationic starch is 5-10 kg / t composition, and the cationic starch is selected from any one or more of corn starch, cassava starch and potato starch.

[0015] In one embodiment, the dosage of the whitening agent is 2-10 kg / t composition, and the whitening agent is selected from any one or more of a fluorescent whitening agent, an inorganic whitening agent and a chemical whitening agent.

[0016] In one embodiment, the dosage of the retention and drainage aid is 0.8-1.2 kg / t composition, and the retention and drainage aid is selected from any one or more of cationic polyacrylamide, anionic polyacrylamide and particulate additives.

[0017] In one embodiment, the dosage of the fungicide is 0.4-0.7 kg / t composition, and the fungicide is selected from any one or more of ether fungicides, alcohol fungicides and ketone fungicides.

[0018] In one embodiment, the dosage of the defoamer is 0.3-0.5 kg / t composition, and the defoamer is selected from any one or more of silicone oil defoamers, polyether defoamers and mineral defoamers.

[0019] The present application also provides a method for preparing the composition comprising any one of the above, the preparation method comprising:

[0020] Step 1, slurry mixing: after the surface layer slurry, the core layer slurry and the bottom layer slurry are mixed, they are diluted to obtain the first product;

[0021] Step 2, adding an auxiliary agent: mixing the first product with an auxiliary agent to obtain a second product;

[0022] Step 3, net forming: the second product is formed by dehydration in the net, and stacked into wet paper sheets to obtain the third product;

[0023] Step 4, dehydration: the wet paper sheets of the third product are dehydrated by shoe pressing to obtain a fourth product;

[0024] Step 5, primary evaporation: evaporating water from the fourth product to obtain a fifth product;

[0025] Step 6, sizing: using a surface sizing agent to apply sizing to the front and back surfaces of the fifth product to obtain a sixth product;

[0026] Step 7, secondary evaporation: evaporating water from the sixth product to obtain the seventh product;

[0027] Step eight, post-processing: the seventh product is subjected to hard calendering, coating and soft calendering to obtain a product.

[0028] In one embodiment, in step one, in the first product after dilution treatment, the concentration of the surface layer slurry is 0.2% to 0.5%, the concentration of the core layer slurry is 0.9% to 1.8%, and the concentration of the bottom layer slurry is 0.2% to 0.5%.

[0029] In one embodiment, in step three, the paper dryness of the third product is less than or equal to 20%.

[0030] In one embodiment, in step 4, the paper dryness of the fourth product is greater than or equal to 45%.

[0031] In one embodiment, in step five, the dryness of the fifth product is 86% to 92%.

[0032] In one of the embodiments, in step six, the solid content of the surface sizing agent is 10% to 20%, and the viscosity of the surface sizing agent is 10 to 15 CPS.

[0033] In one embodiment, in step seven, the paper dryness of the seventh product is 90% to 94%.

[0034] The present application also provides an application of the composition described in any one of the above or the product obtained by the preparation method described in any one of the above in white cardboard.

[0035] In summary, the present application provides a composition, including: a surface layer pulp, a core layer pulp and a bottom layer pulp, wherein the surface layer pulp is composed of coniferous pulp and chemical pulp, the core layer pulp is composed of mechanical pulp and damaged paper recycling pulp, and the bottom layer pulp is composed of coniferous pulp and chemical pulp. The present application also provides a method for preparing the above composition, and the present application also provides an application of the above composition or the product obtained by the above preparation method in white cardboard. In the technical scheme provided by the present application, by controlling the pulp beating degree of the pulp, and controlling the dehydration amount of each step and the product moisture content in combination with the preparation process, and combining with the amount of additives added, the optical roughness of the obtained product is significantly reduced, and when applied to white cardboard, it has high printability and will not have the problem of printing flowery. The product composition, preparation method and application in white cardboard provided by the present application solve the technical defect of printing flowery in the prior art of white cardboard printing. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0037] Figure 1 A schematic flow chart of a method for preparing a composition in the technical solution provided in an embodiment of the present application. DETAILED DESCRIPTION

[0038] The embodiments of the present application provide a composition, a preparation method and application thereof in white cardboard, which are used to solve the technical defect of printing blur in the prior art of white cardboard printing.

[0039] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0040] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0042] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0043] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0044] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0045] See also Figure 1 , Figure 1 The following example is a schematic diagram of the process for preparing the composition. Figure 1 , carry out specific preparation of the composite product.

[0046] Example

[0047] Step 1: Slurry mixing

[0048] The surface layer pulp, the core layer pulp and the bottom layer pulp are mixed and diluted to obtain the first product; in this embodiment, the surface layer pulp is composed of coniferous pulp and chemical pulp, the core layer pulp is composed of mechanical pulp and broken paper recycled pulp, and the bottom layer pulp is composed of coniferous pulp and chemical pulp, wherein the feeding amount of the surface layer pulp is 20 to 23 tons, the feeding amount of the core layer pulp is 60 to 65 tons, and the feeding amount of the bottom layer pulp is 12 to 20 tons. Among them, the refining concentration of chemical pulp is 4.0%~5.0%, and the freeness of chemical pulp is 380~400CSF; the refining concentration of coniferous pulp is 4.0%~5.0%, and the freeness of coniferous pulp is 400~420CSF; the refining concentration of mechanical pulp is 3.5%~4.5%, and the freeness of mechanical pulp is 380~400CSF; the refining concentration of broken paper recycled pulp is 3.0%~4.0%, and the freeness of broken paper recycled pulp is 280~300CSF.

[0049] In this embodiment, taking the surface layer pulp as 100%, the surface layer pulp includes 60% to 70% coniferous pulp, and the remaining component is chemical pulp; taking the core layer pulp as 100%, the core layer pulp includes 70% to 80% mechanical pulp, and the remaining component is damaged paper recycled pulp; taking the bottom layer pulp as 100%, the bottom layer pulp includes 60% to 70% coniferous pulp, and the remaining component is chemical pulp.

[0050] In this embodiment, in the first product obtained after dilution treatment, the concentration of the surface layer slurry is 0.2% to 0.5%, the concentration of the core layer slurry is 0.9% to 1.8%, and the concentration of the bottom layer slurry is 0.2% to 0.5%.

[0051] Step 2: Adding additives

[0052] The first product is mixed with an auxiliary agent to obtain a second product; in this embodiment, the auxiliary agent is selected from: any one or more of dry strength agent, cationic starch, brightener, retention and drainage aid, bactericide and defoamer. Among them, the feeding amount of dry strength agent is 10-20 kg / t composition, and the dry strength agent is selected from: any one or more of cationic polyacrylamide, anionic polyacrylamide and polyacrylamide; the feeding amount of cationic starch is 5-10 kg / t composition, and cationic starch is selected from: any one or more of corn starch, cassava starch and potato starch; the feeding amount of brightener is 2-10 kg / t composition, and the brightener is selected from: any one or more of fluorescent brightener, inorganic brightener and chemical brightener; retention and drainage aid The feeding amount is 0.8-1.2 kg / t composition, the retention and drainage aids are selected from: any one or more of cationic polyacrylamide, anionic polyacrylamide and particulate additives; the feeding amount of the bactericide is 0.4-0.7 kg / t composition, the bactericide is selected from: any one or more of ether bactericides, alcohol bactericides and ketone bactericides; the feeding amount of the defoamer is 0.3-0.5 kg / t composition, and the defoamer is selected from: any one or more of silicone oil defoamers, polyether defoamers and mineral defoamers.

[0053] Step 3: Net forming

[0054] The second product is dehydrated and formed by the wire part, and then laminated into wet paper sheets to obtain the third product; wherein the paper sheet dryness of the third product is less than or equal to 20%.

[0055] Step 4: Dehydration

[0056] The wet paper sheets of the third product are dehydrated by shoe pressing to obtain a fourth product; wherein the paper sheet dryness of the fourth product is greater than or equal to 45%.

[0057] Step 5: Primary Evaporation

[0058] The water of the fourth product is evaporated to obtain the fifth product; wherein the dryness of the fifth product is 86% to 92%.

[0059] Step 6: Gluing

[0060] The surface sizing agent is used to apply surface sizing to the front and back sides of the fifth product to obtain the sixth product, wherein the solid content of the surface sizing agent is 10% to 20%, and the viscosity of the surface sizing agent is 10 to 15 CPS. The sizing step can significantly improve the water absorption resistance of the sixth product.

[0061] Step 7: Secondary evaporation

[0062] The water of the sixth product is evaporated to obtain the seventh product; wherein the paper sheet dryness of the seventh product is 90% to 94%.

[0063] Step 8: Post-processing

[0064] The seventh product is obtained by hard calendering, coating and soft calendering; among them, hard calendering treatment can improve the product's tightness, smoothness, strength and other performance; coating treatment can further improve the product's appearance performance and printing performance. When coating, the product quality and product cost are taken into consideration comprehensively. The front side is coated 3 times and the back side is coated 1 time; soft calendering treatment can further make the product surface flatter and smoother.

[0065] The product prepared in this example is prepared to obtain a quantitative of 200-400 g / m 2 The paper is tested for various properties of the paper, including the following testing methods: whiteness: national standard GB / T7974; interlayer bonding: GB / T26203; printing surface strength: GB / T22365; water absorption value: GB / T1540; smoothness: GB / T456; optical roughness: GB / T22363.

[0066] The measured whiteness is 89±1% ISO, and the interlayer bonding degree is ≥120J / m 2 , printing surface strength ≥1.20m / s, front water absorption value ≤45g / m 2 , water absorption value on the reverse side ≤60g / ㎡, smoothness ≥400s.

[0067] Among them, it should be pointed out that the optical roughness is less than 0.7μm. Compared with the optical roughness of white cardboard less than or equal to 1.5μm in the prior art, the product obtained by the technical solution provided by the present invention has significantly reduced optical roughness, which is conducive to the uniform absorption of ink during the printing process, and there will be no uneven or weak printing blocks. The problem of printing blur during the printing process of white cardboard is effectively avoided, and the waste of white cardboard and printing dyes is avoided. It has high printability and will not cause the problem of printing blur.

[0068] In summary, the present application provides a composition, including: a surface layer pulp, a core layer pulp and a bottom layer pulp, wherein the surface layer pulp is composed of coniferous pulp and chemical pulp, the core layer pulp is composed of mechanical pulp and damaged paper recycling pulp, and the bottom layer pulp is composed of coniferous pulp and chemical pulp. The present application also provides a method for preparing the above composition, and the present application also provides an application of the above composition or the product obtained by the above preparation method in white cardboard. In the technical scheme provided by the present application, by controlling the pulp beating degree of the pulp, and controlling the dehydration amount of each step and the product moisture content in combination with the preparation process, and combining with the amount of additives added, the optical roughness of the obtained product is significantly reduced, and when applied to white cardboard, it has high printability and will not have the problem of printing flowery. The product composition, preparation method and application in white cardboard provided by the present application solve the technical defect of printing flowery in the prior art of white cardboard printing.

[0069] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. At the same time, other implementation methods can be derived from the above-mentioned embodiments, so that structural and logical replacements and changes can be made without departing from the scope of this disclosure.

[0070] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A composition, characterized in that The raw materials of the composition include: surface layer pulp, core layer pulp and bottom layer pulp, wherein the surface layer pulp is composed of coniferous pulp and chemical pulp, the core layer pulp is composed of mechanical pulp and broken paper recycling pulp, and the bottom layer pulp is composed of coniferous pulp and chemical pulp; Among them, the refining concentration of the chemical pulp is 4.0%-5.0%, and the freeness of the chemical pulp is 380-400CSF; the refining concentration of the coniferous pulp is 4.0%-5.0%, and the freeness of the coniferous pulp is 400-420CSF; the refining concentration of the mechanical pulp is 3.5%-4.5%, and the freeness of the mechanical pulp is 380-400CSF; the refining concentration of the broken paper recycled pulp is 3.0%-4.0%, and the freeness of the broken paper recycled pulp is 280-300CSF.

2. The composition according to claim 1, characterized in that Taking the surface layer pulp as 100%, the surface layer pulp includes 60% to 70% of conifer pulp, and the remaining component is chemical pulp.

3. The composition according to claim 1, characterized in that Taking the core layer pulp as 100%, the core layer pulp includes 70% to 80% mechanical pulp, and the remaining component is broken paper recycled pulp.

4. The composition according to claim 1, characterized in that Taking the bottom layer pulp as 100%, the bottom layer pulp includes 60% to 70% of conifer pulp, and the remaining component is chemical pulp.

5. The composition according to any one of claims 1 to 4, characterized in that The raw materials of the composition include, by weight, 20 to 23 parts of surface layer slurry, 60 to 65 parts of core layer slurry and 12 to 20 parts of bottom layer slurry.

6. The composition according to any one of claims 1 to 5, characterized in that The raw materials of the composition also include: an auxiliary agent, and the auxiliary agent is selected from: any one or more of a dry strength agent, a cationic starch, a brightener, a retention and drainage aid, a bactericide and a defoaming agent.

7. The composition according to claim 6, characterized in that The dry strength agent is added in an amount of 10-20 kg / t of the composition, and the dry strength agent is selected from any one or more of cationic polyacrylamide, anionic polyacrylamide and polyacrylamide.

8. The composition according to claim 6, characterized in that The feeding amount of the cationic starch is 5-10 kg / t composition, and the cationic starch is selected from any one or more of corn starch, cassava starch and potato starch.

9. The composition according to claim 6, characterized in that The feeding amount of the whitening agent is 2-10 kg / t composition, and the whitening agent is selected from any one or more of fluorescent whitening agents, inorganic whitening agents and chemical whitening agents.

10. The composition according to claim 6, characterized in that The dosage of the retention and drainage aid is 0.8-1.2 kg / t composition, and the retention and drainage aid is selected from any one or more of cationic polyacrylamide, anionic polyacrylamide and particulate aid.

11. The composition according to claim 6, characterized in that The feeding amount of the bactericide is 0.4-0.7 kg / t composition, and the bactericide is selected from: any one or more of ether bactericides, alcohol bactericides and ketone bactericides.

12. The composition according to claim 6, characterized in that The feeding amount of the defoamer is 0.3-0.5 kg / t composition, and the defoamer is selected from any one or more of silicone oil defoamers, polyether defoamers and mineral defoamers.

13. A method for preparing the composition according to any one of claims 1 to 12, characterized in that: The preparation method is: Step 1, slurry mixing: after the surface layer slurry, the core layer slurry and the bottom layer slurry are mixed, they are diluted to obtain the first product; Step 2, adding an auxiliary agent: mixing the first product with an auxiliary agent to obtain a second product; Step 3, net forming: the second product is formed by dehydration in the net, and stacked into wet paper sheets to obtain the third product; Step 4, dehydration: the wet paper sheets of the third product are dehydrated by shoe pressing to obtain a fourth product; Step 5, primary evaporation: evaporating water from the fourth product to obtain a fifth product; Step 6, sizing: using a surface sizing agent to apply sizing to the front and back surfaces of the fifth product to obtain a sixth product; Step 7, secondary evaporation: evaporating water from the sixth product to obtain the seventh product; Step eight, post-processing: the seventh product is subjected to hard calendering, coating and soft calendering to obtain a product.

14. The preparation method according to claim 13, characterized in that: In step 1, in the first product after dilution treatment, the concentration of the surface layer slurry is 0.2% to 0.5%, the concentration of the core layer slurry is 0.9% to 1.8%, and the concentration of the bottom layer slurry is 0.2% to 0.5%.

15. The preparation method according to claim 13, characterized in that: In step three, the paper dryness of the third product is less than or equal to 20%.

16. The preparation method according to claim 13, characterized in that: In step 4, the paper dryness of the fourth product is greater than or equal to 45%.

17. The preparation method according to claim 13, characterized in that: In step five, the fifth product has a dryness of 86% to 92%.

18. The preparation method according to claim 13, characterized in that: In step six, the solid content of the surface sizing agent is 10% to 20%, and the viscosity of the surface sizing agent is 10 to 15 CPS.

19. The preparation method according to claim 13, characterized in that: In step seven, the paper dryness of the seventh product is 90% to 94%.

20. Use of the composition according to any one of claims 1 to 12 or the product obtained by the preparation method according to any one of claims 13 to 19 in white cardboard.

Citation Information

Patent Citations

  • White cardboard with smooth paper surface and production process thereof

    CN118326746A