Scale, encoder, and scale manufacturing method

By roughening the upper surface of the glass substrate and forming a conductor film on the lower surface, combined with laser processing technology, the problem of damage and noise interference during the processing process is solved, and higher processing reproducibility and electromagnetic shielding effect are achieved.

CN119085718APending Publication Date: 2024-12-06MITUTOYO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410678286.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-05
Filing Date
2024-05-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing scales are prone to damage during laser processing, resulting in defects in the conductor film and components, and it is difficult to suppress noise interference.

Method used

By roughening the upper surface of the glass substrate to form a frosted glass state, and forming a conductor film and element on the lower surface, a conductor pattern is formed on the upper surface by laser processing to avoid laser damage and suppress noise interference.

Benefits of technology

It effectively prevents damage to the conductor film and components during laser processing, improves the processing reproducibility of the conductor pattern and the electromagnetic shielding effect, and reduces noise interference.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119085718A_ABST
    Figure CN119085718A_ABST
Patent Text Reader

Abstract

The invention discloses a scale, an encoder and a scale manufacturing method. The scale includes a glass substrate having a ground glass-like upper surface, a plurality of conductor patterns arranged on the upper surface of the glass substrate at predetermined intervals, and a structure disposed on a lower surface of the glass substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Certain aspects of the embodiments described herein relate to a scale, an encoder, and a method of manufacturing the scale. Background Art

[0002] As a ruler used in an encoder, etc., a ruler is known in which a resin layer is provided on a glass substrate, and repeatedly has a mirror surface concave portion and a rough surface convex portion, and a silicon oxide layer, an aluminum layer and a silicon oxide layer are sequentially provided on the convex portion (see, for example, Japanese Patent Publication No. 6-201906). In addition, the glass surface is treated by dissolving ammonium sulfate, ammonium chloride and ammonium nitrate in hydrofluoric acid alone or in combination, and treating the glass surface with a solution to which sulfuric acid, hydrochloric acid and nitric acid are added alone or in combination as needed. In this case, it is known that fine irregularities are formed on the surface (see, for example, Japanese Patent Application Publication No. 7-237934). Summary of the invention

[0003] In one aspect, an object of the present invention is to make structures such as films and elements provided on the lower surface of a glass substrate difficult to be damaged.

[0004] According to one aspect of the present invention, there is provided a scale comprising: a glass substrate having a frosted glass-like upper surface; a plurality of conductor patterns arranged at predetermined intervals on the upper surface of the glass substrate; and a structure disposed on the lower surface of the glass substrate.

[0005] According to another aspect of the present invention, there is provided an encoder, comprising: the scale as described above.

[0006] According to another aspect of the present invention, a method for manufacturing a ruler is provided, comprising: roughening the upper surface of a glass substrate into a frosted glass state; forming a structure on the lower surface of the glass substrate; and after roughening the upper surface of the glass substrate into the frosted glass state and forming the structure, forming a plurality of conductor patterns arranged at predetermined intervals on the upper surface of the glass substrate by laser processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1A is a diagram showing a configuration of an electromagnetic induction encoder including a scale according to a first embodiment;

[0008] Figure 1B is a diagram showing a detected sinusoidal wave signal;

[0009] Figure 1C is a diagram showing a transmitter coil and a receiver coil;

[0010] Figure 2A is a plan view showing a scale according to a first embodiment;

[0011] Figure 2B is along Figure 2A A cross-sectional view taken along line AA in FIG.

[0012] FIG. 3A to FIG. 3D is a cross-sectional view showing a scale manufacturing method according to a first embodiment;

[0013] FIG. 4A to FIG. 4C is a cross-sectional view illustrating a method for manufacturing a ruler according to Comparative Example 1;

[0014] Figure 5A is a plan view showing a scale according to a second embodiment;

[0015] Figure 5B is along Figure 5A A cross-sectional view taken along line AA in FIG.

[0016] Fig. 6A is a plan view showing a scale according to a third embodiment;

[0017] Figure 6B is along Fig. 6A A cross-sectional view taken along line AA in FIG.

[0018] FIG. 7A to FIG. 7D is a cross-sectional view showing a scale manufacturing method according to a third embodiment;

[0019] FIG. 8A to FIG. 8C is a cross-sectional view showing a method for manufacturing a ruler according to Comparative Example 2;

[0020] Fig. 9A is a plan view showing a scale according to a fourth embodiment;

[0021] Fig. 9B is along Fig. 9A A cross-sectional view taken along line AA in FIG.

[0022] FIG. 10A to FIG. 10D is a cross-sectional view showing a method of manufacturing a scale according to a fourth embodiment;

[0023] FIG. 11A to FIG. 11D are examples of images of the upper surfaces of the glass substrates in samples A to D taken by an optical microscope;

[0024] Fig. 12A and Fig. 12B are cross-sectional views of devices manufactured using glass substrates of samples A to D;

[0025] FIG. 13A to FIG. 13Dare examples of optical microscope images of the upper and lower surfaces of device A manufactured using the glass substrates of samples A to D; and

[0026] Fig.14A and Fig. 14B are examples of optical microscope images of the upper and lower surfaces of device B manufactured using the glass substrates of samples A and D. DETAILED DESCRIPTION

[0027] By forming a conductor pattern for a scale on the upper surface of a glass substrate using laser processing, the processing time when forming the conductor pattern can be shortened and / or the processing reproducibility of the conductor pattern can be improved. When the conductor pattern is formed on the upper surface of the glass substrate, there is a reason to suppress the warping that occurs on the glass substrate. Moreover, in the case of an electromagnetic induction encoder scale, a conductor film can be provided on the lower surface of the glass substrate as an electromagnetic shield for suppressing noise caused by the unevenness of components below the mounting surface of the encoder device. In addition, a scale having a reference point and elements constituting a circuit can be formed on the lower surface of the glass substrate. In this case, when a conductor pattern is formed on the upper surface of the glass substrate using laser processing, objects (such as films and elements) formed on the lower surface of the glass substrate may be damaged by the laser penetrating during processing, and defects may occur on the lower surface of the scale.

[0028] Hereinafter, embodiments will be described with reference to the accompanying drawings.

[0029] (First embodiment) Figure 1A 1 is a diagram showing a configuration of an electromagnetic induction encoder 1000 including a scale 100 according to a first embodiment. Figure 1A As shown, the electromagnetic induction encoder 1000 includes a scale 100 and a detection head 40 that moves relative to the scale 100 in the direction of the measuring axis. The scale 100 and the detection head 40 each have a substantially flat plate shape and are disposed facing each other with a predetermined gap interposed therebetween. The electromagnetic induction encoder 1000 also includes a transmission signal generator 50, a displacement meter 60, and the like. Figure 1A In FIG. 1 , the X axis indicates the displacement direction (measurement axis) of the detection head 40. In the plane formed by the scale 100, the direction perpendicular to the X axis is defined as the Y axis. The direction perpendicular to the plane constituting the scale 100 is defined as the Z axis.

[0030] The detection head 40 is provided with a transmitter coil 42 , a receiver coil 44 , etc. The transmitter coil 42 is a rectangular coil whose length direction is in the X-axis direction. The receiver coil 44 is arranged inside the transmitter coil 42 .

[0031] In the ruler 100, a plurality of conductor patterns 20 made of a conductor are provided on the upper surface 11 of the glass substrate 10. The plurality of conductor patterns 20 are arranged in the X-axis direction with a basic period λ. The basic period λ corresponds to the distance between the centers of two adjacent conductor patterns 20 in the X-axis direction. The conductor pattern 20 is, for example, a plate-like pattern without a hole or a closed-loop coil. The conductor pattern 20 is electromagnetically coupled to the transmitter coil 42 and is also electromagnetically coupled to the receiver coil 44.

[0032] The transmission signal generator 50 generates a single-phase AC transmission signal and supplies the signal to the transmitter coil 42. In this case, a magnetic flux is generated in the transmitter coil 42. As a result, an electromotive force current is generated in the plurality of conductor patterns 20. The plurality of conductor patterns 20 are electromagnetically coupled to the magnetic flux generated by the transmitter coil 42, thereby generating a magnetic flux that changes with a predetermined spatial period in the X-axis direction. The magnetic flux generated by the conductor pattern 20 causes an electromotive force current to be generated in the receiver coil 44. The electromagnetic coupling between the conductor pattern 20 and the receiver coil 44 changes according to the displacement amount of the detection head 40. Thus, as shown in FIG. Figure 1B As shown, a sine wave signal having the same period as the basic period λ is obtained. Therefore, the receiver coil 44 detects the phase of the magnetic flux generated by the plurality of conductor patterns 20 .

[0033] The displacement measuring device 60 can electrically interpolate the sine wave signal to use the signal as a digital quantity with a minimum resolution and measure the displacement of the detection head 40. Figure 1B , the horizontal axis represents the displacement amount of the detection head 40 , and the vertical axis represents the output voltage of the receiver coil 44 .

[0034] The transmitter coil 42, the receiver coil 44 and the conductor pattern 20 that are electromagnetically coupled to each other constitute a track. Therefore, in this embodiment, the electromagnetic induction encoder 1000 includes a track. Note that the electromagnetic induction encoder 1000 can have two tracks arranged at a predetermined interval in the Y-axis direction. In this case, the basic period λ between the two tracks can be different. This allows it to be used as an absolute (ABS) encoder.

[0035] Figure 1C 4 is a diagram showing a transmitter coil 42 and a receiver coil 44 provided in the detection head 40. Figure 1C As shown, the receiver coil 44 is arranged within the transmitter coil 42, forming a rectangular coil. The receiver coil 44 is, for example, a circular coil, but may have other configurations.

[0036] Figure 2A is a plan view showing a scale 100 according to the first embodiment, Figure 2B is along Figure 2A A cross-sectional view taken along line AA in FIG. Figure 2A and Figure 2B As shown, the scale 100 includes, for example, a plurality of conductor patterns 20 provided on the upper surface 11 of the glass substrate 10, and a conductor film 30 provided on the lower surface 12 of the glass substrate 10. The plurality of conductor patterns 20 are arranged at predetermined intervals along the X-axis direction. The plurality of conductor patterns 20 have a substantially rectangular shape, wherein the Y-axis direction is the longitudinal direction when viewed from the +Z direction.

[0037] The glass substrate 10 is formed of, for example, quartz glass, soda-lime glass or alkali-free glass, but may also be made of other materials. Quartz glass is a glass mainly made of silicon dioxide (SiO2) and has very few impurities. Soda-lime glass is a glass whose main component is silicon dioxide (SiO2) and also contains sodium oxide (Na2O) and calcium oxide (CaO). Alkali-free glass is a glass whose main component is silicon dioxide (SiO2) and does not contain alkaline components such as sodium and potassium. The thickness of the glass substrate 10 is, for example, about 0.5 mm to 5.0 mm.

[0038] The conductor pattern 20 is formed of a conductor such as copper, silver, gold or aluminum. The thickness of the conductor pattern 20 is, for example, about 5 μm to 30 μm. The width of the conductor pattern 20 is, for example, about 500 μm to 3000 μm. The interval between the conductor patterns 20 is also, for example, about 500 μm to 3000 μm.

[0039] The conductor film 30 is made of a conductor such as copper, silver, gold or aluminum. For example, the conductor film 30 is made of the same material as the conductor pattern 20. The thickness of the conductor film 30 is, for example, 5 μm to 30 μm. The thickness of the conductor film 30 is, for example, substantially the same as the thickness of the conductor pattern 20, and is 0.8 times or more and 1.2 times or less, and 0.9 times or more and 1.1 times or less of the thickness of the conductor pattern 20.

[0040] The upper surface 11 of the glass substrate 10 is frosted and opaque, and has fine irregularities formed therein. The upper surface 11 has a first area 13 provided with a conductor pattern 20 and a second area 14 located between adjacent conductor patterns 20. In both the first area 13 and the second area 14, the arithmetic mean roughness of the upper surface 11 is 0.20 μm or more. Therefore, the upper surface 11 is in an opaque state in both the first area 13 and the second area 14. The surface roughness of the upper surface 11 in the second area 14 is approximately the same as that in the first area 13, or the surface roughness of the upper surface 11 in the second area 14 is increased due to damage caused by processing. In addition, the second area 14 may be colored due to damage caused by processing. The lower surface 12 of the glass substrate 10 is a substantially smooth surface. The arithmetic mean roughness Ra of the lower surface 12 is, for example, 0.01 μm or less.

[0041] Since the upper surface 11 of the glass substrate 10 is frosted glass, the transmittance of light incident on the upper surface 11 is poor. For example, when red light (wavelength: 630nm to 670nm) is vertically and directly incident on the first area 13 of the upper surface 11 in a state where the conductor pattern 20 and the conductor film 30 are not provided, the transmittance of the red light from the upper surface 11 to the lower surface 12 is 90% or less, may be 87% or less, or may be 85% or less. Even when the red light is vertically and directly incident on the second area 14 of the upper surface 11, the transmittance of the red light from the upper surface 11 to the lower surface 12 is 90% or less, may be 87% or less, or may be 85% or less. The transmittance is the ratio of the intensity of the light emitted from the lower surface 12 to the intensity of the light incident on the upper surface 11.

[0042] The upper surface 11 of the glass substrate 10 has a shape in which the second region 14 is recessed in the -Z direction relative to the first region 13. The second region 14 is formed deeper than the conductor pattern 20 at the boundary with the first region 13. That is, the bottom of the second region 14 at the boundary with the first region 13 is closer to the lower surface 12 of the glass substrate 10 than the conductor pattern 20.

[0043] [Manufacturing method] FIG. 3A to FIG. 3D 1 is a cross-sectional view showing a method of manufacturing the scale 100 according to the first embodiment. Figure 3A As shown, first, a glass substrate 10 is prepared. At this stage, both the upper surface 11 and the lower surface 12 of the glass substrate 10 are smooth surfaces, and the arithmetic mean roughness Ra is, for example, 0.01 μm or less.

[0044] like Figure 3B As shown, the upper surface 11 of the glass substrate 10 is roughened to form a frosted glass-like surface having fine irregularities. For example, the upper surface 11 is roughened by sandblasting or chemical treatment using hydrofluoric acid or the like so that the upper surface 11 looks like frosted glass. By forming the upper surface 11 into a frosted glass shape, light incident on the upper surface 11 is diffusely reflected on the upper surface 11. Therefore, the transmittance of the light incident on the upper surface 11 from the upper surface 11 to the lower surface 12 is reduced. For example, the upper surface 11 is roughened so that the arithmetic mean roughness Ra is 0.20 μm or more to form a frosted glass shape.

[0045] like Figure 3CAs shown, the conductor film 22 is formed on the upper surface 11 of the glass substrate 10, and the conductor film 30 is formed on the lower surface 12. The conductor film 22 and the conductor film 30 are formed, for example, using an electroless plating method. Note that the conductor film 22 and the conductor film 30 can be formed by forming a base conductor layer and then forming a conductor film on the base conductor layer using an electrolytic plating method. It is preferred to form (film-form) the conductor film 22 and the conductor film 30 at the same time. In this case, the conductor film 22 and the conductor film 30 are formed of the same material and have approximately the same thickness.

[0046] like Figure 3D As shown, the conductor film 22 is patterned by laser processing using a laser beam 70 to form a plurality of conductor patterns 20. The laser processing is performed by pulse laser processing using, for example, an infrared (e.g., wavelength 1032 nm), a green (e.g., wavelength 532 nm), or an ultraviolet (e.g., wavelength 355 nm) laser 70. In the pulse laser processing, for example, a pulse width of femtosecond to picosecond order and an energy density of 0.1 to 10 J / cm 2 By repeatedly irradiating the conductor pattern 20 with a short pulse laser at a high speed of 10 kHz to 5 MHz, the side surface of the conductor pattern 20 can be made into a flat tapered surface with an angle of about 60° to 80°.

[0047] Because the upper surface 11 of the glass substrate 10 is roughened and has a frosted glass shape, the laser beam 70 is diffusely reflected on the upper surface 11 and the energy is absorbed on the upper surface 11. Therefore, when the conductor film 22 is etched by the laser beam 70 to form the conductor pattern 20, the second region 14 between the adjacent conductor patterns 20 on the upper surface 11 of the glass substrate 10 is etched by the laser beam 70. When the etching depth reaches the upper surface 11, the surface roughness remains high. Therefore, the laser beam 70 continues to be diffusely reflected on the upper surface 11, and the laser beam 70 is prevented from being transmitted from the upper surface 11 to the lower surface 12 and damaging the conductor film 30 provided on the lower surface 12.

[0048] In addition, the processing conditions may be selected so that the upper surface 11 in the second region 14 is colored from opaque to black by irradiation with the laser 70. The processing conditions include a combination of conditions such as laser intensity, pulse frequency, spot diameter, spot interval, focal depth, processing trajectory, and irradiation timing. If the upper surface 11 of the glass substrate 10 is not frosted, the laser beam 70 irradiates the smooth upper surface 11 of the glass substrate 10 exposed by etching the conductor film 22, so that the laser beam 70 can penetrate the glass substrate 10. However, by roughening the upper surface 11 of the glass substrate 10 in advance so that the upper surface 11 is frosted, even if the upper surface 11 of the glass substrate 10 is exposed during etching with the laser beam 70, the upper surface 11 will remain frosted. Therefore, the laser beam 70 is prevented from penetrating the glass substrate 10.

[0049] In addition, the upper surface 11 of the glass substrate 10 is etched by irradiating with a laser beam 70 so that the second area 14 is more recessed than the first area 13. That is, the upper surface 11 becomes a recessed portion in which the second area 14 is recessed relative to the first area 13. The inner surface of the recess is a rough surface including coloring and unevenness, and may have a conical shape so as to completely reflect the laser beam 70. For example, the angle between the bottom surface and the inner surface of the recess may be 30 degrees or less. A periodic nanometer-sized uneven pattern (laser induced periodic surface structure: LIPSS) having the same wavelength as the laser beam 70 may be formed on the bottom surface of the recess or on the conical surface including the conductor pattern 20. This uneven pattern is formed unintentionally and is not used as part of the scale. In addition, since the uneven pattern is nanometer-sized, the influence on the length measurement using the scale 100 can be suppressed.

[0050] [Comparative Example 1] FIG. 4A to FIG. 4C is a cross-sectional view illustrating a method for manufacturing the scale 500 according to Comparative Example 1. Figure 4A A glass substrate 10 is prepared as shown. The upper surface 11 and the lower surface 12 of the glass substrate 10 are both smooth surfaces. Figure 4B As shown, the conductor film 22 is formed on the upper surface 11 of the glass substrate 10 without roughening the upper surface 11 of the glass substrate 10 to make the upper surface 11 frosted, and the conductor film 30 is formed on the lower surface 12 .

[0051] like Figure 4C As shown, the conductor film 22 is patterned by laser processing using a laser beam 70 to form a plurality of conductor patterns 20. Since the upper surface 11 of the glass substrate 10 is not roughened and is a smooth surface, the laser beam 70 is less likely to be diffusely reflected by the upper surface 11. Therefore, the laser beam 70 is easily transmitted from the upper surface 11 to the lower surface 12. For example, in a portion of the second region 14, the transmittance may be greater than 90%. The laser beam 70 transmitted from the upper surface 11 of the glass substrate 10 to the lower surface 12 may cause damage to the conductor film 30 disposed on the lower surface 12, such as a burnt spot 72. If the burnt spot 72 is formed to protrude from the lower surface of the conductor film 30, the morphology of the glass substrate 10 will change during the subsequent patterning of the conductor film 22, and the focus of the laser beam 70 will shift, making it impossible to perform patterning normally. In addition, when the scale 500 is mounted on a flat mounting surface of the encoder device using an adhesive or the like, the scale 500 may become tilted and cannot be used as a scale. In addition, the scale 500 can be easily peeled off from the mounting surface of the encoder device.

[0052] On the other hand, in the first embodiment, if Figure 3B As shown, the upper surface 11 of the glass substrate 10 is roughened to have a frosted glass shape. Figure 3DAs shown, even when a plurality of conductor patterns 20 are formed on the upper surface 11 of the glass substrate 10 by laser processing using the laser beam 70, the laser beam 70 is diffusely reflected on the upper surface 11. Therefore, the influence of the laser beam 70 on the conductor film 30 formed on the lower surface 12 can be suppressed. Therefore, damage to the conductor film 30 can be suppressed.

[0053] As described above, according to the first embodiment, the glass substrate 10 has the frosted glass-like upper surface 11. Therefore, as described above, even when the conductor pattern 20 is formed by laser processing, the conductor film 30 (molded product) provided on the lower surface 12 of the glass substrate 10 is less likely to be damaged. In addition, since the conductor pattern 20 is provided on the frosted glass-like upper surface 11, the bonding area between the upper surface 11 and the conductor pattern 20 becomes large, and the bonding strength of the conductor pattern 20 is improved.

[0054] Furthermore, in the first embodiment, if Figure 3D As shown, the conductor film 22 formed on the upper surface 11 of the glass substrate 10 is patterned by laser processing using a laser beam 70 to form the conductor pattern 20. Therefore, the upper surface 11 of the glass substrate 10 is also etched by the laser beam 70. As a result, the second region 14 of the upper surface 11 of the glass substrate 10 is recessed relative to the first region 13, and is formed deeper than the conductor pattern 20 at the boundary with the first region 13. This suppresses the generation of edge residues at the lower end of the conductor pattern 20 after the conductor pattern 20 is formed. Therefore, interference in the current flowing through the conductor pattern 20 is suppressed. From the viewpoint of suppressing interference in the current flowing through the conductor pattern 20, the distance L (see Figure 2B ) is preferably set to 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. On the other hand, from the viewpoint of shortening the processing time, the distance L is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less. In addition, since the upper surface 11 of the glass substrate 10 is etched by the laser beam 70, the surface roughness of the second region 14 can be greater than the surface roughness of the first region 13.

[0055] Furthermore, in the first embodiment, after the conductor film 22 is formed on the upper surface 11 of the glass substrate 10 and the conductor film 30 is formed on the lower surface 12, the conductor film 22 is patterned using laser processing to form a plurality of conductor patterns 20. Since both the conductor film 22 and the conductor film 30 are formed, the warping of the glass substrate 10 is suppressed, so that the conductor film 22 can be well patterned using laser processing. Furthermore, for example, if the conductor film 22 is formed only on the upper surface 11, and the conductor film 22 is patterned to form a plurality of conductor patterns 20, and then the conductor film 30 is formed on the lower surface 12, the number of manufacturing steps and the like will increase. On the other hand, by simultaneously forming the conductor film 22 and the conductor film 30, and then patterning the conductor film 22 to form a plurality of conductor patterns 20, an increase in the number of manufacturing steps can be suppressed.

[0056] (Second embodiment) Figure 5A is a plan view showing a scale 200 according to a second embodiment, Figure 5B is along Figure 5A The cross-sectional view is taken along the line AA in FIG. Figure 5A and Figure 5B As shown, in the scale 200, the lower surface 12 of the glass substrate 10 is frosted glass-like and opaque, and has fine irregularities formed therein. For example, the lower surface 12 has a surface roughness that is substantially the same as the surface roughness of the upper surface 11 in the first region 13. The arithmetic mean roughness Ra of the upper surface 11 in the first region 13 and the arithmetic mean roughness Ra of the lower surface 12 may be, for example, 0.20 μm or more, may be 0.25 μm or more, or may be 0.30 μm or more. The arithmetic mean roughness Ra of the lower surface 12 is, for example, 0.9 to 1.1 times, for example, 0.95 to 1.05 times, the arithmetic mean roughness Ra of the upper surface 11 in the first region 13. The rest of the configuration is the same as the scale 100 of the first embodiment, and therefore a description thereof will be omitted.

[0057] [Manufacturing Method] In the scale 200 according to the second embodiment, the Figure 3B In the embodiment, both the upper surface 11 and the lower surface 12 of the glass substrate 10 are roughened, and both the upper surface 11 and the lower surface 12 are formed into frosted glass. The roughening treatment of the lower surface 12 is performed by the same method as the roughening treatment of the upper surface 11. In order to reduce the number of manufacturing steps, it is preferable to roughen the upper surface 11 and the lower surface 12 at the same time (in one processing step). As a result, the upper surface 11 and the lower surface 12 have substantially the same surface roughness. Thereafter, the same method as the first embodiment is performed. Figure 3C and Figure 3D Same steps as in .

[0058] In the second embodiment, as in the first embodiment, the glass substrate 10 has a frosted glass-like upper surface 11. Therefore, even when the conductor pattern 20 is formed on the upper surface 11 of the glass substrate 10 by laser processing using the laser beam 70, the conductor film 30 provided on the lower surface 12 of the glass substrate 10 is less likely to be damaged.

[0059] In addition, in the second embodiment, the lower surface 12 of the glass substrate 10 also has a frosted glass shape. As a result, the laser beam 70 may also be diffusely reflected on the lower surface 12, making it difficult for the conductor film 30 provided on the lower surface 12 to be damaged. In addition, since the surface roughness of the lower surface 12 is large, the bonding area between the lower surface 12 and the conductor film 30 becomes large, thereby improving the bonding strength of the conductor film 30.

[0060] (Third Embodiment) Fig. 6A is a plan view showing a scale 300 according to the third embodiment. Figure 6B is along Fig. 6A The cross-sectional view is taken along the line AA in FIG. Fig. 6A and Figure 6B As shown, in the ruler 300, the lower surface 12 of the glass substrate 10 is also frosted glass, as in the second embodiment. The resin film 80 is provided between the upper surface 11 of the glass substrate 10 and the conductor pattern 20, and the resin film 82 is provided between the lower surface 12 and the conductor film 30. For example, the resin film 80 can be used as an adhesive layer for adhering the glass substrate 10 and the conductor pattern 20, and the resin film 82 can be used as an adhesive layer for adhering the glass substrate 10 and the conductor film 30. The resin films 80 and 82 are made of, for example, epoxy resin, acrylic resin, vinyl acetate resin, etc. The rest of the configuration is the same as the ruler 100 of the first embodiment, so the description thereof will be omitted.

[0061] [Manufacturing method] FIG. 7A to FIG. 7D 1 is a cross-sectional view showing a method of manufacturing the scale 300 according to the third embodiment. Fig. 7A As shown, first, a glass substrate 10 is prepared. At this stage, the upper surface 11 and the lower surface 12 of the glass substrate 10 are both smooth surfaces.

[0062] like Figure 7B As shown, as in the second embodiment, both the upper surface 11 and the lower surface 12 of the glass substrate 10 are roughened so that both the upper surface 11 and the lower surface 12 are frosted.

[0063] like Figure 7CAs shown, the metal foil is attached to the upper surface 11 of the glass substrate 10 using the resin film 80 as an adhesive layer, and the conductor film 22 is formed on the upper surface 11. Similarly, the metal foil is attached to the lower surface 12 of the glass substrate 10 using the resin film 82 as an adhesive layer to form the conductor film 30 on the lower surface 12. The metal foil can be attached using a lamination method or a press processing method. The resin film 80 can be formed on the upper surface 11 of the glass substrate 10 by applying a resin or pasting a sheet-like resin film. Alternatively, the metal foil coated with the resin film 80 can be attached to the upper surface 11 of the glass substrate 10. The same applies to the resin film 82.

[0064] like Fig.7D As shown, the conductor film 22 and the resin film 80 are patterned by laser processing using a laser beam 70 to form a plurality of conductor patterns 20. The laser processing is performed by the method described in the first embodiment. Since the upper surface 11 of the glass substrate 10 is frosted, damage to the resin film 82 and the conductor film 30 provided on the lower surface 12 is suppressed similarly to the first embodiment.

[0065] [Comparative Example 2] FIG. 8A to FIG. 8C is a cross-sectional view showing a method of manufacturing the scale 600 according to Comparative Example 2. Fig. 8A As shown, a glass substrate 10 is prepared. The upper surface 11 and the lower surface 12 of the glass substrate 10 are both smooth surfaces.

[0066] like Figure 8B As shown, the metal foil is attached to the upper surface 11 of the glass substrate 10 using the resin film 80 as an adhesive layer, and the conductor film 22 is formed on the upper surface 11. The metal foil is attached to the lower surface 12 of the glass substrate 10 using the resin film 82 as an adhesive layer, and the conductor film 30 is formed on the lower surface 12.

[0067] like Figure 8C As shown, the conductor film 22 and the resin film 80 are patterned by laser processing using a laser beam 70 to form a plurality of conductor patterns 20. Since the upper surface 11 of the glass substrate 10 is not roughened and does not become frosted glass, similar to Comparative Example 1, the laser beam 70 transmitted from the upper surface 11 of the glass substrate 10 to the lower surface 12 causes burn spots 72 to occur on the resin film 82 and the conductor film 30. In addition, a protrusion 74 may occur in the resin film 82. In this case, as in Comparative Example 1, patterning of the conductor film 22 and the resin film 80 may not be performed normally, or the scale 600 may be placed on the encoder device at an angle, making it impossible to use the scale 600 as a scale.

[0068] On the other hand, in the third embodiment, the glass substrate 10 has a frosted glass-like upper surface 11. Therefore, even if the conductor pattern 20 is formed on the upper surface 11 of the glass substrate 10 by laser processing using the laser beam 70, as in the first embodiment, the influence of the laser beam 70 on the resin film 82 and the conductor film 30 formed on the lower surface 12 can be suppressed, and the resin film 82 and the conductor film 30 can be made less likely to be damaged.

[0069] Furthermore, in the third embodiment, the resin film 82 is provided between the lower surface 12 of the glass substrate 10 and the conductor film 30 (molded product). In this case, as explained in Comparative Example 2, if the upper surface 11 of the glass substrate 10 is not frosted glass-like, the laser beam 70 may cause the protrusion 74 in the resin film 82, making it impossible to use the ruler as a ruler. Therefore, when the resin film 82 is provided, it is preferable to make the upper surface 11 of the glass substrate 10 into a frosted glass shape to suppress the influence of the laser beam 70 on the resin film 82.

[0070] (Fourth embodiment) Fig. 9A is a plan view showing a scale 400 according to a fourth embodiment, Fig. 9B is along Fig. 9A The cross-sectional view is taken along the line AA in FIG. Fig. 9A and Fig. 9B As shown, in the scale 400, the lower surface 12 of the glass substrate 10 is also frosted glass, as in the second embodiment. In the first to third embodiments, on the upper surface 11 of the glass substrate 10, the entire second region 14 is recessed to the same extent relative to the first region 13, but in the fourth embodiment, in the second region 14, the adjacent portion 15 adjacent to the first region 13 is recessed deeper than the central portion 16 located at the center of the X-axis direction. For example, the adjacent portion 15 may be recessed by 5 μm or more relative to the central portion 16, or may be recessed by 10 μm or more. The adjacent portion 15 may be a groove having a V-shaped cross section. The central portion 16 may be slightly recessed relative to the first region 13, or may not be recessed relative to the first region 13, and may have the same height as the first region 13. In addition, the adjacent portion 15 may also have a surface roughness greater than that of the first region 13. The surface roughness of the central portion 16 may be approximately the same as that of the first region 13, or may be greater. The adjacent portion 15 and the central portion 16 may be colored black as in the first embodiment. The rest of the configuration is the same as that of the scale 100 of the first embodiment, and thus a description thereof will be omitted.

[0071] [Manufacturing method] FIG. 10A to FIG. 10D 4 is a cross-sectional view showing a method for manufacturing a scale 400 according to a fourth embodiment. Fig. 10A and Fig. 10BAs shown, the execution of the third embodiment Fig. 7A and Figure 7B Follow the same steps as shown in .

[0072] like Fig. 10C As shown, a plurality of temporary conductor patterns 24 are formed on the upper surface 11 of the glass substrate 10 by applying a conductor paste to the upper surface 11 using screen printing or the like. A conductor film 30 is formed on the lower surface 12 by applying the conductor paste to the lower surface 12 of the glass substrate 10. Since the upper surface 11 is roughened and has a frosted glass shape, defects such as elongation and / or scratching of the conductor paste in the squeegee feeding direction are suppressed.

[0073] When the temporary conductor pattern 24 is formed by applying the conductor paste, the side surface of the temporary conductor pattern 24 may have a tapered shape with a gentle angle. Fig. 10D As shown, the edge portion of the temporary conductor pattern 24 is laser processed using a laser beam 70 to form a conductor pattern 20 having a steeply inclined side surface. Since the upper surface 11 of the glass substrate 10 irradiated with the laser beam 70 is etched, the adjacent portion 15 of the second region 14 adjacent to the first region 13 is recessed relative to the first region 13. In addition, the surface roughness of the adjacent portion 15 may be greater than the surface roughness of the first region 13, or may be a groove with a V-shaped cross section. The central portion 16 of the second region 14 located at the center in the X-axis direction may be irradiated with the laser beam 70 for a short time and slightly recessed relative to the first region 13, or may be irradiated with almost no laser beam 70 and the height may be maintained at approximately the same level as the height of the first region 13 without being recessed relative to the first region 13. When the laser beam 70 is irradiated only for a short time, the surface roughness of the central portion 16 may be greater than the surface roughness of the first region 13, and when the laser beam 70 is hardly irradiated, the surface roughness of the central portion 16 is maintained at the same level as the surface roughness of the first region 13.

[0074] Also in the fourth embodiment, the glass substrate 10 has the frosted glass-like upper surface 11 as in the first embodiment. Therefore, even when the conductor pattern 20 is formed by irradiating the edge portion of the temporary conductor pattern 24 with the laser beam 70 and processing the edge portion of the temporary conductor pattern 24, the influence of the laser beam 70 on the conductor film 30 formed on the lower surface 12 can be suppressed, and the conductor film 30 can be made less likely to be damaged.

[0075] Furthermore, in the fourth embodiment, the conductor pattern 20 is formed by laser processing the edge portion of the temporary conductor pattern 24. Therefore, on the upper surface 11 of the glass substrate 10, the second region 14 has an adjacent portion 15 adjacent to the first region 13, the adjacent portion 15 is recessed relative to the first region 13, and is deeper than the conductor pattern 20 at the boundary with the first region 13. As a result, the lower end portion can be prevented from maintaining a tapered shape on the side surface of the conductor pattern 20, and the current flowing through the conductor pattern 20 can be prevented from being disturbed.

[0076] (Experimental example) FIG. 11A to FIG. 11D is an example of an optical microscope image of the upper surface 11 of the glass substrate 10 in samples A to D. Fig.11A In the sample A shown, the upper surface 11 and the lower surface 12 of the glass substrate 10 are not subjected to roughening treatment, and the upper surface 11 and the lower surface 12 are smooth surfaces. The glass substrate 10 is made of soda-lime glass (the same applies to the glass substrates 10 of samples B to D). The arithmetic mean roughness Ra and the maximum height Rz of the upper surface 11 and the lower surface 12 are 0.00±0.00μm. In addition, when red light is vertically incident on the upper surface 11 of the glass substrate 10, the transmittance of red light from the upper surface 11 to the lower surface 12 is 93%.

[0077] exist Fig. 11B In the sample B shown, the upper surface 11 and the lower surface 12 of the glass substrate 10 are roughened to have a frosted glass appearance. The arithmetic mean roughness Ra of the upper surface 11 and the lower surface 12 is 0.05±0.02μm, and the maximum height Rz is 0.48±0.17μm. In addition, when red light is vertically incident on the upper surface 11 of the glass substrate 10, the transmittance of the red light from the upper surface 11 to the lower surface 12 is 88%.

[0078] exist Fig. 11C In the sample C shown, the upper surface 11 and the lower surface 12 of the glass substrate 10 are roughened so that the upper surface 11 and the lower surface 12 are frosted. The arithmetic mean roughness Ra of the upper surface 11 and the lower surface 12 is 0.30±0.14μm, and the maximum height Rz is 1.43±0.36μm. In addition, when red light is vertically incident on the upper surface 11 of the glass substrate 10, the transmittance of the red light from the upper surface 11 to the lower surface 12 is 87%.

[0079] exist Fig.11DIn the sample D shown, the upper surface 11 and the lower surface 12 of the glass substrate 10 are roughened so that the upper surface 11 and the lower surface 12 are frosted. The arithmetic mean roughness Ra of the upper surface 11 and the lower surface 12 is 0.72±0.08μm, and the maximum height Rz is 2.10±0.47μm. In addition, when red light is vertically incident on the upper surface 11 of the glass substrate 10, the transmittance of the red light from the upper surface 11 to the lower surface 12 is 86%.

[0080] The glass substrate 10 of samples AD was used to manufacture Fig. 12A and Fig. 12B Devices A and B are shown. Fig. 12A In the device A shown, the conductor film 22 is formed on the upper surface 11 of the glass substrate 10, and the resin film 80 is sandwiched between the conductor film 22 and the upper surface 11 of the glass substrate 10. The conductor film 30 is formed on the lower surface 12 of the glass substrate 10, and the resin film 82 is sandwiched between the conductor film 30 and the lower surface 12 of the glass substrate 10. A recess 76 is formed in the upper surface 11 of the glass substrate 10, and the recess 76 penetrates the conductor film 22 and the resin film 80 and penetrates into a part of the glass substrate 10. The recess 76 is formed by laser processing using green laser. For the laser processing, pulse laser processing with a pulse width of about 20ps and a power of about 10W is used. The conductor films 22 and 30 are made of copper. The thickness of the glass substrate 10 is 1.1mm, the thickness of the resin films 80 and 82 is 20μm, and the thickness of the conductor films 22 and 30 is 12μm. The recess 76 has a width of 250μm and a depth of 35μm.

[0081] exist Fig. 12B In the device B shown, the conductor film 22 is formed on the upper surface 11 of the glass substrate 10. The conductor pattern 32 is formed on the lower surface 12 of the glass substrate 10. The recess 78 is formed in the upper surface 11 of the glass substrate 10, penetrating the conductor film 22 and penetrating into a part of the glass substrate 10. The recess 78 is formed by laser processing using a green laser. For the laser processing, a pulse laser processing with a pulse width of about 20 ps and a power of about 10 W is used. The conductor film 22 and the conductor pattern 32 are made of silver. The thickness of the glass substrate 10 is 1.1 mm, and the thickness of the conductor film 22 and the conductor pattern 32 is 12 μm. The width of the recess 78 is 250 μm and the depth is 50 μm.

[0082] FIG. 13A to FIG. 13D is an example of an optical microscope image of the upper and lower surfaces of the device A manufactured using the glass substrates 10 of samples A to D. FIG. 13A to FIG. 13D As shown, it was confirmed that in samples A and B, the conductor film 30 was damaged on the lower surface of the device A, but in samples C and D, damage to the conductor film 30 was suppressed.

[0083] Fig.14A and Fig. 14B is an example of an optical microscope image of the upper and lower surfaces of a device B manufactured using the glass substrate 10 of samples A and D. Fig.14A and Fig. 14B As shown, it was confirmed that in sample A, the conductor pattern 32 was damaged on the lower surface of the device A, but in sample D, damage to the conductor pattern 32 was suppressed.

[0084] like FIG. 13A to FIG. 14B As shown, under the laser processing conditions shown, by setting the transmittance of red light from the upper surface 11 to the lower surface 12 of the glass substrate 10 to 87% or less, it has been confirmed that when the conductor film 22 is processed using laser processing, damage to the conductor film 30 or the conductor pattern 32 provided on the lower surface 12 can be suppressed. In addition, when the upper surface 11 and the lower surface 12 are made into frosted glass by roughening treatment, it has been confirmed that the transmittance of red light transmitted from the upper surface 11 to the lower surface 12 can be reduced to 87% or less by setting the arithmetic mean roughness Ra of the upper surface 11 and the lower surface 12 to 0.16μm or more. At this time, it was confirmed that the maximum height Rz of the upper surface 11 and the lower surface 12 was 1.07μm or more. Note that by using different laser processing conditions in terms of parameters such as the wavelength, power, and pulse density of the laser beam, the conductor film 30 and the like may be damaged unless the transmittance and roughness of the glass substrate 10 are further increased. On the other hand, there is a case where the conductor film 30 and the like are not damaged even if the size is small.

[0085] Note that in the above embodiment, an example is shown in which the solid conductor film 30 is provided as a structure on the lower surface 12 of the glass substrate 10, but the present invention is not limited to this case. The structure provided on the lower surface 12 may be a solid film other than a conductor film, a patterned film, or an element constituting a circuit (such as a sensor element).

[0086] Note that in the above-described embodiment, the case of the electromagnetic induction encoder 1000 is shown as an example, but other cases such as a photoelectric encoder may also be used. In addition, although a scale used in a linear encoder is shown as an example, the scale may be a scale used in a rotary encoder, or a scale used in other encoders or sensors such as an arc encoder.

[0087] although Figure 1A An example is shown in which the electromagnetic induction encoder 1000 includes the scale 100 of the first embodiment, but the electromagnetic induction encoder 1000 may also include the scales of the second to fourth embodiments.

[0088] The present invention is not limited to the specifically disclosed embodiments or examples and variations, but may include other embodiments or examples and variations without departing from the scope of the present invention.

Claims

1. A ruler, comprising: A glass substrate having a frosted glass-like upper surface; a plurality of conductor patterns arranged at predetermined intervals on the upper surface of the glass substrate; as well as A structure is disposed on the lower surface of the glass substrate.

2. The ruler according to claim 1, in, The upper surface of the glass substrate has a first region where the plurality of conductor patterns are disposed and a second region located between the plurality of conductor patterns. wherein at least a portion of the second region adjacent to the first region is recessed relative to the first region, and The second region is formed to be deeper than the plurality of conductor patterns at a boundary with the first region.

3. The ruler according to claim 2, The surface roughness of the bottom surface of at least a portion of the second region adjacent to the first region is greater than the surface roughness of the first region.

4. The scale according to claim 1 or 2, wherein: The lower surface of the glass substrate is in a frosted glass shape.

5. The ruler according to claim 1 or 2, further comprising: a resin film provided between the lower surface of the glass substrate and the structure, The structure is a conductive film.

6. An encoder comprising: A ruler according to claim 1 or 2.

7. A method for manufacturing a ruler, comprising: Roughening the upper surface of the glass substrate into a frosted glass state; forming a structure on the lower surface of the glass substrate; as well as After the upper surface of the glass substrate is roughened into the frosted glass state and the structure is formed, a plurality of conductor patterns arranged at predetermined intervals are formed on the upper surface of the glass substrate by laser processing.

8. The method according to claim 7, further comprising: After roughening the upper surface of the glass substrate into the frosted glass state, forming a conductor film on the upper surface of the glass substrate, In the forming of the plurality of conductor patterns, the conductor film is patterned by laser processing to form the plurality of conductor patterns.

9. The method according to claim 7, further comprising: After roughening the upper surface of the glass substrate into the frosted glass state, forming a plurality of temporary conductor patterns on the upper surface of the glass substrate, When forming the plurality of conductor patterns, edge portions of the plurality of temporary conductor patterns are processed by laser processing, thereby forming the plurality of conductor patterns.