Method for predicting storage performance of positive electrode material

By measuring the viscosity of the positive electrode material slurry and using linear fitting method to predict the capacity loss rate, the problem of evaluating the storage performance of the positive electrode material in the prior art is solved, and a fast and accurate prediction effect is achieved, reducing the development cycle and cost.

CN119086684APending Publication Date: 2024-12-06NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411288190.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to quickly evaluate the storage performance of the positive electrode material, resulting in long development cycles of material products, fluctuating test results and high costs, and it is impossible to effectively optimize the impact of different synthesis processes on storage performance.

Method used

By using the same homogenization method to prepare slurries of different positive electrode materials, their viscosity is measured and capacity loss rate test is performed, and the relationship between slurry viscosity and capacity loss rate is established by using linear fitting method, and the storage performance of the positive electrode material is predicted.

Benefits of technology

It realizes rapid and accurate prediction of the storage performance of the positive electrode material, reduces the development cycle, reduces manpower and material consumption, and improves the stability and accuracy of the test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086684A_ABST
    Figure CN119086684A_ABST
Patent Text Reader

Abstract

The invention discloses a method for predicting the storage performance of a positive electrode material, and the method comprises the following steps: 1) respectively preparing N kinds of slurry by using N kinds of positive electrode materials through the same homogenization method; 2) respectively testing the viscosity of the N slurries to obtain the viscosity eta of the N slurries; (3) preparing batteries from the N types of slurry respectively, and performing battery capacity loss rate test on the batteries respectively to obtain N capacity loss rates CL; 4) according to the N slurry viscosities eta and the N capacity loss rates CL, obtaining a numerical relationship between the capacity loss rates CL and the slurry viscosities eta through a linear fitting method; 5) calculating the capacity loss rate CL by using the slurry viscosity eta according to the numerical relationship; n > 1. The method for predicting the storage performance of the positive electrode material provided by the invention has the characteristics of convenience, rapidness and relatively accurate prediction result.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for predicting storage performance of a positive electrode material, and belongs to the field of new energy. Background Art

[0002] As one of the most critical electrochemical components of the battery, the development of high-stability positive electrode materials is of great significance to battery safety and energy retention. Highly stable positive electrodes can reduce the irreversible loss of capacity when the battery is fully charged and ensure the battery life.

[0003] At present, comparing the capacity retention rate and capacity recovery rate of batteries under different days of high-temperature storage is an important indicator for judging the storage performance of positive electrode materials. High-temperature storage tests are conducted on positive electrode materials with different synthesis processes. The test cycle is long, and it is impossible to quickly evaluate the improvement and optimization effects of different materials, different sintering and treatment processes on storage performance, which leads to a long material product development cycle and is not conducive to product development. In addition, the battery production process has many steps and introduces many variables, which usually leads to fluctuations in test results, consumes a lot of manpower and material resources, and has high requirements on costs.

[0004] Therefore, developing a prediction method that can quickly predict the storage performance of positive electrode materials has become a research direction. Summary of the invention

[0005] The present invention provides a method for predicting the storage performance of a positive electrode material. The method for predicting the storage performance of a positive electrode material has the characteristics of being convenient and fast, and the prediction result is relatively accurate.

[0006] The present invention provides a method for predicting the storage performance of a positive electrode material, wherein the method for predicting the storage performance of a positive electrode material comprises the following steps:

[0007] 1) Using N kinds of positive electrode materials, N kinds of slurries are prepared respectively by the same homogenization method;

[0008] 2) testing the viscosities of the N slurries respectively to obtain N slurry viscosities η;

[0009] 3) The N kinds of slurries are made into batteries respectively, and the battery capacity loss rate is tested respectively to obtain N capacity loss rates C L ;

[0010] 4) According to the N slurry viscosities η and the N capacity loss rates C L , the capacity loss rate C is obtained by linear fitting method. L and the numerical relationship between the slurry viscosity η;

[0011] 5) According to the numerical relationship, the capacity loss rate C is calculated using the slurry viscosity η L ;

[0012] N>1.

[0013] The method for predicting the storage performance of the positive electrode material as described above, wherein in step 4), according to the N slurry viscosities η and the N capacity loss rates C L , through the linear fitting method, the numerical relationship described in formula 1 is obtained:

[0014] C L =γ×η / 10000+β Formula 1;

[0015] in:

[0016] C L is the capacity loss rate, %;

[0017] η is the slurry viscosity, mPa·s;

[0018] γ is the attenuation coefficient;

[0019] β is the correction coefficient;

[0020] Step 5) includes measuring the slurry viscosity η and calculating the capacity loss rate C according to formula 1 L .

[0021] The method for predicting the storage performance of the positive electrode material as described above, wherein the solid contents of the N kinds of slurries are the same; and / or,

[0022] The solid content of the N slurries is 65-75%.

[0023] The method for predicting the storage performance of the positive electrode material as described above, wherein the homogenization method comprises mixing the positive electrode material with a conductive agent and a binder to obtain the slurry;

[0024] The conductive agent is selected from at least one of conductive carbon black SuperP, Ketjen black KB, vapor-grown carbon fiber VGCF, carbon nanotube CNT, and flake graphite KS series materials;

[0025] The adhesive is selected from at least one of Arkema HSV900, Arkema HSV1800, Solvay 5130 and Solvay 6020.

[0026] In the method for predicting the storage performance of the positive electrode material as described above, in step 2), the viscosity test method includes testing the viscosity of the slurry at a temperature of 20-30° C. at a rotation speed of 40-80 rpm.

[0027] The method for predicting the storage performance of the positive electrode material as described above, wherein in step 3), the battery capacity loss rate test also includes recording the initial capacity of the battery and then charging it to 4.3-4.5V, storing it in an environment of 40-70°C for 28-70 days and then performing a capacity test again to obtain the capacity loss rate.

[0028] The method for predicting the storage performance of the positive electrode material as described above, wherein the battery comprises a negative electrode sheet and an electrolyte;

[0029] The negative electrode sheet comprises a copper foil and a negative electrode active layer arranged on two surfaces of the copper foil, wherein the negative electrode active layer comprises a negative electrode material, a conductive agent and an adhesive;

[0030] The negative electrode material is selected from at least one of graphite, silicon-carbon negative electrode material, and silicon-oxygen negative electrode material;

[0031] The conductive agent is selected from at least one of SP, CNT, and KS conductive graphite;

[0032] The adhesive is selected from at least one of PAA, SBR and CMC;

[0033] The electrolyte is selected from at least one of LiPF6, EC, EMC, DEC, and FEC.

[0034] The method for predicting the storage performance of the positive electrode material as described above, wherein the mass ratio of the negative electrode material, the conductive agent, and the adhesive is (93-97): (1.5-3.5): (1.5-3.5).

[0035] The method for predicting the storage performance of the positive electrode material as described above, wherein the method further includes evaluating the difference in the effect of the preparation processes of N positive electrode materials on the capacity loss rate according to the N attenuation coefficients, including:

[0036] The first attenuation coefficient γ1> the second attenuation coefficient γ2, then the influence of the first positive electrode material preparation process on the capacity loss rate is greater than the influence of the second positive electrode material preparation process on the capacity loss rate;

[0037] Among them, the first positive electrode material preparation process and the second positive electrode material preparation process are any two of N different positive electrode material preparation processes, and the first attenuation coefficient γ1 is the attenuation coefficient of the first positive electrode material preparation process, and the second attenuation coefficient γ2 is the attenuation coefficient of the second positive electrode material preparation process.

[0038] The method for predicting the storage performance of the positive electrode material as described above, wherein the method further includes evaluating the difference in the improvement of the storage performance by the preparation processes of the N positive electrode materials according to the N correction coefficients, including:

[0039] The first correction coefficient β1> the second correction coefficient β2, then the improvement of the storage performance by the first positive electrode material preparation process is less than the improvement of the storage performance by the second positive electrode material preparation process;

[0040] Among them, the first positive electrode material preparation process and the second positive electrode material preparation process are any two of N different positive electrode material preparation processes, and the first correction coefficient β1 is the correction coefficient of the first positive electrode material preparation process, and the second correction coefficient β2 is the correction coefficient of the second positive electrode material preparation process.

[0041] The method for predicting the storage performance of the positive electrode material provided by the present invention is convenient and quick, and the prediction result is relatively accurate. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced one by one below. Obviously, the drawings in the following description are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0043] Figure 1 This is a graph showing the relationship between slurry viscosity and capacity loss rate in Example 1;

[0044] Figure 2 is a graph showing the relationship between slurry viscosity and capacity loss rate in Example 2;

[0045] Figure 3 is a graph showing the relationship between slurry viscosity and capacity loss rate in Example 3;

[0046] Figure 4 This is a graph showing the relationship between slurry viscosity and capacity loss rate in Example 4. DETAILED DESCRIPTION

[0047] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0048] A first aspect of the present invention provides a method for predicting the storage performance of a positive electrode material, the method comprising the following steps:

[0049] 1) Using N kinds of positive electrode materials, N kinds of slurries are prepared respectively by the same homogenization method;

[0050] 2) Testing the viscosities of N slurries respectively to obtain N slurry viscosities η;

[0051] 3) Make batteries with N kinds of slurries respectively, and test the battery capacity loss rate respectively to obtain N capacity loss rates C L ;

[0052] 4) According to N slurry viscosities η and N capacity loss rates C L , through the linear fitting method, the capacity loss rate C is obtained L The numerical relationship between η and the slurry viscosity;

[0053] 5) According to the numerical relationship, the capacity loss rate C is calculated using the slurry viscosity η L ;

[0054] N>1.

[0055] The method for predicting the storage performance of the positive electrode material provided by the present invention uses the viscosity of the slurry made from the positive electrode material to predict the storage performance of the battery made from the slurry. Specifically, the present invention does not limit the specific type of positive electrode material, and the positive electrode materials commonly used in the art can be used. For example, in one embodiment, the positive electrode material is a ternary positive electrode material, so that the battery made from the positive electrode material is a ternary lithium battery. The storage performance of the positive electrode material is reflected by the capacity loss rate of the battery. The capacity loss rate of the battery is the ratio of the capacity lost after a period of storage to the initial capacity, that is, the capacity loss rate of the battery has a numerical range of 0-100%. The present invention does not specifically limit the test method for the battery capacity loss rate, and the test method commonly used in the art can be used.

[0056] Specifically, in the method for predicting the storage performance of the positive electrode material provided by the present invention, N different positive electrode materials are first prepared, and the positive electrode materials are subjected to the same homogenization method to obtain N different slurries. The present invention does not specifically limit the homogenization method, and the positive electrode material can be processed using a commonly used homogenization method in the art.

[0057] Furthermore, the viscosities of the N slurries are measured respectively to obtain N slurry viscosities η. The present invention does not limit the test method for the slurry viscosity, and a commonly used test method in the art can be used.

[0058] Further, the N kinds of slurries are prepared into batteries respectively, and the battery capacity loss rate is tested respectively to obtain N capacity loss rates C L The present invention does not specifically limit the test method for the battery capacity loss rate, and a common test method in the art may be used.

[0059] Furthermore, according to N slurry viscosities η and N capacity loss rates C L , through the linear fitting method, the capacity loss rate C is obtainedL The numerical relationship between the capacity loss rate C and the slurry viscosity η. L The linear relationship between C and slurry viscosity η can generally be expressed as L =A×η+B, where A and B are constants obtained through linear fitting. Furthermore, by testing the viscosity of a new slurry and obtaining the viscosity value η, η is substituted into the above linear relationship, and the capacity loss rate of the battery made of the slurry can be predicted using the above linear relationship.

[0060] It is understandable that it is well known in the art that the capacity loss rate of a battery is affected by multiple factors. Therefore, in addition to the fact that N types of positive electrode materials need to use the same homogenization process to prepare the slurry, when using the slurry viscosity to predict the capacity loss rate of the battery, maintaining only a single variable change between other influencing factors such as the composition of the positive electrode material, the preparation method, and the battery preparation method can further improve the accuracy of the prediction. That is, there is only a single variable controlled between the N different positive electrode materials, and the positive electrode material used to predict the capacity loss rate of the battery should also maintain a single variable change with the aforementioned N positive electrode materials.

[0061] For example, in one embodiment, N=5, and the difference between the five positive electrode materials is that the treatment temperatures of the second sintering treatment are different. The treatment temperatures of the second sintering treatment of the five positive electrode materials are 650, 680, 720, 750, and 800°C, respectively. Using the above five positive electrode materials, the viscosities of five slurries and the capacity loss rates of five batteries can be obtained respectively. Using the above five slurry viscosities and the capacity loss rates of five batteries, the capacity loss rate C can be obtained by linear fitting. L and the slurry viscosity η. Further, when the above linear relationship is used to predict the capacity loss rate of a battery with a new positive electrode material, the new positive electrode material is the same as the above five positive electrode materials except for the treatment temperature of the second sintering treatment, and the other components and preparation conditions are the same. After the new positive electrode material is made into a slurry by the same homogenization method, the slurry and the above numerical relationship can be used to predict the capacity loss rate of the battery after the new positive electrode material is made into a battery.

[0062] The method for predicting the storage performance of the positive electrode material provided by the present invention is convenient and quick, and the prediction result is relatively accurate.

[0063] In one embodiment, in step 4), according to N slurry viscosities η and N capacity loss rates C L , through the linear fitting method, the numerical relationship of formula 1 is obtained:

[0064] C L =γ×η / 10000+β Formula 1;

[0065] in:

[0066] C L is the capacity loss rate, %;

[0067] η is the slurry viscosity, mPa·s;

[0068] γ is the attenuation coefficient;

[0069] β is the correction coefficient;

[0070] Step 5) includes measuring the slurry viscosity η and calculating the capacity loss rate C according to formula 1 L .

[0071] The inventors found that the slurry viscosity η and capacity loss rate C L The relationship between can be expressed by formula 1, where γ is the attenuation coefficient. The higher the γ value, the higher the capacity loss rate C. L The faster the rate of increase is, the faster the slurry viscosity η increases; β is the correction coefficient, and the lower the β value is, the higher the battery capacity loss rate C corresponding to the current cathode material composition, preparation process, homogenization process, and battery preparation process. L The smaller.

[0072] Using N slurry viscosities η and N capacity loss rates C L , through linear fitting, the linear relationship shown in Formula 1 can be obtained. Further, after another positive electrode material is made into slurry, the slurry viscosity η is measured, and the capacity loss rate C can be calculated according to Formula 1 L , that is, the storage performance of the positive electrode material is predicted. The above linear relationship is used to more accurately predict the storage performance of the positive electrode material.

[0073] Further, in one embodiment, the solid contents of the N slurries are the same. Keeping the different slurries with the same solid content can reduce the effect of different solid contents on the slurry viscosity, so that the method for predicting the storage performance of the positive electrode material provided by the present invention has higher accuracy. Further, in one embodiment, the solid contents of the N slurries are 65-75%, preferably 65%.

[0074] In one embodiment, the homogenization method includes mixing the positive electrode material with a conductive agent and a binder to obtain a slurry; the conductive agent is selected from at least one of conductive carbon black SuperP, Ketjen black KB, vapor grown carbon fiber VGCF, carbon nanotube CNT, and flaky graphite KS series materials; the binder is selected from at least one of Arkema HSV900, Arkema HSV1800, Solvay 5130, and Solvay 6020.

[0075] The present invention does not limit the specific method of homogenization, and any common homogenization method in the art can be used. In one embodiment, the following homogenization method can be used:

[0076] The positive electrode material and the conductive agent are pre-dry mixed using a double planetary mixer, wherein the stirring revolution speed is 20-50rpm and the dispersion disk dispersion speed is 100-300rpm; a portion of the binder (50-70%) and N-methylpyrrolidone (NMP) are added for kneading process, and the solid content is controlled at 75-85%. First, pre-stir for 5-10 minutes, wherein the revolution speed is 10-30rpm and the dispersion speed is 200-400rpm, and then high-speed stirring is performed, the revolution speed is 20-40rpm, and the dispersion speed is 2000-4 000rpm, during which the material is hung for processing, and the stirring time is 150-200min; the remaining binder (30-50%) and NMP are added for secondary stirring, and the solid content is controlled at 65-75%. First, pre-stir for 5-10min, wherein the revolution speed is 10-30rpm, and the dispersion speed is 200-400rpm, and then high-speed stirring is performed, the revolution speed is 20-40rpm, the dispersion speed is 2000-4000rpm, and the stirring time is 150-200min. After the stirring is completed, the material is discharged to complete the homogenization process.

[0077] In one embodiment, in step 2), the viscosity test method includes testing the viscosity of the slurry at a temperature of 20-30°C at a rotation speed of 40-80 rpm; further, in one embodiment, the viscosity test method in step 2) includes using a rotation viscometer 4# rotor to test the viscosity of the slurry at a temperature of 25°C at a rotation speed of 60 rpm. The above method is simple and convenient, and can make the method for predicting the storage performance of the positive electrode material provided by the present invention more efficient.

[0078] In one embodiment, in step 3), the battery capacity loss rate test further includes recording the initial capacity of the battery and then charging it to 4.3-4.5V, storing it in a 40-70°C environment for 28-70 days and then performing a capacity test again to obtain the capacity loss rate; further, in a preferred embodiment, in step 3), the battery capacity loss rate test further includes recording the initial capacity of the battery and then charging it to 4.4V, storing it in a 70°C environment for 28-70 days and then performing a capacity test again to obtain the capacity loss rate. Storing it in a 70°C environment for 28-70 days can simulate the actual process of capacity decay of the battery in a high temperature environment, so that the prediction method of the storage performance of the positive electrode material provided by the present invention has higher accuracy.

[0079] In one embodiment, a battery for battery capacity loss rate testing includes a negative electrode sheet and an electrolyte;

[0080] The negative electrode sheet includes a copper foil and a negative electrode active layer arranged on two surfaces of the copper foil, and the negative electrode active layer includes a negative electrode material, a conductive agent, and an adhesive;

[0081] The negative electrode material is selected from at least one of graphite, silicon-carbon negative electrode material, and silicon-oxygen negative electrode material;

[0082] The conductive agent is selected from at least one of SP, CNT, and KS conductive graphite;

[0083] The adhesive is selected from at least one of PAA, SBR and CMC;

[0084] The electrolyte is selected from at least one of LiPF6, EC, EMC, DEC, and FEC.

[0085] The mass ratio of the negative electrode material, the conductive agent and the adhesive is (93-97): (1.5-3.5): (1.5-3.5).

[0086] Further, in one embodiment, the mass ratio of graphite, CMC, SP and SBR is 95.5:1.5:1:2, the content of LiPF6 in the electrolyte is 1-1.2M, the volume ratio of EC, EMC and DEC is 1:1:1, and the mass percentage of FEC in the electrolyte is 2%. Using the above battery for testing can make the prediction method of the storage performance of the positive electrode material provided by the present invention have higher accuracy.

[0087] Furthermore, the method for predicting the storage performance of the positive electrode material provided by the present invention also includes evaluating the difference in the effect of N kinds of positive electrode material preparation processes on the capacity loss rate according to N attenuation coefficients, including:

[0088] The first attenuation coefficient γ1> the second attenuation coefficient γ2, then the influence of the first positive electrode material preparation process on the capacity loss rate is greater than the influence of the second positive electrode material preparation process on the capacity loss rate;

[0089] Among them, the first positive electrode material preparation process and the second positive electrode material preparation process are any two of N different positive electrode material preparation processes, and the first attenuation coefficient γ1 is the attenuation coefficient of the first positive electrode material preparation process, and the second attenuation coefficient γ2 is the attenuation coefficient of the second positive electrode material preparation process.

[0090] For Formula 1, C L =γ×η / 10000+β, when β is a constant, C L The vertical axis is η, and the horizontal axis is γ. When the equation 1 is plotted, γ is the slope of the straight line. That is, when the slurry viscosity η increment is the same, the larger the γ value, the greater the capacity loss rate C. LThe larger the increment is. Thus, for two different positive electrode material preparation processes (the first positive electrode material preparation process and the second positive electrode material preparation process), linear fitting obtains formula 1, and compares the first attenuation coefficient γ1 and the second attenuation coefficient γ2. If the first attenuation coefficient γ1> the second attenuation coefficient γ2, the influence of the first positive electrode material preparation process on the capacity loss rate is greater than that of the second positive electrode material preparation process on the capacity loss rate, and vice versa.

[0091] Furthermore, the method for predicting the storage performance of the positive electrode material provided by the present invention evaluates the difference in the improvement of the storage performance by the preparation processes of N positive electrode materials according to N correction coefficients, including:

[0092] The first correction coefficient β1> the second correction coefficient β2, then the improvement of the storage performance by the first positive electrode material preparation process is less than the improvement of the storage performance by the second positive electrode material preparation process;

[0093] The first positive electrode material preparation process and the second positive electrode material preparation process are any two of N different positive electrode material preparation processes, and the first correction coefficient β1 is the correction coefficient of the first positive electrode material preparation process, and the second correction coefficient β2 is the correction coefficient of the second positive electrode material preparation process.

[0094] For Formula 1, C L =γ×η / 10000+β, then when γ is a constant, C L The vertical axis is η, and the horizontal axis is β. When Equation 1 is plotted, β is the intercept of the straight line on the vertical axis. That is, when the slurry viscosity η is the same, the larger the β value, the higher the capacity loss rate C. L The larger the value of . Therefore, for two different positive electrode material preparation processes (the first positive electrode material preparation process and the second positive electrode material preparation process), linear fitting obtains equation 1, and compares the first correction coefficient β1 and the second correction coefficient β2. If the first correction coefficient β1>

[0095] The second correction coefficient β2 means that the improvement of the storage performance by the first cathode material preparation process is less than that by the second cathode material preparation process (that is, the second cathode material preparation process has a lower capacity loss rate C at the same slurry viscosity). L ),vice versa.

[0096] The anaerobic digestion additive provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments:

[0097] Example 1

[0098] The method for evaluating the viscosity and storage performance of the positive electrode material slurry of this embodiment includes the following steps:

[0099] A plurality of positive electrode materials to be evaluated, conductive agents and binders were homogenized at a mass ratio of (94.5:2:1:2.5), wherein the molecular formulas of the plurality of positive electrode materials to be evaluated were

[0100] LiNi 0.69 Co 0.07 Mn 0.23 Zr 0.005 Sr 0.001 Al 0.002 W 0.002 O2 was prepared using the following method:

[0101] Ni 0.7 Co 0.07 Mn 0.23 After (OH)2 is mixed with LiOH, Zr(OH)4, SrO, Al(OH)3, and WO3, the first sintering treatment is carried out at 975°C. After crushing, 1400ppm LiOH and 12000ppm CoOOH are added and mixed based on the total mass of the crushed materials. The second sintering treatment is then carried out at 650, 680, 720, 750, and 800°C, respectively, to obtain a variety of positive electrode active materials.

[0102] The total molar content of metal elements in the cathode material precursor (i.e. Ni 0.7 Co 0.07 Mn 0.23 The ratio of the molar content of nickel, cobalt and manganese elements in (OH)2) to the molar content of lithium in the lithium salt (i.e. the molar content of lithium in LiOH added before the first sintering treatment) is 1:1.05.

[0103] The homogenization process is as follows:

[0104] The positive electrode material and the conductive agent are pre-dry mixed using a double planetary mixer, wherein the stirring revolution speed is 20-50rpm and the dispersion disk dispersion speed is 100-300rpm; a portion of the binder (50-70%) and N-methylpyrrolidone (NMP) are added for kneading process, and the solid content is controlled at 75-85%. First, pre-stir for 5-10 minutes, wherein the revolution speed is 10-30rpm and the dispersion speed is 200-400rpm, and then high-speed stirring is performed, the revolution speed is 20-40rpm, and the dispersion speed is 2000-4 000rpm, during which the material is hung for processing, and the stirring time is 150-200min; the remaining binder (30-50%) and NMP are added for secondary stirring, and the solid content is controlled at 65-75%. First, pre-stir for 5-10min, wherein the revolution speed is 10-30rpm, and the dispersion speed is 200-400rpm, and then high-speed stirring is performed, the revolution speed is 20-40rpm, the dispersion speed is 2000-4000rpm, and the stirring time is 150-200min. After the stirring is completed, the material is discharged to complete the homogenization process.

[0105] In the above process, the conductive agent is conductive carbon black SuperP and flake graphite KS-6, and the mass ratio of the two is conductive carbon black: flake graphite = 2:1; the adhesive is Arkema HSV900.

[0106] After homogenization, the positive electrode active slurry was obtained, and the solid content of the slurry was controlled to 65%. After the slurry temperature returned to room temperature 25° C., the slurry viscosity was recorded using a rotational viscometer with a 4# rotor at 60 rpm.

[0107] The positive electrode slurry is made into an electrode sheet, and the electrode sheet is assembled with the negative electrode sheet to obtain an electrode assembly, the electrode assembly is placed in an outer package, and an electrolyte is injected into the outer package to obtain a battery;

[0108] The negative electrode sheet includes a copper foil and a negative electrode active layer disposed on two surfaces of the copper foil, wherein the negative electrode active layer includes graphite, CMC, SP and SBR, and wherein the mass ratio of graphite, CMC, SP and SBR in the negative electrode active layer is 95.5:1.5:1:2;

[0109] The electrolyte includes LiPF6, EC, EMC, DEC and FEC. The content of LiPF6 in the electrolyte is 1M. The volume ratio of EC, EMC and DEC is 1:1:1. The mass percentage of FEC in the electrolyte is 2%.

[0110] The prepared battery was subjected to a capacity test, and the initial capacity was recorded and the battery was charged to 4.4 V. The battery was placed in a 70°C oven and stored for 28 days. After storage, the capacity test was performed again and the capacity after 28 days was recorded. The capacity loss rate = 1-capacity after 28 days / initial capacity.

[0111] The attenuation rate of the positive electrode material to be evaluated is obtained according to the slurry viscosity and the capacity loss rate after storage, see Table 1, and the linear fitting results are shown in Figure 1 ;

[0112] Table 1

[0113]

[0114] Depend on Figure 1 It can be seen that through linear fitting, the numerical relationship between capacity loss rate and slurry viscosity can be obtained as C L =0.2246η / 10000+0.009, so the attenuation coefficient γ is 0.2246 and the correction coefficient β is 0.009. Based on the above results, we predict the storage performance at a sintering temperature of 780°C. Specifically, when the sintering temperature is 780°C, the measured slurry viscosity is 3054mPa·s. Substituting the slurry viscosity into Figure 1 The numerical relationship obtained is that the 28D capacity loss rate predicted by the attenuation coefficient is 7.75%. The actual 28D capacity loss rate test of the battery made of the slurry is carried out, and the actual 28D capacity loss rate is 7.94%, which is 2.45% different (calculated based on the actual capacity loss rate). The above results are recorded in Table 2. It can be seen from Table 2 that the predicted results are almost the same as the actual test results, and the trends are consistent.

[0115] Table 2

[0116]

[0117] Example 2

[0118] This embodiment is basically the same as Embodiment 1, except that the preparation method of the positive electrode material to be evaluated is different from that in Embodiment 1, and specifically includes:

[0119] The amount of CoOOH added was 4000, 6000, 8000, 10000, and 12000 ppm, the amount of LiOH added was 1400 ppm, and the temperature of the second sintering treatment was 750°C;

[0120] The relevant results are shown in Table 3, and the linear fitting results are shown in Figure 2 ;

[0121] Table 3

[0122]

[0123] Depend on Figure 2 It can be seen that through linear fitting, the numerical relationship between capacity loss rate and slurry viscosity can be obtained as C L=0.3681η / 10000-0.036, so the attenuation coefficient γ is 0.3681 and the correction coefficient β is -0.036. Based on the above results, we predict the storage performance of the bis-calcined coating of 4000ppm. Specifically, when the bis-calcined coating is 4000ppm, the measured slurry viscosity is 2286mPa·s. Substituting the slurry viscosity into Figure 2 The numerical relationship obtained is that the 28D capacity loss rate predicted by the attenuation coefficient is 4.81%. The actual 28D capacity loss rate test of the battery made of the slurry is carried out, and the actual 28D capacity loss rate is 5.07%, which is 5.41% different (calculated based on the actual capacity loss rate). The above results are recorded in Table 4. It can be seen from Table 4 that the predicted results are almost the same as the actual test results and are consistent with the trend.

[0124] Table 4

[0125]

[0126] Example 3

[0127] This embodiment is basically the same as Embodiment 1, except that the preparation method of the positive electrode material to be evaluated is different from that in Embodiment 1, and specifically includes:

[0128] The primary sintering temperatures were 900, 920, 940, 960, 975, and 990°C, the amount of CoOOH added was 12000ppm, the amount of LiOH added was 1400ppm, and the temperature of the second sintering treatment was 750°C;

[0129] The relevant results are shown in Table 5, and the linear fitting results are shown in Figure 3 .

[0130] Table 5

[0131]

[0132] Depend on Figure 3 It can be seen that through linear fitting, the numerical relationship between capacity loss rate and slurry viscosity can be obtained as C L =0.269η / 10000-0.0017, so the attenuation coefficient γ is 0.269 and the correction coefficient β is -0.0017. Based on the above results, we predict the storage performance of the primary sintering temperature of 950℃. Specifically, when the primary sintering temperature is 950℃, the measured slurry viscosity is 3751mPa·s. Substituting the slurry viscosity into Figure 3The numerical relationship obtained is that the 28D capacity loss rate predicted by the attenuation coefficient is 9.92%. The actual 28D capacity loss rate test of the battery made of the slurry is carried out, and the actual 28D capacity loss rate is 10.01%, which differs by 0.91% (calculated based on the actual capacity loss rate). The above results are recorded in Table 6. As can be seen from Table 6, it can be seen that the predicted results are almost the same as the actual test results, and are consistent with the trend.

[0133] Table 6

[0134]

[0135] It can be seen from Examples 1, 2, and 3 that by comparing the change in slurry viscosity with the storage capacity loss rate, it is shown that there is a correlation between slurry viscosity and storage performance. When the secondary sintering coating amount is adjusted, the attenuation coefficient γ is the largest and the correction coefficient β is the most negative, indicating that the process adjustment has the most obvious impact and improvement effect on storage performance.

[0136] Example 4

[0137] This embodiment is basically the same as Embodiment 1, except that the preparation method of the positive electrode material to be evaluated is different from that in Embodiment 1, and specifically includes:

[0138] The secondary sintering additive was replaced by Co(OH)2 from CoOOH, and the addition amount was 8000, 10000, 12000 ppm, respectively. The addition amount of LiOH was 1400 ppm. The temperature of the second sintering treatment was 750°C.

[0139] The relevant results are shown in Table 7, and the linear fitting results are shown in Figure 4 .

[0140] Table 7

[0141]

[0142] Depend on Figure 4 It can be seen that through linear fitting, the numerical relationship between capacity loss rate and slurry viscosity can be obtained as C L =0.3728η / 10000-0.091, so the attenuation coefficient γ is 0.3728 and the correction coefficient β is -0.091.

[0143] It can be seen that after changing the coating additive of the secondary sintering to Co(OH)2, it has a more obvious effect on the storage performance compared to CoOOH at similar slurry viscosity (in Example 1, the correction coefficient β is 0.009; in this embodiment, the correction coefficient β is -0.091, that is, the implementation conditions of this embodiment have a smaller capacity loss rate at the same slurry viscosity).

[0144] In order to further verify the predictive effect of the attenuation coefficient γ on the storage test, this example predicts the storage performance when the Co(OH)2 secondary sintering coating amount is 4000ppm. Specifically, when the Co(OH)2 secondary sintering coating amount is 4000ppm, the measured slurry viscosity is 4143mPa·s. Substituting the slurry viscosity into Figure 4 The numerical relationship obtained is that the 28D capacity loss rate predicted by the attenuation coefficient is 6.34%. The actual 28D capacity loss rate test of the battery made of the slurry is carried out, and the actual 28D capacity loss rate is 6.17%, which is 2.68% different (calculated based on the actual capacity loss rate). The above results are recorded in Table 8. It can be seen from Table 8 that the predicted results are almost the same as the actual test results and are consistent with the trend.

[0145] Table 8

[0146]

[0147] From the above content, it can be seen that the method for predicting the storage performance of the positive electrode material provided by the present invention can not only quickly predict the subsequent storage results through the viscosity test after the front-end homogenization process, but also summarize the differences in the effects of different synthesis processes on the capacity loss rate and the improvement of storage performance, playing a dual role.

[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some or all of the technical features can be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.

Claims

1. A method for predicting the storage performance of a positive electrode material, characterized in that: The following steps are involved: 1) Using N kinds of positive electrode materials, N kinds of slurries are prepared respectively by the same homogenization method; 2) testing the viscosities of the N slurries respectively to obtain N slurry viscosities η; 3) The N kinds of slurries are made into batteries respectively, and the battery capacity loss rate is tested respectively to obtain N capacity loss rates C L ; 4) According to the N slurry viscosities η and the N capacity loss rates C L , the capacity loss rate C is obtained by linear fitting method. L and the numerical relationship between the slurry viscosity η; 5) According to the numerical relationship, the capacity loss rate C is calculated using the slurry viscosity η L ; N>1。 2. The method according to claim 1, characterized in that In step 4), according to the N slurry viscosities η and the N capacity loss rates C L , through the linear fitting method, the numerical relationship described in formula 1 is obtained: C L =γ×η / 10000+β Formula 1; in: C L is the capacity loss rate, %; η is the slurry viscosity, mPa·s; γ is the attenuation coefficient; β is the correction coefficient; Step 5) includes measuring the slurry viscosity η and calculating the capacity loss rate C according to formula 1 L .

3. The method according to claim 1 or 2, characterized in that: The N slurries have the same solid content; and / or, The solid content of the N slurries is 65-75%.

4. The method according to any one of claims 1 to 3, characterized in that The homogenization method comprises mixing the positive electrode material with a conductive agent and a binder to obtain the slurry; The conductive agent is selected from at least one of conductive carbon black SuperP, Ketjen black KB, vapor-grown carbon fiber VGCF, carbon nanotube CNT, and flake graphite KS series materials; The adhesive is selected from at least one of Arkema HSV900, Arkema HSV1800, Solvay 5130 and Solvay 6020.

5. The method according to any one of claims 1 to 4, characterized in that In step 2), the viscosity test method comprises testing the viscosity of the slurry at a temperature of 20-30° C. at a rotation speed of 40-80 rpm.

6. The method according to any one of claims 1 to 5, characterized in that In step 3), the battery capacity loss rate test also includes recording the initial capacity of the battery and then charging it to 4.3-4.5V, storing it in an environment of 40-70°C for 28-70 days and then performing a capacity test again to obtain the capacity loss rate.

7. The method according to any one of claims 1 to 6, characterized in that The battery comprises a negative electrode sheet and an electrolyte; The negative electrode sheet comprises a copper foil and a negative electrode active layer arranged on two surfaces of the copper foil, wherein the negative electrode active layer comprises a negative electrode material, a conductive agent and an adhesive; The negative electrode material is selected from at least one of graphite, silicon-carbon negative electrode material, and silicon-oxygen negative electrode material; The conductive agent is selected from at least one of SP, CNT, and KS conductive graphite; The adhesive is selected from at least one of PAA, SBR and CMC; The electrolyte is selected from at least one of LiPF6, EC, EMC, DEC, and FEC.

8. The method according to claim 7, characterized in that The mass ratio of the negative electrode material, the conductive agent and the adhesive is (93-97): (1.5-3.5): (1.5-3.5).

9. The method according to any one of claims 1 to 8, characterized in that It also includes evaluating the differences in the effects of N cathode material preparation processes on capacity loss rate based on N attenuation coefficients, including: The first attenuation coefficient γ1> the second attenuation coefficient γ2, then the influence of the first positive electrode material preparation process on the capacity loss rate is greater than the influence of the second positive electrode material preparation process on the capacity loss rate; Among them, the first positive electrode material preparation process and the second positive electrode material preparation process are any two of N different positive electrode material preparation processes, and the first attenuation coefficient γ1 is the attenuation coefficient of the first positive electrode material preparation process, and the second attenuation coefficient γ2 is the attenuation coefficient of the second positive electrode material preparation process.

10. The method according to any one of claims 1 to 9, characterized in that It also includes evaluating the differences in storage performance improvement of N cathode material preparation processes according to N correction factors, including: The first correction coefficient β1> the second correction coefficient β2, then the improvement of the storage performance by the first positive electrode material preparation process is less than the improvement of the storage performance by the second positive electrode material preparation process; Among them, the first positive electrode material preparation process and the second positive electrode material preparation process are any two of N different positive electrode material preparation processes, and the first correction coefficient β1 is the correction coefficient of the first positive electrode material preparation process, and the second correction coefficient β2 is the correction coefficient of the second positive electrode material preparation process.