Analysis method for DCR growth of battery

By identifying the source of DCR growth in lithium-ion batteries through contact and interface resistance testing, followed by button cell preparation, the method addresses inefficiencies in existing DCR analysis, enabling targeted electrode modifications for improved battery performance.

CN119087260APending Publication Date: 2024-12-06EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187206.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Current methods for analyzing Direct Current Resistance (DCR) growth in lithium-ion batteries are time-consuming, energy-intensive, and costly, as they require modifying positive or negative electrode materials blindly without identifying the source of DCR growth, leading to inefficient battery performance optimization.

Method used

A method to quickly identify whether DCR growth originates from the positive or negative electrode by testing contact resistance and interface reaction polarization internal resistance, followed by disassembling batteries to prepare button cells for resistance testing, allowing targeted modifications based on the source of DCR increase.

Benefits of technology

This method reduces analysis time, improves production efficiency, and enables targeted improvements to the positive or negative electrode, optimizing battery performance effectively and economically.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087260A_ABST
    Figure CN119087260A_ABST
Patent Text Reader

Abstract

The invention provides an analysis method for DCR growth of a battery, which can quickly identify whether DCR growth of the battery is from a positive electrode or a negative electrode, can specifically modify specific aspects of the positive electrode or the negative electrode according to an identification result, effectively solves the problem that the DCR growth source of the battery is difficult to distinguish and analyze, and is convenient to operate, high in applicability and easy to popularize. The battery circulation DCR analysis time is greatly shortened, the production efficiency is improved, and the method has positive significance in the actual battery production and modification process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to a method for analyzing the DCR growth of a battery. Background Art

[0002] Lithium-ion battery cycle failure is divided into irreversible capacity loss and reversible capacity loss. Irreversible capacity loss comes from the loss of positive and negative electrode materials, which leads to the loss of battery capacity and cannot be restored by a small current. Reversible capacity loss comes from the increase in polarization of the battery itself, and the quantitative parameter is the increase in DCR (direct current resistance). The increase in reversible capacity loss DCR mainly occurs during the cycle process. When the current density increases, the ability of active substances in the electrolyte to participate in the reaction decreases, the electrochemical reaction rate decreases, and the reaction of the electrolyte inside the lithium-ion battery intensifies, resulting in side reactions. The side reactions accumulate on the surface of the positive and negative electrodes, affecting ion transmission, which is ultimately manifested as an increase in DCR.

[0003] Generally speaking, in the composition of the battery, the positive electrode active material and the negative electrode active material are the main reasons affecting the battery performance. Therefore, when facing the above problems, current technicians will directly modify the positive electrode active material or the negative electrode active material, that is, before identifying whether the positive electrode or the negative electrode causes the DCR growth, they will blindly modify the positive electrode active material or the negative electrode active material. For example, the ternary main material is directly doped and coated to improve the stability of the grain boundary of the positive electrode active material, reduce the collapse of the lattice between the metal layers, and reduce the interface reaction. Or the negative electrode main material is directly optimized, such as adjusting the coating method of the silicon-carbon negative electrode. When there is no suitable method to analyze the source of DCR growth, the positive electrode active material or the negative electrode active material is modified by trial and error. Different modified materials need to be matched to form a full battery test, and the DCR growth can only be tested after the finished battery is formed and offline. This traditional DCR growth test method is time-consuming, energy-intensive, and costly. It takes a long time to occupy the test equipment, and the material cost, labor cost, and time cost are high, which invisibly increases the equipment cost.

[0004] In view of this, it is urgent to study a method to quickly analyze the growth of battery cycle DCR, so as to carry out targeted modification of the positive or negative electrode of the battery, effectively optimize the battery performance in a short time, and improve production efficiency. Summary of the invention

[0005] In order to solve the problems and shortcomings in the prior art, the present invention provides a method for analyzing the growth of battery DCR. The method can quickly identify whether the growth of battery DCR comes from the positive electrode or the negative electrode, and can modify specific aspects of the positive electrode or the negative electrode in a targeted manner according to the identification result, effectively solving the problem that the source of battery DCR growth is difficult to distinguish and analyze. The method is easy to operate and has strong applicability, greatly reduces the battery cycle DCR analysis time, improves production efficiency, and has positive significance in actual battery production and modification processes.

[0006] The present invention provides a method for analyzing the DCR growth of a battery, comprising the following steps: S1. testing the contact resistance R10 and the interface reaction polarization internal resistance R1 of the uncirculated battery according to the DCR decomposition process. ct , the contact resistance R20 and interface reaction polarization internal resistance R2 of the cycle failure battery are tested according to the DCR decomposition process. ct ; S2. Calculate the contact resistance change difference ΔR0 = R20-R10, the interface reaction polarization internal resistance change difference ΔR ct =R2 ct -R1 ct , compare ΔR0 with ΔR ct Size, determine whether the increase in battery DCR comes from ΔR0 or ΔR ct ; S3. Disassemble the uncirculated battery after the DCR decomposition process to obtain the first positive electrode sheet and the first negative electrode sheet; at the same time, disassemble the cycle-failed battery after the DCR decomposition process to obtain the second positive electrode sheet and the second negative electrode sheet; S4. Prepare the first button battery, the second button battery, the third button battery, and the fourth button battery with the first positive electrode sheet, the first negative electrode sheet, the second positive electrode sheet, and the second negative electrode sheet, respectively, and use the resistance test program to test the resistance r1 of the first button battery, the resistance r2 of the second button battery, the resistance r3 of the third button battery, and the resistance r4 of the fourth button battery respectively; S5. Calculate the positive electrode resistance change difference Δr p =r3-r1, negative electrode resistance change difference Δr n =r4-r2, compare Δr p With Δr n Size, judge whether the increase of battery DCR comes from the positive electrode or the negative electrode; S6. Combining the results of S2 and S5, when ΔR0>ΔR ct , and Δr p >Δr n , then it is determined that the source of battery DCR growth is the positive electrode contact resistance R 0(p) ; When ΔR0<ΔR ct , and Δr p >Δr n , then it is determined that the source of the battery DCR increase is the positive electrode interface reaction polarization internal resistance R ct(p) ; When ΔR0>ΔR ct , and Δrp <Δr n , then it is determined that the source of the battery DCR increase is the negative electrode contact resistance R 0(n) ; When ΔR0<ΔR ct , and Δr p <Δr n , then it is determined that the source of the battery DCR increase is the negative electrode interface reaction polarization internal resistance R ct(n) During the battery cycle, the internal resistance will increase due to side reactions, material system damage, etc. The degree of increase can be characterized by the increase of DCR, where the increase of DCR includes the increase of ohmic internal resistance (R0), interface reaction polarization internal resistance (R ct ), concentration polarization internal resistance. Since concentration polarization internal resistance does not play a dominant role in energy-type batteries, the present invention only analyzes the growth of these two types of internal resistances, ohmic internal resistance and interface reaction polarization internal resistance, during the battery cycle. Among them, ohmic resistance, also called contact internal resistance, is composed of electrode materials, electrolytes, diaphragm resistance and contact resistance of various parts. Interface reaction polarization internal resistance is related to the electrode-electrolyte interface; it is related to the state of the electrode and the interface of the electrode.

[0007] The design idea of ​​the present invention is to first test the ohmic resistance and interface reaction polarization internal resistance of the uncirculated battery and the cycled failed battery respectively. By comparing the ohmic resistance of the uncirculated battery and the cycled failed battery, and comparing the interface reaction polarization resistance of the uncirculated battery and the cycled failed battery, it can be preliminarily determined whether the increase in DCR during the battery cycle comes from the ohmic resistance or the interface reaction polarization resistance. Then, the uncirculated battery and the cycled failed battery are disassembled, and the positive and negative electrode sheets obtained are used to prepare button batteries, and then the resistance of the button batteries is tested, and this resistance is also the DCR of the button batteries. Because button batteries can be used to test the material properties of the positive or negative electrode, therefore, by using the positive and negative electrode sheets after disassembly of the uncirculated battery and the cycled failed battery to prepare button batteries, and then testing the resistance of these button batteries respectively and comparing the sizes, it can be known whether the increase in DCR of the whole battery comes from the positive electrode or the negative electrode. Finally, combining the above two evaluation results (S2 and S5), it can be further determined that the increase in battery DCR comes from the positive electrode contact resistance R 0(p) , or the positive electrode interface reaction polarization internal resistance R ct(p) , or negative contact resistance R 0(n) , or the negative electrode interface reaction polarization internal resistance R ct(n) In these cases, further targeted improvements can be made to the positive or negative electrode based on the judgment results.

[0008] Generally speaking, if it is determined that the increase in DCR comes from the positive electrode contact resistance R 0(p), improvements can be made in the following aspects: (1) improving the adhesion of the positive electrode sheet and reducing the contact impedance between the positive electrode main material and the foil; (2) optimizing the foil, such as using carbon-coated aluminum foil, which can greatly reduce the contact resistance between the positive / negative electrode material and the current collector and improve the adhesion between the two.

[0009] If it is determined that the increase in DCR comes from the positive electrode interface reaction polarization internal resistance R ct(p) , improvements can be made in the following aspects: (1) improving the stability of the positive electrode main material, such as doping and coating the positive electrode main material; (2) improving the positive electrode interface stability, such as optimizing the electrolyte to form a more stable CEI film.

[0010] If it is determined that the increase in DCR comes from the negative electrode contact resistance R 0(n) , improvements can be made from the following aspects: improving the bonding strength of the negative electrode, such as replacing it with a binder with strong bonding properties.

[0011] If it is determined that the increase in DCR comes from the negative electrode interface reaction polarization internal resistance R ct(n) , improvements can be made from the following aspects: (1) Modification of the negative electrode main material to improve the structural stability of the negative electrode main material, such as fluorination of the graphite surface to form a C-F structure on the graphite surface, which can effectively improve the structural stability of graphite; coating of graphite to improve the structural stability of graphite; (2) Improving the negative electrode interface stability, such as optimizing the electrolyte to form a more stable SEI film.

[0012] It should be noted that the above improvement methods can be adjusted and optimized according to actual conditions. It should also be noted that the above cycle failure battery cycle does not meet the capacity retention rate standard, which is shown as below the standard line and cycle "diving". Below the standard line here means that the capacity retention rate can be referenced. Figure 3 , Figure 3 This is an example of a relevant curve for a battery with a cycle below the standard line; for cycle "diving", please refer to Figure 4 , Figure 4 An example of a relevant curve for a cycle diving battery; Figure 2 This is an example of a relevant curve for a battery with qualified cycles, which can be used for comparative reference.

[0013] From the above analysis, it can be seen that the battery DCR analysis method provided by the present invention can quickly and clearly identify the source of DCR growth, so that further optimization directions can be quickly and targeted, thereby quickly improving the problem of battery DCR growth and further optimizing the electrochemical performance of the battery. It has important guiding significance for battery product optimization and can be optimized in combination with different battery designs.

[0014] When facing the problem of battery failure caused by the increase of battery DCR, because the increase of DCR involves the design of the entire battery, including the positive electrode sheet, the negative electrode sheet, and the electrolyte, there is no effective analysis method in the prior art, and it is difficult to find the source that really causes the increase of battery DCR. Therefore, the traditional improvement method is to directly improve the positive electrode material or the negative electrode material, that is, only the trial method can be adopted to improve the material. Moreover, this traditional method requires different modified materials to be matched to form a full battery test, and it is necessary to wait until the finished battery is formed and offline before the growth of DCR can be tested, which is time-consuming, energy-intensive, and costly. Therefore, compared with the traditional method, the DCR growth analysis method provided by the present invention is time-consuming, energy-intensive, and cost-effective, and has more economic and practical significance.

[0015] Preferably, in S4, the resistance test procedure of the first button battery or the third button battery includes the following steps: S51. Charge to 4.10-4.25V at a constant current of 0.15-0.25C, and stop charging; S52. Let stand for 4-6 minutes; S53. Discharge to 2.4-2.6V at a constant current of 0.15-0.25C, and stop discharging; S54. Let stand for 4-6 minutes; S55. Repeat S51-S53 twice; S56. Let stand for 8-12 minutes. in; S57. Charge at a constant current of 0.15-0.25C to 4.10-4.25V, stop charging; S58. Stand for 4-6min; S59. Discharge at a constant current of 1.4C-1.6C for 28-32s; S510. Stand for 1.8-2.2h; The calculation method of the resistance r1 or r3 of the first button battery or the third button battery is: r1 or r3 = (pre-discharge voltage in S59 - post-discharge voltage in S59) / discharge current in S59;

[0016] The resistance test procedure of the second button cell or the fourth button cell includes the following steps: S51′. Discharge at a constant current of 0.05-0.15C to 4-6mV, and stop discharging; S52′. Let stand for 13-17min; S53′. Charge at a constant current of 0.05-0.15C to 1.4-1.6V, and stop charging; S54′. Let stand for 13-17min; S55′. Repeat S51′-S53′ twice; S56′. Let stand for 8-12min; S57′. Discharge at a constant current of 1.4C-1.6C for 28-32s; S58′. Let stand for 1.8-2.2h; The calculation method of the resistance R2 or R4 of the second button cell or the fourth button cell is: R2 or R4 = (voltage before discharge in S57′-voltage after discharge in S57′) / discharge current in S57′.

[0017] The DCR of the whole battery is tested in a pulse discharge mode. The button battery can also be tested in this way. Generally, the button battery is tested at a current of 0.2C. Then we use a large current of 1.5C to discharge. After standing still, the voltage will rebound obviously. The rebound voltage value is divided by the current to get the DCR value of the button battery (r1, r2, r3, r4). If we set it to 0.2C current for testing, the trend is not obvious. Polarization is easy to show under large current. The polarization quantification parameter is the DCR value. Therefore, the present invention can effectively test and obtain the DCR value of the button battery by discharging with a larger current.

[0018] Among them, in the first button cell or the third button cell, these two button cells are prepared based on the positive electrode sheets disassembled from the uncycled battery and the cycle-failed battery. In S51, charging is first performed to ensure that the lithium in the positive electrode material runs to the metallic lithium to prepare for discharge; in S52, standing for a certain time is to reduce the polarization voltage and avoid measurement errors caused by polarization; in S53, discharging is performed with a small current to ensure that the battery is fully activated; in S54, standing for a certain time is to reduce the polarization voltage and avoid measurement errors caused by polarization; in S55, cycling twice is to ensure that the prepared button cell has no leakage voltage and other problems; in S56, standing for a certain time is to reduce the polarization voltage and avoid measurement errors caused by polarization; in S57, it is a normal charging step; in S58, standing for a certain time is to reduce the polarization voltage and avoid measurement errors caused by polarization; in S59, charging with a large current can observe obvious polarization, so it can be used to calculate the resistance value (DCR); S590 is a normal standing step, and it is retrieved after standing. In the second button cell or the fourth button cell, these two button cells are prepared based on the negative electrode sheets disassembled from uncycled batteries and cycle-failed batteries. The discharge in S51′ is to replenish lithium to the negative electrode in preparation for subsequent tests; the standing time in S52′ is to reduce the polarization voltage and avoid measurement errors caused by polarization; the discharge with a small current in S53′ ensures that the battery is fully activated; the standing time in S54′ is to reduce the polarization voltage and avoid measurement errors caused by polarization; the cycle in S55′ is repeated twice to ensure that the prepared button cell has no leakage voltage or other problems; the standing time in S56′ is to reduce the polarization voltage and avoid measurement errors caused by polarization; in S57′, obvious polarization can be observed by charging with a large current, so it can be used to calculate the resistance value (DCR); S58′ is a normal standing step, and it is retrieved after standing.

[0019] In short, steps S51 to S55 (or S51′ to S55′) are activation steps for button cells, ensuring that the prepared button cells are problem-free and can be charged and discharged well. Steps S57 to S510 (or S57′ to S58′) are resistance test steps, which are key steps. The button cells are discharged with a large current. Under the condition of large current discharge, the voltage drop of batteries with large resistance values ​​is large, and the voltage of batteries with small resistance values ​​is reduced. The resistance value of the button cell can be obtained according to this step. The discharge time and discharge current are crucial. The discharge current and discharge time can be appropriately adjusted for batteries of different capacities. After the above steps are tested, the resistance of the button cell can be tested more accurately, so it can be more accurately judged whether the DCR increase of the whole battery comes from the positive electrode or the negative electrode, which provides a basis for further analysis of the source of battery DCR increase.

[0020] Preferably, in S4, the resistance test procedure of the first button battery or the second button battery includes the following steps: S51. charging to 4.25V at a constant current of 0.2C, and stopping charging; S52. standing for 5 minutes; S53. discharging to 2.5V at a constant current of 0.2C, and stopping discharging; S54. standing for 5 minutes; S55. repeating S51 to S53 twice; S56. standing for 10 minutes; S57. charging to 4.25V at a constant current of 0.2C, and stopping charging; S58. standing for 5 minutes; S59. discharging at a constant current of 1.5C for 30 seconds; S510. standing for 2 hours;

[0021] The resistance test procedure of the second button cell or the fourth button cell includes the following steps: S51′. Discharge at a constant current of 0.1C to 5mV, and stop discharging; S52′. Let stand for 15min; S53′. Charge at a constant current of 0.1C to 1.5V, and stop charging; S54′. Let stand for 15min; S55′. Repeat S51′ to S53′ twice; S56′. Let stand for 10min; S57′. Discharge at a constant current of 1.5C for 30s; S58′. Let stand for 2h.

[0022] Preferably, in S1, the DCR decomposition process comprises the following steps: S11. Discharge at a constant current of 0.15-0.25C to 2.4-2.6V, and stop discharging; S12. Stand for 8-12min; S13. First charge at a constant current of 0.9-1.1C to 4.10-4.25V, then charge at a constant voltage of 4.10-4.25V to a current of 0.09-0.11A, and stop charging; S14. Stand for 55-65min; S15. Discharge at a constant current of 0.9-1.1C to a battery capacity of 88-92%; S16. Stand for 1.8-2.2h; S17 .Discharge at a constant current of 1 to 1.5C for 9 to 11 seconds, then stop discharging; S18. Stand for 38 to 42 seconds; S19. Charge at a constant current of 1 to 1.5C for 9 to 11 seconds, then stop charging; S110. Stand for 38 to 42 seconds; S111. Repeat S15 to S110 until the voltage is 2.4 to 2.6V; The contact resistance of an uncirculated battery or a cycle-failed battery is R10 or R20 = V1 / ΔI1, where ΔV1 is the discharge start voltage in S17 minus the voltage after S16 is stationary, and I1 is the current value of S17; The interface reaction polarization internal resistance R1 of an uncirculated battery or a cycle-failed battery ct or R2 ct =ΔV2 / I1, ΔV2 is the difference between the voltage at the 1st second and the voltage at the 3rd second of the discharge start in S17, and I1 is the current value of S17. After the above steps of testing, the ohmic resistance and interface reaction polarization internal resistance of the uncycled battery and the cycle-failed battery can be tested more accurately, and then it can be more accurately judged that the DCR growth of the whole battery comes from the ohmic resistance and interface reaction polarization internal resistance, which provides a basis for further analysis of the source of battery DCR growth.

[0023] Preferably, in S1, the DCR decomposition process comprises the following steps: S11. Discharge the battery at a constant current of 0.2C to 2.5V, and stop discharging; S12. Let stand for 10 minutes; S13. First charge at a constant current of 1C to 4.2V, then charge at a constant voltage of 4.2V to a current of 0.1A, and stop charging; S14. Let stand for 60 minutes; S15. Discharge at a constant current of 1C to 90% of the battery capacity; S16. Let stand for 2 hours; S17. Discharge at a constant current of 1C for 10s, and stop discharging; S18. Let stand for 40s; S19. Charge at a constant current of 1C for 10s, and stop charging; S110. Let stand for 40s; S111. Repeat S15 to S110 until the voltage is 2.5V.

[0024] Preferably, in the first positive electrode sheet or the second positive electrode sheet, the positive electrode active material includes at least one of a lithium cobalt oxide positive electrode material, a lithium manganate positive electrode material, a nickel cobalt manganate positive electrode material, a nickel cobalt aluminum oxide positive electrode material, a lithium iron phosphate positive electrode material, and a lithium manganese iron phosphate positive electrode material. The battery cycle DCR growth analysis method provided by the present invention is applicable to a variety of positive electrode active materials, and can effectively analyze the source of DCR growth for batteries prepared using these active materials, so as to quickly and accurately optimize battery performance in a targeted manner.

[0025] Preferably, the positive electrode active material includes at least one of a nickel cobalt manganese oxide positive electrode material, a lithium iron phosphate positive electrode material, and a lithium iron manganese phosphate positive electrode material. For the above-mentioned several positive electrode active materials that are commonly used in the market, the battery DCR growth analysis method provided by the present invention has greater adaptability, and therefore has very important guiding significance for solving the DCR growth problem in the current lithium battery field.

[0026] Preferably, in the first negative electrode sheet or the second negative electrode sheet, the negative electrode active material includes at least one of a graphite negative electrode material, a graphene negative electrode material, a disordered carbon negative electrode material, a silicon-based negative electrode material, and a lithium titanate negative electrode material; the graphite negative electrode material includes at least one of natural graphite, artificial graphite, composite graphite, and mesophase carbon microspheres; the disordered carbon negative electrode material includes at least one of hard carbon and soft carbon; the silicon-based negative electrode material includes at least one of a silicon-oxygen negative electrode material, a silicon-carbon negative electrode material, and a silicon-based alloy negative electrode material. The battery DCR growth analysis method provided by the present invention is applicable to a variety of negative electrode active materials, and can effectively analyze the source of DCR growth for batteries prepared using these active materials, so as to quickly and accurately optimize battery performance in a targeted manner.

[0027] Preferably, the negative electrode active material includes at least one of natural graphite, artificial graphite, composite graphite, silicon-oxygen negative electrode material, and silicon-carbon negative electrode material. For the above-mentioned negative electrode active materials that are commonly used in the market, the battery DCR growth analysis method provided by the present invention has greater adaptability, and therefore has very important guiding significance for solving the DCR growth problem in the current lithium battery field.

[0028] Preferably, in the first button cell or the third button cell, the lithium sheet is used as the negative electrode of the first button cell or the third button cell; in the second button cell or the fourth button cell, the lithium sheet is used as the positive electrode of the second button cell or the fourth button cell. When the button cells are subjected to relevant performance tests, the button cells prepared with the above materials can well reflect the performance of the positive electrode or negative electrode in the full battery (uncycled battery, cycle-failed battery). Therefore, the resistance of the tested button cell can well reflect the resistance of the positive electrode or negative electrode, and the DCR increase of the full battery can be more accurately judged whether it comes from the positive electrode or the negative electrode according to the resistance of the button cell test, which lays a good foundation for the next step of analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The contact resistance R10 and R20 of the uncycled battery and the cycle-failed battery in Example 1, and the interface reaction polarization internal resistance R1 ct , R2 ct The test curve.

[0030] Figure 2 is an example of a relevant curve for a battery that has passed the cycle test.

[0031] Figure 3 is an example of a relevant curve for a battery that cycles below the standard line.

[0032] Figure 4 is an example of a relevant curve for a cycle diving battery. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0034] Example 1

[0035] In this embodiment, the uncirculated battery and the cycle-failed battery are a certain type of battery with a capacity of 2600maAh, the main material of the positive electrode is NCM (NCM811), and the mass ratio of each raw material of the positive electrode active material layer in the positive electrode sheet is NCM (NCM811): carbon nanotube CNT (conductive agent): polyvinylidene fluoride PVDF (binder) = 97:2:1. The main material of the negative electrode is graphite, and the mass ratio of each raw material of the negative electrode active material layer in the negative electrode sheet is graphite: conductive carbon black SP (conductive agent): styrene butadiene rubber SBR (binder) = 97:1:2.

[0036] Follow the steps below to analyze the battery DCR growth:

[0037] S1. Test the contact resistance R10 and interface reaction polarization internal resistance R1 of the uncycled battery according to the DCR decomposition process ct , the contact resistance R20 and interface reaction polarization internal resistance R2 of the cycle failure battery are tested according to the DCR decomposition process. ct ; The DCR decomposition process includes the following steps:

[0038] S11. Discharge the battery at a constant current of 0.2C to 2.5V, and stop discharging;

[0039] S12. Let stand for 10 min;

[0040] S13. First charge at a constant current of 1C to 4.2V, then charge at a constant voltage of 4.2V to a current of 0.1A, and stop charging;

[0041] S14. Let stand for 60 min;

[0042] S15. Discharge at a constant current of 1C until the battery capacity is 90%;

[0043] S16. Let stand for 2 hours;

[0044] S17. Discharge at a constant current of 1C for 10s, and then stop discharging;

[0045] S18. Let stand for 40 seconds;

[0046] S19. Charge at a constant current of 1C for 10s, then stop charging;

[0047] S110. Let stand for 40 seconds;

[0048] S111. Repeat S15 to S110 until the voltage reaches 2.5V;

[0049] The contact resistance of an uncycled battery or a cycle-failed battery is R10 or R20 = ΔV1 / I1, where ΔV1 is the discharge start voltage in S17 minus the voltage after S16 is stationary, and I1 is the current value of S17;

[0050] Interface reaction polarization internal resistance R1 of uncycled battery or cycle-failed battery ct or R2 ct =ΔV2 / I1, ΔV2 is the difference between the voltage at the 1st second and the voltage at the 3rd second of the discharge start in S17, and I1 is the current in S17;

[0051] S2. Calculate the contact resistance change difference ΔR0 = R20-R10, the interface reaction polarization internal resistance change difference ΔR ct =R2 ct -R1 ct , compare ΔR0 with ΔR ct Size, determine whether the increase in battery DCR comes from ΔR0 or ΔR ct ;

[0052] S3. Disassemble the uncirculated battery after the DCR decomposition process to obtain a first positive electrode sheet and a first negative electrode sheet; at the same time, disassemble the cycle-failed battery after the DCR decomposition process to obtain a second positive electrode sheet and a second negative electrode sheet;

[0053] S4. Prepare a first button cell, a second button cell, a third button cell, and a fourth button cell using the first positive electrode sheet, the first negative electrode sheet, the second positive electrode sheet, and the second negative electrode sheet, respectively, and use a resistance test program to test the resistance r1 of the first button cell, the resistance r2 of the second button cell, the resistance r3 of the third button cell, and the resistance r4 of the fourth button cell;

[0054] The resistance test procedure of the first button cell or the second button cell includes the following steps:

[0055] S51. Charge at a constant current of 0.2C until the voltage reaches 4.25V, then stop charging;

[0056] S52. Let stand for 5 minutes;

[0057] S53. Discharge at a constant current of 0.2C to 2.5V, and stop discharging;

[0058] S54. Let stand for 5 minutes;

[0059] S55. Repeat S51 to S53 twice;

[0060] S56. Let stand for 10 minutes;

[0061] S57. Charge at a constant current of 0.2C until the voltage reaches 4.25V, then stop charging;

[0062] S58. Let stand for 5 minutes;

[0063] S59. Discharge at a constant current of 1.5C for 30s;

[0064] S510. Let stand for 2 hours;

[0065] The resistance r1 or r3 of the first button battery or the third button battery is calculated as follows: r1 or r3 = (pre-discharge voltage in S59 - post-discharge voltage in S59) / discharge current in S59;

[0066] The resistance test procedure of the second or fourth button cell includes the following steps:

[0067] S51 'discharge at a constant current of 0.1C to 5mV, stop discharging;

[0068] S52′. Let stand for 15 min;

[0069] S53 '. Charge to 1.5V at a constant current of 0.1C, and stop charging;

[0070] S54′. Let stand for 15 min;

[0071] S55'. Repeat S51'~S53' twice;

[0072] S56′. Let stand for 10 min;

[0073] S57′. Discharge at a constant current of 1.5C for 30s;

[0074] S58′. Let stand for 2 hours;

[0075] The resistance r2 or r4 of the second button cell or the fourth button cell is calculated as follows: r2 or r4 = (pre-discharge voltage in S57' - post-discharge voltage in S57') / discharge current in S57'.

[0076] S5. Calculate the positive electrode resistance change difference Δr p =r3-r1, negative electrode resistance change difference Δr n =r4-r2, compare Δr p With Δr n Size, to determine whether the increase in battery DCR comes from the positive electrode or the negative electrode;

[0077] S6. Combining the results of S2 and S5, it is further determined that the increase in battery DCR comes from one of the following situations: positive electrode contact resistance R 0(p) , positive electrode interface reaction polarization internal resistance R ct(p) , Negative electrode contact resistance R 0(n) , negative electrode interface reaction polarization internal resistance R ct(n) According to the judgment result, targeted improvements are made to the positive or negative electrode.

[0078] In the above test step S4, in the first button cell or the third button cell, the lithium sheet is used as the negative electrode of the first button cell or the third button cell; the specific preparation process is: wipe one side of the positive electrode with NMP (N-methylpyrrolidone), cut the original sheet with a diameter of 11 mm with an 11 mm punching machine, and assemble it according to the negative electrode shell-metal lithium sheet-diaphragm-electrolyte-pole sheet-gasket-spring sheet-positive electrode shell.

[0079] In the second button cell or the fourth button cell, a lithium sheet is used as the positive electrode of the second button cell or the fourth button cell; the specific preparation process is: wipe one side of the negative electrode with pure water, cut the original sheet with a diameter of 12 mm with a 12 mm punching machine, and assemble it according to the negative electrode shell-metal lithium sheet-diaphragm-electrolyte-pole sheet-gasket-spring sheet-positive electrode shell.

[0080] After the DCR decomposition process of S1 above, the contact resistance R10 and interface reaction polarization internal resistance R1 of the uncycled battery are calculated. ct , the contact resistance R20 and the interface reaction polarization internal resistance R2 of the cycle failure battery ct As shown in Table 1, the test contact resistance R10, R20, interface reaction polarization internal resistance R1 of the uncycled battery or cycle failure battery ct , R2 ct The test curve is as follows Figure 1 shown.

[0081] Table 1 Contact resistance and interface reaction polarization internal resistance data of uncycled batteries and cycle-failed batteries

[0082]

[0083]

[0084] As shown in Table 1, the R0 change value before and after the battery cycle is 21.1mΩ, and the R ct The change value is 39.05mΩ, where R ct The change value of is larger than that of R0, so it can be inferred that the increase of battery cycle DCR mainly comes from R ct growth.

[0085] Further, in the above S4, the test results of the resistance (DCR) of the button battery are shown in Table 2, that is, the results of r1, r2, r3, and r4 are shown in Table 2. Because the button battery is relatively small, the positive and negative electrodes after disassembly of the full battery (uncycled battery and cycle-failed battery) can be used. Through appropriate sampling and cutting, multiple button battery samples based on the positive electrode sheet or negative electrode sheet of the same full battery can be prepared. In this embodiment, for each disassembled positive and negative electrode sheet, three parallel sample button batteries are prepared, and the resistance data of the button batteries are shown in Table 2.

[0086] Table 2 Resistance data of positive and negative button cells

[0087] type Sample 1 Sample 2 Sample 3 The first button battery resistance r1, Ω 19.51 21.68 21.32 The second button battery resistance r2, Ω 69.89 70.85 69.49 The third button battery resistor r3, Ω 65.87 74.99 61.95 The fourth button battery resistor r4, Ω 73.82 74.48 72.81 <![CDATA[Δr p , that is, r3-r1, Ω]]> 46.36 53.31 40.63 <![CDATA[Δr n , that is, r4-r2, Ω]]> 3.93 3.63 3.32

[0088] It can be seen from Table 2 that after the cycle failure, the positive electrode changes by 46.8Ω compared with the uncycled positive electrode, which is 224% compared with the uncycled positive electrode; after the cycle failure, the negative electrode changes by 3.63Ω ​​compared with the uncycled negative electrode, which is 5.2% compared with the uncycled positive electrode; therefore, it can be determined that the increase in DCR comes from the increase in the positive electrode.

[0089] Furthermore, combined with the results in Table 1 and Table 2, it is judged that the DCR increase of this type of battery comes from the positive electrode interface reaction polarization internal resistance R ct(p) .

[0090] For the identified positive electrode interface reaction polarization internal resistance R ct(p) The increase in the DCR of this type of battery leads to an increase in the interface reaction polarization internal resistance and the electrode-electrolyte interface, which is related to the structural stability of the positive electrode main material. Therefore, measures are taken to optimize the positive electrode main material. The optimization of the positive electrode main material is specifically: reducing the positive electrode main material particles and matching the positive electrode main material coating.

[0091] For the optimized positive electrode main material, the battery is re-prepared with similar preparation steps as the previous uncycled battery or cycle-failed battery (that is, only the positive electrode main material is replaced with the optimized positive electrode main material, and the rest is the same), and the DCR change rate of the optimized battery is tested, and the data are shown in Table 3.

[0092] Table 3 Contact resistance and interface reaction polarization internal resistance data of uncycled batteries and cycle-failed batteries after optimization of the main positive electrode material

[0093] type Uncycled battery, mΩ Cycle failure battery, mΩ Change value, mΩ <![CDATA[R0]]> 21.55 42.1 20.55 <![CDATA[R ct ]]> 10.25 14.45 4.2

[0094] It can be seen from Table 3 that in the optimized battery, R ct The rate of change of is significantly reduced, from a change value of 39.05mΩ to 4.2mΩ, indicating that the analysis method for the increase of battery DCR provided by the present invention can quickly and clearly identify the cause of the increase of DCR, and modify specific aspects of the positive or negative electrode in a targeted manner according to the identification result. From the data results in Table 3, it can be seen that the performance of the battery is obviously and effectively optimized, indicating that the analysis method of the present invention has high accuracy and strong operability, and has important guiding significance for actual production.

[0095] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. A method for analyzing battery DCR growth, characterized in that: The steps include: S1. Test the contact resistance R10 and interface reaction polarization internal resistance R1 of the uncycled battery according to the DCR decomposition process ct , the contact resistance R20 and interface reaction polarization internal resistance R2 of the cycle failure battery are tested according to the DCR decomposition process. ct ; S2. Calculate the contact resistance change difference ΔR0 = R20-R10, the interface reaction polarization internal resistance change difference ΔR ct =R2 ct -R1 ct , compare ΔR0 with ΔR ct Size, determine whether the increase in battery DCR comes from ΔR0 or ΔR ct ; S3. dismantle the uncirculated battery after the DCR decomposition process to obtain a first positive electrode sheet and a first negative electrode sheet; and dismantle the cycle-failed battery after the DCR decomposition process to obtain a second positive electrode sheet and a second negative electrode sheet; S4. Prepare a first button battery, a second button battery, a third button battery, and a fourth button battery with the first positive electrode sheet, the first negative electrode sheet, the second positive electrode sheet, and the second negative electrode sheet, respectively, and use a resistance test program to test the resistance r1 of the first button battery, the resistance r2 of the second button battery, the resistance r3 of the third button battery, and the resistance r4 of the fourth button battery; S5. Calculate the positive electrode resistance change difference Δr p =r3-r1, negative electrode resistance change difference Δr n =r4-r2, compare Δr p With Δr n Size, to determine whether the increase in battery DCR comes from the positive electrode or the negative electrode; S6. Combining the results of S2 and S5, when ΔR0>ΔR ct , and Δr p >Δr n , then it is determined that the source of battery DCR growth is the positive electrode contact resistance R 0(p) ; When ΔR0<ΔR ct , and Δr p >Δr n , then it is determined that the source of the battery DCR increase is the positive electrode interface reaction polarization internal resistance R ct(p) ; When ΔR0>ΔR ct , and Δr p <Δr n , then it is determined that the source of the battery DCR increase is the negative electrode contact resistance R 0(n) ; When ΔR0<ΔR ct , and Δr p <Δr n , then it is determined that the source of the battery DCR increase is the negative electrode interface reaction polarization internal resistance R ct(n) .

2. The method for analyzing the battery DCR growth according to claim 1, characterized in that: In S4, the resistance test procedure of the first button battery or the third button battery includes the following steps: S51. Charge at a constant current of 0.15-0.25C until the voltage reaches 4.10-4.25V, then stop charging; S52. Let stand for 4 to 6 minutes; S53. Discharge at a constant current of 0.15-0.25C to 2.4-2.6V, and stop discharging; S54. Let stand for 4 to 6 minutes; S55. Repeat S51 to S53 twice; S56. Let stand for 8 to 12 minutes; S57. Charge at a constant current of 0.15-0.25C until the voltage reaches 4.10-4.25V, then stop charging; S58. Let stand for 4 to 6 minutes; S59. Discharge at a constant current of 1.4C to 1.6C for 28 to 32 seconds; S510. Let stand for 1.8 to 2.2 hours; The resistance r1 or r3 of the first button battery or the third button battery is calculated as follows: r1 or r3 = (pre-discharge voltage in S59 - post-discharge voltage in S59) / discharge current in S59; The resistance test procedure of the second button cell or the fourth button cell comprises the following steps: S51 '. Discharge at a constant current of 0.05 ~ 0.15C to 4 ~ 6mV, and stop discharging; S52′. Let stand for 13 to 17 minutes; S53 '. Charge to 1.4 ~ 1.6V at a constant current of 0.05 ~ 0.15C, and stop charging; S54′. Let stand for 13 to 17 minutes; S55'. Repeat S51'~S53' twice; S56′. Let stand for 8 to 12 minutes; S57′. Discharge at a constant current of 1.4C to 1.6C for 28 to 32 seconds; S58′. Let stand for 1.8 to 2.2 hours; The resistance r2 or r4 of the second button battery or the fourth button battery is calculated as follows: r2 or r4 = (pre-discharge voltage in S57' - post-discharge voltage in S57') / discharge current in S57'.

3. The method for analyzing the battery DCR growth according to claim 2, characterized in that: In S4, the resistance test procedure of the first button battery or the second button battery includes the following steps: S51. Charge at a constant current of 0.2C until the voltage reaches 4.25V, then stop charging; S52. Let stand for 5 minutes; S53. Discharge at a constant current of 0.2C to 2.5V, and stop discharging; S54. Let stand for 5 minutes; S55. Repeat S51 to S53 twice; S56. Let stand for 10 minutes; S57. Charge at a constant current of 0.2C until the voltage reaches 4.25V, then stop charging; S58. Let stand for 5 minutes; S59. Discharge at a constant current of 1.5C for 30s; S510. Let stand for 2 hours; The resistance test procedure of the second button cell or the fourth button cell comprises the following steps: S51 'discharge at a constant current of 0.1C to 5mV, stop discharging; S52′. Let stand for 15 min; S53 '. Charge to 1.5V at a constant current of 0.1C, and stop charging; S54′. Let stand for 15 min; S55'. Repeat S51'~S53' twice; S56′. Let stand for 10 min; S57′. Discharge at a constant current of 1.5C for 30s; S58′. Let stand for 2 hours.

4. The method for analyzing the battery DCR growth according to claim 1, characterized in that: In S1, the DCR decomposition process includes the following steps: S11. Discharge at a constant current of 0.15-0.25C until the voltage reaches 2.4-2.6V, then stop discharging; S12. Let stand for 8 to 12 minutes; S13. First charge at a constant current of 0.9-1.1C to 4.10-4.25V, then charge at a constant voltage of 4.10-4.25V to a current of 0.09-0.11A, and stop charging; S14. Let stand for 55 to 65 minutes; S15. Discharge at a constant current of 0.9 to 1.1C until the battery capacity is 88 to 92%; S16. Let stand for 1.8 to 2.2 hours; S17. Discharge at a constant current of 1 to 1.5C for 9 to 11 seconds, and then stop discharging; S18. Let stand for 38 to 42 seconds; S19. Charge at a constant current of 1 to 1.5C for 9 to 11 seconds, then stop charging; S110. Let stand for 38-42 seconds; S111. Repeat S15 to S110 until the voltage is 2.4 to 2.6 V; The contact resistance of the uncirculated battery or the cycle-failed battery is R10 or R20 = ΔV1 / I1, where ΔV1 is the discharge start voltage in S17 minus the voltage after S16 is stationary, and I1 is the current value of S17; The interface reaction polarization internal resistance R1 of the uncirculated battery or the cycle-failed battery ct or R2 ct =ΔV2 / I1, ΔV2 is the difference between the voltage at the 1st second and the voltage at the 3rd second from the start of discharge in S17, and I1 is the current value in S17.

5. The method for analyzing the battery DCR growth according to claim 4, characterized in that: In S1, the DCR decomposition process includes the following steps: S11. Discharge the battery at a constant current of 0.2C to 2.5V, and stop discharging; S12. Let stand for 10 minutes; S13. First charge at a constant current of 1C to 4.2V, then charge at a constant voltage of 4.2V to a current of 0.1A, and stop charging; S14. Let stand for 60 min; S15. Discharge at a constant current of 1C until the battery capacity is 90%; S16. Let stand for 2 hours; S17. Discharge at a constant current of 1C for 10s, and then stop discharging; S18. Let stand for 40 seconds; S19. Charge at a constant current of 1C for 10s, then stop charging; S110. Let stand for 40 seconds; S111. Repeat S15 to S110 until the voltage reaches 2.5V.

6. The method for analyzing the DCR growth of a battery as claimed in claim 1, characterized in that: In the first positive electrode sheet or the second positive electrode sheet, the positive electrode active material includes at least one of lithium cobalt oxide positive electrode material, lithium manganese oxide positive electrode material, nickel cobalt lithium manganese oxide positive electrode material, nickel cobalt aluminum oxide lithium positive electrode material, lithium iron phosphate positive electrode material, and lithium iron manganese phosphate positive electrode material.

7. The method for analyzing the increase in DCR of a battery as claimed in claim 6, characterized in that: The positive electrode active material includes at least one of a lithium nickel cobalt manganese oxide positive electrode material, a lithium iron phosphate positive electrode material, and a lithium iron manganese phosphate positive electrode material.

8. The method for analyzing the battery DCR growth according to claim 1, characterized in that: In the first negative electrode sheet or the second negative electrode sheet, the negative electrode active material includes at least one of a graphite negative electrode material, a graphene negative electrode material, a disordered carbon negative electrode material, a silicon-based negative electrode material, and a lithium titanate negative electrode material; The graphite negative electrode material includes at least one of natural graphite, artificial graphite, composite graphite, and mesophase carbon microspheres; The disordered carbon negative electrode material includes at least one of hard carbon and soft carbon; The silicon-based negative electrode material includes at least one of a silicon-oxygen negative electrode material, a silicon-carbon negative electrode material, and a silicon-based alloy negative electrode material.

9. The method for analyzing the battery DCR growth as claimed in claim 8, characterized in that: The negative electrode active material includes at least one of natural graphite, artificial graphite, composite graphite, silicon-oxygen negative electrode material, and silicon-carbon negative electrode material.

10. The method for analyzing the battery DCR growth according to claim 1, characterized in that: In the first button battery or the third button battery, a lithium sheet is used as a negative electrode of the first button battery or the third button battery; In the second button cell or the fourth button cell, a lithium sheet is used as the positive electrode of the second button cell or the fourth button cell.