Wire bonding life prediction method considering intermetallic compound evolution
Through temperature cycling test and finite element simulation, a model of the impact of IMC type and thickness on wire bonding life was established, which solved the limitations of IMC growth on life evaluation in the prior art, and achieved accurate prediction of wire bonding life.
Patent Information
- Application Number
- CN202411212533.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively identify the growth thickness of intermetallic compounds (IMC) with temperature cycle cycles, and the impact of IMC evolution on wire bonding life is not considered, resulting in a significant heterostructure life evaluation of IMC growth under high and low temperature cycles. There are limitations.
Through the design of temperature cycle test, the mapping relationship between intermetallic compounds and temperature cycle cycles was established, and the equivalent plastic strain amplitude model was established using finite element simulation. Combined with the Coffin-Manson model, considering the influence of IMC types and thicknesses, the lead bonding life was achieved. predictions.
A wire bonding life prediction model considering IMC evolution was established, and the impact of IMC type and thickness on bonding life was comprehensively considered, which improved the accuracy and reliability of wire bonding life evaluation under high and low temperature cycles.
Smart Images

Figure CN119089745A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of wire bonding lifetime assessment methods in microelectronic packaging. Background Art
[0002] Wire bonding technology is a key process for connecting semiconductor chips to the I / O leads of microelectronic packages or metal wiring pads on substrates. As electronic packaging develops towards miniaturization and high-density integration, the number of wire bonds integrated in the package continues to increase, and the failure of a single bonding wire will cause abnormal system functions of the entire integrated circuit. Since wire bonding is mostly heterogeneous interconnection, the thermal expansion coefficients of various materials are different, and under the action of high and low temperature cyclic loads, intermetallic compounds (IMC) will overgrow, which will cause large stress / strain accumulation in the bonding area and induce crack initiation and expansion, ultimately leading to wire bonding failure. Therefore, it is of great significance to study and establish a life prediction model that takes into account the influence of IMC evolution and predict the life of wire bonding under service environment, which is of great significance to evaluate the reliability of the overall system.
[0003] The paper "Lifting-off of Al bonding wires in IGBT modules under power cycling: failure mechanism and lifetime model, YL Huang, YJ Jia, YF Luo, F. Xiao, BL Liu, IEEE Journ Al of Emerging and Selected Topics in Power Electronics, 2020, 8 (3): 3162-3173" discloses a modified Coffin-Manson lifetime prediction model that takes into account the coupling effects of multiple factors such as current, heating time, and temperature difference, and verifies the high reliability of the model and applies it to the lifetime assessment of Al wires. However, the influence of IMC evolution on the quality of the connection interface is not involved, and the influence of IMC thickness and type on the lifetime prediction model is not considered in the modeling process. This method has great limitations in the application of this method to the lifetime assessment of heterostructures with significant IMC growth under high and low temperature cycles.
[0004] That is, it is difficult for existing technologies to identify how the IMC growth thickness of a material changes with temperature cycling, and it is even more difficult to effectively reveal the impact of IMC evolution on wire bonding life. Summary of the invention
[0005] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a method for predicting the life of wire bonds that takes into account the evolution of intermetallic compounds. The method provides a mapping relationship between different types of intermetallic compounds and temperature cycles, and establishes an equivalent plastic strain amplitude model that takes into account the influence of the type and thickness of the intermetallic compounds through finite element simulation, thereby realizing the prediction of the life of wire bonds.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a wire bonding life prediction method considering the evolution of intermetallic compounds, comprising the following steps:
[0007] Step 1: Design a temperature cycle test for wire bonding samples, obtain wire bonding samples with different intermetallic compound characteristic parameters after different temperature cycle times, and establish a mapping relationship model between different intermetallic compound characteristic parameters of wire bonding and temperature cycle according to the diffusion equation;
[0008] At the same time, a three-dimensional geometric model of the wire bonding sample is established, and the three-dimensional geometric model is given the same material properties as the wire bonding sample and the temperature cycle load of the temperature cycle test, that is, a three-dimensional finite element model of the wire bonding under temperature cycle is obtained;
[0009] Step 2: Perform finite element analysis based on the wire bonding three-dimensional finite element model to determine the stress and strain concentration area in the wire bonding three-dimensional finite element model; then use the finite element sub-model method to segment the stress and strain concentration area in the wire bonding three-dimensional finite element model to obtain a three-dimensional finite element model of the stress and strain concentration area under temperature cycling;
[0010] Step 3: Perform finite element analysis on the three-dimensional finite element model of the stress and strain concentration area to obtain the equivalent plastic strain amplitude corresponding to the characteristic parameters of different intermetallic compounds, and then establish an equivalent plastic strain amplitude model of the stress and strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds;
[0011] Step 4: The mapping relationship model between the characteristic parameters of different intermetallic compounds of the wire bonding and the temperature cycle and the equivalent plastic strain amplitude model considering the influence of the characteristic parameters of the intermetallic compounds in the stress and strain concentration area are coupled to the Coffin-Manson model, that is, a wire bonding life prediction model considering the characteristic parameters of the intermetallic compounds in the stress and strain concentration area is established, and the wire bonding life prediction of the evolution of intermetallic compounds under temperature cycling is realized.
[0012] Furthermore, the characteristic parameters of the intermetallic compound in step 1 are the type and thickness of the intermetallic compound, and the diffusion equation in step 1 is:
[0013] d=d0+an b ,
[0014] Wherein, d represents the thickness of the intermetallic compound when the number of temperature cycles is n; d0 represents the thickness of the intermetallic compound under the initial conditions; a represents the growth constant; b represents the index related to the number of temperature cycles;
[0015] The mapping relationship model between the thickness d of different intermetallic compounds and the number of temperature cycles n is established as follows:
[0016] d=f(n).
[0017] Furthermore, the process conditions of the temperature cycle test described in step 1 are:
[0018] Raise the temperature from room temperature to 125-175°C, keep warm for 20-30 min, lower the temperature to -90--40°C at a rate of 10-30°C / min, keep warm for 20-30 min, continue to raise the temperature from -90--40°C to 125-175°C, keep warm for 20-30 min. This is one cycle and must be repeated at least three times.
[0019] Furthermore, in the step of establishing the three-dimensional finite element model of wire bonding under temperature cycling described in step 1, the material physical property parameters of the wire bonding sample include the corresponding physical property parameters of the wire, the intermetallic compound of the bonding interface, the pad and the substrate;
[0020] The material property parameters are Young's modulus, Poisson's ratio, density, thermal expansion coefficient, yield strength and tangent modulus of the wire bonding sample; the temperature cycle load is -65 to 150°C.
[0021] Furthermore, the specific analysis steps for determining the stress and strain concentration area in the wire bonding three-dimensional finite element model in the step 2 are: performing stress and strain analysis on the wire bonding three-dimensional finite element model under the temperature cycle obtained in the step 1, and determining the stress and strain concentration area according to the effective stress and equivalent plastic strain distribution in the wire bonding three-dimensional finite element model, which means that cracks are likely to initiate and expand in this area, eventually leading to wire bonding failure; using the finite element sub-model method, dividing the stress and strain concentration area in the wire bonding three-dimensional finite element model to obtain a three-dimensional finite element model of the stress and strain concentration area under the temperature cycle, and then changing the characteristic parameters of the intermetallic compounds in the three-dimensional finite element model of the stress and strain concentration area to obtain a mapping relationship between the characteristic parameters of different intermetallic compounds and the equivalent plastic strain amplitude, so as to establish an equivalent plastic strain amplitude model of the stress and strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds.
[0022] Furthermore, the step three is specifically as follows:
[0023] By changing the characteristic parameters of the intermetallic compounds in the three-dimensional finite element model of the wire bonding stress and strain concentration area under the temperature cycle, and combining the finite element simulation to obtain the simulation results, the characteristic parameters d1, d2, ..., d m , and the mapping relationship with the equivalent plastic strain amplitude Δε is:
[0024] Δε=f(d1,d2,…,d m ),
[0025] Subsequently, based on the above mapping relationship, an equivalent plastic strain amplitude model is established in the stress-strain concentration area considering the influence of characteristic parameters of intermetallic compounds.
[0026] Furthermore, the equivalent plastic strain amplitude model of the stress and strain concentration region considering the influence of the characteristic parameters of the intermetallic compounds is obtained from the mapping relationship of the equivalent plastic strain amplitudes corresponding to the characteristic parameters of different intermetallic compounds in the stress and strain concentration region, specifically:
[0027] Quantitative statistics when the number of temperature cycles is n k When k is an integer greater than 1, the thickness of different types of intermetallic compounds are This is used as the thickness of different intermetallic compound phases in the three-dimensional finite element model of the wire bonding stress and strain concentration area under the temperature cycle. Finite element numerical simulation is performed on the three-dimensional finite element model of the stress and strain concentration area under high and low temperature cyclic loading, and the intermetallic compound thickness is obtained. The equivalent plastic strain amplitude Δε k ;
[0028] Then the equivalent plastic strain amplitude model of the stress-strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds is obtained as follows:
[0029]
[0030] Where, d i ,d j Expressed as the thickness of the i-th and j-th intermetallic compounds; β0, β i ,β ij Represented as a material parameter in the model.
[0031] Furthermore, the wire bonding life prediction model considering the characteristic parameters of the intermetallic compound in the stress and strain concentration area established in step 4 is:
[0032]
[0033] Where N f It is expressed as the life of wire bonding under temperature cycling; Δε is expressed as the equivalent plastic strain amplitude; εf is expressed as the fatigue toughness coefficient, and ε f =0.325; c is the fatigue toughness index, which is related to the average temperature T of the temperature cycle avg is related to the frequency f, and c = -0.442-6×10 -4 T avg +1.74×10 -2 ln(1+f);d i ,d j ,d m Expressed as the thickness of the i, j, and m intermetallic compounds when the number of temperature cycles is n; β0, β i ,β ij Expressed as material parameters; It is expressed as the thickness of the i, j, and m intermetallic compounds under the initial conditions; a i , a j , a m Expressed as the growth constant of the i, j, and m intermetallic compounds; b i , b j , b m It is expressed as an index related to the number of temperature cycles of the i, j, and m intermetallic compounds.
[0034] Furthermore, the stress and strain concentration area in the wire bonding three-dimensional finite element model obtained in step 2 is the bonding interface area of the wire bonding or the wire or pad or substrate area.
[0035] Furthermore, the wire bonding interface is an Al-Au wire bonding interface, or the wire bonding sample is a wire bonding sample composed of Al or Cu or Au or Si-Al or Ag or alloy wires, Au / TiW / NiCr or Au or Cu or Al pads and Si or ceramic substrates.
[0036] The method also includes step 4 of using the intermetallic compound thickness value of the wire bonding interface that varies with the number of temperature cycles as non-sample data to perform reliability verification on the wire bonding life prediction model.
[0037] The beneficial effects of the present invention are as follows: the present invention takes into account the evolution of intermetallic compounds during temperature cycling, comprehensively considers the changes in the types and thicknesses of intermetallic compounds during temperature cycling, establishes a functional relationship between the thicknesses of different intermetallic compounds and the number of temperature cycles, and explores the influence of the number of temperature cycles on the thicknesses of different intermetallic compounds. The present invention also considers the influence of the types and thicknesses of intermetallic compounds on the life of wire bonding during temperature cycling, establishes a functional relationship between the types and thicknesses of intermetallic compounds and the equivalent plastic strain amplitude, studies the influence of the types and thicknesses of intermetallic compounds on the stress-strain field of the bonding interface, thereby establishing a finite element numerical simulation system for wire bonding under high and low temperature cycles, and then obtains a wire bonding life prediction model that considers the influence of the evolution of intermetallic compounds, providing a basis for the life prediction of wire bonding. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The overall equivalent plastic strain distribution of the stress-strain concentration region model of the Al-Au wire bonding after the temperature cycle of the present invention is completed;
[0039] Figure 2 It is the equivalent plastic strain distribution of the bottom of the Al wire in the stress-strain concentration area model of the Al-Au wire bonding after the temperature cycle of the present invention is completed. DETAILED DESCRIPTION
[0040] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0041] In order to achieve the above object, the present invention provides the following specific implementation methods:
[0042] Embodiment 1: A method for predicting wire bonding life considering the evolution of intermetallic compounds, comprising the following steps:
[0043] S1. The process conditions of the temperature cycle test are: heating from room temperature to 125-175°C, keeping warm for 20-30 minutes, cooling down to -90--40°C at a rate of 10-30°C / min, keeping warm for 20-30 minutes, and continuing to heat from -90--40°C to 125-175°C, keeping warm for 20-30 minutes, as a cycle, and at least three cycles, to conduct multiple temperature cycle tests on the wire bonding sample, and obtain wire bonding samples with different intermetallic compound characteristic parameters after different temperature cycle times;
[0044] The wire bonding interface is an Al-Au wire bonding interface, or the wire bonding sample is a wire bonding sample consisting of Al or Cu or Au or Si-Al or Ag or alloy wires, Au / TiW / NiCr or Au or Cu or Al pads, and Si or ceramic substrates.
[0045] S2. According to the characteristic parameters of the intermetallic compound, namely the type and thickness of the intermetallic compound, according to the diffusion equation:
[0046] d=d0+an b ,
[0047] Wherein, d represents the thickness of the intermetallic compound when the number of temperature cycles is n; d0 represents the thickness of the intermetallic compound under the initial conditions; a represents the growth constant; b represents the index related to the number of temperature cycles;
[0048] The mapping relationship model between the thickness d of different intermetallic compounds and the number of temperature cycles n is established as follows:
[0049] d=f(n).
[0050] S3, establishing a three-dimensional geometric model of the wire bonding sample, giving the three-dimensional geometric model the same material properties as the wire bonding sample and the temperature cycle load of the temperature cycle test, that is, obtaining a three-dimensional finite element model of the wire bonding under temperature cycling;
[0051] The material physical property parameters of the wire bonding sample include the corresponding physical property parameters of the wire, the intermetallic compound at the bonding interface, the pad and the substrate;
[0052] The physical property parameters are Young's modulus, Poisson's ratio, density, thermal expansion coefficient, yield strength and tangent modulus of the wire bonding sample; the temperature cycle load is -65 to 150°C.
[0053] S4. Perform stress-strain analysis on the wire bonding three-dimensional finite element model obtained under the temperature cycle. According to the distribution of equivalent stress and equivalent plastic strain in the wire bonding three-dimensional finite element model, the stress-strain concentration area is determined, which means that cracks are likely to initiate and propagate in this area, and eventually lead to wire bonding failure, specifically the bonding interface area.
[0054] S5. Using a finite element sub-model method, a stress and strain concentration region is divided in the wire bonding three-dimensional finite element model, where the stress and strain concentration region is a wire bonding lead or pad or substrate region, so as to obtain a three-dimensional finite element model of the stress and strain concentration region under a temperature cycle corresponding to the specific stress and strain concentration region;
[0055] S6. By changing the characteristic parameters of the intermetallic compounds in the three-dimensional finite element model of the stress and strain concentration area, the characteristic parameters d1, d2, ..., d m , and the mapping relationship with the equivalent plastic strain amplitude Δε is:
[0056] Δε=f(d1,d2,...,dm );
[0057] S7, the equivalent plastic strain amplitude model of the stress-strain concentration region considering the influence of the characteristic parameters of the intermetallic compounds obtained from the mapping relationship of the equivalent plastic strain amplitudes corresponding to the characteristic parameters of the different intermetallic compounds, specifically:
[0058] Quantitative statistics when the number of temperature cycles is n k When k is an integer greater than 1, the thickness of different types of intermetallic compounds are This is used as the thickness of different intermetallic compound phases in the three-dimensional finite element model of the wire bonding stress and strain concentration area under the temperature cycle. Finite element numerical simulation is performed on the three-dimensional finite element model of the stress and strain concentration area under high and low temperature cyclic loading, and the intermetallic compound thickness is obtained. The equivalent plastic strain amplitude Δε k ;
[0059] Then the equivalent plastic strain amplitude model of the stress-strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds is obtained as follows:
[0060]
[0061] Where, d i ,d j Expressed as the thickness of the i-th and j-th intermetallic compounds; β0, β i ,β ij Represented as a material parameter in the model.
[0062] S8. The mapping relationship model between the characteristic parameters of different intermetallic compounds of the wire bonding and the temperature cycle and the equivalent plastic strain amplitude model considering the influence of the characteristic parameters of the intermetallic compounds in the stress and strain concentration area are coupled to the Coffin-Manson model, that is, the wire bonding life prediction model considering the characteristic parameters of the intermetallic compounds in the stress and strain concentration area is established as follows:
[0063]
[0064] Where N f It is expressed as the life of wire bonding under temperature cycling; Δε is expressed as the equivalent plastic strain amplitude; ε f is expressed as the fatigue toughness coefficient, and ε f =0.325; c is the fatigue toughness index, which is related to the average temperature T of the temperature cycle avg is related to the frequency f, and c = -0.442-6×10 -4 T avg +1.74×10 -2 ln(1+f);d i ,dj ,d m Expressed as the thickness of the i, j, and m intermetallic compounds when the number of temperature cycles is n; β0, β i ,β ij Expressed as material parameters; It is expressed as the thickness of the i, j, and m intermetallic compounds under the initial conditions; a i , a j , a m Expressed as the growth constant of the i, j, and m intermetallic compounds; b i , b j , b m It is expressed as an index related to the number of temperature cycles of the i, j, and m intermetallic compounds.
[0065] In order to further illustrate the technical solution, the present invention provides the following specific test examples:
[0066] The Al-Au wire bonding sample was used as a specific implementation object, wherein the bonding wire was an Al wire with a diameter of 40 μm, containing 1% Si, and the Au layer was deposited on the Si substrate by magnetron sputtering, with a thickness of about 700-800 nm. The bonded sample was kept at 125°C for 96 hours.
[0067] Step 1: Design a temperature cycle test with a test temperature of -65 to 150°C, a high and low temperature holding time of 25 minutes, a heating / cooling rate of 20°C / min, and 100, 200, 500, 600, 800, and 1000 temperature cycles, respectively. Through experimental characterization, it was determined that there were two types of IMCs at the Al-Au wire bonding interface during the temperature cycle. The types of IMCs are AuAl2 and Au2Al. The thickness of IMCs under different times of temperature cycles is shown in Table 1.
[0068] Table 1 Effect of temperature cycle times on IMC thickness of Al-Au wire bonding interface
[0069]
[0070] Based on the diffusion equation and combined with the quantitative results, the material parameters are calculated and expressed as:
[0071]
[0072] In the formula, Expressed as the thickness of Au2Al in μm; It is expressed as the thickness of AuAl2 in μm; n is the number of temperature cycles.
[0073] Step 2: Construct a three-dimensional geometric model based on the actual size of the Al-Au wire bonding, and perform a temperature cycle finite element numerical simulation. The temperature load setting is the same as the actual temperature cycle test, with a temperature range of -65 to 150°C, a high and low temperature insulation time of 25 minutes, a heating / cooling rate of 20°C / min, and five temperature cycles. By analyzing the equivalent stress / plastic strain distribution during the temperature cycle, it is found that the equivalent stress and equivalent plastic strain at the bottom of the Al wire are small in the middle and large at the edge, and the maximum values of the equivalent stress and equivalent plastic strain are both located on the contact surface between Al and Au, indicating that the Al-Au wire bonding interface is a stress and strain concentration area.
[0074] Furthermore, according to Table 1, seven three-dimensional finite element models of stress and strain concentration areas of Al-Au wire bonding containing IMC were established.
[0075] Step 3: If Figure 1 , Figure 2 As shown in the figure, the three-dimensional finite element model of the seven wire bonding stress and strain concentration areas containing IMC was further refined to divide the mesh, and then the temperature cycle finite element numerical simulation was carried out. The temperature load setting is the same as the actual temperature cycle test, the temperature range is -65 ~ 150 ℃, the high and low temperature insulation time is 25min, the heating / cooling rate is 20℃ / min, and five temperature cycles are set. Analyzing the numerical simulation results, it can be seen that the plastic strain is mainly generated at the contact interface between IMC and Al lead. The maximum value of the equivalent plastic strain is located in the area close to the arc end of the contact surface between Al and IMC, and the closer to the contact edge of the Al lead and IMC, the larger the equivalent plastic strain value, as shown in the figure. Figure 1 , Figure 2 As shown in the figure, since the yield strength of Al lead is low, the stress required for plastic deformation is small, while IMC is a hard and brittle phase, and greater stress is required for plastic deformation. However, the stress concentration caused by temperature changes during temperature cycling cannot reach the yield strength of Al-Au IMC, so plastic deformation mainly occurs in Al lead. The contact interface between Al lead and IMC not only has stress concentration, but also undergoes large plastic deformation. Moreover, since the stress caused by temperature cycle load is concentrated in two areas near the wire tail end and wire arc end, the plastic deformation in these two areas is more severe, which will produce larger plastic strain. Therefore, cracks are easy to initiate and expand in the wire tail end and wire arc end area, eventually leading to wire bonding failure.
[0076] The equivalent plastic strain data of the fifth cycle of the stress and strain concentration area during the temperature cycle was extracted to obtain the equivalent plastic strain amplitude. The corresponding equivalent plastic strain amplitude and life prediction results in the three-dimensional finite element model of each stress and strain concentration area are shown in Table 2:
[0077] Table 2 Equivalent plastic strain amplitude of the three-dimensional finite element model of the stress-strain concentration area of the Al-Au wire bonding with different IMC thicknesses
[0078]
[0079]
[0080] Step 4: According to Table 2, establish the equivalent plastic strain amplitude model considering the influence of IMC type and thickness in the stress and strain concentration area:
[0081]
[0082] Where Δε represents the equivalent plastic strain amplitude.
[0083] Step 5: Couple the equivalent plastic strain amplitude model value to the Coffin-Manson model, and consider the evolution of IMC during temperature cycling to establish an Al-Au wire bonding life prediction model that considers the influence of IMC type and thickness:
[0084]
[0085] Where N f Expressed as the life of wire bonding under temperature cycling; ε f is expressed as the fatigue toughness index, and ε f =0.325; c is the fatigue toughness index, which is related to the average temperature T of the temperature cycle avg is related to the frequency f, and c = -0.442-6×10 -4 Tavg+1.74×10 -2 ln(1+f).
[0086] In order to test the accuracy of the life prediction model, as shown in Table 3:
[0087] Table 3 Comparison of experimental and calculated values of stress-strain concentration area life of Al-Au wire bonding
[0088]
[0089] It can be seen from the table that the maximum relative error of the model is 15.37%, the minimum relative error is 0.14%, the average relative error is 5.27%, and the correlation coefficient R 2 It is 0.94, indicating that the prediction accuracy of the model is good.
[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A wire bonding life prediction method considering the evolution of intermetallic compounds, characterized in that: The following steps are involved: Step 1: Design a temperature cycle test for wire bonding samples, obtain wire bonding samples with different intermetallic compound characteristic parameters after different temperature cycle times, and establish a mapping relationship model between different intermetallic compound characteristic parameters of wire bonding and temperature cycle according to the diffusion equation; At the same time, a three-dimensional geometric model of the wire bonding sample is established, and the three-dimensional geometric model is given the same material properties as the wire bonding sample and the temperature cycle load of the temperature cycle test, that is, a three-dimensional finite element model of the wire bonding under temperature cycle is obtained; Step 2: Perform finite element analysis based on the wire bonding three-dimensional finite element model to determine the stress and strain concentration area in the wire bonding three-dimensional finite element model; then use the finite element sub-model method to segment the stress and strain concentration area in the wire bonding three-dimensional finite element model to obtain a three-dimensional finite element model of the stress and strain concentration area under temperature cycling; Step 3: Perform finite element analysis on the three-dimensional finite element model of the stress and strain concentration area to obtain the equivalent plastic strain amplitude corresponding to the characteristic parameters of different intermetallic compounds, and then establish an equivalent plastic strain amplitude model of the stress and strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds; Step 4: The mapping relationship model between the characteristic parameters of different intermetallic compounds of the wire bonding and the temperature cycle and the equivalent plastic strain amplitude model considering the influence of the characteristic parameters of the intermetallic compounds in the stress and strain concentration area are coupled to the Coffin-Manson model, that is, a wire bonding life prediction model considering the characteristic parameters of the intermetallic compounds in the stress and strain concentration area is established, and the wire bonding life prediction of the evolution of intermetallic compounds under temperature cycling is realized.
2. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: The characteristic parameters of the intermetallic compound in step 1 are the type and thickness of the intermetallic compound, so the diffusion equation in step 1 is: d=d0+an b , Wherein, d represents the thickness of the intermetallic compound when the number of temperature cycles is n; d0 represents the thickness of the intermetallic compound under the initial conditions; a represents the growth constant; b represents the index related to the number of temperature cycles; The mapping relationship model between the thickness d of different intermetallic compounds and the number of temperature cycles n is established as follows: d=f(n).
3. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: The process conditions of the temperature cycle test described in step 1 are: Raise the temperature from room temperature to 125-175°C, keep warm for 20-30 min, lower the temperature to -90--40°C at a rate of 10-30°C / min, keep warm for 20-30 min, continue to raise the temperature from -90--40°C to 125-175°C, keep warm for 20-30 min. This is one cycle and must be repeated at least three times.
4. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: In the step of establishing the three-dimensional finite element model of wire bonding under temperature cycling described in step 1, the material physical property parameters of the wire bonding sample include the corresponding physical property parameters of the wire, the intermetallic compound at the bonding interface, the pad and the substrate; The material property parameters are Young's modulus, Poisson's ratio, density, thermal expansion coefficient, yield strength and tangent modulus of the wire bonding sample; the temperature cycle load is -65 to 150°C.
5. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: The specific analysis steps for determining the stress and strain concentration area in the wire bonding three-dimensional finite element model in the step 2 are: performing stress and strain analysis on the wire bonding three-dimensional finite element model under the temperature cycle obtained in the step 1, and determining the stress and strain concentration area according to the distribution of equivalent stress and equivalent plastic strain in the wire bonding three-dimensional finite element model, that is, indicating that cracks are likely to initiate and expand in this area, and eventually lead to the failure of the wire bonding; By using the finite element sub-model method, the stress and strain concentration area is cut out in the wire bonding three-dimensional finite element model to obtain the three-dimensional finite element model of the stress and strain concentration area under temperature cycling. Subsequently, by changing the characteristic parameters of the intermetallic compounds in the three-dimensional finite element model of the stress and strain concentration area, the mapping relationship between the characteristic parameters of different intermetallic compounds and the equivalent plastic strain amplitude is obtained, and the equivalent plastic strain amplitude model of the stress and strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds can be established.
6. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: The step three is specifically as follows: By changing the characteristic parameters of the intermetallic compounds in the three-dimensional finite element model of the wire bonding stress and strain concentration area under the temperature cycle, and combining the finite element simulation to obtain the simulation results, the characteristic parameters d1, d2, ..., d m , and the mapping relationship with the equivalent plastic strain amplitude Δε is: Δε=f(d1,d2,...,d m ), Subsequently, based on the above mapping relationship, an equivalent plastic strain amplitude model is established in the stress-strain concentration area considering the influence of characteristic parameters of intermetallic compounds.
7. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 6, characterized in that: The equivalent plastic strain amplitude model of the stress-strain concentration region considering the influence of the characteristic parameters of the intermetallic compounds is obtained from the mapping relationship of the equivalent plastic strain amplitudes corresponding to the characteristic parameters of different intermetallic compounds in the stress-strain concentration region, specifically: Quantitative statistics when the number of temperature cycles is n k When k is an integer greater than 1, the thickness of different types of intermetallic compounds are This is used as the thickness of different intermetallic compound phases in the three-dimensional finite element model of the wire bonding stress and strain concentration area under the temperature cycle. Finite element numerical simulation is performed on the three-dimensional finite element model of the stress and strain concentration area under high and low temperature cyclic loading, and the intermetallic compound thickness is obtained. The equivalent plastic strain amplitude Δε k ; Then the equivalent plastic strain amplitude model of the stress-strain concentration area considering the influence of the characteristic parameters of the intermetallic compounds is obtained as follows: Where, d i ,d j Expressed as the thickness of the i-th and j-th intermetallic compounds; β0, β i ,β ij Represented as a material parameter in the model.
8. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: The wire bonding life prediction model considering the characteristic parameters of intermetallic compounds in the stress and strain concentration area established in step 4 is: Where N f It is expressed as the life of wire bonding under temperature cycling; Δε is expressed as the equivalent plastic strain amplitude; ε f is expressed as the fatigue toughness coefficient, and e f =0.325; c is the fatigue toughness index, which is related to the average temperature T of the temperature cycle avg is related to the frequency f, and c = -0.442-6×10 -4 T avg +1.74×10 -2 ln(1+f);d i ,d j ,d m It is expressed as the thickness of the i, j, and m intermetallic compounds when the number of temperature cycles is n; β0, β i ,β ij Expressed as material parameters; It is expressed as the thickness of the i, j, and m intermetallic compounds under the initial conditions; a i , a j , a m Expressed as the growth constant of the i, j, and m intermetallic compounds; b i , b j , b m It is expressed as an index related to the number of temperature cycles of the i, j, and m intermetallic compounds.
9. The wire bonding life prediction method considering the evolution of intermetallic compounds according to claim 1, characterized in that: The stress and strain concentration area in the wire bonding three-dimensional finite element model obtained in step 2 is the bonding interface area of the wire bonding or the wire or pad or substrate area.
10. The wire bonding life prediction method considering the evolution of intermetallic compounds according to any one of claims 1 to 9, characterized in that: The wire bonding interface is an Al-Au wire bonding interface, or the wire bonding sample is a wire bonding sample consisting of Al or Cu or Au or Si-Al or Ag or alloy wires, Au / TiW / NiCr or Au or Cu or Al pads and Si or ceramic substrates.