Positive electrode material and preparation method thereof, positive plate and secondary battery

By using ABO3 type cladding material and LiCoaMbAzBwO2 interface on lithium cobalt oxide positive electrode material, the problem of structural instability of lithium cobalt oxide and the shedding of the cladding substance at high voltage is solved, and a more stable cladding layer and improved electricity are achieved. Chemical properties extend the service life of the battery.

CN119092661APending Publication Date: 2024-12-06ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017220.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The structure of lithium cobalt oxide cathode material is unstable at high voltage, which easily leads to structural collapse and cobalt ion dissolution, thereby reducing specific capacity and shortening battery life. The existing covering substances are not in a firm contact with the substrate and are prone to fall off, resulting in deterioration of performance.

Method used

The chemical formula of the coating material is ABO3, A is La, Y, Zr, B is Co, Ni, Mn, Ti, the matrix material is LiCoxMyO2, M is Mo6+, W6+, forming the LiCoaMbAzBwO2 interface, and doping it through high-valent metal ions. Mixed and long-term firing to form a stable coating layer, enhancing the stability and electrochemical properties of lithium cobalt oxide.

Benefits of technology

It improves the stability of the coating layer, prevents the coating substance from falling off, reduces electrolyte corrosion, enhances the low-temperature stability and electrochemical performance of lithium cobalt oxide, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092661A_ABST
    Figure CN119092661A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode material and a preparation method thereof, a positive plate and a secondary battery, the positive electrode material comprises a base material and a coating material coating the outer surface of the base material, the chemical general formula of the coating material is ABO3, A is one of La, Y and Zr, and B is one of Co, Ni, Mn and Ti; the chemical general formula of the base material is LiCoxMyO2, M is one or more of Mo < 6 + >, W < 6 + > and Se < 6 + >, and x + y = 1; an interface with a chemical general formula of LiCoaMbAzBwO2 is formed between the matrix material and the coating material, wherein a + b + z + w = 1. According to the lithium cobalt oxide positive electrode material disclosed by the invention, the stability of the coating layer is enhanced by doping + 6-valence high-valence ions, so that the coating layer is effectively prevented from falling off in the stirring, rolling and repeated charging processes, and electrolyte corrosion is reduced, thereby improving the low-temperature stability of the material and the electrochemical performance of the material under high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet, and a secondary battery. Background Art

[0002] At present, the lithium cobalt oxide positive electrode material with a layered structure is widely used in the market. Under normal circumstances, the normal charging cut-off voltage of lithium cobalt oxide LiCoO2 is 4.2V, and the specific capacity is about 140mAh / g, which is only 50% of the theoretical specific capacity of 274mAh / g. Increasing the charging cut-off voltage of the material can increase the specific capacity of lithium cobalt oxide. 4.4V high-voltage lithium cobalt oxide materials have begun to be widely used in the market. However, lithium cobalt oxide materials have two shortcomings under high voltage, which limit the application of lithium cobalt oxide materials in large lithium-ion batteries: First, when the charging cut-off voltage is greater than 4.2V, the Li in LiCoO2 + A large amount of Co ions will be deintercalated, causing the +3-valent Co ions in the structure to be converted into +4-valent Co ions, thereby forming oxygen defects, weakening the binding force between cobalt and oxygen, and ultimately causing the layered crystal structure of the material to collapse and be destroyed. During charge and discharge, Li ions cannot be deintercalated normally, reducing the specific capacity of the material. Second, under high-voltage charge and discharge conditions, Co ions are easily dissolved into the electrolyte, and +4-valent Co ions have relatively strong oxidizing properties, which will cause the electrolyte to oxidize and decompose, shortening the battery life.

[0003] In order to solve the structural collapse and cobalt dissolution problems of lithium cobalt oxide positive electrode materials during high voltage charging and discharging, people have adopted a large number of modification means and methods, mainly doping and surface coating of lithium cobalt oxide materials. However, due to the weak contact between the coating material and the lithium cobalt oxide matrix in the existing technology, the coating material is easy to fall off from the lithium cobalt oxide matrix under the repeated action of stress, and once the lithium cobalt oxide loses the coating of the coating material, the side reactions on its surface will be more intense, and the performance of the lithium cobalt oxide will deteriorate more significantly.

[0004] In view of this, it is indeed necessary to provide a technical solution to the above problems. Summary of the invention

[0005] One of the purposes of the present invention is to provide a positive electrode material to address the deficiencies of the prior art, so as to improve the problems of the current lithium cobalt oxide material having unstable structure under high pressure, enhanced surface oxidation of lithium cobalt oxide and increased side reactions with the electrolyte.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A positive electrode material, comprising a base material and a coating material coated on the outer surface of the base material, wherein the coating material has a chemical formula of ABO3, wherein A is one of La, Y, and Zr, and B is one of Co, Ni, Mn, and Ti; the base material has a chemical formula of LiCo x M y O2, where M is Mo 6+ , W 6+ 、Se 6+ One or more of the following, wherein x+y=1; a chemical formula of LiCo is formed between the matrix material and the coating material. a M b A z B w The interface of O2, where a+b+z+w=1.

[0008] Preferably, the coating material ABO3 is a cubic or octahedral perovskite.

[0009] Preferably, the molar ratio of the element A in the coating material to the element M in the matrix material is 0.0002 to 0.002.

[0010] Preferably, the matrix material LiCo x M y The molar ratio of Li, Co and M in O2 is 1.05:1:0.001~0.03.

[0011] The second object of the present invention is to provide a method for preparing a positive electrode material, comprising the following steps:

[0012] S1. Weigh the cobalt oxide, lithium salt and M oxide according to the molar ratio, then mix the materials evenly, then place the materials in a tube furnace for firing, crush the fired materials, and obtain a semi-finished lithium cobalt oxide doped with M after powdering;

[0013] S2, dissolve the soluble salt of A(NO3)3·6H2O and B in the alcohol solution, then add the doped M lithium cobalt oxide semi-finished product prepared in S1, stir evenly, place until the alcohol solution is completely volatilized, and then put the materials into the tube furnace for firing. At this time, LiCo x Mo y ABO3 coating material will be generated in situ on the surface of O2;

[0014] S3, heating the material obtained in S2 to 500-1100°C at 3-5°C / min, sintering it in an air atmosphere for 8-55h, and then crushing the material to obtain the positive electrode material.

[0015] Preferably, in step S1, the molar ratio of Co in the cobalt oxide to Li in the lithium salt is Li:Co=1.05:1-1.15:1, and the molar ratio of Co in the cobalt oxide to M in the M oxide is M:Co=0.01-0.03.

[0016] Preferably, in step S1, the firing process is to first heat the tube furnace to 600-800°C at 8-10°C / min, then sinter at a constant temperature and air atmosphere for 5-7 hours, then heat to 1000-1200°C at 3-5°C / min, and then sinter at a constant temperature and air atmosphere for 18-22 hours.

[0017] Preferably, in step S2, the firing process is to heat the tube furnace to 900-1100° C. at 3-5° C. / min, and then sinter for 4-6 hours.

[0018] The third object of the present invention is to provide a positive electrode sheet, comprising the positive electrode material mentioned above,

[0019] A fourth object of the present invention is to provide a secondary battery comprising the above-mentioned positive electrode sheet.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: the lithium cobalt oxide positive electrode material prepared by the present invention is doped with +6 high-valent ions to improve the stability of the coating, and at the same time, the coating material of the present invention is firmly connected to the surface of the lithium cobalt oxide substrate, effectively preventing the coating material from falling off from the lithium cobalt oxide substrate during stirring, rolling, and repeated charging, thereby ensuring the stability of the lithium cobalt oxide surface. In the long-term cycle process, the surface coating layer can reduce the erosion of the electrolyte on the surface of the lithium cobalt oxide, and the LiCo generated between the substrate material and the coating material a M b A z B w The O2 (a+b+z+w=1) phase interface can improve the low-temperature stability of lithium cobalt oxide and improve the electrochemical performance of lithium cobalt oxide at high voltage. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM image of the positive electrode material of Example 1 of the present invention;

[0022] Figure 2 This is a TEM image of the positive electrode material of Example 1 of the present invention;

[0023] Figure 3 This is the secondary ion mass spectrum of the positive electrode material of Example 1 of the present invention. DETAILED DESCRIPTION

[0024] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods and accompanying drawings, but the implementation methods of the present invention are not limited thereto.

[0025] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0026] The first aspect of the present invention is to provide a positive electrode material, comprising a base material and a coating material coated on the outer surface of the base material, wherein the coating material has a chemical formula of ABO3, wherein A is one of La, Y, and Zr, and B is one of Co, Ni, Mn, and Ti; the base material has a chemical formula of LiCo x M y O2, where M is Mo 6+ , W 6+ 、Se 6+ One or more of the following, wherein x+y=1; a chemical formula of LiCo is formed between the matrix material and the coating material. a M b A z B w The interface of O2, where a+b+z+w=1. The valence of the metal ions doped in the present invention is +6, and the high-valence metal ions doped into the Co site can stabilize the Co 3+ The high-valent ion doping can form coordination bonds with the electrons of more oxygen atoms in lithium cobalt oxide, thereby enhancing the oxygen fixation ability and the stability of lithium cobalt oxide. In addition, the radius of +6 valent metal ions is larger than that of Co 3+ , which will increase the c-axis spacing and enhance Li + diffusion rate.

[0027] Wherein, a chemical formula of LiCo is formed between the base material and the coating material. a M b A z B w O2 interface, so that the coating material and the surface of the lithium cobalt oxide substrate are firmly connected, which can effectively prevent the coating material from falling off from the lithium cobalt oxide substrate during stirring, rolling, and repeated charging, ensure the stability of the lithium cobalt oxide surface, and prevent the electrolyte from corroding the lithium cobalt oxide surface. In addition, the interface can also accelerate the surface Li + The diffusion rate of lithium cobalt oxide is improved, thereby improving the low-temperature performance of lithium cobalt oxide.

[0028] Wherein, the coating material ABO3 is a cubic or octahedral perovskite. Perovskite-type composite oxide ABO3 is a new type of inorganic non-metallic material with unique physical and chemical properties. The A position is generally a rare earth or alkaline earth element ion, and the B position is a transition element ion. Both the A position and the B position can be partially replaced by other metal ions with similar radii while keeping their crystal structure basically unchanged. This type of compound has a stable crystal structure.

[0029] In some embodiments, the molar ratio of the element A in the coating material to the element M in the matrix material is 0.0002 to 0.002.

[0030] In some embodiments, the matrix material LiCo x M y The molar ratio of Li, Co, and M in O2 is 1.05:1:0.001-0.03. The proportion of Li element is greater than that of Co and M elements. Li will be lost in the subsequent sintering process, and the excess Li element can replenish the consumed Li.

[0031] The second aspect of the present invention is to provide a method for preparing the above-mentioned positive electrode material, comprising the following steps:

[0032] S1. Weigh the cobalt oxide, lithium salt and oxide of the M element according to the molar ratio, then mix the materials evenly, then place the materials in a tube furnace for firing, crush the fired materials, and obtain a semi-finished lithium cobalt oxide doped with M after powdering;

[0033] S2, dissolve the soluble salt of A(NO3)3·6H2O and B in the alcohol solution, then add the doped M lithium cobalt oxide semi-finished product prepared in S1, stir evenly, place until the alcohol solution is completely volatilized, and then put the materials into the tube furnace for firing. At this time, LiCo x Mo y ABO3 coating material will be generated in situ on the surface of O2;

[0034] S3, heating the material obtained in S2 to 500-1100°C at 3-5°C / min, sintering it in an air atmosphere for 8-55h, and then crushing the material and powdering it to obtain the positive electrode material.

[0035] In some embodiments, in step S1, the molar ratio of Co in the cobalt oxide to Li in the lithium salt is Li:Co=1.05:1-1.15:1, and the molar ratio of Co in the cobalt oxide to M in the M oxide is M:Co=0.01-0.03.

[0036] In some embodiments, in step S1, the firing process is to first heat the tube furnace to 600-800°C at 8-10°C / min, then sinter at a constant temperature and air atmosphere for 5-7 hours, then heat to 1000-1200°C at 3-5°C / min, and then sinter at a constant temperature and air atmosphere for 18-22 hours.

[0037] In some embodiments, in step S2, the firing process is to heat the tube furnace to 900-1100° C. at 3-5° C. / min, and then sinter for 4-6 hours.

[0038] The present invention adopts step-by-step firing, firstly forms a coating of ABO3 perovskite material in situ on the surface of the base material, and then adopts a coating process of long-term calcination. At the same time, due to the presence of high-valent large ion radius doping element M, the Co layer spacing is large. Under the action of long-term thermal driving force, the coating elements A and B can be formed on the LiCo x M y O2 shallow surface forms A and B doping, A and B elements occupy the Co position, and finally in the cobalt oxide LiCo x M y LiCo is formed between O2 and the coating material ABO3 a M b A z B w Compared with the traditional coating materials and coating methods of lithium cobalt oxide, the coating effect of the present invention is firmer and better.

[0039] The third aspect of the present invention is to provide a positive electrode sheet, the positive electrode material mentioned above.

[0040] A fourth aspect of the present invention is to provide a secondary battery comprising the above-mentioned positive electrode sheet.

[0041] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods and accompanying drawings, but the implementation methods of the present invention are not limited thereto.

[0042] Example 1

[0043] A positive electrode material, comprising a base material and a coating material coated on the outer surface of the base material, wherein the coating material has a chemical formula of ABO3, wherein A is La and B is Mn; and the base material has a chemical formula of LiCo x M y O2, where M is Mo 6+ , wherein x+y=1; a chemical formula of LiCo is formed between the base material and the coating material 0.99 1Mo 0.007 La 0.001Mn 0.001 The O2 interface.

[0044] The preparation method of the positive electrode material is:

[0045] 1) Co3O4, Li2CO3 and MoO3 are weighed according to a Li:Co molar ratio of 1.05:1 and a Mo:Co molar ratio of 0.007, and the materials are mixed evenly by a high-speed mixer, and then the materials are placed in a tube furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6h, and then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20h, and then the materials are crushed and powdered to obtain a Mo-doped lithium cobalt oxide semi-finished product;

[0046] 2) dissolving La(NO3)3·6H2O and Mn(NO3)3 in ethanol, adding the Mo-doped lithium cobalt oxide semi-finished product obtained in step 1), stirring evenly, and placing at 80°C until the ethanol is completely volatilized; placing the materials in a tube furnace, heating to 1000°C at 4°C / min, and sintering at 1000°C for 5h, at which time a LaMnO3 coating material is in situ generated on the surface of the Mo-doped lithium cobalt oxide semi-finished product; wherein the molar ratio of La to Mn is 1, and the molar ratio of La to Mo in the matrix material is 0.001; the matrix material refers to the Mo-doped lithium cobalt oxide semi-finished product, and the same is true below, which will not be repeated;

[0047] 3) The material obtained in step 2) is heated to 1000°C at 5°C / min, and then sintered at 1000°C in an air atmosphere for 10 hours, and the material is crushed to obtain finished lithium cobalt oxide. Figure 2 TEM and secondary ion mass spectrometry tests show that the finished lithium cobalt oxide contains LiCo 0.991 Mo 0.007 La 0.001 Mn 0.001 O2 interface.

[0048] Preparation of positive electrode sheet: The positive electrode material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) prepared above are fully stirred in a N-methyl methyl pyrrolidone solvent system at a mass ratio of 96:2.5:1.5. After stirring evenly, a positive electrode slurry is obtained, and the slurry is coated on Al foil, baked, rolled, and cut into strips to obtain a positive electrode sheet.

[0049] Preparation of negative electrode sheet: Graphite, conductive agent carbon nanotube, binder styrene butadiene rubber, and thickener sodium carboxymethyl cellulose are stirred and mixed in deionized water at a mass ratio of 96.5:1.5:1:1. After being mixed evenly, the negative electrode slurry is coated on Cu foil, baked, rolled, and cut into strips to obtain a negative electrode sheet.

[0050] Preparation of isolation membrane: Polyethylene (PE) polymer film is used as isolation membrane.

[0051] Preparation of electrolyte: The organic solvents are uniformly mixed according to the mass ratio to obtain an organic solvent mixture, the specific mass ratio is: ethylene carbonate (EC): propyl propionate (PP): vinylene carbonate (VC): diethyl carbonate (DEC): propylene carbonate (PC) = 20:28:2:30:20. Lithium salt LiPF6 is added to the organic solvent mixture, the mass ratio of LiPF6 to the organic solvent mixture is 9:91, and the electrolyte of the lithium ion battery is obtained after uniform mixing.

[0052] Preparation of lithium-ion batteries: stack the positive electrode sheet, separator, and negative electrode sheet in order, and wind them to obtain an electrode assembly. When folding the electrode sheets, pay attention to the separator to completely separate the positive and negative electrode sheets. Put the electrode assembly in a packaging shell, inject electrolyte into the packaging shell and package it, and finally obtain a lithium-ion battery.

[0053] Example 2

[0054] The difference from Example 1 is that the sintering time in the preparation step 3) is 24 hours.

[0055] The rest is the same as in Example 1 and will not be described again here.

[0056] Example 3

[0057] The difference from Example 1 is that the sintering time in the preparation step 3) is 55 h.

[0058] The rest is the same as in Example 1 and will not be described again here.

[0059] Example 4

[0060] The difference from Example 1 is that the sintering time in the preparation step 3) is 60 hours.

[0061] The rest is the same as in Example 1 and will not be described again here.

[0062] Example 5

[0063] The difference from Example 1 is that in the preparation step 3), the temperature is first raised to 500°C at 5°C / min, and then sintered in an air atmosphere at 500°C for 55h.

[0064] The rest is the same as in Example 1 and will not be described again here.

[0065] Example 6

[0066] The difference from Example 1 is that in the preparation step 3), the temperature is first raised to 700° C. at 5° C. / min, and then sintered at 700° C. in an air atmosphere for 55 hours.

[0067] The rest is the same as in Example 1 and will not be described again here.

[0068] Example 7

[0069] The difference from Example 6 is that in the preparation step 1), the raw materials are Co3O4, Li2CO3 and SeO3 with a Li:Co molar ratio of 1.05:1 and a Se:Co molar ratio of 0.007.

[0070] The rest is the same as in Example 6 and will not be described again here.

[0071] Example 8

[0072] The difference from Example 1 is that in preparation step 2), the molar ratio of La to Mo in the matrix material is 0.0005; in step 3), the temperature is first raised to 700° C. at 5° C. / min, and then sintered at 700° C. in air atmosphere for 55 hours.

[0073] The rest is the same as in Example 6 and will not be described again here.

[0074] Example 9

[0075] The difference from Example 1 is that in preparation step 2), the molar ratio of La to Mo in the matrix material is 0.0015; in step 3), the temperature is first raised to 700° C. at 5° C. / min, and then sintered at 700° C. in air atmosphere for 55 hours.

[0076] The rest is the same as in Example 6 and will not be described again here.

[0077] Example 10

[0078] The difference from Example 1 is that in preparation step 2), the molar ratio of La to Mo in the matrix material is 0.002; in step 3), the temperature is first raised to 700° C. at 5° C. / min, and then sintered at 700° C. in air atmosphere for 55 hours.

[0079] The rest is the same as in Example 6 and will not be described again here.

[0080] Embodiment 11

[0081] The difference from Example 1 is that in preparation step 2), the molar ratio of La to Mo in the matrix material is 0.003; in step 3), the temperature is first raised to 700° C. at 5° C. / min, and then sintered at 700° C. in air atmosphere for 55 hours.

[0082] The rest is the same as in Example 6 and will not be described again here.

[0083] Comparative Example 1

[0084] After Co3O4 and Li2CO3 are weighed according to a Li:Co molar ratio of 1.05:1, the materials are mixed evenly using a high-speed mixer, and then placed in a tubular furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6 hours, then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20 hours, the material is crushed and powdered to obtain a finished lithium cobalt oxide product.

[0085] Comparative Example 2

[0086] 1) Co3O4, Li2CO3 and Mg2(OH)2CO3 are weighed according to a Li:Co molar ratio of 1.05:1 and a Mg:Co molar ratio of 0.007, and the materials are mixed evenly using a high-speed mixer. The materials are then placed in a tubular furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6 hours, then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20 hours, and then the materials are crushed and powdered to obtain a Mg-doped lithium cobalt oxide semi-finished product.

[0087] 2) The semi-finished lithium cobalt oxide obtained in step 1) is homogenized with Al2O3, wherein the molar ratio of Al to Co is 0.001, and then the temperature is raised to 1000°C at 5°C / min, and then sintered for 10 hours in an air atmosphere at 1000°C, the material is crushed, and a finished lithium cobalt oxide product doped with Mg and coated with Al is obtained after powdering.

[0088] Comparative Example 3

[0089] 1) Co3O4, Li2CO3 and Al2O3 are weighed according to a Li:Co molar ratio of 1.05:1 and an Al:Co molar ratio of 0.007, and the materials are mixed evenly using a high-speed mixer. The materials are then placed in a tubular furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6 hours, then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20 hours, and then the materials are crushed and powdered to obtain an Al-doped lithium cobalt oxide semi-finished product.

[0090] 2) The semi-finished lithium cobalt oxide obtained in step 1) is mixed evenly with Al2O3, wherein the molar ratio of Al to Co is 0.001, and then the temperature is increased to 1000°C at 5°C / min, and then sintered at 1000°C in an air atmosphere for 10 hours, the material is crushed, and powdered to obtain a finished lithium cobalt oxide product doped with Al and coated with Al.

[0091] Comparative Example 4

[0092] 1) Co3O4, Li2CO3 and TiO2 are weighed according to a Li:Co molar ratio of 1.05:1 and a Ti:Co molar ratio of 0.007, and the materials are mixed evenly using a high-speed mixer. The materials are then placed in a tubular furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6 hours, then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20 hours. The materials are then crushed and powdered to obtain a Ti-doped lithium cobalt oxide semi-finished product.

[0093] 2) The semi-finished lithium cobalt oxide obtained in step 1) is homogenized with Al2O3, wherein the molar ratio of Al to Co is 0.001, and then sintered at 1000°C in an air atmosphere for 10 hours, the material is crushed, and powdered to obtain a finished lithium cobalt oxide product doped with Ti and coated with Al.

[0094] Comparative Example 5

[0095] The difference from Comparative Example 3 is that the sintering time in step 2) is 55 h.

[0096] The rest is the same as Comparative Example 3 and will not be described again.

[0097] Comparative Example 6

[0098] 1) Co3O4, Li2CO3 and MoO3 are weighed according to a Li:Co molar ratio of 1.05:1 and a Mo:Co molar ratio of 0.007, and the materials are mixed evenly using a high-speed mixer. The materials are then placed in a tubular furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6 hours, then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20 hours, and then the materials are crushed and powdered to obtain a Mo-doped lithium cobalt oxide semi-finished product.

[0099] 2) The semi-finished lithium cobalt oxide obtained in step 1) is homogenized with Al2O3, wherein the molar ratio of Al to Co is 0.001, and then sintered at 1000°C in an air atmosphere for 10 hours. The material is crushed and powdered to obtain a finished lithium cobalt oxide product doped with Mo and coated with Al.

[0100] Comparative Example 7

[0101] 1) Co3O4, Li2CO3 and Al2O3 are weighed according to a Li:Co molar ratio of 1.05:1 and an Al:Co molar ratio of 0.007, and the materials are mixed evenly using a high-speed mixer. The materials are then placed in a tubular furnace, first heated to 800°C at 10°C / min, and then sintered at 800°C in an air atmosphere for 6 hours, then heated to 1100°C at 5°C / min, and then sintered at 1100°C in an air atmosphere for 20 hours, and then the materials are crushed and powdered to obtain an Al-doped lithium cobalt oxide semi-finished product.

[0102] 2) Dissolve La(NO3)3·6H2O and Mn(NO3)3 in ethanol, add the Al-doped lithium cobalt oxide semi-finished product prepared in step 1), wherein the molar ratio of La to Co is 0.001; the mass of La(NO3)3·6H2O added is 0.002% of the mass of the Al-doped lithium cobalt oxide semi-finished product; after stirring evenly, place at 80°C until the ethanol is completely volatilized. Place the material in a tubular furnace, heat to 1000°C at 4°C / min, and sinter at 1000°C for 10 hours to obtain a finished lithium cobalt oxide product doped with Al and coated with LaMnO3.

[0103] The performance of the positive electrode materials obtained in the above Examples 1 to 11 and Comparative Examples 1 to 7 was tested.

[0104] The test results are shown in Table 1 below.

[0105] (1) Low temperature test

[0106] At room temperature, the soft-pack battery cell is charged to 4.53V at a constant current and constant voltage of 0.5C, with a cut-off current of 0.02C, and discharged to 3.0V at a constant current of 0.2C at room temperature. The room temperature discharge capacity is recorded as Cap1;

[0107] At room temperature, the soft-pack battery cell is charged to 4.53V at 0.5C constant current and constant voltage, with a cut-off current of 0.02C, and discharged to 3.0V at -10℃ at 0.2C constant current. The obtained -10℃ discharge capacity is recorded as Cap2;

[0108] Low temperature performance is the value of Cap2 / Cap1

[0109] (2) Cycle performance test: The soft pack battery cell is placed in a 45°C environment, charged at 3C constant current and constant voltage to 4.53V, the cut-off current is 0.05C, and discharged at 0.7C constant current to 3.0V. This step of charge and discharge is recorded as one cycle. Repeat this cycle until the capacity retention rate of the battery cell is less than 80%. The battery cell is stopped from being tested and the cycle number of this battery cell is recorded. The test results are shown in Table 1 below.

[0110] Table 1

[0111]

[0112]

[0113] As shown in Table 1, the present invention can effectively improve the cycle performance and low temperature stability of lithium cobalt oxide by doping +6 high-valent ions in the positive electrode material and coating the surface of the positive electrode material with ABO3 (A is one of La, Y, and Zr), and improve the electrochemical performance of lithium cobalt oxide under high voltage.3+ The more lattice oxygen next to the position enhances the stability of lithium cobalt oxide, and because the ionic radius is larger than Co 3+ , which will increase the c-axis spacing and enhance the diffusion rate of Li+; the positive electrode material prepared by the ABO3 type coating has a more stable structure and better electrical performance.

[0114] From the test results of the above embodiments and comparative examples, it can be seen that the positive electrode material of the comparative example does not contain LiCo a M b A z B w O2 (a + b + z + w = ​​1) phase interface, its cycle performance and low temperature performance are significantly worse than the positive electrode material of the embodiment. In addition, the performance of the positive electrode material is related to the type of doping elements, the type of coating material, the sintering process, and the element ratio of the material. It can be seen from Examples 1-6 that too short or too long coating time, as well as too high sintering temperature, will affect the LiCo a M b A z B w The formation effect of O2 interface, LiCo a M b A z B w O2 can accelerate Li + migration and affects the low temperature properties of the material.

[0115] It can be seen from Examples 6 and 8-11 that when the molar ratio of the A element (La or Se) in the coating material to the M element (Mo) in the matrix material is 0.0002 to 0.002, the positive electrode material has better cycle performance and low temperature performance.

[0116] Compared with Comparative Examples 2 to 6, Comparative Example 1 has better low temperature performance. The reason is that Comparative Examples 2 to 6 use Al2O3 coating, which forms an inert coating layer on the surface of lithium cobalt oxide particles, affecting the Li + de-embedding, thus affecting the performance of the material.

[0117] In summary, the positive electrode material provided by the present invention has better structural stability and electrochemical performance. The lithium cobalt oxide positive electrode material prepared by the present invention, doping with +6 high-valent ions can improve the stability of the coating, and at the same time, the coating material is firmly connected to the surface of the lithium cobalt oxide substrate, which can effectively prevent the lithium cobalt oxide coating material from falling off from the lithium cobalt oxide substrate during stirring, rolling, and repeated charging, and ensure the stability of the lithium cobalt oxide surface. The coating layer on the surface can reduce the corrosion of the lithium cobalt oxide surface by the electrolyte during the long-term circulation of lithium cobalt oxide, and the coating material falls off from the lithium cobalt oxide substrate. The phase interface generated between the matrix material and the coating material can improve the low-temperature stability of lithium cobalt oxide and improve the electrochemical performance of lithium cobalt oxide under high voltage.

[0118] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A positive electrode material, characterized in that: The invention comprises a base material and a coating material coated on the outer surface of the base material, wherein the coating material has a chemical formula of ABO3, wherein A is one of La, Y, and Zr, and B is one of Co, Ni, Mn, and Ti; and the base material has a chemical formula of LiCo x M y O2, where M is Mo 6+ , W 6+ 、Se 6+ One or more of the following, wherein x+y=1; a chemical formula of LiCo is formed between the matrix material and the coating material. a M b A z B w The interface of O2, where a+b+z+w=1.

2. The positive electrode material according to claim 1, characterized in that The coating material ABO3 is a cubic or octahedral perovskite.

3. The positive electrode material according to claim 1, characterized in that The molar ratio of the element A in the coating material to the element M in the base material is 0.0002 to 0.

002.

4. The positive electrode material according to claim 1, characterized in that The matrix material LiCo x M y The molar ratio of Li, Co and M in O2 is 1.05:1:0.001~0.

03.

5. A method for preparing a positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Weigh the cobalt oxide, lithium salt and M oxide according to the molar ratio, then mix the materials evenly, then place the materials in a tube furnace for firing, crush the fired materials, and obtain a semi-finished lithium cobalt oxide doped with M after powdering; S2, dissolving A(NO3)3·6H2O and soluble salt of B in an alcohol solution, then adding the doped M lithium cobalt oxide semi-finished product prepared in S1, stirring evenly, leaving it until the alcohol solution is completely volatilized, and then placing the materials in a tube furnace for firing; S3, heating the material obtained in S2 to 500-1100°C at 3-5°C / min, sintering it in an air atmosphere for 8-55h, and then crushing the material to obtain the positive electrode material.

6. The method for preparing the positive electrode material according to claim 5, characterized in that: In step S1, the molar ratio of Co in the cobalt oxide to Li in the lithium salt is Li:Co=1.05:1-1.15:1, and the molar ratio of Co in the cobalt oxide to M in the M oxide is M:Co=0.01-0.

03.

7. The method for preparing the positive electrode material according to claim 5, characterized in that: In step S1, the firing process is to first heat the tube furnace to 600-800°C at 8-10°C / min, then sinter at a constant temperature and air atmosphere for 5-7h, then heat to 1000-1200°C at 3-5°C / min, and then sinter at a constant temperature and air atmosphere for 18-22h.

8. The method for preparing the positive electrode material according to claim 5, characterized in that: In step S2, the firing process is to heat the tube furnace to 900-1100°C at 3-5°C / min, and then sinter for 4-6h.

9. A positive electrode sheet, characterized in that: The positive electrode material comprises the positive electrode material according to any one of claims 1 to 4.

10. A secondary battery, characterized in that: Including the positive electrode sheet as described in claim 9.