Substrate, negative electrode material, and secondary battery
By controlling the particle size distribution of the matrix and negative electrode materials, ensuring uniform deposition of active substances and reducing particle gaps, using carbon materials to prepare spherical negative electrode materials, solving the expansion rate and energy density of negative electrode materials in the charge and discharge cycle, and improving the battery cycling performance and charge and discharge efficiency.
Patent Information
- Application Number
- CN202411385249.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
The uneven deposition of silicon materials on the porous substrate leads to an increase in the expansion rate and cracking and powdering risk of the negative electrode material during the charge and discharge cycle, and the gap between the particles of the negative electrode material is large, which reduces the energy density of the electrode sheet and the charge and discharge efficiency of the battery. .
By controlling the average and standard deviation of the particle size of the matrix and negative electrode materials, we ensure uniform deposition of active substances, reduce particle gaps, and improve the distribution uniformity of conductive agents and electrolytes. Carbon materials or their composite materials are used as the matrix, combined with electrostatic spraying method Prepare the negative electrode material to form a spherical structure to optimize the particle size distribution.
It reduces the expansion rate and cracking and powdering risk of the negative electrode material, improves the cycle performance and charge and discharge efficiency of the battery, and enhances the energy density and dynamic performance of the battery.
Smart Images

Figure CN119092693A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical energy storage, and in particular to a substrate, a negative electrode material and a secondary battery. Background Art
[0002] The negative electrode material may include a matrix and active materials deposited in the pores of the matrix, such as silicon materials. However, the silicon material may be deposited unevenly on the porous matrix, resulting in uneven stress distribution after the active ions are embedded, increasing the expansion rate and cracking and pulverization risk of the negative electrode material during cycling, and accelerating capacity decay. In addition, when the above-mentioned negative electrode material is prepared into an electrode sheet, there will be large gaps between the negative electrode material particles, which reduces the energy density of the electrode sheet, and these larger pores will also affect the contact and infiltration of the electrolyte with the negative electrode material, reducing the charge and discharge efficiency and kinetic performance of the battery. Summary of the invention
[0003] In view of this, the present application provides a substrate, a negative electrode material and a secondary battery to solve at least one of the above technical problems.
[0004] To achieve the above objectives, in a first aspect, the present application provides a substrate having pores, the substrate comprising a carbon material, the average particle size D0 of the substrate being 5.5 μm to 9.5 μm, and the standard deviation S0 of the particle size of the substrate being 0.08 to 0.35.
[0005] In some possible implementations, the relative standard deviation S0 / D0 of the particle size of the matrix is 0.008 to 0.064.
[0006] In some possible implementations, the matrix has a spherical structure, and the sphericity of the matrix is 0.9 to 1.0.
[0007] In some possible implementations, the total pore volume of the matrix is 0.5 cm 3 / g to 2.0 cm 3 / g.
[0008] In some possible implementations, the average pore size of the matrix is 0.1 nm to 8 nm.
[0009] In some possible implementations, the carbon material includes one or more of artificial graphite, amorphous carbon, activated carbon, and mesophase carbon microbeads.
[0010] In a second aspect, the present application provides a negative electrode material, which includes a matrix and an active substance, the matrix has pores, at least part of the active substance is disposed in the pores of the matrix, the average particle size D1 of the negative electrode material is 5.5 μm to 9.5 μm, and the standard deviation S1 of the particle size of the negative electrode material is 0.1 to 0.35.
[0011] In some possible implementations, the relative standard deviation S1 / D1 of the particle size of the negative electrode material is 0.010 to 0.064.
[0012] In some possible implementations, based on the mass of the negative electrode material, the mass proportion of oxygen element in the negative electrode material is 0.05% to 4.0%.
[0013] In some possible implementations, the specific surface area of the negative electrode material is less than or equal to 10 m 2 / g.
[0014] In some possible implementations, the powder conductivity of the negative electrode material is 0.05 S / m to 5 S / m.
[0015] In some possible implementations, the surface capacity density of the negative electrode material is 4.55 mAh / cm 2 Up to 6.10 mAh / cm 2 .
[0016] In some possible implementations, the pore volume of the negative electrode material is less than or equal to 0.15 cm 3 / g.
[0017] In some possible implementations, the average pore size of the negative electrode material is less than or equal to 10 nm.
[0018] In some possible implementations, the negative electrode material has a quasi-spherical structure, and the sphericity of the negative electrode material is 0.9 to 1.0.
[0019] In some possible implementations, the average value D0 of the particle size of the matrix is 5.5 μm to 9.5 μm, and the standard deviation S0 of the particle size of the matrix is 0.08 to 0.35.
[0020] In some possible implementations, the relative standard deviation S0 / D0 of the particle size of the matrix is 0.008 to 0.064.
[0021] In some possible implementations, the matrix has a spherical structure, and the sphericity of the matrix is 0.9 to 1.0.
[0022] In some possible implementations, the total pore volume of the matrix is 0.5 cm 3 / g to 2.0 cm 3 / g.
[0023] In some possible implementations, the average pore size of the matrix is 0.1 nm to 8 nm.
[0024] In some possible implementations, the matrix includes a carbon material, and the carbon material includes one or more of artificial graphite, amorphous carbon, activated carbon, and mesophase carbon microbeads.
[0025] In some possible implementations, the matrix includes a non-carbon material, and the non-carbon material includes at least one of metal oxides, silicides, silicates, phosphates, titanates and aluminum borates; the metal oxides include one or more of aluminum oxide, zirconium oxide, germanium dioxide and manganese dioxide; the silicides include one or more of silicon carbide and silicon nitride; the silicates include one or more of cordierite, mullite and zeolite; the phosphates include one or more of aluminum phosphate, magnesium phosphate, calcium phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate and lanthanum phosphate; the titanates include one or more of calcium titanate, iron titanate, lithium titanate and barium titanate.
[0026] In some possible implementations, the active material includes one or more of Si, Li, Na, K, Sn, Ge, Fe, Mg, Ti, Zn, Al, P, and Cu.
[0027] In some possible implementations, the matrix includes a carbon matrix, the active substance includes a silicon material, the silicon material includes one or more of amorphous silicon, crystalline silicon, silicon oxide, silicon alloy, and a composite of crystalline silicon and amorphous silicon, and based on the mass of the negative electrode material, the mass proportion of carbon element in the negative electrode material is 30% to 70%.
[0028] In some possible implementations, based on the mass of the negative electrode material, the mass proportion of silicon element in the negative electrode material is 30% to 80%.
[0029] In a third aspect, the present application further provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer comprises the above-mentioned negative electrode material.
[0030] In a fourth aspect, the present application also provides a secondary battery, comprising the above-mentioned negative electrode sheet.
[0031] In the present application, by controlling the average value of the particle size of the matrix or the negative electrode material and the standard deviation of the particle size to meet the preset conditions, the active material can be deposited more evenly on the matrix, so that when the negative electrode material embeds active ions during the charge and discharge cycle, it helps to make the stress distribution in the negative electrode material particles more uniform, reduce the expansion rate and the risk of cracking and pulverization of the negative electrode material during the cycle, help maintain a stable capacity and improve the cycle performance; at the same time, when the preset conditions are met, it is helpful to reduce the gap between the negative electrode material particles, thereby helping to improve the volume energy density of the negative electrode sheet prepared from the negative electrode material, and also help to improve the distribution uniformity of the conductive agent and the electrolyte between the negative electrode material, improve the contact and infiltration between the electrolyte and the negative electrode material, and help to improve the charge and discharge efficiency and kinetic performance of the resulting secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application during charging.
[0033] Figure 2 A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application during discharge.
[0034] Figure 3 This is a scanning electron microscope image of the negative electrode material provided in Example 1 of the present application.
[0035] Figure 4 This is a scanning electron microscope image of the negative electrode material particles provided in Example 1 of the present application.
[0036] Figure 5 This is an energy dispersive X-ray spectrum of the carbon element in the negative electrode material particles provided in Example 1 of the present application.
[0037] Figure 6 This is the energy dispersive X-ray spectrum of the silicon element in the negative electrode material particles provided in Example 1 of the present application.
[0038] Main component symbols Electrode assembly 100 Positive electrode 101 Negative electrode 102 Isolation film 103. DETAILED DESCRIPTION
[0039] The embodiments of the present application are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application; it should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present application; in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other; many specific details are elaborated in the following description to facilitate a full understanding of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0040] An embodiment of the present application provides a secondary battery, comprising a housing, an electrode assembly and an electrolyte. The electrode assembly and the electrolyte are both located in the housing.
[0041] The outer shell may be a packaging bag encapsulated by an encapsulation film (such as an aluminum-plastic film), for example, a soft-pack battery. In other embodiments, it may also be a steel shell battery, an aluminum shell battery, etc.
[0042] See also Figure 1 and Figure 2The electrode assembly 100 includes a positive electrode sheet 101, a negative electrode sheet 102 and a separator 103. The separator 103 is disposed between the positive electrode sheet 101 and the negative electrode sheet 102. When an electrolyte (not shown) is provided, when charging, refer to Figure 1 , active ions (such as lithium ions) are deintercalated from the lattice of the positive electrode material (such as the lithiated intercalation compound) of the positive electrode sheet 101, pass through the separator 103 through the electrolyte, reach the negative electrode sheet 102 and insert into the lattice of the negative electrode material. Figure 2 , active ions (such as lithium ions) are deintercalated from the lattice of the negative electrode material of the negative electrode sheet 102, pass through the isolation membrane 103 through the electrolyte, reach the positive electrode sheet 101 and are embedded in the lattice of the positive electrode material (such as the lithiated intercalation compound), generating electrons that travel from the negative electrode sheet 102 through the external circuit to the positive electrode sheet 101, and the reverse movement of the electrons forms an electric current that can be used by electrical appliances.
[0043] In some embodiments, the electrode assembly 100 may be a laminated structure, which is formed by alternately stacking the positive electrode sheet 101, the separator 103, and the negative electrode sheet 102. In other embodiments, the electrode assembly 100 may also be a wound structure, which is formed by stacking the positive electrode sheet 101, the separator 103, and the negative electrode sheet 102 in sequence and then winding them.
[0044] Positive electrode The positive electrode sheet 101 includes a positive electrode current collector and a positive electrode material active layer provided on at least one surface of the positive electrode current collector. The positive electrode current collector may be made of aluminum foil or nickel foil, or may be any composite current collector disclosed in the prior art, such as but not limited to the current collector formed by combining the aforementioned conductive foil and a polymer substrate. The positive electrode material active layer includes a positive electrode active material, and the positive electrode active material includes a compound that can reversibly embed and deintercalate lithium ions (i.e., a lithiated intercalation compound). In some embodiments, the positive electrode active material may include a lithium transition metal composite oxide. The lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese and nickel. In some embodiments, the positive electrode active material may include but is not limited to lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material (NCM), lithium manganese oxide (LiMn2O4), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4) or at least one of lithium iron phosphate (LiFePO4).
[0045] The positive electrode material active layer also includes a binder to bond the positive electrode active material particles to facilitate the formation of a film layer, and at the same time, it can also improve the bonding force between the positive electrode material active layer and the positive electrode current collector. In some embodiments, the binder may include but is not limited to at least one of polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon.
[0046] The positive electrode material active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0047] Negative plate The negative electrode sheet 102 includes a negative electrode current collector and a negative electrode material active layer disposed on at least one surface of the negative electrode current collector. The negative electrode current collector may be at least one of copper foil, nickel foil, stainless steel foil, titanium foil or a carbon-based current collector, or may be any composite current collector disclosed in the prior art, such as but not limited to a current collector formed by combining the aforementioned conductive foil and a polymer substrate.
[0048] The negative electrode material active layer includes a negative electrode material, the negative electrode material includes a matrix and an active material, the matrix has pores, at least part of the active material is disposed in the pores of the matrix, the average value D1 of the particle size of the negative electrode material is 5.5 μm to 9.5 μm, and the standard deviation S1 of the particle size of the negative electrode material is 0.1 to 0.35. For example, the average value D1 of the particle size of the negative electrode material can be 5.5 μm, 6.0 μm, 6.5 μm, 7.0 μm, 7.5 μm, 8.0 μm, 8.5 μm, 9.0 μm, 9.5 μm, or any value within the range formed by any two of the above values. The standard deviation S1 of the particle size of the negative electrode material can be 0.1, 0.15, 0.20, 0.25, 0.30, 0.35, or any value within the range formed by any two of the above values.
[0049] In the present application, when the average value D1 of the particle size of the negative electrode material constituting the negative electrode sheet 102 and the standard deviation S1 of the particle size meet the above conditions, it is conducive to making the active material more evenly deposited on the substrate, so that when the negative electrode material embeds active ions during the charge and discharge cycle, it helps to make the stress distribution in the negative electrode material particles more uniform, reduce the expansion rate and cracking and pulverization risk of the battery prepared by the negative electrode material during the cycle, help maintain the stable capacity of the battery prepared by the negative electrode material and improve the cycle performance of the battery prepared by the negative electrode material; at the same time, when the above conditions are met, it is conducive to reducing the gap between the negative electrode material particles, thereby helping to improve the volume energy density of the negative electrode sheet 102, and also conducive to improving the uniformity of the distribution of the conductive agent and the electrolyte between the negative electrode material, improving the contact and infiltration effect between the electrolyte and the negative electrode material, and helping to improve the charge and discharge efficiency and kinetic performance of the battery prepared by the negative electrode material.
[0050] It should be noted that, on the one hand, when the average value D1 of the particle size of the negative electrode material constituting the negative electrode sheet 102 is too small, such as less than 5.5 μm, it reflects that the particle size of the negative electrode material particles is relatively small as a whole. The formation of such a negative electrode material will be accompanied by poor pore uniformity of the matrix in the negative electrode material and a relatively large specific surface area, resulting in uneven deposition of the active substance on the matrix, which in turn leads to uneven distribution of expansion stress of the negative electrode material during the charge and discharge cycle, and an increase in the expansion rate. The relatively large specific surface area easily increases the contact between the active substance and the electrolyte, resulting in oxidation of the active substance (such as silicon material), resulting in a decrease in the surface capacity density and the first coulomb efficiency of the negative electrode material. When the average value D1 of the particle size of the negative electrode material constituting the negative electrode sheet 102 is too large, such as greater than 9.5 μm, it reflects that the particle size of the negative electrode material particles is too large, resulting in a small pore volume of the matrix in the negative electrode material, and a small space available for adsorbing active substances, which will lead to a decrease in the surface capacity density. At this time, it is also easy to form a large gap between the negative electrode materials, which is not conducive to the uniform distribution of the conductive agent and the electrolyte between the negative electrode materials, and will also lead to uneven expansion stress, and may further cause an increase in the expansion rate and a decrease in the first coulomb efficiency. On the other hand, when the standard deviation S1 of the particle size of the negative electrode material constituting the negative electrode sheet 102 is too large, it means that the discrete degree of the particle size distribution of the negative electrode material particles is too large. Even if the average value of the particle size of the negative electrode material meets the set conditions, there are a certain amount of negative electrode material particles with too large or too small particle sizes inside. As mentioned above, these negative electrode material particles with too large or too small particle sizes will have adverse effects.
[0051] Therefore, the average value D1 and the standard deviation S1 of the particle size of the negative electrode material constituting the negative electrode sheet 102 are controlled to meet the predetermined conditions, so that the negative electrode material constituting the negative electrode sheet 102 has a suitable particle size as a whole and the dispersion of the particle size distribution is low, which can reduce the risk of high expansion rate caused by deposition or uneven distribution of active materials in the negative electrode material, and can also reduce the risk of decreased charge and discharge efficiency caused by uneven distribution of conductive agents or electrolytes between negative electrode materials. Therefore, it is beneficial to improve the charge and discharge efficiency and kinetic performance of the secondary battery.
[0052] In some embodiments, the relative standard deviation S1 / D1 of the particle size of the negative electrode material satisfies 0.010≤S1 / D1≤0.064. For example, S1 / D1 can be 0.010, 0.020, 0.025, 0.030, 0.035, 0.040, 0.045, 0.050, 0.055, 0.060, 0.064, or any value within the range formed by any two of the above values. When the above conditions are met, it is conducive to forming a smaller gap between the negative electrode materials, reducing the risk of forming a larger gap between the negative electrode materials, thereby improving the uniform distribution of the electrolyte or conductive agent between the substrates, and further promoting the uniform distribution of the expansion stress.
[0053] In some embodiments, based on the mass of the negative electrode material, the mass percentage of oxygen in the negative electrode material is 0.05% to 4.0%. For example, the mass percentage of oxygen in the negative electrode material can be 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or any value within the range formed by any two of the above values. The oxygen in the negative electrode material includes oxygen in the oxygen-containing functional groups on the matrix and oxygen formed after oxidation of the active material (such as silicon material). Controlling the mass percentage of oxygen in the negative electrode material within the above range is conducive to reducing the oxidation of the active material (such as silicon material), thereby helping to reduce the risk of a decrease in the surface capacity density of the negative electrode material.
[0054] In some embodiments, the specific surface area of the negative electrode material is less than or equal to 10 m 2 / g. For example, the specific surface area of the negative electrode material can be 1 m 2 / g, 2 m 2 / g, 3 m 2 / g, 4 m 2 / g, 5 m 2 / g, 6 m 2 / g, 7 m 2 / g, 8 m 2 / g, 9 m 2 / g, 10 m 2 / g or any value within the range formed by any two of the above values. Controlling the specific surface area of the negative electrode material within the above range can reduce the formation of SEI on the surface of the negative electrode material, thereby improving the first coulombic efficiency of the battery prepared with the negative electrode material. When the specific surface area of the negative electrode material is too large, the contact between the active material and the electrolyte in the negative electrode material increases, which makes it easier to cause oxidation of the active material and reduce the surface capacity density of the negative electrode material.
[0055] In some embodiments, the pore volume of the negative electrode material is less than or equal to 0.15 cm 3 / g. For example, the pore volume of the negative electrode material can be 0.15 cm 3 / g, 0.13 cm 3 / g, 0.11 cm 3 / g, 0.09 cm 3 / g, 0.08 cm 3 / g, 0.07 cm 3 / g, 0.06 cm 3 / g, 0.05 cm 3 / g or any value within the range formed by any two of the above values. The pore volume of the negative electrode material within the above range indicates that the active material is well deposited in the pores of the matrix, and such pore volume can further improve the surface capacity density of the negative electrode material.
[0056] In some embodiments, the surface capacity density of the negative electrode material is 4.55 mAh / cm 2 Up to 6.10 mAh / cm 2 For example, the surface capacity of the negative electrode material can be 4.55 mAh / cm 2 、4.60 mAh / cm 2 、4.65 mAh / cm 2 、4.70 mAh / cm 2 、4.80mAh / cm 2 、5.10 mAh / cm 2 、5.50 mAh / cm 2 、5.90 mAh / cm 2 、6.10 mAh / cm 2 Or any value within the range formed by any two of the above values.
[0057] In some embodiments, the powder conductivity of the negative electrode material is 0.05 S / m to 5 S / m. For example, the powder conductivity of the negative electrode material can be 0.05 S / m, 1 S / m, 1.5 S / m, 2 S / m, 2.5 S / m, 3 S / m, 3.5 S / m, 4 S / m, 4.5 S / m, 5 S / m, or any value within the range formed by any two of the above values.
[0058] In some embodiments, the average pore size of the negative electrode material is less than or equal to 10 nm. For example, the average pore size of the negative electrode material can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any value within the range formed by any two of the above values.
[0059] In some embodiments, the negative electrode material has a spherical structure, and the sphericity of the negative electrode material is 0.9 to 1.0. Compared with the negative electrode material formed by the irregular polyhedron matrix, the negative electrode material with a spherical structure has a relatively smaller specific surface area, which is conducive to adjusting the contact and wettability between the negative electrode material and the electrolyte or the conductive agent, and when the negative electrode material has a spherical structure, it is conducive to forming a smaller gap between the negative electrode materials, thereby improving the uniform distribution of the electrolyte or the conductive agent between the negative electrode materials, and further promoting the uniform distribution of the expansion stress.
[0060] In some embodiments, the average value D0 of the particle size of the matrix is 5.5 μm to 9.5 μm, and the standard deviation S0 of the particle size of the matrix is 0.08 to 0.35. For example, the average value D0 of the particle size of the matrix can be 5.5 μm, 6.0 μm, 6.5 μm, 7.0 μm, 7.5 μm, 8.0 μm, 8.5 μm, 9.0 μm, 9.5 μm, or any value within the range composed of any two of the above values. The standard deviation S0 of the particle size of the matrix can be 0.08, 0.1, 0.15, 0.20, 0.25, 0.30, 0.35, or any value within the range composed of any two of the above values. Since the active material is distributed in the pores of the matrix to form the negative electrode material, it can be understood that when the average value of the particle size of the matrix is controlled to be within the above range, it is helpful to form a negative electrode material whose average value of the particle size meets the conditions. In some embodiments, the relative standard deviation S0 / D0 of the particle size of the matrix is 0.008 to 0.064.
[0061] In some embodiments, the substrate has a spherical structure, and the sphericity of the substrate is 0.9 to 1.0. Compared with the substrate of an irregular polyhedron, the substrate of a spherical structure has a relatively smaller specific surface area, which is conducive to adjusting the contact and wettability between the negative electrode material and the electrolyte or the conductive agent. When the substrate has a spherical structure, the negative electrode materials formed are conducive to forming a smaller gap, thereby improving the uniform distribution of the electrolyte or the conductive agent between the negative electrode materials, and further promoting the uniform distribution of the expansion stress.
[0062] In some embodiments, the total pore volume of the matrix is 0.5 cm 3 / g to 2.0 cm 3 / g. For example, the total pore volume of the matrix can be 0.5 cm3 / g, 0.7 cm 3 / g, 0.9 cm 3 / g, 1.1 cm 3 / g, 1.3 cm 3 / g, 1.5 cm 3 / g, 1.7 cm 3 / g, 1.9 cm 3 / g, 2.0 cm 3 / g or any value within the range formed by any two of the above values. Since the matrix has pores, a certain total pore volume provides sufficient deposition space for the active material. The present application also finds that when the total pore volume of the matrix is controlled within the above range, it is conducive to the deposition of the active material and improves the surface capacity density of the negative electrode material based on such a matrix.
[0063] In some embodiments, the average pore size of the matrix is 0.1 nm to 8 nm. For example, the average pore size of the matrix can be 0.1 nm, 0.5 nm, 1 nm, 2 nm, 3 nm, 5 nm, 6 nm, 7 nm, 8 nm, or any value within the range of any two of the above values. Since micropores (pore size <2 nm) are commonly present in the matrix, when the average pore size of the matrix is too large, it means that there are more mesopores (pore size of 2~50 nm) or macropores (pore size >50 nm), which may lead to poor pore uniformity of the pores formed in the matrix. The present application found that when the pore uniformity of the matrix is poor, it may be accompanied by an average value of the particle size of the matrix that is too small, and the deposition of the active substance in the relatively more mesopores or macropores is not conducive to its uniform distribution on the matrix, which increases the risk of uneven crushing of the matrix expansion stress.
[0064] In some embodiments, the substrate comprises a carbon material. In some embodiments, the carbon material comprises one or more of artificial graphite, amorphous carbon, activated carbon, and mesocarbon microbeads.
[0065] In some embodiments, the matrix includes a non-carbon material. In some embodiments, the non-carbon material includes at least one of a metal oxide, a silicide, a silicate, a phosphate, a titanate, and an aluminum borate. Among them, the metal oxide includes one or more of aluminum oxide, zirconium oxide, germanium dioxide, and manganese dioxide. Silicides include one or more of silicon carbide and silicon nitride. Silicates include one or more of cordierite, mullite, and zeolite. Phosphates include one or more of aluminum phosphate, magnesium phosphate, calcium phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate, and lanthanum phosphate. Titanates include one or more of calcium titanate, iron titanate, lithium titanate, and barium titanate.
[0066] In some embodiments, the active material includes one or more of Si, Li, Na, K, Sn, Ge, Fe, Mg, Ti, Zn, Al, P, and Cu.
[0067] In some embodiments, the substrate is a carbon substrate, the active material is a silicon material, and the silicon material includes one or more of amorphous silicon, crystalline silicon, silicon oxide, silicon alloy, and a composite of crystalline silicon and amorphous silicon.
[0068] In some embodiments, based on the mass of the negative electrode material, the mass proportion of the carbon element of the negative electrode material is 30% to 70%. For example, the mass proportion of the carbon element of the negative electrode material can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70% or any value within the range composed of any two of the above values. The mass proportion of the carbon element of the negative electrode material is within the above range, which is conducive to providing sufficient conductivity for the negative electrode material. In some embodiments, based on the mass of the negative electrode material, the mass proportion of the silicon element of the negative electrode material is 30% to 80%. For example, the mass proportion of the silicon element of the negative electrode material can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80% or any value within the range composed of any two of the above values. The mass proportion of the silicon element of the negative electrode material is within the above range, which is conducive to improving the surface capacity density of the negative electrode material, thereby improving the first coulombic efficiency.
[0069] The negative electrode material active layer also includes a binder to bind the negative electrode active material particles to facilitate the formation of a film layer, and can also improve the binding force between the negative electrode material active layer and the negative electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylic (ester) styrene butadiene rubber, epoxy resin or nylon, etc.
[0070] The negative electrode material active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0071] Isolation film The isolation membrane 103 includes a membrane layer with a porous structure, and its material includes but is not limited to at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, the isolation membrane can be a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane.
[0072] Electrolytes The electrolyte has the function of conducting ions between the positive electrode sheet and the negative electrode sheet. The state of the electrolyte can be one or more of a gel state, a solid state and a liquid state. In some embodiments, the electrolyte is an electrolyte. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet. In some embodiments, the electrolyte includes a lithium salt and an organic solvent. The lithium salt can be selected from but not limited to one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium tetraphenylborate (LiB(C6H5)4), lithium methanesulfonate (LiCH3SO3), lithium bis(trifluoromethanesulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethylsulfonyl)imide (LiN(SO2CF3)2, tris(trifluoromethylsulfonyl)methyl lithium (LiC(SO2CF3)3), lithium bis(oxalatoborate) (LiBOB) and lithium difluorophosphate (LiPO2F2). For example, the lithium salt is selected from LiPF6 because it can give high ionic conductivity and improve cycle characteristics. The organic solvent can be a carbonate compound, a carboxylate compound, an ether compound, Compounds, nitrile compounds, other organic solvents or combinations thereof. Examples of carbonate compounds include, but are not limited to, diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.
[0073] Another embodiment of the present application further provides a method for preparing a negative electrode material, comprising: The first step: providing a carbon source solution, the mass concentration of the carbon source is 2% to 5%, spraying the carbon source solution into the solidifying liquid by electrostatic spraying to obtain a mixed solution, the voltage of the electrostatic spraying is 1 V to 30 V, the flow rate of the electrostatic spraying is 0.5 mL / h to 5 mL / h, filtering the mixed solution to obtain a carbon precursor.
[0074] In the present application, taking the carbon matrix as an example, in the stage of obtaining the carbon precursor, by controlling the carbon source concentration, spray voltage and spray flow rate within a specific range, the particle size of the sprayed carbon precursor can be controlled to form more spherical carbon precursor particles, thereby affecting the subsequent activation, active material adsorption and densification treatment, and thus helping to obtain a carbon matrix with an average particle size D and a particle size standard deviation S that meet the range or a spherical negative electrode material that further adsorbs active substances, thereby preparing a negative electrode material with excellent surface density, expansion rate and first coulomb efficiency.
[0075] Specifically, on the one hand, when the carbon source concentration is too low, the spray particles are in the process of removing the solvent, and the solvent volatilization easily makes the prepared carbon precursor particle size smaller. At the same time, a large amount of solvent volatilization easily causes the carbon precursor to sink, resulting in a deterioration in the uniformity of the particle size, a large standard deviation of the particle size, and a large relative standard deviation of the particle size. When the carbon source concentration is too high, the carbon source in the particles sprayed by the electrostatic spray is too concentrated, which easily leads to a larger particle size of the particles sprayed. On the one hand, when the electrostatic spray voltage is too low, the discharge frequency and intensity are low, so that the number of spherical carbon precursors ejected is reduced and the particle size is larger. When the electrostatic spray voltage is too high, the discharge frequency and intensity are high, which can increase the number of spherical carbon precursors ejected, but the particle size is small and the particle size uniformity is poor, the particle size standard deviation is large, and the relative standard deviation of the particle size is also large. On the other hand, when the spray flow rate is too low, the ejected spherical precursors are less, and the particle size is small, the uniformity is poor, the particle size standard deviation is large, and the relative standard deviation of the particle size is also large. When the spray flow rate is too high, although the number of spherical precursors sprayed out can be increased, it is easy to cause the particle size of the sprayed particles to be too large.
[0076] In some embodiments, the carbon source in the carbon source solution includes one or more of chitosan, resin, starch, and asphalt.
[0077] In some embodiments, the solvent in the carbon source solution includes one or more of water, ethanol, ethyl acetate, petroleum ether, tetrahydrofuran, acetone, dimethylformamide and dichloromethane.
[0078] In some embodiments, the solidifying liquid includes one or more of concentrated sulfuric acid, aldehydes, alcohols, amines, and calcium salt solutions.
[0079] Step 2: Carbonize and activate the carbon precursor to obtain a porous carbon matrix.
[0080] The role of carbonization includes maintaining the morphology and structural stability of the carbon precursor and reducing the disintegration of the carbon precursor during the activation process. The role of activation includes etching the carbonized structure to generate pores, thereby obtaining a porous carbon matrix and increasing the adsorption capacity of the carbon matrix to nano-silicon.
[0081] In some embodiments, the carbonization is carried out in an inert gas atmosphere, the carbonization temperature is 500°C to 900°C, and the carbonization time is 1 h to 6 h. For example, the carbonization temperature can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, or any value within the range formed by any two of the above values. The carbonization time can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, or any value within the range formed by any two of the above values.
[0082] In some embodiments, the activation is carried out in water vapor with a flow rate of 1 L / min to 15 L / min, the activation temperature is 700°C to 900°C, and the activation time is 5 h to 24 h. For example, the steam flow rate can be 1 L / min, 3 L / min, 5 L / min, 7 L / min, 9 L / min, 11 L / min, 13 L / min, 15 L / min, or any value in the range of any two of the above values. The activation time is 5 h, 8 h, 12 h, 15 h, 18 h, 21 h, 24 h, or any value in the range of any two of the above values.
[0083] Step 3: Provide a gas flow containing nano-silicon, and use a porous carbon matrix to adsorb the gas flow to obtain a composite precursor.
[0084] In some embodiments, providing the nano-silicon gas flow includes cracking silane gas in an inert gas atmosphere at a temperature of 400° C. to 800° C. For example, the temperature for cracking the silane gas can be 400° C., 450° C., 500° C., 550° C., 600° C., 650° C., 700° C., 750° C., 800° C., or any value within the range formed by any two of the above values.
[0085] In some embodiments, the adsorption temperature is 400°C to 800°C, and the adsorption time is 1 h to 12 h. For example, the adsorption temperature can be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, or any value in the range of any two of the above values. The adsorption time can be 1 h, 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, or any value in the range of any two of the above values.
[0086] Step 4: Densify the composite precursor to obtain the negative electrode material.
[0087] The role of densification includes rearranging the carbon atoms on the surface of the composite precursor at high temperature to fill the empty pores, which is beneficial to reduce its specific surface area, thereby obtaining a negative electrode material.
[0088] In some embodiments, the densification treatment includes placing the composite material in an inert gas atmosphere at a temperature of 500°C to 950°C for 2 hours to 6 hours. For example, the temperature of the densification treatment can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, or any value in the range formed by any two of the above values. The time of the densification treatment can be 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, or any value in the range formed by any two of the above values.
[0089] The scheme of the present application will be explained below in conjunction with the embodiments. Those skilled in the art will understand that the following examples are only used to explain the present application and cannot be construed as limiting the present application. Unless otherwise stated, the reagents, software and instruments not specifically stated in the following embodiments are all conventional commercial products or open source.
[0090] Embodiment 1: A negative electrode material, the preparation method comprising: S1, dissolving chitosan in pure water to form a chitosan solution with a mass concentration of 2%, and then spraying the chitosan solution into a 1% glutaraldehyde curing liquid by electrostatic spraying, the voltage of the electrostatic spraying is 10 kV, the flow rate of the electrostatic spraying is 1 mL / h, and filtering the curing liquid to obtain a carbon precursor.
[0091] S2, the carbon precursor was carbonized at 800 °C for 2 h in 300 L / h nitrogen, and then activated at 800 °C for 10 h at a steam flow rate of 10 L / min to obtain a porous carbon material.
[0092] S3, 100 sccm silane gas is cracked at 700 °C in a 200 sccm argon atmosphere to produce a gas flow containing nano-silicon, and then the gas flow is adsorbed using a spherical porous carbon material at 650 °C for 6 h to obtain a composite precursor.
[0093] S4, densifying the composite precursor at 900 °C for 2 h in 500 sccm argon to obtain a negative electrode material.
[0094] Figure 3This is a scanning electron microscope image of the negative electrode material obtained in Example 1. Figure 3 It can be seen that the obtained negative electrode material has a suitable particle size, and the discreteness of the particle size distribution is low. The negative electrode material has a spherical structure, and the gaps formed between the negative electrode material particles are small.
[0095] See also Figure 4 , Figure 5 and Figure 6 ,right Figure 4 The captured negative electrode material particles are subjected to energy dispersive X-ray spectroscopy analysis, which clearly shows that there are carbon elements ( Figure 5 ) and silicon ( Figure 6 ), indicating that the preparation method of Example 1 successfully prepared a negative electrode material with a carbon material as a porous matrix and silicon material attached thereto.
[0096] Embodiment 2: The difference from Example 1 is that in S1, chitosan is dissolved and dispersed in pure water to form a 3% chitosan solution.
[0097] Embodiment 3: The difference from Example 1 is that in S1, chitosan is dissolved and dispersed in pure water to form a 5% chitosan solution.
[0098] Embodiment 4: The difference from Example 1 is that in S1, the voltage of the electrostatic spray is set to 30 kV.
[0099] Embodiment 5: The difference from Example 1 is that in S1, the voltage of the electrostatic spray is set to 30 kV, and the flow rate of the electrostatic spray is set to 0.5 mL / h.
[0100] Embodiment 6: The difference from Example 1 is that in S1, chitosan is dissolved and dispersed in pure water to form a 5% chitosan solution, and the voltage of the electrostatic spray is set to 1 kV.
[0101] Embodiment 7: The difference from Example 1 is that in S1, chitosan is dissolved and dispersed in pure water to form a 5% chitosan solution, the voltage of the electrostatic spray is set to 1 kV, and the flow rate of the electrostatic spray is set to 5 mL / h.
[0102] Comparative Example 1: The difference from Example 5 is that in S1, chitosan is dissolved and dispersed in pure water to form a 1% chitosan solution.
[0103] Comparative Example 2: The difference from Example 7 is that in S1, chitosan is dissolved and dispersed in pure water to form a 6% chitosan solution.
[0104] Comparative Example 3: The difference from Example 5 is that in S1, the voltage of the electrostatic spray is set to 32 kV.
[0105] Comparative Example 4: The difference from Example 7 is that in S1, the voltage of the electrostatic spray is set to 0.8 kV.
[0106] Comparative Example 5: The difference from Example 5 is that in S1, the flow rate of the electrostatic spray is set to 0.4 mL / h.
[0107] Comparative Example 6: The difference from Example 7 is that in S1, the flow rate of electrostatic spray is set to 6 mL / h.
[0108] Please refer to Table 1 for some preparation parameters of Examples 1-7 and Comparative Examples 1-6 of the present application.
[0109] Table 1. Some preparation parameters of Examples 1-7 and Comparative Examples 1-6 of the present application Performance Testing (1) Etching treatment: Taking silicon material as the active material as an example, 150 mL of 20% HF acid solution by mass is added dropwise into 10 g of negative electrode material under stirring, which will produce SiF4 and H2 gases and release heat. After no gas is generated, the supernatant acid solution is removed by centrifugation, and 150 mL of 20% HF acid solution by mass is added to the negative electrode material again. After stirring for 12 hours, the supernatant acid solution is removed by centrifugation again, and then the negative electrode material is washed with pure water until it is neutral and dried to obtain the negative electrode material after removing the silicon material, that is, the matrix.
[0110] (2) Test method for specific surface area of negative electrode material or substrate: The specific surface area was measured using a Micromeritics TriStar 3000 specific surface area and pore size analyzer.
[0111] (3) Testing methods for pore volume and pore size of negative electrode materials or substrates: The test was carried out using ASAP 2460 equipment from Micromeritics, USA, and the pore volume V was calculated using the BJH Desorption cumulative volume of pores model in the pore diameter range of 17 Å~3000 Å.
[0112] Micromeretics ASAP 2460 was used for micropore and mesopore analysis. At liquid nitrogen temperature, the equilibrium adsorption of nitrogen on the surface of an object is related to its pore size and other characteristics. Combined with the law of the change of adsorption amount with relative pressure during adsorption, multiple models can be fitted to calculate the pore size. The report generated by the software uses the density functional theory (abbreviated as DFT) method to calculate the pore size distribution, average pore size, total pore volume, and pore volume within a certain range.
[0113] (4) Test method for mass content of carbon element in negative electrode material: Use Germany's Bruker's G4 ICARUS HF infrared carbon and sulfur analyzer: the sample burns in a high-temperature, oxygen-rich state, and the carbon and sulfur elements it contains are oxidized into carbon dioxide and sulfur dioxide, respectively. The generated gases enter the infrared detector with the carrier gas, and the carbon and sulfur content can be calculated by quantitatively analyzing the changes in the carbon dioxide signal and the sulfur dioxide signal.
[0114] (5) Test method for mass content of silicon in negative electrode materials: Use Nanyang Xinyu SA2-9-17TP box-type atmosphere furnace: burn in an oxygen atmosphere to make the silicon and silicon oxide in the sample react to form silicon dioxide, and the carbon is burned and turned into carbon dioxide and discharged, and the silicon content is calculated by weighing.
[0115] (6) Test method for the mass content of oxygen in negative electrode materials: Using the German Verder ONH 2000 oxygen, nitrogen and hydrogen element analyzer, the sample is wrapped in flux and melted in an inert atmosphere. The oxygen element it contains is reduced to carbon dioxide by the carbon in the graphite crucible. The generated carbon dioxide enters the infrared detector with the carrier gas. The change of the carbon dioxide signal is quantitatively counted to calculate the oxygen content.
[0116] (7) Negative electrode material powder conductivity test: The MCP-PD51 powder conductivity meter from Mitsubishi Chemical of Japan was used. The system used the four-probe method to measure the volume resistivity of the sample. The instrument can measure the resistance of the powder, and then the computer automatically calculates the conductivity and resistivity of the powder. The conductivity was tested at five pressure points: 4, 8, 12, 16, and 20 kN.
[0117] (8) Electrochemical performance test: 1) The test method for the first discharge specific capacity and the first coulombic efficiency (ICE) is as follows: the negative electrode material, conductive carbon black, and polyacrylic acid (PPA) are prepared into a negative electrode slurry in a mass ratio of 75:15:10, coated on copper foil, and dried to form a negative electrode sheet. A metal lithium sheet is used as the counter electrode and assembled into a button cell in an argon-filled glove box. The button cell is charged and discharged at a current density of 0.1C in the charge and discharge range of 0.01V-5V to obtain the first discharge specific capacity and the first coulombic efficiency (ICE) of the button cell.
[0118] 2) The test method for the capacity retention rate and the electrode thickness expansion rate after 50 cycles is as follows: the negative electrode slurry is prepared according to the mass ratio of the negative electrode active material, conductive carbon black (Super-P), conductive graphite (KS-6), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) of 92:2:2:2:2, coated on copper foil, and dried to form a negative electrode sheet. The negative electrode active material is a mixture of the negative electrode material and graphite of the present application, wherein the proportion of the negative electrode material and graphite is determined by the first reversible specific capacity of the two and the capacity required to be matched between the two. A metal lithium sheet is used as the counter electrode and assembled into a button cell in an argon-filled glove box. The button cell is subjected to 50 repeated charge and discharge tests in the charge and discharge range of 0.01 V-5 V at a current density of 1C to obtain the capacity retention rate and the electrode thickness expansion rate after 50 cycles of the battery.
[0119] The present application tests and statistics the average particle size of the negative electrode materials of Examples 1-7 and Comparative Examples 1-6. The test method and statistical method include: using a Japanese Hitachi S-4800 electron scanning microscope to take pictures of the samples under the conditions of 3.0 kV 8.2 mm×1.0 K, and measuring and counting the particle size in the sample pictures on nano measure, randomly selecting a certain square area, dividing the area into nine squares, selecting a total of 200 particles in the four corners and the middle square for particle size measurement, and statistically analyzing the particle size measurement results through software Image J to obtain the average particle size D0 and particle size standard deviation S0 of the carbon matrix. The average particle size D1, particle size standard deviation S1 and particle size relative standard deviation S1 / D1 of the negative electrode material are obtained.
[0120] The present application also mixes the negative electrode materials of Examples 1-7 and Comparative Examples 1-6 with conductive carbon black (Super-P) and acrylonitrile multi-polymer aqueous binder (LA133) in a ratio of 70:15:15 to form a slurry and evenly applies it to the copper foil, and prepares the electrode sheet after drying. The thickness of the copper foil is measured by a caliper. , the thickness of the electrode is measured to be , assembled into button cells and tested their surface capacity density and first coulombic efficiency on the Blue Electric Battery Test Cabinet M340A. After 50 cycles, the pole pieces were removed, cleaned and dried, and the thickness of the pole pieces was measured with a caliper. , then the calculation formula of the expansion rate after 50 cycles is as follows: Please refer to Table 2 for the above test or statistical results.
[0121] Table 2. Performance parameters of Examples 1-7 and Comparative Examples 1-6 of the present application Embodiment 1-7 can control the particle size of the carbon precursor formed by the spray by controlling the carbon source concentration, the electrostatic spray voltage and the electrostatic spray flow rate within a certain range, and form spherical carbon precursor particles. Through subsequent activation, active material adsorption and densification treatment, the average particle size D1 and the particle size standard deviation S1 of the prepared negative electrode material meet the predetermined range. On the one hand, it is beneficial to make the active material more evenly deposited on the substrate, so that when the negative electrode material is embedded with active ions during the charge and discharge cycle, it helps to make the stress distribution in the negative electrode material particles more uniform, reducing the expansion rate and cracking and pulverization risk of the battery prepared by the negative electrode material during the cycle. Therefore, the expansion rate is low, which helps to maintain the stable capacity of the battery prepared by the negative electrode material and improve the cycle performance of the battery prepared by the negative electrode material. On the other hand, it is beneficial to reduce the gaps between the negative electrode material particles, thereby helping to increase the volume energy density of the negative electrode sheet, thereby making the surface density higher. It is also beneficial to improve the uniformity of distribution of the conductive agent and the electrolyte between the negative electrode materials, improve the contact and wetting effect between the electrolyte and the negative electrode material, and help to improve the charge and discharge efficiency and kinetic performance of the battery prepared with the negative electrode material, and have a higher first coulombic efficiency.
[0122] Compared with Example 5, the carbon source concentration in Comparative Example 1 is relatively low. Under the condition that other conditions are the same, during the process of removing the solvent from the spray particles, the volatilization of the solvent is likely to cause the particle size of the prepared carbon precursor to become smaller. At the same time, a large amount of solvent volatilization is likely to cause the carbon precursor to sink, thereby causing the particle size uniformity to deteriorate and the particle size standard deviation to be larger. Therefore, the average values of the particle sizes of the carbon matrix and the negative electrode material obtained in Comparative Example 1 are both smaller than the set lower limit, while the particle size standard deviations of the carbon matrix and the negative electrode material are both larger than the set upper limit.
[0123] Compared with Example 5, the electrostatic spray voltage of Comparative Example 3 is relatively high, which results in a smaller particle size and a larger standard deviation of the particle size when other conditions are the same. Therefore, the average particle size of the carbon matrix and the negative electrode material obtained in Comparative Example 3 is less than the set lower limit, while the standard deviation of the particle size of the carbon matrix and the negative electrode material is greater than the set upper limit.
[0124] Compared with Example 5, the electrostatic spray flow rate of Comparative Example 5 is lower. Under the condition that other conditions are the same, the particle size of the sprayed particles is smaller, the standard deviation of the particle size is larger, and the number of spherical carbon precursors is reduced. Therefore, the average particle size of the carbon matrix and the negative electrode material obtained in Comparative Example 5 is less than the set lower limit, while the standard deviation of the particle size of the carbon matrix and the negative electrode material is greater than the set upper limit.
[0125] The carbon precursors of Comparative Examples 1, 3, and 5 above have too small particle sizes, and steam activation is fast, resulting in uneven pores and a large specific surface area. The uneven pores lead to uneven distribution of expansion stress in the prepared negative electrode material, an increase in the expansion rate, and a large specific surface area leads to a decrease in the first coulombic efficiency and nano-silicon oxidation, which in turn causes a decrease in the surface capacity density. In addition, the carbon precursors of Comparative Examples 1, 3, and 5 above have too large a standard deviation in particle size, which also leads to uneven distribution of the conductive agent and the electrolyte among the particles, which leads to uneven expansion stress, and further causes an increase in the expansion rate of the negative electrode sheet and a decrease in the first coulombic efficiency of the secondary battery.
[0126] Compared with Example 7, the carbon source concentration in Comparative Example 2 is relatively high. Under the same other conditions, the carbon source in the particles sprayed by electrostatic spraying is too concentrated, resulting in the particle size of the sprayed particles being generally larger. Therefore, the average particle size of the carbon matrix and the negative electrode material obtained in Comparative Example 2 is greater than the set upper limit value.
[0127] Compared with Example 7, the electrostatic spray voltage in Comparative Example 4 is relatively low. Under the condition that other conditions are the same, the particle size of the sprayed particles is generally larger, and the number of spherical carbon precursors is reduced. Therefore, the average particle size of the carbon matrix and the negative electrode material obtained in Comparative Example 4 is greater than the set upper limit value.
[0128] Compared with Example 7, the electrostatic spray flow rate in Comparative Example 6 is higher, which results in the particle size of the sprayed particles being generally larger when other conditions are the same. Therefore, the average particle sizes of the carbon matrix and the negative electrode material obtained in Comparative Example 6 are both greater than the set upper limit value.
[0129] The carbon precursors of Comparative Examples 2, 4 and 6 have too large particle sizes, slow steam activation, small pore volumes produced by activation, less adsorbed nano-silicon, and larger gaps between particles, which in turn leads to a decrease in the surface capacity density of the negative electrode material.
[0130] The above results show that when the average particle size D1 and the particle size standard deviation S1 of the negative electrode material meet the predetermined range, the surface density of the negative electrode material is higher, the expansion rate of the negative electrode sheet is lower, and the first coulombic efficiency of the secondary battery is higher.
[0131] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A substrate, characterized in that: The substrate has pores, the substrate includes a carbon material, The average value D0 of the particle size of the matrix is 5.5 μm to 9.5 μm, and the standard deviation S0 of the particle size of the matrix is 0.08 to 0.
35.
2. The substrate according to claim 1, characterized in that The substrate satisfies at least one of the following conditions: (1) The relative standard deviation S0 / D0 of the particle size of the matrix is 0.008 to 0.064; (2) The matrix has a spherical structure, and the sphericity of the matrix is 0.9 to 1.0; (3) The total pore volume of the matrix is 0.5 cm 3 / g to 2.0 cm 3 / g; (4) The average pore size of the matrix is 0.1 nm to 8 nm; (5) The carbon material includes one or more of artificial graphite, amorphous carbon, activated carbon, and mesophase carbon microspheres.
3. A negative electrode material, comprising a substrate and an active substance, wherein the substrate has pores, and at least part of the active substance is disposed in the pores of the substrate, characterized in that: The average value D1 of the particle size of the negative electrode material is 5.5 μm to 9.5 μm, and the standard deviation S1 of the particle size of the negative electrode material is 0.1 to 0.
35.
4. The negative electrode material according to claim 3, characterized in that The negative electrode material satisfies at least one of the following conditions: (1) The relative standard deviation S1 / D1 of the particle size of the negative electrode material is 0.010 to 0.064; (2) Based on the mass of the negative electrode material, the mass percentage of oxygen element in the negative electrode material is 0.05% to 4.0%; (3) The specific surface area of the negative electrode material is less than or equal to 10 m 2 / g; (4) The powder conductivity of the negative electrode material is 0.05 S / m to 5 S / m; (5) The surface capacity density of the negative electrode material is 4.55 mAh / cm 2 Up to 6.10 mAh / cm 2 ; (6) The pore volume of the negative electrode material is less than or equal to 0.15 cm 3 / g; (7) The average pore size of the negative electrode material is less than or equal to 10 nm; (8) The negative electrode material has a quasi-spherical structure, and the sphericity of the negative electrode material is 0.9 to 1.
0.
5. The negative electrode material according to claim 3, characterized in that The substrate satisfies at least one of the following conditions: (1) The average particle size D0 of the matrix is 5.5 μm to 9.5 μm, and the standard deviation S0 of the particle size of the matrix is 0.08 to 0.35; (2) The relative standard deviation S0 / D0 of the particle size of the matrix is 0.008 to 0.064; (3) The matrix has a spherical structure, and the sphericity of the matrix is 0.9 to 1.0; (4) The total pore volume of the matrix is 0.5 cm 3 / g to 2.0 cm 3 / g; (5) The average pore size of the matrix is 0.1 nm to 8 nm.
6. The negative electrode material according to claim 3, characterized in that The substrate includes at least one of a carbon material and a non-carbon material; The carbon material includes one or more of artificial graphite, amorphous carbon, activated carbon, and mesophase carbon microspheres; The non-carbon material includes at least one of metal oxides, silicides, silicates, phosphates, titanates and aluminum borates; the metal oxide includes one or more of aluminum oxide, zirconium oxide, germanium dioxide and manganese dioxide; the silicide includes one or more of silicon carbide and silicon nitride; the silicate includes one or more of cordierite, mullite and zeolite; the phosphate includes one or more of aluminum phosphate, magnesium phosphate, calcium phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate and lanthanum phosphate; the titanate includes one or more of calcium titanate, iron titanate, lithium titanate and barium titanate.
7. The negative electrode material according to claim 3, characterized in that The active material includes one or more of Si, Li, Na, K, Sn, Ge, Fe, Mg, Ti, Zn, Al, P and Cu.
8. The negative electrode material according to claim 3, characterized in that The matrix is a carbon matrix, the active material is a silicon material, the silicon material includes one or more of amorphous silicon, crystalline silicon, silicon oxide, silicon alloy, and a composite of crystalline silicon and amorphous silicon, and the negative electrode material satisfies at least one of the following conditions: (1) Based on the mass of the negative electrode material, the mass proportion of carbon element in the negative electrode material is 30% to 70%; (2) Based on the mass of the negative electrode material, the mass proportion of silicon element in the negative electrode material is 30% to 80%.
9. A negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, characterized in that: The negative electrode active material layer comprises the negative electrode material according to any one of claims 3 to 8.
10. A secondary battery, characterized in that: Comprising the negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Negative electrode material for lithium ion secondary battery, method for producing same, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
CN116686108A
Negative electrode material for lithium ion secondary battery, method for evaluating same, method for producing same, negative electrode for lithium ion secondary
CN116783727A
Negative electrode material for lithium ion secondary battery, negative electrode material composition for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
CN116897447A
Negative electrode material, preparation method thereof and lithium ion battery
CN117352673A
Negative electrode material and battery
CN117457880A
Cited By
Negative electrode material and battery
WO2025236650A1