Sodium-rich sodium polyvanadate material, preparation method thereof, positive plate and battery
By introducing cationic defects into polyvanadate materials, the sodium-polyvanadate-rich sodium polyvanadate material Na2+xV6O16·2.9H2O was prepared by simple precipitation method, which solved the poor dynamic behavior and structure of polyvanadate materials in magnesium ion batteries. Stability issues enable high capacity and long life of magnesium ion battery positive electrode material.
Patent Information
- Application Number
- CN202411220897.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing polyvanadate materials have poor kinetic behavior, low ionic conductivity and poor structural stability in magnesium-ion batteries or magnesium-based hybrid ion batteries, resulting in low battery capacity and short cycle life.
The sodium-rich sodium polyvanadate material Na2+xV6O16·2.9H2O was prepared by simple precipitation method. By controlling the concentration, pH value and water bath conditions of sodium metavanadate, a sodium-rich sodium-poly with anisotropic single crystal nanoribbon structure was generated. Sodium vanadate material improves its structural stability and ion diffusion kinetics.
It significantly improves the conductivity and structural stability of the positive electrode, improves the cycle life and actual capacity of the battery, and shows excellent electrochemical performance and rate performance.
Smart Images

Figure CN119092699A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrode materials, and in particular to a sodium-rich sodium polyvanadate material and a preparation method thereof, a positive electrode sheet and a battery. Background Art
[0002] In magnesium ion batteries, due to the divalent Mg 2+ There is a strong interaction between the host cathode material and the magnesium ion, which results in a very slow embedding / de-embedding cycle process on the cathode material, seriously affecting the electrochemical performance of magnesium ion batteries. + and Na + ), can effectively promote ion diffusion kinetics and improve the charge storage capacity and cycle stability of the battery. This method of adding monovalent exogenous cations (such as Li + and Na + ), the energy storage system formed is called a magnesium-based hybrid ion battery. And because the abundance of lithium resources in the earth's crust is limited, magnesium-sodium hybrid ion batteries are more economical than magnesium-lithium hybrid ion batteries, and therefore have higher application potential. Although magnesium-based hybrid ion batteries exhibit superior electrochemical potential compared to magnesium-ion batteries, the positive electrode materials that can be used for magnesium-based hybrid ion batteries are still very limited. In addition, these existing positive electrode materials generally have problems of low ion conductivity and poor structural stability, resulting in low actual capacity of the battery and short cycle life. Therefore, there is an urgent need to develop advanced positive electrode materials with rapid ion diffusion channels and high structural stability to improve the performance of magnesium-sodium hybrid ion batteries.
[0003] Vanadium oxides, due to their rich redox states and VO bond distortion, have derived a large number of high-capacity, structure-rich polyvanadate materials, which are widely used in various metal ion batteries. For example, CN202210724649.2 prepared copper hydroxypyrovanadate cathode material by hydrothermal method and applied it to magnesium secondary battery, and showed excellent reversible capacity (current density of 0.2A g -1 The specific capacity is 277.31 mAh g -1 ) and excellent cycle stability (capacity retention rate after 400 cycles is 96.97%, and Coulomb efficiency is always stable at 100%). However, the positive effect of exogenous cations in standard stoichiometric ratio on polyvanadate positive electrode is very limited, especially in terms of structural stability and ionic conductivity, which still limits the application of polyvanadate in magnesium secondary batteries and magnesium-based hybrid ion batteries. Summary of the invention
[0004] In view of the above deficiencies in the prior art, the purpose of the present invention is to provide a sodium-rich sodium polyvanadate material to solve the problems that when existing polyvanadate materials are used as the positive electrode of a magnesium ion battery or a magnesium-based hybrid ion battery, they have poor kinetic behavior, low ionic conductivity, and poor structural stability, resulting in a low battery capacity and a short cycle service life.
[0005] Furthermore, a preparation method of the sodium-rich sodium polyvanadate material, as well as a positive electrode sheet and a battery containing the sodium-rich sodium polyvanadate material, are provided.
[0006] To solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0007] A sodium-rich sodium polyvanadate material, with the chemical formula Na 2+x V6O 16 ·2.9H2O, where 0 < X < 4, and the microscopic morphology is an anisotropic single-crystal nanobelt structure.
[0008] The preparation method of the sodium-rich sodium polyvanadate material includes the following steps:
[0009] (1) Dissolve sodium metavanadate in deionized water, and stir until sodium metavanadate is completely dissolved to obtain a sodium metavanadate solution, denoted as solution A;
[0010] (2) Under stirring conditions, add an acid solution to solution A and adjust the pH to 2 - 3.5, and the resulting solution is denoted as solution B;
[0011] (3) Place solution B under a water bath condition, stir it to react fully, then cool it naturally, filter, wash, and dry to obtain the sodium-rich sodium polyvanadate material.
[0012] The present invention uses a simple precipitation method to prepare the sodium-rich sodium polyvanadate material, which is simple, efficient, and low-cost. During specific preparation, by controlling the concentration of sodium metavanadate, the pH value of the solution, and the water bath conditions, the sodium metavanadate undergoes a condensation reaction under acidic conditions to generate the corresponding phase, thereby realizing the preparation of the sodium-rich sodium polyvanadate material.
[0013] Furthermore, in step (1), the concentration of the sodium metavanadate solution is 5 g / L - 35 g / L. If the concentration of the sodium metavanadate solution is lower than this range, the sodium ions in the original reaction solution are insufficient and the required sodium-rich phase cannot be formed; conversely, if the concentration of the sodium metavanadate solution is too high, sodium metavanadate will not be completely dissolved at room temperature, resulting in waste of raw materials.
[0014] Furthermore, the mass concentration of the acid solution in step (2) is 5% to 30%. If the concentration of the acid solution is lower than this range, the sodium ion concentration in the original reaction solution will be reduced, affecting the formation of the sodium-rich phase; while if the concentration of the acid solution is too high, the sodium metavanadate reaction will not be complete, reducing the yield of sodium-rich sodium polyvanadate and increasing the difficulty of pH value control.
[0015] Furthermore, in step (3), the water bath temperature is 60-130° C., and the stirring time is 3-12 hours. A water bath temperature outside this range or a stirring time that is too short may result in a decrease in product purity. Experiments have shown that 8 hours is sufficient for a complete reaction, and no longer reaction time is required, so the preferred stirring time is 8 hours.
[0016] Furthermore, in step (3), the drying temperature is 60 to 100° C. and the drying time is 3 to 8 hours.
[0017] Furthermore, the acid solution in step (2) is one or more of sulfuric acid, nitric acid, hydrochloric acid and boric acid.
[0018] Furthermore, it is preferred that the pH in step (2) is adjusted to 2.0 to 2.5.
[0019] A battery positive electrode sheet comprises the sodium-rich sodium polyvanadate material.
[0020] A battery comprises the positive electrode sheet, wherein the battery comprises a mixed ion battery, a sodium ion battery, a magnesium ion battery or a zinc ion battery.
[0021] A magnesium-based hybrid ion battery with Na + / Mg 2+ The double salt electrolyte is used as the electrolyte, and the positive electrode sheet is used as the positive electrode.
[0022] Further, the Mg 2+ / Na + The concentration of the double salt electrolyte is 0.5 to 3M.
[0023] Furthermore, in the double salt electrolyte, Na + / Mg 2+ The molar ratio is 1 to 2.5:1.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention adopts a simple precipitation method to introduce cation defects (Na + ), increasing V 5+ With V 4+The conversion ratio between vanadates and vanadates is increased, which enhances the electron transition and significantly improves the conductivity of the material, thereby improving the rate performance of the positive electrode. The cation defect further acts as an interlayer pillar to limit the migration path of magnesium ions, enhance the structural stability and ion diffusion kinetics of the sodium polyvanadate material, and thus improve the cycle life and actual capacity of the battery.
[0026] 2. The sodium-rich sodium polyvanadate material prepared by the present invention has excellent ionic conductivity, electronic conductivity and structural stability. The magnesium ion battery assembled using the sodium-rich sodium polyvanadate material prepared by the present invention as the positive electrode exhibits excellent electrochemical performance. 2+ 、Na + The invention has good compatibility, and the magnesium-based mixed ion full battery assembled using the sodium-rich sodium polyvanadate material prepared by the invention as the positive electrode still exhibits excellent charge storage performance and cycle stability.
[0027] 3. Na obtained by the present invention 2+x V6O 16 · When 2.9H2O material is used as the positive electrode material of magnesium ion battery, at 0.05Ag -1 The specific capacity is as high as 155 mAh g at a current density of -1 ; Increase the current density to 5.0Ag -1 Time 2+x V6O 16 ·2.9H2O cathode specific capacity remains at 39mAh g -1 ; at 0.5Ag -1 After 300 cycles at the current density, the capacity retention rate is as high as 78%, showing excellent rate performance and long-cycle stability. It is a highly promising high-capacity, long-life magnesium-ion battery positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a process flow chart for preparing the sodium-rich sodium polyvanadate material;
[0029] Figure 2 TEM and SAED images of the sodium-rich sodium polyvanadate material prepared in Example 1 of the present invention;
[0030] Figure 3 This is the XRD pattern of the sodium-rich sodium polyvanadate material prepared in Example 1 of the present invention;
[0031] Figure 4 This is a TGA graph of the sodium-rich sodium polyvanadate material prepared in Example 1 of the present invention;
[0032] Figure 5This is a graph of specific capacity at different current densities when the sodium-rich sodium polyvanadate material prepared in Example 1 of the present invention is used as a positive electrode material for a magnesium ion battery;
[0033] Figure 6 When the sodium-rich sodium polyvanadate material prepared in Example 1 of the present invention is used as the positive electrode material of the magnesium ion battery, at 0.5A g -1 Long cycle test diagram under current density;
[0034] Figure 7 When the sodium-rich sodium polyvanadate material prepared in Example 1 of the present invention is used as the positive electrode material of the magnesium-sodium mixed ion full battery, the magnesium-sodium mixed ion full battery has a positive electrode material of 8.0 mV s -1 Cyclic voltammetry curves at different scan rates;
[0035] Figure 8 For the application example 1, the magnesium-sodium mixed ion full battery is used at 0.1Ag -1 Long cycle test diagram under current density;
[0036] Fig. 9 For the application example 2, the magnesium-sodium mixed ion full battery is used at 0.1Ag -1 Long cycle test diagram under current density;
[0037] Fig.10 For the application example 3, the magnesium-sodium mixed ion full battery is used at 0.1Ag -1 Long cycle test diagram under current density. DETAILED DESCRIPTION
[0038] The specific implementation modes of the present invention are further described in detail below in conjunction with specific examples.
[0039] The numerical ranges in the present invention are understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any intermediate value in the stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0040] Unless otherwise stated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of conflict with any incorporated document, the content of this specification shall prevail. Regarding "comprising", "including", "having", "containing", etc. used herein, they are all open terms, which means including but not limited to.
[0041] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods.
[0042] The materials, reagents, etc. used in the present invention can be purchased or synthesized by known methods unless otherwise specified.
[0043] In the quantitative tests of the present invention, three repeated experiments are set, and the results are averaged.
[0044] See Figure 1 , the present invention provides a method for preparing a sodium-rich polyvanadate material, comprising the following steps:
[0045] (1) Dissolve sodium metavanadate in deionized water and stir until sodium metavanadate is completely dissolved to obtain a sodium metavanadate solution;
[0046] (2) Under stirring conditions, add an acid solution to the sodium metavanadate solution obtained in step (1) until the pH is 2 to 3.5;
[0047] (3) Place the solution obtained in step (2) under a water bath condition, stir to make it react fully, then naturally cool, filter, wash, and dry to obtain the sodium-rich polyvanadate material.
[0048] The obtained sodium-rich polyvanadate material has the chemical formula Na 2+x V6O 16 ·2.9H2O, where 0 < X < 4, and the microscopic morphology is an anisotropic nanobelt structure, which is a typical single crystal structure.
[0049] I. Examples
[0050] Example 1
[0051] This example provides a method for preparing a sodium-rich polyvanadate material, comprising the following steps:
[0052] Dissolve 15 g of sodium metavanadate in 2000 mL of deionized water and stir at room temperature until homogeneous; then, under stirring conditions, add a sulfuric acid solution with a mass concentration of 10% until a homogeneous orange-red transparent solution with pH = 2.0 is obtained. Place the obtained homogeneous orange-red transparent solution in a water bath pot and stir at 70 °C for 9 h under water bath conditions. After the reaction is completed, let it cool naturally and then filter. Wash the obtained precipitate product three times by suction filtration with deionized water and place it in a drying oven at 70 °C for 8 h to obtain the sodium-rich polyvanadate material.
[0053] Example 2
[0054] This example provides a method for preparing a sodium-rich polyvanadate material, comprising the following steps:
[0055] Dissolve 30g of sodium metavanadate in 2000mL of deionized water and stir at room temperature until uniform; then add a 5% sulfuric acid solution under stirring until a uniform orange-red transparent solution with a pH of 2.0 is obtained. Place the obtained uniform orange-red transparent solution in a water bath and stir it for 12h under 60℃ water bath conditions. After the reaction is completed, let it cool naturally and filter it. The obtained precipitated product is washed three times with deionized water by suction, and placed in a drying oven at 80℃ for 6h to obtain a sodium-rich sodium polyvanadate material.
[0056] Example 3
[0057] This embodiment provides a method for preparing a sodium-rich sodium polyvanadate material, comprising the following steps:
[0058] Dissolve 15g of sodium metavanadate in 2000mL of deionized water and stir at room temperature until uniform; then add nitric acid solution with a mass concentration of 15% under stirring until a uniform orange-red transparent solution with a pH of 2.5 is obtained. The uniform orange-red transparent solution is placed in a water bath and stirred for 7h under 80℃ water bath conditions. After the reaction is completed, it is filtered after natural cooling. The obtained precipitated product is washed three times with deionized water by suction, and placed in a drying oven at 80℃ for 6h to obtain a sodium-rich sodium polyvanadate material.
[0059] Example 4
[0060] This embodiment provides a method for preparing a sodium-rich sodium polyvanadate material, comprising the following steps:
[0061] Dissolve 20g of sodium metavanadate in 2000mL of deionized water and stir at room temperature until uniform; then add a 30% boric acid solution under stirring until a uniform orange-red transparent solution with a pH of 2.8 is obtained. Place the obtained uniform orange-red transparent solution in a water bath and stir it for 3h under 130℃ water bath conditions. After the reaction is completed, let it cool naturally and filter it. The obtained precipitated product is washed three times with deionized water by suction, and placed in a drying oven at 100℃ for 3h to obtain a sodium-rich sodium polyvanadate material.
[0062] Example 5
[0063] This embodiment provides a method for preparing a sodium-rich sodium polyvanadate material, comprising the following steps:
[0064] Dissolve 15g of sodium metavanadate in 2000mL of deionized water and stir at room temperature until uniform; then add a 10% hydrochloric acid solution under stirring until a uniform orange-red transparent solution with a pH of 3.5 is obtained. Place the obtained uniform orange-red transparent solution in a water bath and stir it for 9h under 70℃ water bath conditions. After the reaction is completed, let it cool naturally and filter it. The obtained precipitated product is washed three times with deionized water by suction, and placed in a drying oven at 70℃ for 8h to obtain a sodium-rich sodium polyvanadate material.
[0065] 2. Results and Analysis
[0066] (I) Structural characterization of the prepared sodium-rich sodium polyvanadate material
[0067] (1) TEM characterization
[0068] Figure 2 The transmission electron microscope image (TEM image) and selected area electron diffraction image (SAED image) of the sodium-rich sodium polyvanadate material obtained in Example 1 are shown in FIG. Figure 2 It can be seen that the microscopic morphology of the sodium-rich sodium polyvanadate material obtained in Example 1 is an anisotropic nanobelt structure and a typical single crystal structure with good crystallinity.
[0069] The sodium-rich sodium polyvanadate materials prepared in Examples 2 to 5 were tested using the same method, and the results were substantially consistent with those of Example 1.
[0070] (2) XRD characterization
[0071] Figure 3 The X-ray diffraction analysis diagram (XRD diagram) of the sodium-rich sodium polyvanadate material obtained in Example 1 is shown in FIG. Figure 3 It can be seen that the sodium-rich sodium polyvanadate material prepared in Example 1 is consistent with the X-ray diffraction standard card JCPDS#16-0601 (chemical formula is Na2V6O 16 ·3H2O) are compared, and the physical phases of the two are completely consistent. All diffraction peaks are consistent with those of monoclinic crystal Na2V6O 16 The 3H2O standard peak is completely consistent, indicating that the introduced interlayer cation defects have not changed the original sodium polyvanadate phase composition.
[0072] Compared with the peak position of the (001) crystal plane of the standard card JCPDS#16-0601, the XRD curve of the sample in this embodiment has an obvious rightward angle shift, corresponding to a decrease in the interlayer spacing, indicating that the excess sodium is located between the layers and acts as an interlayer pillar, which enhances the interlayer connection, resulting in a decrease in the interlayer spacing, thereby enhancing the structural stability of the positive electrode material.
[0073] The sodium-rich sodium polyvanadate materials prepared in Examples 2 to 5 were tested using the same method, and the results were substantially consistent with those of Example 1.
[0074] (3) TGA and ICP characterization
[0075] Figure 4 Thermogravimetric analysis (TGA) of the sodium-rich sodium polyvanadate material obtained in Example 1 is shown in FIG. Figure 4 It can be seen that the sodium-rich sodium polyvanadate material prepared in Example 1 contains about 2.9 water molecules in each product molecule.
[0076] The sodium-rich sodium polyvanadate materials prepared in Examples 2 to 5 were subjected to thermogravimetric analysis, and the results were substantially consistent with those of Example 1.
[0077] Table 1 is an ICP test result table of the sodium-rich sodium polyvanadate material prepared in the present invention.
[0078] Table 1 ICP test results of sodium-rich sodium polyvanadate materials.
[0079] Example element Na / V (atomic ratio) Example 1 Na / V 3.7:6 Example 2 Na / V 4.5:6 Example 3 Na / V 3.8:6 Example 4 Na / V 4.0:6 Example 5 Na / V 3.7:6
[0080] Combining the thermogravimetric analysis results of the sodium-rich sodium polyvanadate material and Table 1, it can be seen that the chemical formulas of the sodium-rich sodium polyvanadate materials prepared in different embodiments are shown in Table 2.
[0081] Table 2 Chemical formula of sodium-rich sodium polyvanadate material obtained in Example
[0082] Example Chemical formula Example 1 <h2 style=";text-align:left;direction:ltr"><![CDATA[Na <h2 style=";text-align:left;direction:ltr"> 3.7 <h2 style=";text-align:left;direction:ltr"> V6O<h2 style=";text-align:left;direction:ltr"> 16 <h2 style=";text-align:left;direction:ltr"> 2.9H2O<h2 style=";text-align:left;direction:ltr"> Example 2 <h2 style=";text-align:left;direction:ltr"><![CDATA[Na <h2 style=";text-align:left;direction:ltr"> 4.5 <h2 style=";text-align:left;direction:ltr"> V6O<h2 style=";text-align:left;direction:ltr"> 16 <h2 style=";text-align:left;direction:ltr"> 2.9H2O<h2 style=";text-align:left;direction:ltr"> Example 3 <h2 style=";text-align:left;direction:ltr"><![CDATA[Na <h2 style=";text-align:left;direction:ltr"> 3.8 <h2 style=";text-align:left;direction:ltr"> V6O<h2 style=";text-align:left;direction:ltr"> 16 <h2 style=";text-align:left;direction:ltr"> 2.9H2O<h2 style=";text-align:left;direction:ltr"> Example 4 <h2 style=";text-align:left;direction:ltr"><![CDATA[Na <h2 style=";text-align:left;direction:ltr"> 4.0 <h2 style=";text-align:left;direction:ltr"> V6O<h2 style=";text-align:left;direction:ltr"> 16 <h2 style=";text-align:left;direction:ltr"> 2.9H2O<h2 style=";text-align:left;direction:ltr"> Example 5 <h2 style=";text-align:left;direction:ltr"><![CDATA[Na <h2 style=";text-align:left;direction:ltr"> 3.7 <h2 style=";text-align:left;direction:ltr"> V6O<h2 style=";text-align:left;direction:ltr"> 16 <h2 style=";text-align:left;direction:ltr"> 2.9H2O<h2 style=";text-align:left;direction:ltr">
[0083] (II) Electrochemical performance test of sodium-rich sodium polyvanadate materials
[0084] (1) Magnesium ion battery
[0085] The present invention uses the sodium-rich sodium polyvanadate material prepared in Example 1 to be loaded on a carbon paper current collector as the positive electrode, activated carbon is loaded on a carbon cloth current collector as the negative electrode, 0.5M Mg(TFSI)2 is used as the electrolyte, and assembled into a 2032 button cell for electrochemical performance testing. A constant current charge and discharge (GCD) test is performed on the sodium-rich sodium polyvanadate positive electrode using a charge and discharge test system (Neware-CT8000).
[0086] Figure 5 is Na obtained in Example 1 of the present invention 3.7 V6O 16 ·2.9Specific capacity diagram of H2O material as positive electrode material of magnesium ion battery at different current densities. Figure 5 It can be seen that at 0.05Ag -1 At current density, Na 3.7 V6O 16 ·2.9H2O cathode specific capacity up to 155mAh g -1 ; Increase the current density to 5.0Ag-1 When, Na 3.7 V6O 16 ·2.9H2O cathode specific capacity remains at 39mAh g -1 It can be seen that the Na 3.7 V6O 16 ·2.9H2O material has excellent rate performance when used as the positive electrode of magnesium ion battery.
[0087] Figure 6 The Na obtained in Example 1 of the present invention 3.7 V6O 16 · When 2.9H2O material is used as the positive electrode material of magnesium ion battery, at 0.5Ag -1 Long cycle test diagram under current density. Figure 6 It can be seen that Na 3.7 V6O 16 ·2.9H2O positive electrode at 0.5Ag -1 After 300 cycles at the same current density, the capacity retention rate reached 78%, showing the Na 3.7 V6O 16 ·2.9H2O cathode has excellent long cycle stability.
[0088] (2) Magnesium-sodium mixed ion battery
[0089] The present invention uses the sodium-rich sodium polyvanadate material prepared in Example 1 to be loaded on a carbon paper current collector as the positive electrode, 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA) to be loaded on a carbon cloth current collector as the negative electrode, and 1.5M NaTFSI / Mg(TFSI)2 as the electrolyte (in the electrolyte, Na + / Mg 2+ The molar ratio was 1:1), and the 2032 button cells were assembled for electrochemical performance testing. Cyclic voltammetry (CV) test of the sodium-rich sodium polyvanadate positive electrode was performed using an electrochemical workstation (CHI660e).
[0090] Figure 7 The Na obtained in Example 1 of the present invention 3.7 V6O 16 When 2.9H2O material is used as the positive electrode material of magnesium-sodium mixed ion full battery, the magnesium-sodium mixed ion full battery has a high conductivity at 8.0mV s -1 The cyclic voltammetry curves of the first three cycles at the scan rate. Figure 7 It can be seen that in the first three cycles, the area and shape of the cyclic voltammetry curve did not change significantly, indicating that Mg 2+ 、Na + In Na 3.7 V6O 16 ·2.9H2O can undergo reversible insertion / extraction cycles in the positive electrode, with good reversibility.
[0091] The sodium-rich sodium polyvanadate materials prepared in Examples 2 to 5 were used to perform the above electrochemical performance test and had similar electrochemical performance.
[0092] It can be seen that the Na prepared by the present invention 2+x V6O 16 ·When 2.9H2O material is used as the positive electrode material of magnesium-ion batteries and magnesium-based mixed-ion batteries, it shows excellent electrochemical performance, which provides a direction for the research of high-capacity and long-life magnesium-ion batteries and magnesium-based mixed-ion batteries.
[0093] 3. Application Examples
[0094] Application Example 1
[0095] A magnesium-sodium mixed ion battery, comprising:
[0096] Na prepared in Example 1 of the present invention 3.7 V6O 16 ·2.9H2O material is loaded on carbon paper current collector as positive electrode, 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA) is loaded on carbon cloth current collector as negative electrode, and 1.5M NaTFSI / Mg(TFSI)2 electrolyte is used as electrolyte to assemble into magnesium-sodium mixed ion full battery. + / Mg 2+ The molar ratio is 1:1.
[0097] The battery capacity and coulombic efficiency of the battery assembled in this embodiment are as follows: Figure 8 As shown by Figure 8 It can be seen that in Na + / Mg 2+ In the NaTFSI / Mg(TFSI)2 electrolyte with a molar ratio of 1:1, the hybrid ion battery -1 Provides 28mAh g -1 The initial specific capacity is as high as 90% in 200 cycles.
[0098] Application Example 2
[0099] A magnesium-sodium mixed ion battery, comprising:
[0100] Na prepared in Example 1 of the present invention 3.7 V6O 16·2.9H2O material is loaded on carbon paper current collector as positive electrode, 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA) is loaded on carbon cloth current collector as negative electrode, and 1.5M NaTFSI / Mg(TFSI)2 electrolyte is used as electrolyte to assemble into magnesium-sodium mixed ion full battery. + / Mg 2+ The molar ratio is 2:1.
[0101] The battery capacity and coulombic efficiency of the battery assembled in this embodiment are as follows: Fig. 9 As shown by Fig. 9 It can be seen that in Na + / Mg 2+ In the NaTFSI / Mg(TFSI)2 electrolyte with a molar ratio of 2:1, the hybrid ion battery -1 Provides 28mAh g -1 The initial specific capacity of the battery decreased to about 70% after 200 cycles.
[0102] Application Example 3
[0103] A magnesium-sodium mixed ion battery, comprising:
[0104] Na prepared in Example 1 of the present invention 3.7 V6O 16 ·2.9H2O material is loaded on carbon paper current collector as positive electrode, 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA) is loaded on carbon cloth current collector as negative electrode, and 1.5M NaTFSI / Mg(TFSI)2 electrolyte is used as electrolyte to assemble into magnesium-sodium mixed ion full battery. + / Mg 2+ The molar ratio is 2.5:1.
[0105] The battery capacity and coulombic efficiency of the battery assembled in this embodiment are as follows: Fig.10 As shown by Fig.10 It can be seen that in Na + / Mg 2 + In the NaTFSI / Mg(TFSI)2 electrolyte with a molar ratio of 2.5:1, the average coulombic efficiency of the hybrid ion battery after 200 cycles is about 90%, but its -1 The initial specific capacity was reduced to 21 mAh g -1 .
[0106] By comparative analysis, Na + / Mg 2+When the molar ratio is 1:1, the magnesium-sodium mixed ion full battery has both the optimal capacity and the optimal coulombic efficiency.
[0107] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A sodium-rich sodium polyvanadate material, characterized in that: Its chemical formula is Na 2+x V6O 16 ·2.9H2O, where 0 < X < 4, and the microscopic morphology is an anisotropic single-crystal nanobelt structure.
2. The method for preparing the sodium-rich sodium polyvanadate material according to claim 1, characterized in that: The following steps are involved: (1) dissolving sodium metavanadate in deionized water and stirring until the sodium metavanadate is completely dissolved to obtain a sodium metavanadate solution, which is referred to as solution A; (2) Under stirring conditions, add an acid solution to solution A and adjust the pH to 2-3.
5. The resulting solution is recorded as solution B. (3) Solution B is placed in a water bath, stirred to allow for sufficient reaction, cooled naturally, filtered, washed, and dried to obtain a sodium-rich sodium polyvanadate material.
3. The method for preparing a sodium-rich sodium polyvanadate material according to claim 2, wherein: The concentration of the sodium metavanadate solution in step (1) is 5 g / L to 35 g / L.
4. The method for preparing a sodium-rich sodium polyvanadate material according to claim 2, wherein: The mass concentration of the acid solution in step (2) is 5% to 30%.
5. The method for preparing a sodium-rich sodium polyvanadate material according to claim 2, wherein: In the step (3), the water bath temperature is 60 to 130° C., and the stirring time is 3 to 12 hours.
6. A positive electrode sheet for a battery, characterized in that: The invention comprises the sodium-rich sodium polyvanadate material as described in claim 1.
7. A battery, characterized in that: Including the positive electrode sheet as claimed in claim 6.
8. A magnesium-based hybrid ion battery, based on Na + / Mg 2+ The double salt electrolyte is an electrolyte characterized in that The positive electrode sheet according to claim 6 is used as the positive electrode.
9. The magnesium-based hybrid ion battery according to claim 8, characterized in that: The Mg 2+ / Na + The concentration of the double salt electrolyte is 0.5 to 3M.
10. The magnesium-based hybrid ion battery according to claim 8, characterized in that: In the double salt electrolyte, Na + / Mg 2+ The molar ratio is 1 to 2.5:1.
Citation Information
Patent Citations
Preparation method of magnesium ion battery positive electrode material
CN114368783A
Magnesium-doped sodium-rich sodium polyvanadate material as well as preparation method and application thereof