Battery pole piece, preparation method thereof and secondary battery

By designing a structure including a current collector, an active material layer and a conductive material auxiliary layer in the lithium-ion secondary battery electrode sheet, the problem of poor bonding in the edge area of ​​the battery electrode sheet is solved, and the ion conduction and cycling performance are improved. Extends the battery life.

CN119092706APending Publication Date: 2024-12-06BYD CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411153629.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The thickness direction of the edge area of ​​the lithium-ion secondary battery has poor fit, resulting in poor ion conduction performance and poor charging capacity and cycling performance.

Method used

The battery electrode design is adopted which includes a current collector, an active material layer and an auxiliary layer. The active material layer consists of a first part and a second part, the second part is located on one side of the first part, the auxiliary layer is made of a conductive material, and the auxiliary layer is located on the The second part is away from the side of the current collector and contacts the second part to improve the thickness and ion conduction properties of the edge region.

Benefits of technology

By increasing the thickness and ion conduction performance of the edge area of ​​the battery pole plate, the ion conductivity and cyclic stability of the battery pole plate are improved, and the service life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092706A_ABST
    Figure CN119092706A_ABST
Patent Text Reader

Abstract

The invention discloses a battery pole piece, a preparation method thereof and a secondary battery, relates to the technical field of batteries, and aims to solve the problem that the edge area of the battery pole piece is poorer in lamination in the thickness direction. The battery pole piece comprises a current collector, an active material layer and at least one auxiliary layer, the active material layer is arranged on the surface of the current collector; the active material layer comprises a first part and at least one second part, the second part is positioned on one side of the first part along a first direction, and the first direction is intersected with the thickness direction of the battery pole piece; an average thickness of the first portion is greater than an average thickness of the second portion. The auxiliary layer is arranged on one side, far away from the current collector, of the second part and is in contact with the second part; the material of the auxiliary layer includes a conductive material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a battery pole piece and a preparation method thereof, and a secondary battery. Background Art

[0002] As a green, efficient and reliable energy storage device, lithium-ion secondary batteries have broad application prospects in the fields of energy, transportation, military, etc. Battery poles are an important component of lithium-ion secondary batteries, which not only affect the capacity, cycle life and safety of the battery, but also affect the charge and discharge performance of the battery. Therefore, the research and optimization of battery poles is the key to improving the performance of lithium-ion secondary batteries.

[0003] During the preparation of battery pole pieces, when the wet slurry made of positive and negative electrode materials is coated, due to the casting effect of the wet slurry itself, the coating amount at the edge of the pole piece is less than that in the middle area of ​​the pole piece, resulting in the thickness of the slurry in the edge area of ​​the pole piece being too thin and the expansion force being low, resulting in poor adhesion in the thickness direction of the edge area of ​​the battery pole piece, causing the ion conductivity of the edge area of ​​the battery pole piece to be poor during the battery charge and discharge cycle, thereby worsening the charging capacity and cycle performance, and affecting the battery performance. Summary of the invention

[0004] The purpose of the present application is to provide a battery pole piece and a method for preparing the same, and a secondary battery, aiming to solve the problem of poor bonding in the thickness direction of the edge area of ​​the battery pole piece.

[0005] In order to achieve the above objectives, this application adopts the following technical solutions:

[0006] In a first aspect, the present application provides a battery pole piece. The battery pole piece includes a current collector, an active material layer and at least one auxiliary layer. The active material layer is disposed on the surface of the current collector; the active material layer includes a first part and at least one second part, the second part is located on one side of the first part along a first direction, and the first direction intersects with the thickness direction of the battery pole piece; the average thickness of the first part is greater than the average thickness of the second part. The auxiliary layer is disposed on the side of the second part away from the current collector and in contact with the second part; the material of the auxiliary layer includes a conductive material.

[0007] In the battery electrode provided in the embodiment of the present application, the auxiliary layer is arranged on the second part. The auxiliary layer can be used to increase the overall thickness of the edge area of ​​the battery electrode, so that the thickness difference of the area where the active material layer is arranged in the battery electrode is relatively small, and the fitting effect in the thickness direction of the edge area of ​​the battery electrode can be improved. Moreover, the material of the auxiliary layer includes conductive material, which can realize ion conduction between the second part and the auxiliary layer, thereby improving the ion conductivity performance of the edge area of ​​the battery electrode, thereby improving the ion conductivity performance of the battery electrode.

[0008] In some embodiments, the conductive material includes a conductive polymer material, and the conductive polymer material is configured to form a conductive polymer gel under a first predetermined condition.

[0009] In some embodiments, the conductive polymer material includes at least one of a polyoxyethylene-based conductive polymer material, a polyacrylonitrile-based conductive polymer material, a polymethyl methacrylate-based conductive polymer material, a polyvinylidene fluoride-based conductive polymer material, and a polyvinylidene fluoride-hexafluoropropylene-based conductive polymer material.

[0010] In some embodiments, under room temperature conditions, the viscosity of the conductive polymer material ranges from 500 mPa·s to 8000 mPa·s.

[0011] In some embodiments, the active material layer is disposed on the first surface of the current collector. The distance between the surface of the auxiliary layer away from the first surface and the first surface is a first size. The distance between the surface of the first portion away from the first surface and the first surface is a second size. The ratio between the first size and the second size is greater than or equal to a first threshold.

[0012] In some embodiments, a ratio between the first dimension and the second dimension is greater than or equal to 92%.

[0013] In some embodiments, the dimension of the second portion along the thickness direction of the battery electrode sheet is a first thickness, and the first thickness gradually decreases in a direction away from the first portion.

[0014] In some embodiments, the dimension of the auxiliary layer along the thickness direction of the battery electrode sheet is a second thickness, and the second thickness gradually increases in a direction away from the first portion.

[0015] In some embodiments, along the first direction, second portions are disposed on both sides of the first portion, and auxiliary layers are disposed on two second portions located on both sides of the first portion.

[0016] In some embodiments, the current collector includes: a coating portion and a lug portion, the active material layer covers the coating portion, and the lug portion is adjacent to the coating portion and is not covered by the active material layer, wherein the auxiliary layer extends onto the lug portion.

[0017] In some embodiments, under the second preset condition, the peel strength of the surfaces of the auxiliary layer and the active material layer is greater than or equal to 0.1 N / 40 mm.

[0018] In the second aspect, the application provides a method for preparing a battery pole piece. The method for preparing a battery pole piece includes: providing a current collector; forming an active material layer on the surface of the current collector, the active material layer including a first part and at least one second part, the second part is located on one side of the first part along a first direction, the first direction intersects with the thickness direction of the battery pole piece, and the average thickness of the first part is greater than the average thickness of the second part; forming at least one auxiliary layer, the auxiliary layer is arranged on the side of the second part away from the current collector, and the auxiliary layer is in contact with the second part. The material of the auxiliary layer includes a conductive material.

[0019] In some embodiments, forming at least one auxiliary layer includes: forming an initial auxiliary layer by a coating process, the initial auxiliary layer including a portion located on a side of the second portion away from the current collector and contacting the second portion, and heating the initial auxiliary layer to form the auxiliary layer.

[0020] In some embodiments, forming the active material layer includes: forming an initial active material layer by a coating process; and heating the initial active material layer to form the active material layer. The initial auxiliary layer and the initial active material layer are formed by the same coating process.

[0021] In some embodiments, forming at least one auxiliary layer includes: forming a composite film, the composite film including an intermediate layer and a release film located on both sides of the intermediate layer, the material of the intermediate layer being the same as the material of the auxiliary layer; and peeling off the release film to cover the intermediate layer on the side of the second part away from the current collector.

[0022] In some embodiments, forming the composite film includes: composite the initial intermediate layer and the release film to obtain the initial composite film; and adopting a rolling process and a winding process to obtain a rolled initial composite film.

[0023] In some embodiments, forming the composite film further comprises: heating the initial composite film so that the initial intermediate layer forms the intermediate layer. Alternatively, heating the rolled initial composite film so that the initial intermediate layer forms the intermediate layer.

[0024] In some embodiments, the material of the release film includes at least one of polypropylene and polyethylene terephthalate.

[0025] In a third aspect, the present application provides a secondary battery. The secondary battery includes a battery housing, a battery core and an electrolyte, wherein the battery core and the electrolyte are arranged in the inner cavity of the battery housing. The battery core includes a battery pole sheet as in any of the above embodiments. Alternatively, the battery core includes a battery pole sheet obtained by the preparation method as in any of the above embodiments.

[0026] In some embodiments, the battery electrode sheet includes at least one auxiliary layer, in which an electrolyte is swollen.

[0027] In some embodiments, the battery core is a wound battery core or a laminated battery core.

[0028] In some embodiments, when the battery core is a laminated battery core, the difference between the maximum value of the dimension of the battery core along the second direction and the minimum value of the dimension of the battery core along the second direction ranges from 0 to 0.04 mm; the second direction is the thickness direction of the battery plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0030] Figure 1 Schematic diagram of the coating thinning area of ​​the positive electrode sheet in some embodiments;

[0031] Figure 2 Schematic diagram of the coating thinning area of ​​the negative electrode plate in some embodiments;

[0032] Figure 3 It is a structural diagram of a battery electrode in some embodiments;

[0033] Figure 4 The structure diagram of the battery pole piece in some other embodiments;

[0034] Figure 5 The structure diagram of the battery pole piece in some other embodiments;

[0035] Figure 6 A flowchart of a method for preparing a battery electrode sheet in some embodiments;

[0036] Figure 7 A schematic diagram of a battery pole piece coating process in some embodiments;

[0037] Figure 8 Schematic diagram of a battery electrode coating process in some embodiments;

[0038] Fig. 9 A structural diagram of a secondary battery in some embodiments;

[0039] Fig.10 Schematic diagram of the structure of a secondary battery in some embodiments. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0041] In the description of this application, it should be understood that the terms "upper", "lower", "left", "right", "front", "back", "inside", "outside", etc. indicate directions or positional relationships based on the directions or relative positional relationships shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on this application. Unless otherwise specified, the above-mentioned directional description can be flexibly set in the process of actual application under the condition that the relative positional relationship shown in the accompanying drawings is met.

[0042] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, "plurality" means two or more.

[0043] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection. It can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0044] In the present application, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, article or device. In the absence of further restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the process, article or device including the element.

[0045] In the embodiments of the present application, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.

[0046] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0047] It should be noted that, for example, 11-1 in the drawings of this application indicates that component 11 belongs to component 1, for example, Figure 3 111 to 110 indicate that the tabs 111 belong to the current collector 110. For example, 1 / 2 in the drawings of the present disclosure indicates that both component 1 and component 2 can refer to the component, for example, Fig. 9 200A / 200 indicates that the laminated pole core 200A and the pole core 200 can be represented by this component. Other similar reference numerals appearing in the drawings also follow the above description.

[0048] In order to make the technical problems, technical solutions and beneficial effects solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0049] like Fig. 9 and Fig.10 As shown, the secondary battery 300 includes a battery housing 310 , a battery core 200 and an electrolyte 320 , and the battery core 200 and the electrolyte 320 are sealed and accommodated in the inner cavity of the battery housing 310 .

[0050] Exemplarily, the battery core 200 includes a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode. The positive electrode is prepared from a positive electrode sheet. The negative electrode is prepared from a negative electrode sheet. The positive electrode sheet includes a current collector and a positive electrode material loaded on the current collector. The negative electrode sheet includes a current collector and a negative electrode material loaded on the current collector.

[0051] Exemplarily, the preparation method of the positive electrode sheet is to mix the positive electrode material, the conductive agent and the binder in a certain proportion in a solvent to obtain the required positive electrode slurry, and then apply the positive electrode slurry on the current collector, and obtain the positive electrode after drying and pressing.

[0052] Exemplarily, the preparation process of the negative electrode sheet is to mix the negative electrode material and the binder in a certain proportion in a solvent to obtain the desired negative electrode slurry, and then apply the negative electrode slurry on the current collector, and obtain the negative electrode sheet after drying and pressing.

[0053] In some implementations, when preparing a battery electrode sheet (e.g., a positive electrode sheet or a negative electrode sheet) and applying a wet slurry (e.g., a positive electrode slurry or a negative electrode slurry), the wet slurry has a smaller coating amount at the edge of the battery electrode sheet due to its own casting effect, such as Figure 1 The positive electrode sheet 10 shown shows an edge thinning region Q, such as Figure 2 The negative electrode plate 11 shown shows an edge thinning area P, which leads to edge bursting or low edge surface density after coating and winding, resulting in poor bonding effect in the thickness direction of the edge area of ​​the battery plate. During the charge and discharge cycle of the secondary battery, the expansion force of the edge thinning area Q and / or the edge thinning area P is limited, resulting in poor ion conductivity, and sometimes causing abnormal N / P ratio problems, resulting in poor charging capacity and cycle performance, affecting the performance of the secondary battery.

[0054] In some other embodiments, when applying the wet slurry, a stainless steel gasket is used to design a corresponding chamfer at the edge of the pole piece for adjustment to increase the amount of wet slurry applied to the edge of the battery pole piece. However, when using the stainless steel gasket for adjustment, it is usually necessary to stop the machine and adjust the horizontality of the bolts. This operation is time-consuming and cannot accurately control the amount of coating on the edge of the pole piece. It may also cause a significant thinning of the slurry thickness in the edge of the battery pole piece, even up to 5mm to 50mm wide, affecting battery performance and causing a large design waste.

[0055] Based on this, firstly, Figure 3 As shown, the embodiment of the present application provides a battery electrode 100. The battery electrode 100 includes a current collector 110, an active material layer 120 and at least one auxiliary layer 130.

[0056] The active material layer 120 is disposed on at least one surface of the current collector 110; the active material layer 120 includes a first portion 121 and at least one second portion 122, the second portion 122 is located on one side of the first portion 121 along a first direction X, and the first direction X intersects with the thickness direction of the battery electrode; the average thickness of the first portion 121 is greater than the average thickness of the second portion 122. Figure 3 The dotted line in represents a boundary line between the first portion 121 and the second portion 122 .

[0057] The auxiliary layer 130 is disposed on a side of the second portion 122 away from the current collector 110 and in contact with the second portion 122 ; the material of the auxiliary layer 130 includes a conductive material.

[0058] In some examples, the battery electrode sheet 100 may be a positive electrode sheet. In this case, the material of the active material layer 120 may include a positive electrode material, a conductive agent, and a binder.

[0059] In some other examples, the battery electrode sheet 100 may be a negative electrode sheet. In this case, the material of the active material layer 120 may include a negative electrode material and a binder.

[0060] It can be understood that the auxiliary layer 130 is arranged on the second part 122, and the auxiliary layer 130 can be used to increase the overall thickness of the edge area of ​​the battery electrode 100, so that the thickness difference of the area where the active material layer 120 is arranged in the battery electrode 100 is relatively small, and the fitting effect in the thickness direction of the edge area of ​​the battery electrode 100 can be improved. Moreover, the material of the auxiliary layer 130 includes conductive material, which can realize ion conduction between the second part 122 and the auxiliary layer 130, so that the ion conductivity performance of the edge area of ​​the battery electrode 100 is improved, thereby improving the ion conductivity performance of the battery electrode 100.

[0061] In some implementations, when the edge thinning region (e.g. Figure 1 The area indicated by the symbol Q or Figure 2 When the expansion force of the area indicated by the middle mark P is low and the current density of the edge thinning area is large, the edge thinning area consumes the electrolyte prematurely, resulting in excessive loss of active materials, which in turn causes battery cycle failure and affects battery performance.

[0062] In some embodiments, the conductive material includes a conductive polymer material, and the conductive polymer material is configured to form a conductive polymer gel under a first predetermined condition.

[0063] For example, the first preset condition may be placing the conductive polymer material in a liquid environment, such as an electrolyte environment. Alternatively, the first preset condition may be heating to above 60°C.

[0064] In the relevant technology, conductive polymer materials have high conductivity, good flexibility and toughness, and can adapt to various deformations such as bending and stretching; conductive polymer materials also have excellent chemical stability and can remain stable in a wide temperature range; in addition, conductive polymer materials also have certain corrosion resistance and protection, and can protect metal and other substrates from the influence of the external environment. In addition, conductive polymers have good processability and can be prepared into materials of different forms through various methods such as solution self-assembly, printing, coating, hot pressing, spinning, etc.

[0065] On this basis, after the conductive polymer material forms a conductive polymer gel, in addition to having the properties of the above-mentioned conductive polymer material, it also has better liquid retention performance due to the porous structure in the conductive polymer gel or the loose inorganic particle layer that may exist. In this way, the conductive polymer material can swell the electrolyte to form a conductive polymer gel. In this way, the conductive polymer gel can swell a certain amount of electrolyte to form a liquid retention effect, so that the electrolyte in the edge area of ​​the active material layer 120 is consumed more slowly, reducing the loss of active substances and ensuring the circulation of the secondary battery. Moreover, the conductive polymer material does not fall off or pulverize due to swelling of the electrolyte, and can be immersed in the electrolyte for 10 years without falling off or pulverizing.

[0066] In some embodiments, the conductive polymer material includes at least one of a polyoxyethylene-based conductive polymer material, a polyacrylonitrile-based conductive polymer material, a polymethyl methacrylate-based conductive polymer material, a polyvinylidene fluoride-based conductive polymer material, and a polyvinylidene fluoride-hexafluoropropylene-based conductive polymer material.

[0067] In practical applications, the above conductive polymer material can be modified to improve the performance of the conductive polymer material, such as adhesion, stability or conductivity, etc. For example, when the conductive polymer material is a polymethyl methacrylate-based conductive polymer material, the polymethyl methacrylate-based conductive polymer material can be modified to improve the conductivity of the polymethyl methacrylate-based conductive polymer material.

[0068] It can be understood that the above conductive polymer material has the advantages of being easy to obtain, low cost, strong conductivity, and being able to form a conductive polymer gel, and can be used as the material of the auxiliary layer 130 .

[0069] In some embodiments, under room temperature conditions, the viscosity of the conductive polymer material ranges from 500 mPa·s to 8000 mPa·s.

[0070] For example, at room temperature, the viscosity of the conductive polymer material may be 500 mPa·s, 2000 mPa·s, 3500 mPa·s, 5000 mPa·s, 6500 mPa·s or 8000 mPa·s, etc., but is not limited thereto.

[0071] When the viscosity of the conductive polymer material is relatively large (for example, greater than 8000mPa·s), the castability of the conductive polymer material may be affected, causing the auxiliary layer 130 to be uneven in thickness or agglomerate; when the viscosity of the conductive polymer material is relatively small (for example, less than 500mPa·s), the auxiliary layer 130 may not be effectively attached to the active material layer 120, or the bonding force between the auxiliary layer 130 and the active material layer 120 may be relatively weak, resulting in shedding or peeling. Therefore, by setting the viscosity of the conductive polymer material to a range of 500mPa·s to 8000mPa·s, the conductive polymer can be uniformly adhered to the active material layer 120, and the bonding force between the auxiliary layer 130 and the active material layer 120 can be improved, forming a good bonding interface and improving the bonding strength.

[0072] In some embodiments, Figure 4 As shown, the active material layer 120 is disposed on the first surface A of the current collector 110. The distance between the surface of the auxiliary layer 130 away from the first surface A and the first surface A is a first size L 1 The distance between the surface of the first portion 121 away from the first surface and the first surface is the second dimension L 2 .

[0073] Among them, the first dimension L 1 With the second size L 2 The ratio between them is greater than or equal to the first threshold.

[0074] It can be understood that by setting the ratio between the first size and the second size to be greater than or equal to the first threshold value, the thickness of the area in the battery electrode 100 where the active material layer 120 is provided can be made more uniform, and the fitting effect in the thickness direction of the edge area of ​​the battery electrode 100 can be improved, thereby improving the ion conductivity of the edge area of ​​the battery electrode 100, thereby improving the ion conductivity of the battery electrode 100, and further improving the battery cycle performance.

[0075] In some embodiments, the first dimension L 1 With the second size L 2 The ratio between them is greater than or equal to 92%.

[0076] For example, the first dimension L 1 With the second size L 2 The ratio between them can be 92%, 94%, 96%, 98%, 99% or 102%, etc., which is not limited here.

[0077] In some embodiments, Figure 4 As shown, the dimension of the second portion 122 along the thickness direction of the battery electrode 100 is a first thickness D 1 The first thickness D1 The width of the first portion 121 gradually decreases in a direction away from the first portion 121 .

[0078] In some embodiments, Figure 4 As shown, the dimension of the auxiliary layer 130 along the thickness direction of the battery electrode 100 is the second thickness D 2 The second thickness D 2 The width of the first portion 121 gradually increases in a direction away from the first portion 121 .

[0079] It can be understood that, through the above configuration, the second thickness D 2 The variation trend of the first thickness D 1 The changing trend is opposite to that of the first portion 122 . More material of the auxiliary layer 130 can be filled in the thinner portion of the second portion 122 , and less material of the auxiliary layer 130 can be filled in the thicker portion of the second portion 122 . In this way, the thickness of the area where the active material layer 120 is provided in the battery electrode 100 can be made more uniform, and the fitting effect in the thickness direction of the edge area of ​​the battery electrode 100 can be improved.

[0080] In some examples, the thickness of the auxiliary layer 130 to be set can be determined according to the coating speed and coating amount of the wet slurry, and the coating speed and coating amount of the auxiliary layer 130 can be adjusted according to the determined thickness of the auxiliary layer 130, so that the dimension of the auxiliary layer 130 along the thickness direction of the battery electrode 100 is the second thickness D2. The second thickness D2 gradually increases in the direction away from the first portion 121.

[0081] In some embodiments, Figure 3 to Figure 6 As shown, along the first direction X, the second parts 122 are disposed on both sides of the first part 121 , and the auxiliary layer 130 is disposed on the two second parts 121 located on both sides of the first part 121 .

[0082] It can be understood that, through the above arrangement, the bonding effect of the two edge regions of the battery pole piece in the thickness direction can be improved, so that the ionic conductivity performance of the battery pole piece can be improved as a whole.

[0083] In some embodiments, Figure 5 As shown, the current collector 110 includes a coating portion 111 and a lug portion 112 . The active material layer 120 covers the coating portion 111 ; the lug portion 112 is adjacent to the coating portion 111 and is not covered by the active material layer 120 ; wherein the auxiliary layer 130 also includes a portion covering the lug portion 112 .

[0084] In some embodiments, under the second preset condition, the peel strength of the surfaces of the auxiliary layer 130 and the active material layer 120 is greater than or equal to 0.1 N / 40 mm.

[0085] Exemplarily, the second preset condition may be: peeling is performed at a peeling angle greater than 45° at room temperature.

[0086] For example, the peel strength between the auxiliary layer 130 and the active material layer 120 may be 0.1 N / 40 mm, 0.3 N / 40 mm, 0.5 N / 40 mm, 0.7 N / 40 mm, or 1.0 N / 40 mm, etc., which is not limited here.

[0087] It can be understood that, through the above configuration, the bonding strength between the auxiliary layer 130 and the active material layer 120 can be increased, making the connection between the auxiliary layer 130 and the active material layer 120 closer, which is helpful for ion transmission, thereby improving the stability of the battery cycle.

[0088] In a second aspect, the present application provides a method for preparing a battery electrode 100. Figure 6 As shown, the method for preparing the battery electrode 100 includes: S1 to S3.

[0089] S1: providing a current collector 110 .

[0090] S2: forming an active material layer 120 on the surface of the current collector 110. The active material layer 120 includes a first portion 121 and at least one second portion 122, wherein the second portion 122 is located on one side of the first portion 121 along a first direction X, and the first direction X intersects with the thickness direction of the battery electrode 100. The average thickness of the first portion 121 is greater than the average thickness of the second portion 122.

[0091] S3: forming at least one auxiliary layer 130. The auxiliary layer 130 is disposed on a side of the second portion 122 away from the current collector 110, and the auxiliary layer 130 is in contact with the second portion 122. The material of the auxiliary layer 130 includes a conductive material.

[0092] In some embodiments, S3 forming the auxiliary layer 130 includes: S3.1A to S3.2A.

[0093] S3.1A: forming an initial auxiliary layer by a coating process, wherein the initial auxiliary layer includes a portion located on a side of the second portion 122 away from the current collector 110 and in contact with the second portion 122 .

[0094] S3.2A: Heat the initial auxiliary layer to form the auxiliary layer 130 .

[0095] Regarding the S3.1A coating process, before coating, the coating amount and coating width of the conductive polymer material can be adjusted accordingly according to the width and thickness of the second portion 122 collected in the early stage, so as to better fit the battery pole piece 100 and improve the battery performance. In particular, the coating speed and coating amount can also be adjusted accordingly according to the width and thickness of the second portion 122, so as to stably coat the second portion 122 corresponding to the battery pole piece.

[0096] In some embodiments, S2 forming an active material layer includes: S2.1 to S2.2.

[0097] S2.1: Forming an initial active material layer by a coating process.

[0098] S2.2: heating the initial active material layer to form the active material layer 120 .

[0099] Figure 7 Schematic diagram of the battery electrode coating process in some embodiments. Figure 7 In the figure, M represents a conductive polymer material feeding device. The process of coating the conductive polymer material by the conductive polymer material feeding device M can be performed after the active material layer 120 is coated, or can be performed during the coating process of the active material layer 120.

[0100] To this end, in some embodiments, the initial auxiliary layer and the initial active material layer are formed by a same coating process.

[0101] It can be understood that, through the above configuration, the process of forming the auxiliary layer 130 can be simplified.

[0102] In some embodiments, Figure 8 As shown, forming at least one auxiliary layer 130 includes: S3.1B to S3.2B.

[0103] S3.1B: forming a composite film, wherein the composite film includes an intermediate layer 130 i and release films R located on both sides of the intermediate layer 130 i . The material of the intermediate layer 130 i is the same as that of the auxiliary layer 130 .

[0104] S3.2B: Peel off the release film R, and cover the intermediate layer 130 i on the side of the second portion 122 away from the current collector 110 .

[0105] It can be understood that, through the above arrangement, the auxiliary layer 130 can be formed in a prefabricated manner, which is conducive to the large-scale production of the auxiliary layer 130 .

[0106] In some embodiments, forming a composite film (ie, S3.1B) includes: S3.11B to S3.12B.

[0107] S3.11B: Compounding the initial intermediate layer and the release film to obtain an initial composite film.

[0108] S3.12B: A rolled initial composite film is obtained by using a rolling process and a winding process.

[0109] Here, the roll pressing process is to pressurize the initial composite film by a roll-to-roll method.

[0110] It can be understood that, through the above arrangement, a rolled initial composite film can be formed, and the portability of the initial composite film can be improved.

[0111] In some embodiments, forming a composite membrane (ie, S3.1B) further comprises S3.13B.

[0112] S3.13B: Heating the initial composite film so that the initial intermediate layer forms an intermediate layer.

[0113] It should be understood that, in the case where forming the composite film further includes S3.13B, S3.13B may be performed after S3.11B and before S3.12B.

[0114] In some embodiments, forming a composite membrane (ie, S3.1B) further includes S3.14B.

[0115] S3.14B: Heating the rolled initial composite film so that the initial intermediate layer forms an intermediate layer.

[0116] It should be understood that, in the case where forming the composite film further includes S3.14B, S3.14B may be performed after S3.12B.

[0117] In some embodiments, the material of the release film R includes at least one of polypropylene and polyethylene terephthalate.

[0118] It can be understood that the above-mentioned materials are easy to obtain, low in cost, and easy to release, which can prevent the initial intermediate layer from adhering to the release film, and is beneficial to improving the process feasibility of the auxiliary layer 130 .

[0119] In a third aspect, the present application provides a secondary battery. Fig. 9 and Fig.10 As shown, the secondary battery 300 includes a battery housing 310, a battery core 200 and an electrolyte 320, and the battery core 200 and the electrolyte 320 are arranged in the inner cavity of the battery housing 310. The battery core 200 includes a battery pole piece 100 as in any of the above embodiments. Alternatively, the battery core 200 includes a battery pole piece 100 obtained by the preparation method of any of the above embodiments.

[0120] In some embodiments, the battery electrode sheet 100 includes at least one auxiliary layer 130. The auxiliary layer 130 is swollen with electrolyte.

[0121] It can be understood that when the auxiliary layer 130 is swollen with electrolyte, the auxiliary layer 130 can realize the liquid retention function. In this way, the amount of electrolyte in the edge area of ​​the battery electrode 100 can be increased to prevent the edge area of ​​the battery electrode 100 from consuming the electrolyte too early, thereby avoiding the battery cycle failure caused by excessive loss of active materials in the edge area of ​​the battery electrode 100, thereby improving the performance of the secondary battery.

[0122] In some embodiments, the battery core 200 is a wound battery core 200B or a laminated battery core 200A.

[0123] It can be understood that according to the description of the above-mentioned conductive polymer material, the conductive polymer material can make the material on the battery pole piece 100 fit well with the current collector 110, and has high flexibility, and can also increase the flexibility of the battery pole piece 100. Therefore, whether it is made into a wound battery pole core or a stacked battery pole core, it can reduce defects such as material falling off, cracking, curling and bursting in the electrode manufacturing process, which is beneficial to improving the performance of the secondary battery.

[0124] In some embodiments, when the battery electrode core 200 is a laminated battery electrode core 200A, the difference between the maximum value of the dimension H of the battery electrode core 200A along the second direction Y and the minimum value of the dimension H of the battery electrode core 200A along the second direction Y is in the range of 0 to 0.04 mm; the second direction Y is the thickness direction of the battery electrode sheet 100.

[0125] In practical applications, a hot pressing process can be used when forming the battery core 200A, and a specific temperature and pressure can be set to ensure that the two ends and the middle large surface of the battery core maintain a uniform thickness. For example, the maximum value of the dimension H of the battery core 200A along the second direction Y and the minimum value of the dimension H of the battery core 200A along the second direction Y are in the range of 0 to 0.04 mm.

[0126] Exemplarily, the difference between the maximum value of the dimension H of the battery pole core 200A along the second direction Y and the minimum value of the dimension H of the battery pole core 200A along the second direction Y can be 0, 0.01mm, 0.02mm, 0.03mm or 0.04mm, etc., which is not limited here.

[0127] Through the above-mentioned setting, the thickness of the battery core 200A can be made more uniform and consistent, ensuring that the current is more evenly distributed in the battery core 200A. It can also reduce the deformation and stress concentration of the battery core 200A during the charging and discharging process, reduce the cracking or powdering of the battery core 200A, and thus improve the cycle life and stability of the battery.

[0128] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A battery electrode, It is characterized in that include: current collector; An active material layer is disposed on the surface of the current collector; The active material layer includes a first portion and at least one second portion, wherein the second portion is located on one side of the first portion along a first direction, wherein the first direction intersects with a thickness direction of the battery electrode sheet; and an average thickness of the first portion is greater than an average thickness of the second portion; as well as, at least one auxiliary layer; The auxiliary layer is disposed on a side of the second portion away from the current collector and in contact with the second portion; the material of the auxiliary layer includes a conductive material.

2. The battery electrode according to claim 1, It is characterized in that The conductive material includes a conductive polymer material, and the conductive polymer material is configured to form a conductive polymer gel under a first preset condition.

3. The battery electrode according to claim 2, It is characterized in that The conductive polymer material comprises at least one of a polyoxyethylene-based conductive polymer material, a polyacrylonitrile-based conductive polymer material, a polymethyl methacrylate-based conductive polymer material, a polyvinylidene fluoride-based conductive polymer material, and a polyvinylidene fluoride-hexafluoropropylene-based conductive polymer material.

4. The battery electrode according to claim 2, It is characterized in that Under normal temperature conditions, the viscosity of the conductive polymer material ranges from 500 mPa·s to 8000 mPa·s.

5. The battery electrode according to any one of claims 1 to 4, It is characterized in that The active material layer is disposed on the first surface of the current collector; the distance between the surface of the auxiliary layer away from the first surface and the first surface is a first size; the distance between the surface of the first portion away from the first surface and the first surface is a second size; The ratio of the first size to the second size is greater than or equal to a first threshold.

6. The battery electrode according to claim 5, It is characterized in that A ratio between the first size and the second size is greater than or equal to 92%.

7. The battery electrode according to any one of claims 1 to 4, It is characterized in that The dimension of the second portion along the thickness direction of the battery electrode sheet is a first thickness, and the first thickness gradually decreases in a direction away from the first portion.

8. The battery electrode according to any one of claims 1 to 4, It is characterized in that The dimension of the auxiliary layer along the thickness direction of the battery electrode sheet is a second thickness; the second thickness gradually increases in a direction away from the first portion.

9. The battery electrode according to any one of claims 1 to 4, It is characterized in that Along the first direction, the second parts are disposed on both sides of the first part, and the auxiliary layer is disposed on both second parts located on both sides of the first part.

10. The battery electrode according to any one of claims 1 to 4, It is characterized in that The current collector comprises: a coating portion, the active material layer covering the coating portion; and a pole ear portion, adjacent to the coating portion and not covered by the active material layer; Wherein, the auxiliary layer extends onto the pole lug portion.

11. The battery electrode according to any one of claims 1 to 4, It is characterized in that Under the second preset condition, the peeling strength between the surfaces of the auxiliary layer and the active material layer is greater than or equal to 0.1 N / 40 mm.

12. A method for preparing a battery electrode. It is characterized in that include: providing a current collector; forming an active material layer on a surface of the current collector; The active material layer includes a first portion and at least one second portion, wherein the second portion is located on one side of the first portion along a first direction, wherein the first direction intersects with a thickness direction of the battery electrode sheet; and an average thickness of the first portion is greater than an average thickness of the second portion; At least one auxiliary layer is formed. The auxiliary layer is disposed on a side of the second portion away from the current collector and in contact with the second portion. The material of the auxiliary layer includes a conductive material.

13. The method for preparing a battery electrode according to claim 12, It is characterized in that The forming of at least one auxiliary layer comprises: forming an initial auxiliary layer by a coating process, wherein the initial auxiliary layer includes a portion located on a side of the second portion away from the current collector and in contact with the second portion; and The initial auxiliary layer is heated to form the auxiliary layer.

14. The method for preparing a battery electrode according to claim 13, It is characterized in that The forming of the active material layer comprises: forming an initial active material layer by a coating process; and, heating the initial active material layer to form the active material layer; Wherein, the initial auxiliary layer and the initial active material layer are formed by a same coating process.

15. The method for preparing a battery electrode according to claim 12, It is characterized in that The forming of the auxiliary layer comprises: forming a composite film; the composite film comprises an intermediate layer and release films located on both sides of the intermediate layer, the material of the intermediate layer is the same as that of the auxiliary layer; and, The release film is peeled off, and the intermediate layer is covered on a side of the second portion away from the current collector.

16. The method for preparing a battery electrode according to claim 15, It is characterized in that The forming of the composite film comprises: Compounding the initial intermediate layer and the release film to obtain an initial composite film; and, The rolled initial composite film is obtained by adopting a rolling process and a winding process.

17. The method for preparing a battery electrode according to claim 16, It is characterized in that The forming of the composite film further comprises: heating the initial composite film so that the initial intermediate layer forms an intermediate layer; or, The rolled initial composite film is heated so that the initial intermediate layer forms an intermediate layer.

18. The method for preparing a battery pole piece according to any one of claims 15 to 17, It is characterized in that The material of the release film includes at least one of polypropylene and polyethylene terephthalate.

19. A secondary battery, It is characterized in that include: Battery housing; as well as, The battery core and electrolyte are arranged in the inner cavity of the battery shell; Wherein, the battery pole core comprises a battery pole piece as claimed in any one of claims 1 to 7; or, The battery pole core comprises a battery pole piece obtained by the preparation method according to any one of claims 8 to 11.

20. The secondary battery according to claim 19, It is characterized in that The battery pole piece includes at least one auxiliary layer; the electrolyte is swollen in the auxiliary layer.

21. The secondary battery according to claim 19, It is characterized in that The battery core is a wound battery core or a laminated battery core.

22. The secondary battery according to claim 21, It is characterized in that When the battery pole core is a laminated battery pole core, the difference between the maximum value of the dimension of the battery pole core along the second direction and the minimum value of the dimension of the battery pole core along the second direction ranges from 0 to 0.04 mm; the second direction is the thickness direction of the battery pole sheet.

Citation Information

Cited By

  • Electrode sheet and manufacturing method therefor, secondary battery and electrical apparatus

    WO2025232355A1