Diaphragm coating, diaphragm, preparation method of diaphragm and negative-electrode-free battery of diaphragm
By using ZnO and LiNO3 coated with PMMA in a negative electrode-free lithium metal battery, the problems of lithium dendrites and battery cycle stability are solved, and the battery resistance reduction and cycle stability are improved, and the process is simplified. Reduced costs.
Patent Information
- Application Number
- CN202411188141.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The battery safety and cycle stability problems caused by the formation and growth of lithium dendrites of the negative electrode are difficult to effectively solve in the entire life cycle of the existing technology, and the three-dimensional porous copper foam is high in cost and the modified SEI film has a large impedance. LiNO3 has limited solubility, and the process of increasing the physicochemical process of the positive electrode material is complicated.
By coating ZnO and LiNO3 in PMMA, the separator coating is prepared, dendrite formation is inhibited, the battery resistance is reduced, and the lithium ion conductivity and negative electrode cycle stability is improved. The PMMA is used to coat the separator coating of ZnO and LiNO3, and the PMMA is circulating. During the process, it participates in the deposition and dissolution of metal lithium, ZnO releases Li-Zn alloy, and LiNO3 forms a stable SEI component.
Effectively suppress dendrite formation, reduce battery resistance, improve negative electrode cycle stability and battery capacity retention, simplify process and reduce costs.
Smart Images

Figure BDA0005014151020000191
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to a diaphragm coating, a diaphragm and a preparation method thereof and a negative electrode-free battery thereof. Background Art
[0002] Traditional lithium batteries based on lithium-ion intercalation chemistry can no longer meet the energy density requirements of lithium batteries in various emerging fields. Lithium metal batteries (LMBs), which have a relatively high theoretical specific capacity and are known for their high energy density, have once again attracted people's attention as a promising next-generation advanced energy storage technology. Among them, anode-free lithium metal batteries (AF-LMBs) eliminate the use of initial anode active materials, which increases the battery energy density to the limit while reducing the battery production cost. They have the advantages of high energy density, low cost, and high safety, and are one of the most promising next-generation high-energy density battery systems. Similar to general lithium metal batteries, anode-free batteries also face problems such as battery safety and cycle stability caused by the formation and growth of lithium dendrites. The metal lithium deposited on the anode has extremely high reactivity and causes huge volume changes, which in turn leads to problems such as lithium dendrite growth, dead lithium generation and accumulation, and side reactions between metal lithium and electrolyte. In addition, the activation energy of lithium deposited on most current collectors is relatively high. When lithium is plated on the current collector, a large nucleation barrier needs to be overcome. Excessive overpotential may lead to uneven lithium deposition morphology, and the uneven initial morphology will seriously affect the subsequent release of lithium from the deposited layer and the deposition process in the next cycle, making it difficult to form a stable negative electrode interface, which ultimately accelerates the consumption of active lithium and causes battery failure.
[0003] At present, the research directions of the negative electrode-free battery mainly focus on the following issues: (1) Leveling the surface morphology of initial lithium deposition: three-dimensional porous copper foam, carbon nanotube sponge, and carbon nanorod array with appropriate submicron skeleton structure can reduce the local current density and provide abundant nucleation sites, which can effectively accommodate lithium into the three-dimensional current collector without generating dendrites; current collector design can improve the lithium affinity of foil, reduce the nucleation potential, and improve the morphology of lithium deposition; 2) Optimizing the SEI layer by modifying the electrolyte: optimizing the electrolyte with appropriate concentration, additives, salt combination, solvent, etc., and inducing the formation of a stable and strong SEI layer, such as LiNO3. 3) Over-lithiation of the positive electrode material: during the first cycle of charging, lithium ions are released from the positive electrode and deposited as metallic lithium on the negative electrode current collector. During the subsequent discharge, the potential is controlled to dissolve part of the metallic lithium and embed it back into the positive electrode material. At this time, some metallic lithium still exists on the negative electrode current collector, which can replenish the lithium source consumed by the side reactions in the subsequent cycles, thereby improving the battery cycle life.
[0004] However, the above scheme still has the following shortcomings: 1. The cost of three-dimensional porous copper foam as a current collector is high; 2. The modified SEI membrane design can improve the cycle life, but the impedance is large, and it can only control the initial SEI membrane uniformity and chemical stability; it is impossible to achieve SEI membrane repair throughout the life cycle; 3. Due to the limited solubility of LiNO3 in ester solvents, the amount added to the electrolyte is low and it cannot play a role throughout the life cycle; 4. The physical and chemical processes of the positive electrode material increase. Summary of the invention
[0005] In order to overcome the above technical problems, the present invention provides a diaphragm coating, a diaphragm and a preparation method thereof, and a negative electrode-free battery. The present invention prepares a diaphragm coating by coating ZnO and any LiNO3 in PMMA, which can better inhibit dendrite formation, reduce the resistance of the battery system, improve the rate performance of the battery cell, enhance the lithium ion conductivity, and enhance the cycle stability of the negative electrode.
[0006] Specifically, the first aspect of the present invention provides a diaphragm coating, wherein the coating contains PMMA and ZnO, wherein PMMA encapsulates the ZnO; wherein the mass ratio of PMMA to ZnO is (92-98):(2-5).
[0007] In one or more embodiments, the diaphragm coating further contains LiNO3, and the PMMA covers the ZnO and LiNO3; wherein, in the diaphragm coating, the mass ratio of PMMA, ZnO and LiNO3 is (92-98):(2-5):(0.5-6), preferably (92-98):(2-5):(0.5-4).
[0008] In one or more embodiments, the diaphragm coating has a thickness of 2-5 nm.
[0009] A second aspect of the present invention provides a method for preparing a diaphragm coating as described in any embodiment of the present invention, characterized in that the method comprises the following steps:
[0010] (1) Providing an aqueous solution of PMMA microspheres and an aqueous solution of ZnO
[0011] (2) mixing the ammonia solution of the PMMA microspheres and the ZnO aqueous solution, stirring for a period of time, and centrifugally drying to obtain a PMMA-coated ZnO composite material;
[0012] (3) The composite material is mixed with a solvent to obtain a coating liquid, and the coating liquid is coated on at least one surface of a substrate, and the diaphragm coating is obtained after curing.
[0013] In one or more embodiments, when the separator coating further contains LiNO 3 , the step (1) includes providing an aqueous solution containing ZnO and LiNO 3 , or further providing an aqueous solution of LiNO 3 .
[0014] In one or more embodiments, the preparation of the ammonia aqueous solution of PMMA microspheres comprises the following steps: uniformly dispersing PMMA microspheres in an ammonia aqueous solution to form an ammonia aqueous solution containing PMMA microspheres; preferably, the mass concentration of PMMA is 20-24wt%, such as 25-35wt% or 28-32wt%.
[0015] In one or more embodiments, the preparation of the aqueous solution of ZnO comprises the following steps: dispersing ZnO in water to form an aqueous solution containing ZnO; preferably, in the aqueous solution containing ZnO, the mass concentration of ZnO is 2.0-4.0wt%, such as 2.5-4.0wt% or 2.5-3.6wt%.
[0016] In one or more embodiments, the preparation of the aqueous solution containing ZnO and LiNO3 comprises the following steps: dispersing ZnO in deionized water containing LiNO3 to form an aqueous lithium nitrate solution containing ZnO; preferably, in the solution, the mass concentration of ZnO is 2.0-4.0wt%, for example, 2.5-4.0wt% or 2.5-3.6wt%; the mass concentration of LiNO3 is 0.5-3.0wt%, for example, 0.5-2.7wt%.
[0017] In one or more embodiments, the mass ratio of the aqueous ammonia solution containing PMMA microspheres to the aqueous solution containing ZnO and optionally LiNO3 is (2.0-3.0):1, for example (2.5-3.0):1.
[0018] In one or more embodiments, the solvent mixed with the composite material is selected from one or more of N,N-dimethylacetamide, acetone and N-methylpyrrolidone.
[0019] In one or more embodiments, the curing temperature is 5-80°C, such as 15-30°C.
[0020] The third aspect of the present invention provides a diaphragm, which includes a substrate layer and a diaphragm coating as described in any embodiment of the present invention coated on the substrate layer; the substrate layer is preferably a PP film, a PE film, an aramid diaphragm, or a composite film of PP and PE.
[0021] A fourth aspect of the present invention provides a lithium-ion battery, comprising a positive electrode sheet, an electrolyte and a separator, wherein the separator is the separator as described in any embodiment of the present invention.
[0022] In one or more embodiments, the ratio of the mass of LiNO3 in the separator to the mass of the positive electrode material of the positive electrode sheet is 0.2 to 0.5 wt%.
[0023] In one or more embodiments, the mass ratio of ZnO in the separator to the mass ratio of the positive electrode material of the positive electrode sheet is 2-3 wt %.
[0024] In one or more embodiments, the electrolyte includes an additive LiI, and the mass concentration of LiI in the electrolyte is preferably 30-50 mM.
[0025] In one or more embodiments, the negative electrode of the lithium ion battery is a negative electrode current collector, and the negative electrode current collector is, for example, copper foil or aluminum foil.
[0026] The fifth aspect of the present invention provides the use of the diaphragm coating as described in any embodiment of the present invention in improving the cycle performance of the battery, especially improving the battery capacity retention rate;
[0027] A sixth aspect of the present invention provides the use of the diaphragm coating as described in any embodiment herein in the preparation of a lithium ion battery, especially a negative electrode-free lithium ion battery. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this article. Unless otherwise specified, all technical and scientific terms used in this article are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this article shall prevail.
[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0030] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0031] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0032] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0033] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0034] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0035] The present invention prepares a diaphragm coating by coating ZnO and any LiNO3 in PMMA. During the lithium battery cycle, PMMA reversibly participates in the deposition and dissolution process of metallic lithium. Before deposition, the lithium ions captured by PMMA can be preferentially reduced to form initial lithium seeds, inducing changes in the morphology of metallic lithium deposition; the ZnO and any LiNO3 coated by PMMA are gradually released, and ZnO can form a Li-Zn alloy, providing an ideal choice for the deposition and growth of Li, and better inhibiting the formation of dendrites; at the same time, due to its high electron mobility, ZnO can also reduce the resistance of the battery system, thereby improving the rate performance of the battery cell. NO3 in LiNO3 - Can decompose to form Li3N and N x O y - Good SEI components such as NH4+ and NH4+ are beneficial to improving lithium ion conductivity; in addition, the Li-N bond can continuously form a uniform interface, thereby improving the cycle stability of the negative electrode. Therefore, the lithium ion battery made by using the diaphragm coating of the present invention has an improved battery capacity retention rate.
[0036] In the present invention, the full name of PMMA is polymethyl methacrylate.
[0037] Diaphragm coating
[0038] Therefore, the present invention provides a diaphragm coating, which contains PMMA and ZnO. In the diaphragm coating, ZnO encapsulates PMMA, and PMMA forms a protective layer. During the circulation process, ZnO is released as PMMA dissolves.
[0039] In the diaphragm coating of the present invention, the mass ratio of PMMA to ZnO can be (92-98):(2-5), such as (93-98):(2-4.5) or (94-98):(2-5).
[0040] In some embodiments, the diaphragm coating of the present invention may also contain LiNO3. Similarly, LiNO3 is coated in the PMMA of the diaphragm. LiNO3 is not restricted by its solubility in the electrolyte and can be slowly released throughout the life cycle to achieve long-term regulation of the negative electrode interface. Preferably, when contained, the mass ratio of PMMA and LiNO3 can be (92-98): (0.5-6), for example (92-98): (0.5-4) or (92-98): (0.5-3).
[0041] In some embodiments, the diaphragm coating of the present invention contains PMMA, ZnO and optional LiNO3, wherein ZnO and LiNO3 are coated in PMMA. In the diaphragm coating, the mass ratio of PMMA, ZnO and LiNO3 may be (92-98): (2-5): (0-6). In some embodiments, in the diaphragm coating, the mass ratio of PMMA, ZnO and LiNO3 may be (92-98): (2-5): (0-4). In some embodiments, in the diaphragm coating, the mass ratio of PMMA, ZnO and LiNO3 may be (92-98): (2-5): (0.5-6), or (92-98): (2-5): (0.5-4).
[0042] In some embodiments, the thickness of the membrane coating of the present invention is 2-5 nm.
[0043] Preparation method of diaphragm coating
[0044] The method for preparing the diaphragm coating of the present invention may include the following steps:
[0045] (1) providing an aqueous ammonia solution of PMMA microspheres and an aqueous solution of ZnO;
[0046] (2) mixing the ammonia solution of the PMMA microspheres and the ZnO aqueous solution, stirring for a period of time, and centrifugally drying to obtain a PMMA-coated ZnO composite material;
[0047] (3) The composite material is mixed with a solvent to obtain a coating liquid, and the coating liquid is coated on at least one surface of a substrate, and the diaphragm coating is obtained after curing.
[0048] In some embodiments, when the separator coating further contains LiNO 3 , the step (1) comprises providing an aqueous solution containing ZnO and LiNO 3 , or further providing an aqueous solution of LiNO 3 .
[0049] In some embodiments, PMMA microspheres are uniformly dispersed in an ammonia solution to form an ammonia solution containing PMMA microspheres. The concentration of the ammonia solution may be 0.5-1.0 mol / L. In some embodiments, the mass concentration of PMMA in the ammonia solution containing PMMA microspheres may be 20-24 wt%, such as 25-35 wt% or 28-32 wt%.
[0050] In some embodiments, ZnO is dispersed in water (preferably deionized water) to form an aqueous solution containing ZnO. Preferably, in the aqueous solution containing ZnO, the mass concentration of ZnO may be 2.0-4.0wt%, such as 2.5-4.0wt% or 2.5-3.6wt%.
[0051] In some embodiments, LiNO3 is dispersed in water (preferably deionized water) to form an aqueous solution containing LiNO3. Preferably, in the aqueous solution containing LiNO3, the mass concentration of LiNO3 may be 0.5-3.0wt%, for example, 0.5-2.7wt%.
[0052] In some embodiments, ZnO is dispersed in deionized water containing LiNO3 to form an aqueous lithium nitrate solution containing ZnO. Preferably, in the solution, the mass concentration of ZnO may be 2.0-4.0wt%, such as 2.5-4.0wt% or 2.5-3.6wt%; the mass concentration of LiNO3 may be 0.5-3.0wt%, such as 0.5-2.7wt%.
[0053] In step (2), there is no particular restriction on the mass ratio of the solution for providing PMMA microspheres, the solution for providing ZnO, and the solution for providing LiNO3, as long as the mass percentages of PMMA, ZnO, and LiNO3 (when contained) in the composite material finally prepared are within the range described in the present invention. In some embodiments, the mass ratio of the aqueous ammonia solution containing PMMA microspheres to the aqueous solution containing ZnO and optionally LiNO3 can be (2.0-3.0):1, for example (2.5-3.0):1.
[0054] In step (2), the obtained mixed solution can be stirred at a temperature of 45-60° C. for 20-60 min, for example, 30-60 min. In some embodiments, the temperature can be provided by a water bath. The mixture can be stirred in a conventional manner, and the rotation speed can be determined according to the actual production situation. After the stirring is completed, the mixture is centrifuged and dried to obtain a composite material of ZnO and optionally LiNO3 coated with PMMA.
[0055] In step (3), the type of solvent is not particularly limited, and can be selected from the types of solvents conventionally used in the art, for example, one or more selected from N,N-dimethylacetamide, acetone and N-methylpyrrolidone. In some embodiments, the solvent is selected from N,N-dimethylacetamide.
[0056] In step (3), the curing temperature is 5-80° C., such as 15-30° C., such as about 25° C. The curing time can be determined according to actual conditions, for example, it can be 30 min-2 h, such as 50 min-1.5 h. The curing can be carried out by a coagulation bath curing method well known in the art.
[0057] Step (3), after curing, it can be washed with water first and then dried. There is no particular limitation on the washing method, and it can be carried out by a conventional washing method in the art. In some embodiments, deionized water is used for washing. The purpose of drying is to remove the solvent. There is no particular limitation on the drying method, and it can be carried out by a conventional drying method in the art, such as, for example, drying.
[0058] Diaphragm
[0059] The present invention also provides a diaphragm, which includes a substrate layer and a diaphragm coating as described herein coated on the substrate layer. The material of the substrate layer is not particularly limited, and conventional base film types in the art can be used, such as PP film, PE film, aramid diaphragm, or a composite film of PP and PE.
[0060] Lithium-ion battery
[0061] The present invention provides an electrochemical device, such as a lithium ion battery, comprising the separator of the present invention. The lithium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet. The lithium ion battery of the present invention is characterized in that it comprises the separator of the present invention as a separator. The separator of the present invention is applicable to various types of lithium ion batteries, including lithium ion batteries without negative electrodes.
[0062] Lithium ion battery electrolyte contains organic solvent and lithium salt. Organic solvent commonly used in electrolyte is carbonate solvent and ether solvent. Suitable ether solvent includes but is not limited to low melting point ether, tetraethylene glycol dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,3-dioxolane, tetrafluorohydrolanthane, etc. Exemplary low melting point ethers such as ether, dodecyl ether, butyl ether, etc. Suitable carbonate solvent includes but is not limited to one or more selected from ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), preferably two or more. The lithium salt in the electrolyte of the present invention can be a lithium salt commonly used in the art, including but not limited to lithium hexafluorophosphate (LiPF6), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bis(fluorosulfonyl) imide (LiFSI), lithium bisoxalate borate (LiBOB), lithium difluorooxalate borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium fluoride (LiF), lithium trifluoromethanesulfonate (LiCF3SO3), etc. In some embodiments, the lithium salt is LiPF6 and LiFSI. The concentration of the lithium salt in the electrolyte can be 0.5 to 2 mol / L, for example 0.8 mol / L, 1 mol / L, 1.2 mol / L.
[0063] In some embodiments, the electrolyte also includes additives. Additives commonly used in electrolytes include, but are not limited to, one or more selected from vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, vinyl sulfite, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) phosphite, and adiponitrile. In some preferred embodiments, the electrolyte of the present invention includes the additive LiI. The concentration of LiI is preferably 30-50mM. In the present invention, LiI is introduced as an additive in the electrolyte additive, and I can be reversibly converted into I during the cycle. 3- , which constitutes a redox medium (I - / I 3- ) and shuttles between the positive and negative electrodes through the electrolyte. 3- It can react chemically with dead lithium to eliminate and activate dead lithium, thereby dynamically maintaining the interface stability during the battery cycle. In the present invention, if the concentration of LiI is higher than 50mM, it may cause excessive self-discharge of the battery and reduce the coulombic efficiency.
[0064] The negative electrode sheet in the lithium-ion battery generally includes a negative electrode current collector and a negative electrode material layer formed on the surface of the negative electrode current collector. The negative electrode current collector may be copper foil or aluminum foil. The negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder. The negative electrode material layer is obtained by coating a negative electrode slurry containing a negative electrode active material, a conductive agent, a binder and a solvent onto a positive electrode current collector, and then rolling and baking. The solvent of the negative electrode slurry may be water. The negative electrode active material is conventionally used in sodium ion batteries in the art, including materials that can accept and release sodium ions, such as soft carbon, hard carbon, acetylene black, sodium titanate and one or more metals that can form alloys with sodium. The negative electrode conductive agent may be one or more selected from acetylene black, carbon nanotubes, carbon black and conductive graphite. The negative electrode binder may be one or more selected from polytetrafluoroethylene emulsion (PTFE), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinylidene fluoride emulsion (PVDF). The mass ratio of each component in the negative electrode material layer can be conventional, for example, the mass fraction of the negative electrode active material can be 90%-98%, such as 93%, 95%, 95.7%, 96%, 97%. The mass fraction of the conductive agent can be 0.5%-5%, such as 1%, 1.5%, 2%, 3%, 4%. The mass fraction of the binder can be 0.5%-5%, such as 1%, 1.5%, 2%, 3%, 4%.
[0065] In some embodiments, the negative electrode sheet in the lithium ion battery may also include only the negative electrode current collector, and such lithium ion batteries may be referred to as negative electrode-free lithium ion batteries. The negative electrode current collector may be copper foil or aluminum foil. The separator of the present invention is preferably suitable for negative electrode-free lithium ion batteries.
[0066] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer (also called a positive electrode material layer) disposed on the positive electrode current collector. The positive electrode current collector can be aluminum foil, copper foil, titanium foil, nickel foil, iron foil, zinc foil, etc. The positive electrode active material layer includes a positive electrode active material (also called a positive electrode material). The positive electrode active material may include a compound that can reversibly embed and deintercalate lithium ions. The positive electrode active material may be selected from a composite oxide containing lithium and at least one selected from cobalt, manganese, nickel and iron, preferably a composite oxide containing lithium. The lithium-containing composite oxide is preferably LiM x O y and LiM x PO4, wherein M is a combination of one or more transition metals, 0<x≤3, 0<y≤4. Examples of positive electrode active materials include lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium iron phosphate (LiFePO4), etc.
[0067] The positive electrode active material layer may also include one or two selected from a conductive agent and a binder. The conductive agent is used to improve the conductivity of the electrode. Examples of the conductive agent of the positive electrode include one or more of conductive carbon black, carbon fiber (CF), acetylene black, Ketjen black, graphene and carbon nanotubes. The binder of the positive electrode improves the bonding performance between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples of the binder of the positive electrode include at least one of a fluorine-containing resin, a polypropylene resin, a fiber-type binder, a rubber-type binder and a polyimide-type binder. In some embodiments, the conductive agent in the positive electrode active material layer is conductive carbon black, and the binder is polyvinylidene fluoride.
[0068] The content ratio of each component in the positive electrode active material layer can be conventional. The mass fraction of the positive electrode active material in the positive electrode active material layer can be 90%-98%, for example, 91%, 93%, 93.5%, 94%, 94.7%, 95%, 95.2%, 96%, 97%. The mass fraction of the conductive agent can be 0.5%-5%, for example, 1%, 1.5%, 1.8%, 2%, 3%, 4%. The mass fraction of the binder can be 0.5%-5%, for example, 1%, 1.5%, 1.6%, 2%, 3%, 4%.
[0069] The positive electrode active material layer is obtained by coating a positive electrode slurry containing the components of the positive electrode active material layer and a solvent onto a positive electrode current collector, followed by drying and pressing. The solvent of the positive electrode slurry can be N-methylpyrrolidone (NMP). The surface density of the coating can be 10-22 mg / cm 2 , for example, 12 mg / cm 2 、13mg / cm 2 、14mg / cm 2 、15mg / cm 2 、16mg / cm 2 、16.5mg / cm 2 、17mg / cm 2 、18mg / cm 2 、19mg / cm 2 , 20mg / cm 2 The purpose of drying is to remove the solvent in the negative electrode active slurry. Drying can be oven drying. The drying temperature can be 80-120°C, for example, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C. The drying time can be 0.5-2h, for example, 0.8h, 1h, 1.2h, 1.5h, 1.8h.
[0070] In the present invention, in some embodiments, the mass ratio of ZnO in the separator to the mass ratio of the positive electrode material is 2-3wt%. The mass ratio of LiNO3 in the separator to the positive electrode material is 0.2-0.5wt%, such as 0.25wt%, 0.3wt%, 0.45wt%. Controlling the mass ratio of ZnO and optionally LiNO3 in the separator to the mass ratio of the positive electrode material within the above range can effectively and better inhibit dendrite formation, reduce the resistance of the battery system, improve the rate performance of the battery cell, and enhance the lithium ion conductivity and the cycle stability of the negative electrode.
[0071] The positive electrode sheet, the negative electrode sheet and the separator are stacked or wound according to the design requirements, and then packaged in a shell, and then dried, injected (injected with the hydrogel electrolyte of the present invention), sealed, formed, aged, and divided into different volumes to obtain an electrochemical device, such as a lithium ion battery. The form of the lithium ion battery of the present invention is not particularly limited, and can be a cylindrical lithium ion battery, a soft-pack lithium ion battery, or an aluminum shell lithium ion battery.
[0072] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0073] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
[0074] Example 1
[0075] Preparation of diaphragm
[0076] (1) PMMA microspheres were added into an ammonia solution (the concentration of the ammonia solution was 0.7 mol / L), and stirred to be uniformly dispersed in the solution to form an ammonia solution containing PMMA microspheres; in the ammonia solution containing PMMA microspheres, the mass concentration of PMMA was 31 wt %.
[0077] ZnO is dispersed in deionized water containing LiNO3 to form a lithium nitrate aqueous solution containing ZnO; the mass concentration of ZnO is 2.37wt%; the mass concentration of LiNO3 is 2.63wt%.
[0078] (2) The ammonia solution containing PMMA microspheres and the lithium nitrate solution containing ZnO were mixed in a mass ratio of 3:1, and reacted in a water bath at a reaction temperature of 50°C. After stirring for 30 minutes, the resulting solution was centrifuged and dried to obtain a composite material of PMMA-coated ZnO and LiNO3. In the composite material, the mass ratio of PMMA, ZnO and LiNO3 was 95:2.37:2.63.
[0079] (3) The composite material is added to a dimethylacetamide (DMAC) solvent, stirred evenly, and dispersed at high speed to obtain a solvent-based coating liquid. The coating liquid is coated on a polyethylene porous base film (Enjie, thickness of 7 μm) by a coating machine, and then cured in a coagulation bath (the temperature of the coagulation bath curing is 25°C; the curing time is 1 hour), washed with deionized water, and dried to obtain a diaphragm containing a PMMA coating. The thickness of the PMMA coating is 3 nm.
[0080] Cathode sheet preparation
[0081] Lithium iron phosphate, conductive agent SP, and binder PVDF are mixed in a certain proportion through stirring, coating, cold pressing, slitting and other processes to form the positive electrode sheets required for winding; specifically, LiFePO4, conductive carbon black and polyvinylidene fluoride are dispersed in N-methylpyrrolidone to form a positive electrode active material slurry. Among them, the mass fraction ratio of LiFePO4: conductive carbon black: polyvinylidene fluoride is 96.5%: 1.8%: 1.7%, and the solid content of the slurry is 50%. The slurry is coated on aluminum foil with a surface density of 16mg / cm 2 , and then dried at 90°C for 60 minutes to obtain a positive electrode sheet.
[0082] Electrolyte preparation
[0083] The electrolyte used is lithium salt LiPF6 and LiFSI, the solvent is ethylene glycol dimethyl ether (DME), and the additives are FEC (fluoroethylene carbonate) and LiI. Among them, the concentration of LiI is 50mM. The concentration of LiPF6 is 1.2M. The concentration of LiFSI is 0.4M. The concentration of FEC is 4wt%.
[0084] Lithium battery preparation
[0085] The copper foil is used as the negative electrode current collector; the separator is the separator prepared in the above step (3), wherein the PE base film is coated with a PMMA coating, the coating is coated with ZnO particles and LiNO3 particles, and the amount of ZnO and LiNO3 added to the separator is 2wt% and 0.2wt% of the LFP positive electrode material, respectively. The positive electrode, the separator, the negative electrode current collector and the pole piece are wound into a winding core, the winding core is coated with an insulating coating film, and is placed in a square aluminum shell. After baking, liquid injection, formation, capacity and other processes, a 50Ah battery cell is prepared.
[0086] Example 2
[0087] Preparation of diaphragm
[0088] (1) PMMA microspheres are added into an ammonia solution (the concentration of the ammonia solution is 0.5 mol / L), and stirred to be uniformly dispersed in the solution to form an ammonia solution containing PMMA microspheres; in the ammonia solution containing PMMA microspheres, the mass concentration of PMMA is 30 wt %.
[0089] ZnO is dispersed in deionized water containing LiNO3 to form a lithium nitrate aqueous solution containing ZnO; the mass concentration of ZnO is 2.37wt%; the mass concentration of LiNO3 is 2.64wt%.
[0090] (2) The ammonia solution containing PMMA microspheres and the lithium nitrate solution containing ZnO were mixed in a mass ratio of 2.85:1, and reacted in a water bath at a reaction temperature of 50°C. After stirring for 30 minutes, the resulting solution was centrifuged and dried to obtain a composite material of PMMA-coated ZnO and LiNO3. In the composite material, the mass ratio of PMMA, ZnO and LiNO3 was 94.9:2.37:2.64.
[0091] (3) The composite material is added to a dimethylacetamide (DMAC) solvent, stirred evenly, and dispersed at high speed to obtain a solvent-based coating liquid. The coating liquid is coated on a polyethylene porous base film (Enjie, 7 μm) using a coating machine, and then cured in a coagulation bath (the coagulation bath curing temperature is 25°C; the curing time is 1 h), washed with deionized water, and dried to obtain a diaphragm containing a PMMA coating. The thickness of the PMMA coating is 3 nm.
[0092] Cathode sheet preparation
[0093] The steps for preparing the positive electrode sheet of Example 2 are the same as those of Example 1.
[0094] Electrolyte preparation
[0095] The steps for preparing the electrolyte in Example 2 are the same as those in Example 1.
[0096] Lithium battery preparation
[0097] Copper foil is used as the negative electrode current collector; the separator is the separator prepared in the above step (3), wherein the PE base film is coated with a PMMA coating, the coating is coated with ZnO particles and LiNO3 particles, and the amount of ZnO and LiNO3 added to the separator is 2wt% and 0.3wt% of the positive electrode material of the LFP positive electrode sheet, respectively. The positive electrode, the separator, the negative electrode current collector and the electrode sheet are wound into a winding core, the winding core is coated with an insulating coating film, and is placed in a square aluminum shell. After baking, liquid injection, formation, capacity and other processes, a 50Ah battery cell is prepared.
[0098] Example 3
[0099] Preparation of diaphragm
[0100] (1) PMMA microspheres are added into an ammonia solution (the concentration of the ammonia solution is 1.0 mol / L), and stirred to be uniformly dispersed in the solution to form an ammonia solution containing PMMA microspheres; in the ammonia solution containing PMMA microspheres, the mass concentration of PMMA is 30 wt %.
[0101] ZnO is dispersed in deionized water to form an aqueous solution containing ZnO; the mass concentration of ZnO is 3.6 wt%.
[0102] (2) The ammonia solution containing PMMA microspheres and the lithium nitrate solution containing ZnO were mixed in a mass ratio of 2.8:1, and reacted in a water bath at a reaction temperature of 50°C. After stirring for 30 minutes, the resulting solution was centrifuged and dried to obtain a PMMA-coated ZnO composite material. In the composite material, the mass ratio of PMMA to ZnO was 96.4:3.6.
[0103] (3) The composite material is added to a dimethylacetamide (DMAC) solvent, stirred evenly, and dispersed at high speed to obtain a solvent-based coating liquid. The coating liquid is coated on a polyethylene porous base film (Enjie, thickness of 7 μm) using a coating machine, and then cured in a coagulation bath (the temperature of the coagulation bath curing is 25°C; the curing time is 1 h), washed with deionized water, and dried to obtain a diaphragm containing a PMMA coating. The thickness of the PMMA coating is 3 nm.
[0104] Cathode sheet preparation
[0105] The steps for preparing the positive electrode sheet of Example 3 are the same as those of Example 1.
[0106] Electrolyte preparation
[0107] The electrolyte used is lithium salt LiPF6 and LiFSI, the solvent is ethylene glycol dimethyl ether (DME), and the additives are FEC (fluoroethylene carbonate) and LiI. Among them, the concentration of LiI is 30mM. The concentration of LiPF6 is 1.2M. The concentration of LiFSI is 0.4M. The concentration of FEC is 4wt%.
[0108] Lithium battery preparation
[0109] The copper foil is used as the negative electrode current collector; the separator is the separator prepared in the above step (3), wherein the PE base film is coated with a PMMA coating, the coating is coated with ZnO particles and LiNO3 particles, and the amount of ZnO added to the separator is 3wt% of the mass of the positive electrode material of the LFP positive electrode. The positive electrode, the separator, the negative electrode current collector and the pole piece are wound into a winding core, the winding core is coated with an insulating coating film, and is placed in a square aluminum shell. After baking, liquid injection, formation, capacity and other processes, a 50Ah battery cell is prepared.
[0110] Example 4
[0111] Preparation of diaphragm
[0112] (1) PMMA microspheres are added into an ammonia solution (the concentration of the ammonia solution is 0.5 mol / L), and stirred to be uniformly dispersed in the solution to form an ammonia solution containing PMMA microspheres; in the ammonia solution containing PMMA microspheres, the mass concentration of PMMA is 30 wt %.
[0113] ZnO is dispersed in deionized water containing LiNO3 to form a lithium nitrate aqueous solution containing ZnO; the mass concentration of ZnO is 3.592wt%; the mass concentration of LiNO3 is 0.598wt%.
[0114] (2) The ammonia solution containing PMMA microspheres and the lithium nitrate solution containing ZnO were mixed in a mass ratio of 2.81:1, and reacted in a water bath at a reaction temperature of 50°C. After stirring for 30 minutes, the resulting solution was centrifuged and dried to obtain a composite material of PMMA-coated ZnO and LiNO3. In the composite material, the mass ratio of PMMA, ZnO and LiNO3 was 95.81:3.592:0.598.
[0115] (3) The composite material is added to a dimethylacetamide (DMAC) solvent, stirred evenly, and dispersed at high speed to obtain a solvent-based coating liquid. The coating liquid is coated on a polyethylene porous base film using a coating machine, and then cured in a coagulation bath (the coagulation bath curing temperature is 25°C; the curing time is 1 hour), washed with deionized water, and dried to obtain a PMMA-coated diaphragm. The thickness of the PMMA coating is 3 nm.
[0116] Cathode sheet preparation
[0117] The steps for preparing the positive electrode sheet of Example 4 are the same as those of Example 1.
[0118] Electrolyte preparation
[0119] Electrolyte preparation
[0120] The electrolyte used is lithium salt LiPF6 and LiFSI, the solvent is ethylene glycol dimethyl ether (DME), and the additives are FEC (fluoroethylene carbonate) and LiI. Among them, the concentration of LiI is 30mM. The concentration of LiPF6 is 1.2M. The concentration of LiFSI is 0.4M. The concentration of FEC is 4wt%.
[0121] Lithium battery preparation
[0122] Copper foil is used as the negative electrode current collector; the separator is the separator prepared in the above step (3), wherein the PE base film is coated with a PMMA coating, the coating is coated with ZnO particles and LiNO3 particles, and the amount of ZnO and LiNO3 added to the separator is 2wt% and 0.3wt% of the mass of the positive electrode material of the LFP positive electrode sheet, respectively. The positive electrode, the separator, the negative electrode current collector and the electrode sheet are wound into a winding core, the winding core is coated with an insulating coating film, and is placed in a square aluminum shell. After baking, liquid injection, formation, capacity and other processes, a 50Ah battery cell is prepared.
[0123] Example 5
[0124] The only difference between Example 5 and Example 4 is that the mass ratio of PMMA:ZnO:LiNO3 in the separator is 97:2.4:0.6. The added amounts of ZnO and LiNO3 are 2wt% and 0.5wt% of the mass of the positive electrode material of the LFP positive electrode sheet, respectively. The remaining operating conditions and steps are the same as those of Example 4.
[0125] Example 6
[0126] The only difference between Example 6 and Example 3 is that in the preparation of the electrolyte, the electrolyte used is lithium salt LiPF6 and LiFSI, the solvent is ethylene glycol dimethyl ether (DME), the additive is FEC (fluoroethylene carbonate), and LiI is not added. The remaining operating conditions and steps are the same as those in Example 3.
[0127] Comparative Example 1
[0128] Compared with Example 6, a PE-based film from Enjie is used as the separator, which has a thickness of 7 μm and no coating; the rest is the same as Example 6.
[0129] Comparative Example 2
[0130] Preparation of diaphragm
[0131] Add PMMA particles to dimethylacetamide (DMAC) solvent, stir evenly, and disperse at high speed to obtain a solvent-based coating liquid. Use a coating machine to apply the coating liquid to a polyethylene porous base film (Enjie, thickness of 7μm), solidify in a coagulation bath (solidification bath curing temperature is 25°C; curing time is 1h), wash with deionized water, and dry to obtain a diaphragm containing a PMMA coating. The thickness of the coating is 3nm.
[0132] Cathode sheet preparation
[0133] The steps for preparing the positive electrode sheet of Comparative Example 2 are the same as those of Example 1.
[0134] Electrolyte preparation
[0135] The electrolyte preparation steps of Comparative Example 2 are the same as those of Example 1.
[0136] Lithium battery preparation
[0137] The preparation steps are the same as those in Example 1, except that the diaphragm prepared in this comparative example is used.
[0138] Comparative Example 3
[0139] Diaphragm
[0140] The PE-based membrane from Enjie was used as the separator, which had a thickness of 7 μm and no coating.
[0141] Cathode sheet preparation
[0142] The steps for preparing the positive electrode sheet of Comparative Example 3 are the same as those of Example 1.
[0143] Electrolyte preparation
[0144] The electrolyte used is lithium salt LiPF6, LiFSI, the solvent is ethylene glycol dimethyl ether (DME), and the additives are FEC (fluoroethylene carbonate) and LiI. Among them, the concentration of LiI is 80mM. The concentration of LiPF6 is 1.2M. The concentration of LiFSI is 0.4M. The concentration of FEC is 4wt%.
[0145] Lithium-ion battery
[0146] The preparation steps of the lithium ion battery are the same as those in Example 1.
[0147] Comparative Example 4
[0148] Preparation of diaphragm
[0149] (1) adding PMMA microspheres into an ammonia solution and stirring the microspheres to uniformly disperse the microspheres in the solution to form an ammonia solution containing PMMA microspheres; the mass concentration of PMMA in the ammonia solution containing PMMA microspheres is 30 wt %.
[0150] LiNO3 is dissolved in deionized water to form a lithium nitrate aqueous solution; the mass concentration of LiNO3 is 0.3%wt%.
[0151] (2) The ammonia solution containing PMMA microspheres and the lithium nitrate solution were mixed in a mass ratio of 2.7:1, and reacted in a water bath at a reaction temperature of 50°C. After stirring for 30 minutes, the obtained solution was centrifuged and dried to obtain a PMMA-coated LiNO3 composite material. In the composite material, the mass ratio of PMMA to LiNO3 was 99.7:0.3.
[0152] (3) The composite material is added to a dimethylacetamide (DMAC) solvent, stirred evenly, and dispersed at high speed to obtain a solvent-based coating liquid. The coating liquid is coated on a polyethylene porous base film using a coating machine, and then cured in a coagulation bath (the coagulation bath curing temperature is 25°C; the curing time is 1 hour), washed with deionized water, and dried to obtain a PMMA-coated diaphragm. The thickness of the PMMA coating is 3 nm.
[0153] Cathode sheet preparation
[0154] The steps for preparing the positive electrode sheet of Comparative Example 4 are the same as those of Example 1.
[0155] Electrolyte preparation
[0156] The electrolyte used is lithium salt LiPF6, LiFSI, the solvent is ethylene glycol dimethyl ether (DME), and the additives are FEC (fluoroethylene carbonate) and LiI. Among them, the concentration of LiI is 50mM. The concentration of LiPF6 is 1.2M. The concentration of LiFSI is 0.4M. The concentration of FEC is 4wt%.
[0157] Lithium-ion battery
[0158] The preparation steps of the lithium ion battery are the same as those in Example 1.
[0159] Comparative Example 5
[0160] Preparation of diaphragm
[0161] (1) adding PMMA microspheres into an ammonia solution and stirring the microspheres to uniformly disperse the microspheres in the solution to form an ammonia solution containing PMMA microspheres; the mass concentration of PMMA in the ammonia solution containing PMMA microspheres is 30 wt %.
[0162] (2) Al2O3 was dispersed in deionized water, and the mass concentration of Al2O3 was 3.6wt%.
[0163] (3) The ammonia solution containing PMMA microspheres and the Al2O3 aqueous solution are mixed in a mass ratio of 3.2:1, and reacted in a water bath at a reaction temperature of 50°C. After stirring for 30 minutes, the resulting solution is centrifuged and dried to obtain PMMA-coated ceramic microspheres. In the microspheres, the mass ratio of PMMA to Al2O3 is 96.4:3.6.
[0164] (3) The composite material is added to a dimethylacetamide (DMAC) solvent, stirred evenly, and dispersed at high speed to obtain a solvent-based coating liquid. The coating liquid is coated on a polyethylene porous base film using a coating machine, and then cured in a coagulation bath (the coagulation bath curing temperature is 25°C; the curing time is 1 hour), washed with deionized water, and dried to obtain a PMMA-coated diaphragm. The thickness of the PMMA coating is 3 nm.
[0165] Cathode sheet preparation
[0166] The steps for preparing the positive electrode sheet of Comparative Example 4 are the same as those of Example 1.
[0167] Electrolyte preparation
[0168] The electrolyte used is lithium salt LiPF6 and LiFSI, the solvent is ethylene glycol dimethyl ether (DME), and the additive is FEC (fluoroethylene carbonate). The concentration of LiPF6 is 1.2M, the concentration of LiFSI is 0.4M, and the concentration of FEC is 4wt%.
[0169] Lithium-ion battery
[0170] The preparation steps of the lithium ion battery are the same as those in Example 1. The amount of Al2O3 added to the separator is 3 wt% of the mass of the positive electrode material of the LFP positive electrode sheet.
[0171] Test Case
[0172] The battery performance tests were performed on the batteries of Examples 1-6 and Comparative Examples 1-5:
[0173] (1) First efficiency test:
[0174] The battery was charged and discharged under the condition of 25℃, charged at 1C constant current to 3.65V, and constant voltage to 0.05C cut-off; left to stand for 10min; discharged at 1C constant current to 2.5V; left to stand for 10min; the charging capacity and discharging capacity of the battery were recorded, and the ratio of the discharge capacity to the charging capacity was the first efficiency.
[0175] (2) Test of battery capacity retention at 25°C
[0176] At 25°C, charge the battery to 3.65V at 1C and leave it for 5 minutes. Discharge the battery to 2.5V at 1C and leave it for 5 minutes. Repeat the above steps 100 times to obtain the capacity of the battery after 100 cycles. The capacity retention rate after 100 cycles is calculated by the following formula:
[0177] Capacity retention rate = (discharge capacity after 100th cycle / discharge capacity at first cycle)*100%.
[0178] (3) 72h battery capacity retention test
[0179] At 25℃, charge the battery to 3.65V at 1C, then leave it for 5 minutes; discharge the battery to 2.5V at 1C, record the initial discharge capacity of the battery, then leave it for 5 minutes; charge the battery to 3.65V at 1C; store the battery at 45℃ for 72h; discharge the battery to 2.5V at 1C, record the discharge capacity after storage; the ratio of the discharge capacity after storage to the initial discharge capacity of the battery is the 72h capacity retention rate.
[0180] The battery performance test results of Examples 1-6 and Comparative Examples 1-5 are shown in Table 1 below.
[0181] Table 1: Battery performance test results of Examples 1-6 and Comparative Examples 1-5
[0182]
Claims
1. A diaphragm coating, characterized in that: The coating contains PMMA and ZnO, wherein the mass ratio of PMMA to ZnO is (92-98):(2-5).
2. The diaphragm coating according to claim 1, characterized in that The diaphragm coating also contains LiNO3; wherein, in the diaphragm coating, the mass ratio of PMMA, ZnO and LiNO3 is (92-98): (2-5): (0.5-6), preferably (92-98): (2-5): (0.5-4).
3. The diaphragm coating according to claim 1 or 2, characterized in that: The PMMA covers the ZnO, or the PMMA covers the ZnO and LiNO3; and / or The thickness of the diaphragm coating is 2-5 nm.
4. The method for preparing the diaphragm coating according to claim 1, characterized in that: The method comprises the following steps: (1) Providing an aqueous solution of PMMA microspheres and an aqueous solution of ZnO (2) mixing the ammonia solution of the PMMA microspheres and the ZnO aqueous solution, stirring for a period of time, and centrifugally drying to obtain a PMMA-coated ZnO composite material; (3) The composite material is mixed with a solvent to obtain a coating liquid, and the coating liquid is coated on at least one surface of a substrate, and the diaphragm coating is obtained after curing.
5. The method for coating a diaphragm according to claim 4, characterized in that: The preparation of the ammonia solution of PMMA microspheres comprises the following steps: uniformly dispersing PMMA microspheres in the ammonia solution to form an ammonia solution containing PMMA microspheres; preferably, the mass concentration of PMMA is 20-24wt%, such as 25-35wt% or 28-32wt%; and / or The preparation of the aqueous solution of ZnO comprises the following steps: dispersing ZnO in water to form an aqueous solution containing ZnO; preferably, in the aqueous solution containing ZnO, the mass concentration of ZnO is 2.0-4.0wt%, such as 2.5-4.0wt% or 2.5-3.6wt%.
6. The method for diaphragm coating according to claim 4, characterized in that: The diaphragm coating further contains LiNO3, and the step (1) includes providing an aqueous solution containing ZnO and LiNO3, or further includes providing an aqueous solution of LiNO3; Preferably, the preparation of the aqueous solution containing ZnO and LiNO3 The method comprises the following steps: dispersing ZnO in water containing LiNO3 to form a lithium nitrate aqueous solution containing ZnO; preferably, in the solution, the mass concentration of ZnO is 2.0-4.0wt%, such as 2.5-4.0wt% or 2.5-3.6wt%; the mass concentration of LiNO3 is 0.5-3.0wt%, such as 0.5-2.7wt%; Preferably, the preparation of the aqueous solution of LiNO3 comprises dissolving LiNO3 in water to form an aqueous solution of LiNO3; preferably, in the solution, the mass concentration of LiNO3 is 0.5-3.0wt%, such as 0.5-2.7wt%.
7. The method for diaphragm coating according to any one of claims 4 to 6, characterized in that: The method has one or more of the following features: The mass ratio of the ammonia solution containing PMMA microspheres to the aqueous solution containing ZnO and optionally LiNO3 is (2.0-3.0):1, for example (2.5-3.0):1; The solvent mixed with the composite material is selected from one or more of N,N-dimethylacetamide, acetone and N-methylpyrrolidone; The curing temperature is 5-80°C, such as 15-30°C.
8. A diaphragm, characterized in that: The diaphragm comprises a substrate layer and a diaphragm coating as claimed in any one of claims 1 to 3 coated on the substrate layer; the substrate layer is preferably a PP film, a PE film, an aramid diaphragm, or a composite film of PP and PE.
9. A lithium ion battery comprising a positive electrode sheet, a negative electrode current collector, an electrolyte and a separator, characterized in that: The diaphragm is the diaphragm according to claim 8.
10. The lithium ion battery according to claim 9, characterized in that The lithium-ion battery has one or more of the following features: The mass ratio of ZnO in the separator to the mass ratio of the positive electrode material of the positive electrode sheet is 2-3wt%; The mass ratio of LiNO3 in the separator to the mass ratio of the positive electrode material of the positive electrode sheet is 0.2-0.5wt%; The electrolyte includes LiI; preferably, the mass concentration of LiI is 30-50mM; The negative electrode of the lithium-ion battery is a negative electrode current collector, and the negative electrode current collector is, for example, copper foil or aluminum foil. 11.Select from the following applications: (1) Use of the diaphragm coating as claimed in claims 1 to 3 in improving battery cycle performance, especially improving battery capacity retention rate; (2) Use of the diaphragm coating as described in claims 1-3 in the preparation of lithium-ion batteries, especially negative electrode-free lithium-ion batteries.
Citation Information
Patent Citations
Lithium-rich lithium ion battery diaphragm
CN109950459A
Negative-electrode-free lithium battery with high energy density
CN113964454A
Battery
CN114628851A
Coating diaphragm and preparation method thereof
CN115954617A
Ceramic microsphere, diaphragm containing ceramic microsphere and lithium ion battery containing diaphragm
CN117423957A